A method for removing a nickel-platinum coating
By employing a three-step synergistic mechanism of electrolytic softening of interfacial bonding force, thermal stress-induced coating lifting, and ultrasonic low-force scraping, combined with a dilute phosphoric acid-sulfuric acid mixed electrolyte and corrosion inhibitor to protect the substrate, the problem of substrate damage during nickel-platinum coating removal is solved, achieving efficient coating removal and substrate protection.
Patent Information
- Application Number
- CN202611469338.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies are difficult to remove nickel-platinum coatings efficiently without damaging the substrate, and also result in resource waste.
A three-step synergistic mechanism is adopted, which involves electrolytic softening of the interface bonding force, thermal stress inducing coating lifting, and ultrasonic low-force scraping. The substrate is protected by a mixed electrolyte of dilute phosphoric acid and sulfuric acid and a corrosion inhibitor, and the coating is peeled off by an ultrasonic scraper.
It achieves efficient removal of nickel-platinum plating, maintains the dimensional accuracy and surface integrity of the substrate, reduces the loss of precious metals, and is suitable for processing workpieces of different sizes and shapes.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of machining technology, and specifically relates to a method for removing nickel-platinum plating. Background Technology
[0002] Platinum group metals (including platinum, palladium, rhodium, iridium, osmium, and ruthenium) possess excellent corrosion resistance, good ductility, superior electrical conductivity, and high light reflectivity. Their chemical stability far exceeds that of most metallic elements, giving them an irreplaceable position in the fields of precision and functional materials. Nickel-platinum plating combines the advantages of nickel plating—strong adhesion, high hardness, and relatively controllable cost—with platinum plating—excellent corrosion resistance, oxidation resistance, catalytic activity, and electrical contact stability. It is widely used in critical applications such as petrochemical catalyst supports, fuel cell bipolar plates, precision electronic connectors, reactors and stirring components, and aerospace high-temperature protection components, playing a particularly important role in ensuring the performance and service life of workpieces.
[0003] However, in engineering practice, nickel-platinum plating inevitably exhibits failure phenomena such as localized wear, microcrack propagation, pitting corrosion, and catalytic activity decline after long-term service. Furthermore, quality issues such as uneven thickness and substandard adhesion may arise during plating preparation, requiring rework. All of these situations necessitate the complete removal of the nickel-platinum plating from the workpiece surface to allow for replating on the substrate or recycling of the precious metal resources. It is worth noting that workpieces bearing nickel-platinum plating (such as stainless steel reactor bodies, precision valve bodies, and catalyst support frameworks) often have high manufacturing costs and excellent substrate materials; scrapping them solely due to plating failure would result in significant resource waste. Therefore, developing a stripping method that can efficiently remove nickel-platinum plating while maximally protecting the substrate from damage has significant engineering application value and economic significance.
[0004] Currently, there are several main methods for removing nickel-platinum precious metal plating from workpiece surfaces, but all have significant shortcomings: First, the traditional alkaline-acid chemical stripping method. This method first uses a strong alkaline solution for alkaline washing, followed by acid washing with strong acids such as hydrochloric acid, nitric acid, or aqua regia to dissolve the plating. Since the thickness of the nickel-platinum plating is usually only on the micrometer scale, the acid solution can easily penetrate the plating defects and directly corrode the stainless steel substrate, causing pitting corrosion, dimensional deviations, and even structural damage; strong alkalis may also cause intergranular corrosion and alkali embrittlement of the substrate under high temperature conditions. In addition, this method involves many steps, consumes a lot of auxiliary materials, and has high waste liquid treatment costs. Second, the concentrated acid immersion method. This method involves directly immersing the workpiece in strong acids such as concentrated hydrochloric acid, concentrated nitric acid, or aqua regia to dissolve the plating. However, concentrated acids have a comprehensive corrosive effect on the stainless steel substrate, significantly increasing the surface roughness of the workpiece and severely compromising dimensional accuracy; acid residues in the internal cavities and crevices of complex workpieces are difficult to remove, leading to continuous post-corrosion. In particular, platinum is only soluble in a few media such as aqua regia, while aqua regia also has a strong dissolving ability for elements such as chromium, nickel, and iron in stainless steel. Workpieces are often severely damaged before the coating is completely removed, making it impractical for industrial applications. Third, mechanical stripping. This method uses sandblasting, grinding, scraping, etc., to directly remove the coating. Because the coating has a strong bond with the substrate, a large force is required during stripping, inevitably causing scratches, deformation, and micro-cracks on the substrate surface. Thin-walled or precision workpieces are prone to dimensional deviations. Furthermore, this method cannot effectively handle the internal cavities and hidden areas of workpieces with complex geometries. Summary of the Invention
[0005] Therefore, the purpose of this invention is to provide a method for removing nickel-platinum plating.
[0006] The present invention provides a method for removing nickel-platinum plating, comprising the following steps: S1. Spray corrosion inhibitor solution onto the non-plated area and the damaged area of the workpiece, and after standing and drying, the treated workpiece is obtained. S2. The treated workpiece is used as the anode and the titanium plate is used as the cathode. The workpiece is placed in an electrolytic cell containing electrolyte and immersed. After immersion, electrolysis is performed to obtain the electrolyzed workpiece. The composition of the electrolyte is: the mass ratio of concentrated phosphoric acid, concentrated sulfuric acid and water is (60~70):(15~20):(15~20). S3. The workpiece after electrolysis is baked to cause the nickel-platinum coating to peel off. Then, the nickel-platinum coating is peeled off by ultrasonication and the coating is collected to obtain a workpiece with the coating partially or completely removed. S4. Repeat steps S1 to S3 for the workpiece where the plating layer was partially removed in step S3, until the nickel-platinum plating layer is completely removed.
[0007] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) This invention achieves efficient removal of nickel-platinum coatings through a three-step synergistic mechanism: electrolytic softening of interfacial bonding force, thermal stress-induced coating lifting, and ultrasonic low-force scraping. After a single synergistic treatment, the coating removal rate is not less than 75% (up to 80% in Example 1). For residual coatings that cannot be completely removed in a single treatment, the coating can be completely removed by repeated synergistic treatment.
[0008] (2) This invention uses a dilute phosphoric acid-sulfuric acid mixed electrolyte, which is far less corrosive than strong acids such as hydrochloric acid, concentrated nitric acid, or aqua regia used in existing technologies. Combined with corrosion inhibitors, it provides pre-protection for non-plated areas and damaged plating areas of the workpiece, effectively inhibiting the erosion of the stainless steel substrate by the electrolyte during electrolysis. The purpose of electrolysis is not to dissolve the plating, but to generate microbubbles and osmotic pressure differences at the plating-substrate interface through anodic reactions, weakening the interfacial bonding force. The electrolysis process is mild and controllable, avoiding pitting corrosion, intergranular corrosion, and other damage to the substrate. The subsequent baking temperature (200~230℃) is far lower than the sensitization temperature of stainless steel, preventing changes in the substrate structure and thermal deformation. The ultrasonic scraper achieves physical peeling of the plating with micron-level amplitude and extremely low contact force, without causing scratches, deformation, or stress concentration on the substrate surface. Therefore, this method can effectively maintain the dimensional accuracy and surface integrity of the workpiece while thoroughly removing the plating, protecting the workpiece from corrosion damage and enabling its reuse.
[0009] (3) This invention collects nickel-platinum plating fragments primarily through physical stripping. The plating is peeled off in solid form rather than dissolved entirely in the electrolyte, with platinum group metals mainly recovered as solid concentrates. The nickel component partially dissolves with the electrolyte and can be recovered separately through conventional electrolysis or precipitation. The platinum grade in the solid concentrate is significantly higher than that of the original plating, greatly simplifying the subsequent refining process. This is significantly superior to the chemical dissolution method, which requires the extraction and recovery of precious metals from complex waste liquids, effectively reducing the loss of precious metals.
[0010] (4) The process of this invention is simple, the operating conditions are mild, and the equipment requirements are low (conventional electrolytic cells, electric heating fans, and ultrasonic scrapers can be used). The process parameters are easy to control, and the repeatability and stability are good. The electrolysis time can be adjusted according to the time and thickness relationship of this invention within the range of 10~50μm of coating thickness, and it can be applied to the processing of workpieces of different sizes and shapes, and has good prospects for industrial promotion and application. Detailed Implementation
[0011] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.
[0012] The present invention provides a method for removing nickel-platinum plating, comprising the following steps: S1. Spray corrosion inhibitor solution onto the non-plated area and the damaged area of the workpiece, and after standing and drying, the treated workpiece is obtained. S2. The treated workpiece is used as the anode and the titanium plate is used as the cathode. The workpiece is placed in an electrolytic cell containing electrolyte and immersed. After immersion, electrolysis is performed to obtain the electrolyzed workpiece. The composition of the electrolyte is: the mass ratio of concentrated phosphoric acid, concentrated sulfuric acid and water is (60~70):(15~20):(15~20). S3. The workpiece after electrolysis is baked to cause the nickel-platinum coating to peel off. Then, the nickel-platinum coating is peeled off by ultrasonication and the coating is collected to obtain a workpiece with the coating partially or completely removed. S4. Repeat steps S1 to S3 for the workpiece where the plating layer was partially removed in step S3, until the nickel-platinum plating layer is completely removed.
[0013] This invention achieves systematic, low-damage protection of the substrate workpiece through overall process design. Before entering the electrolysis process, a corrosion inhibitor is sprayed onto the non-plated areas and areas with damaged plating on the workpiece, forming a dense protective film on the substrate surface. This prevents direct contact between the electrolyte and the substrate from the source, avoiding the risk of the electrolyte corroding the substrate through plating defects. In the electrolysis process, a dilute acid mixture of phosphoric acid and sulfuric acid is selected as the electrolyte. Its corrosiveness is far lower than that of strong acid systems such as hydrochloric acid, concentrated nitric acid, and aqua regia used in existing technologies. Moreover, the purpose of electrolysis is not to dissolve the plating, but to weaken the interfacial bonding force by generating microbubbles and osmotic pressure differences at the interface between the plating and the substrate through short-time, low-current-density controlled electrolysis. The electrochemical dissolution of the substrate is minimal. In the baking process, the baking temperature is controlled far below the sensitization temperature of stainless steel. The difference in the thermal expansion coefficients between the plating and the substrate causes the plating to lift off on its own after the interfacial bonding force has been weakened, without causing changes in the substrate structure or thermal deformation. In the final stripping process, an ultrasonic scraper is used to remove the loose, raised coating. The high-frequency, low-amplitude ultrasonic vibrations allow the scraper to complete the stripping with extremely low contact force, preventing scratches, deformation, or stress concentration on the substrate surface. This invention, through the progressive and synergistic effects of each step, comprehensively reduces damage to the substrate from three dimensions: chemical corrosion, electrochemical corrosion, and mechanical damage, achieving a balance between efficient coating removal and preservation of substrate integrity.
[0014] In some embodiments, in step S1, the substrate of the workpiece is stainless steel.
[0015] In some embodiments, in step S1, the corrosion inhibitor is sodium chromate, and the mass concentration of the corrosion inhibitor solution is 1.5~2.5%, including but not limited to: 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, etc.
[0016] In some embodiments, the time for static drying in step S1 is 30 to 40 minutes, including but not limited to: 30 minutes, 32 minutes, 35 minutes, 38 minutes, 40 minutes, etc.
[0017] In some embodiments, in step S2, the mass concentration of phosphoric acid is 83~85wt%, including but not limited to: 83wt%, 83.5wt%, 84wt%, 84.5wt%, 85wt%, etc.; the concentration of concentrated sulfuric acid is 96~98wt%, including but not limited to: 96wt%, 96.5wt%, 97wt%, 97.5wt%, 98wt%, etc.
[0018] In some embodiments, the soaking time in step S2 is 8 to 12 minutes, including but not limited to: 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, etc.
[0019] In some embodiments, in step S2, the electrolysis voltage is 10-15V, including but not limited to: 10V, 11V, 12V, 13V, 14V, 15V, etc.; the electrolysis temperature is 65-80℃, including but not limited to: 65℃, 68℃, 70℃, 72℃, 75℃, 78℃, 80℃, etc.; and the electrolysis time is 5-8min, including but not limited to: 5min, 6min, 7min, 8min, etc.
[0020] In some embodiments, in step S3, the baking is performed using an electric heating fan; wherein: the power of the electric heating fan is 800~1200W, including but not limited to: 800W, 900W, 1000W, 1100W, 1200W, etc.; the distance from the plating layer is 20~30cm, including but not limited to: 20cm, 22cm, 25cm, 28cm, 30cm, etc.; the baking is performed until the surface temperature of the workpiece reaches 200~230℃, including but not limited to: 200℃, 205℃, 210℃, 215℃, 220℃, 225℃, 230℃, etc.; and the workpiece is kept at this temperature for 5~10min, including but not limited to: 5min, 6min, 7min, 8min, 9min, 10min, etc.
[0021] In some embodiments, in step S3, an ultrasonic scalpel is used to ultrasonically peel off the nickel-platinum coating. The frequency of the ultrasonic scalpel is 20 to 30 kHz, including but not limited to: 20 kHz, 22 kHz, 25 kHz, 28 kHz, 29 kHz, 30 kHz, etc.
[0022] In some embodiments, in step S3, nickel and platinum metals are recovered from the collected coating.
[0023] In some embodiments, in steps S3 and S4, the workpiece with all the coating removed is cleaned, then sandblasted, and finally cleaned again to obtain a regenerated workpiece.
[0024] In some embodiments, the specific process of the sandblasting treatment is as follows: first, sandblasting is performed with corundum, and then sandblasting is performed with glass beads and glass sand in a mass ratio of (1~2):(1~2).
[0025] Example 1 S1. Take a stainless steel workpiece with a nickel-platinum coating. The workpiece weighs 668.56g. The supplier provides data: the stainless steel substrate weighs 470g, that is, the coating weighs 198.56g, and the average coating thickness is 25μm. Spray a 2% sodium chromate solution on the non-coating area and the damaged area of the nickel-platinum coated stainless steel workpiece. After standing and drying for 35 minutes, the pretreated workpiece is obtained.
[0026] S2. Using the pretreated workpiece as the anode and the titanium plate as the cathode, the workpiece is placed in an electrolytic cell containing electrolyte and soaked for 10 minutes. After soaking, it is electrolyzed for 7 minutes to obtain the electrolyzed workpiece. The electrolyte is prepared by mixing concentrated phosphoric acid, concentrated sulfuric acid and water in a mass ratio of 65:17.5:17.5, with a phosphoric acid concentration of 85 wt% and a sulfuric acid concentration of 98 wt%. The electrolysis voltage is 12 V and the electrolysis temperature is 75 °C.
[0027] S3. Use an electric heating fan to bake the electrolyzed workpiece. The power of the electric heating fan is 1000W, and the distance between the electric heating fan and the workpiece is controlled to be about 25cm. This causes the nickel-platinum plating to peel off. Bake until the surface temperature of the workpiece reaches 220±10℃ and hold for 6 minutes. At this time, the peeled area accounts for about 80% of the total plating area. Then, while it is still hot, use an ultrasonic scalpel to ultrasonically treat the workpiece. The ultrasonic frequency is 25kHz, which causes the nickel-platinum plating to fall off, resulting in a workpiece with a plating removal rate of about 80%. Collect the peeled plating for nickel-platinum extraction.
[0028] S4. Repeat steps S1 to S3 once for the workpiece with a coating removal rate of about 80% in step S3, to obtain a workpiece with complete coating removal.
[0029] S5. The workpiece with the coating completely removed is cleaned with pure water, dried, and then weighed. The mass of the workpiece is 463.89g, the substrate loss is 6.11g, and the loss rate is 1.30%.
[0030] S6. The cleaned workpiece in step S5 is first sandblasted with corundum, and then sandblasted with glass beads and glass sand at a mass ratio of 1:1. After sandblasting, it is cleaned with pure water to obtain the regenerated workpiece.
[0031] Comparative Example 1 A stainless steel workpiece with a nickel-platinum plating layer was taken, weighing 688.89g. The supplier provided data showing the stainless steel substrate weighed 484g. The workpiece was immersed in a 40wt% nitric acid solution for 80 minutes. After removal and drying, the plating was peeled off using a scraper, removing approximately 90% of the plating area. Aqua regia was sprayed onto the remaining 10% of the plating area, and the workpiece was left to stand for 20 minutes. The remaining plating was then peeled off using a scraper, followed by rinsing with pure water and drying. The workpiece was then weighed, yielding a weight of 453.46g, with a substrate loss of 30.54g, resulting in a loss rate of 6.31%.
[0032] By comparing the effects of Example 1 and Comparative Example 1, it can be seen that although the method in Comparative Example 1 is simple, it results in significant wear and tear on the workpiece, reaching 6.31%, making it difficult to reuse the workpiece. In contrast, the wear and tear on the workpiece in Example 1 is less than 2%, allowing for the re-preparation of a nickel-platinum coating for reuse.
[0033] Comparative Example 2 It is basically the same as Example 1, except that step S1 is omitted; that is, in step S1, sodium chromate solution is not sprayed in the non-plating area and the plating damaged area.
[0034] The corresponding preparation methods are as follows: S1. Take a stainless steel workpiece with a nickel-platinum plating layer. The workpiece weighs 560.85g. The supplier provides the following data: the stainless steel substrate weighs 394g, the plating layer weighs 166.85g, and the average plating thickness is approximately 24μm. Do not apply sodium chromate solution.
[0035] S2 is basically the same as step S2 in Example 1, except that a stainless steel workpiece with a nickel-platinum coating is used instead of the pretreated workpiece.
[0036] S3, the same as step S3 in Example 1, yields a workpiece with a coating removal rate of approximately 83%.
[0037] S4, the same as step S4 in Example 1.
[0038] S5, same as step S5 in Example 1, the corresponding workpiece mass is 369.41g, the substrate loss is 24.59g, and the loss rate is 6.24%.
[0039] Comparing the effects of Example 1 and Comparative Example 2, the initial coating removal effect of Comparative Example 2 is better than that of Example 1, but its workpiece loss rate is higher; this may be because without the protection of sodium chromate solution, the surface of the workpiece at the damaged location is dissolved during electrolysis.
[0040] Comparative Example 3 It is basically the same as Example 1, except that in step S2, electrolysis is not performed, but soaking is used.
[0041] The corresponding preparation methods are as follows: S1. Take a stainless steel workpiece with a nickel-platinum coating. The workpiece weighs 634.47g. The supplier provides the following data: the stainless steel substrate weighs 446g, the coating weighs 188.47g, and the average coating thickness is approximately 24μm. Spray a 2% sodium chromate solution onto the non-coating area and the damaged area of the nickel-platinum coated stainless steel workpiece. After standing and drying for 35 minutes, the pretreated workpiece is obtained.
[0042] S2. Immerse the pretreated workpiece in the electrolyte for 80 minutes to obtain the immersed workpiece. The electrolyte is prepared by mixing concentrated phosphoric acid, concentrated sulfuric acid and water in a mass ratio of 65:17.5:17.5, with the concentration of concentrated phosphoric acid being 85wt% and the concentration of concentrated sulfuric acid being 98wt%.
[0043] S3 is basically the same as step S3 in Example 1, except that the workpiece after electrolysis is replaced by the workpiece after immersion; the corresponding workpiece has a coating removal rate of about 40%.
[0044] S4 is the same as step S4 in Example 1; the difference is that steps S1 to S3 are repeated twice.
[0045] S5, same as step S5 in Example 1, the corresponding workpiece mass is 430.57g, the substrate loss is 15.43g, and the loss rate is 3.46%.
[0046] Comparing Example 1 and Comparative Example 3, the coating removal time in Comparative Example 3 was longer and the loss was higher; this indicates that simply immersing in electrolyte without electrolysis resulted in poor coating removal.
[0047] Comparative Example 4 The process is basically the same as in Example 1, except that the electrolyte in step S2 is prepared by mixing concentrated hydrochloric acid, concentrated sulfuric acid and water in a mass ratio of 65:17.5:17.5, with the concentration of concentrated hydrochloric acid being 37 wt% and the concentration of concentrated sulfuric acid being 98 wt%.
[0048] The corresponding preparation methods are as follows: S1 is basically the same as step S1 in Example 1, except that: a stainless steel workpiece with a nickel-platinum plating is taken, the workpiece mass is 671.24g, and the supplier provides the following data: the stainless steel substrate mass is 472.35g, the plating mass is 198.89g, and the average plating thickness is about 25μm.
[0049] S2 is basically the same as step S2 in Example 1, except that the electrolyte is different.
[0050] S3, the same as step S3 in Example 1, yields a workpiece with a coating removal rate of approximately 61%.
[0051] S4, same as step S4 in Example 1.
[0052] S5, same as step S5 in Example 1. The corresponding workpiece mass is 422.16g, the substrate loss is 50.19g, and the loss rate is 10.63%.
[0053] Comparing Example 1 and Comparative Example 4, it can be seen that using concentrated hydrochloric acid instead of concentrated phosphoric acid results in a poorer coating removal effect and very high loss.
[0054] Comparative Example 5 The process is basically the same as in Example 1, except that the electrolyte in step S2 is prepared by mixing concentrated phosphoric acid and water in a mass ratio of 82.5:17.5, with the concentration of concentrated phosphoric acid being 85 wt%.
[0055] The corresponding preparation methods are as follows: S1 is basically the same as step S1 in Example 1, except that: a stainless steel workpiece with nickel-platinum plating is taken, the workpiece mass is 667.83g, and the supplier provides the following data: the stainless steel substrate mass is 469.52g, the plating mass is 198.31g, and the average plating thickness is about 25μm.
[0056] S2 is basically the same as step S2 in Example 1, except that the electrolyte is different.
[0057] S3, same as step S3 in Example 1; correspondingly, a workpiece with a coating removal rate of approximately 70% is obtained.
[0058] S4, same as step S4 in Example 1.
[0059] S5, same as step S5 in Example 1; the mass of the corresponding workpiece is 441.07g, the substrate loss is 28.45g, and the loss rate is 6.06%.
[0060] Comparing Example 1 and Comparative Example 5, it can be seen that using phosphoric acid alone in the electrolyte does not result in good coating removal and causes significant workpiece loss.
[0061] Comparative Example 6 The process is basically the same as in Example 1, except that the electrolyte in step S2 is prepared by mixing concentrated sulfuric acid and water in a mass ratio of 82.5:17.5, with the concentration of concentrated sulfuric acid being 98 wt%.
[0062] The corresponding preparation methods are as follows: S1 is basically the same as step S1 in Example 1, except that: a stainless steel workpiece with nickel-platinum plating is taken, the workpiece mass is 669.42g, and the supplier provides the following data: the stainless steel substrate mass is 470.86g, the plating mass is 198.56g, and the average plating thickness is about 25μm.
[0063] S2 is basically the same as step S2 in Example 1, except that the electrolyte is different.
[0064] S3, same as step S3 in Example 1; correspondingly, a workpiece with a coating removal rate of approximately 60% is obtained.
[0065] S4, same as step S4 in Example 1.
[0066] S5, same as step S5 in Example 1; the corresponding workpiece mass is 429.32g, the substrate loss is 41.54g, and the loss rate is 8.82%.
[0067] Comparing Example 1 and Comparative Example 6, it can be seen that using sulfuric acid alone in the electrolyte does not result in good plating removal, and the workpiece wear increases significantly.
[0068] Example 2 The process is basically the same as in Example 1, except that in step S2, the electrolyte is prepared by mixing concentrated phosphoric acid, concentrated sulfuric acid and water in a mass ratio of 60:20:20, with the concentrated phosphoric acid having a mass concentration of 85 wt% and the concentrated sulfuric acid having a mass concentration of 98 wt%.
[0069] The corresponding preparation methods are as follows: S1 is basically the same as step S1 in Example 1, except that: a stainless steel workpiece with nickel-platinum plating is taken, the workpiece mass is 670.15g, and the supplier provides the following data: the stainless steel substrate mass is 471.62g, the plating mass is 198.53g, and the average plating thickness is about 25μm.
[0070] S2 is basically the same as step S2 in Example 1, except that the electrolyte is different.
[0071] S3, same as step S3 in Example 1; correspondingly, a workpiece with a coating removal rate of approximately 78% is obtained.
[0072] S4, same as step S4 in Example 1.
[0073] S5, same as step S5 in Example 1; the mass of the corresponding workpiece is 464.26g, the substrate loss is 7.36g, and the loss rate is 1.56%.
[0074] Example 3 The process is basically the same as in Example 1, except that in step S2, the electrolyte is prepared by mixing concentrated phosphoric acid, concentrated sulfuric acid and water in a mass ratio of 70:15:15, with the concentrated phosphoric acid having a mass concentration of 85 wt% and the concentrated sulfuric acid having a mass concentration of 98 wt%.
[0075] The corresponding preparation methods are as follows: S1 is basically the same as step S1 in Example 1, except that: a stainless steel workpiece with nickel-platinum plating is taken, the workpiece mass is 669.34g, and the supplier provides the following data: the stainless steel substrate mass is 470.78g, the plating mass is 198.56g, and the average plating thickness is about 25μm.
[0076] S2 is basically the same as step S2 in Example 1, except that the electrolyte is different.
[0077] S3, same as step S3 in Example 1; correspondingly, a workpiece with a coating removal rate of approximately 76% is obtained.
[0078] S4, same as step S4 in Example 1.
[0079] S5, same as step S5 in Example 1; the corresponding workpiece mass is 463.15g, the substrate loss is 7.63g, and the loss rate is 1.62%.
[0080] Comparing Examples 1, 2, and 3, adjusting the ratio of concentrated phosphoric acid, concentrated sulfuric acid, and water resulted in slight fluctuations in the coating removal effect, but all showed good overall performance. Overall, Example 1 exhibited the best coating removal effect with a lower loss rate.
[0081] Example 4 S1. Take a stainless steel workpiece with a nickel-platinum coating. The workpiece weighs 668.92g. The supplier provides data: the stainless steel substrate weighs 470.31g, that is, the coating weighs 198.61g, and the average coating thickness is about 25μm. Spray a 1.5% sodium chromate solution on the non-coating area and the damaged area of the nickel-platinum coated stainless steel workpiece. After standing and drying for 40 minutes, the pretreated workpiece is obtained.
[0082] S2. Using the pretreated workpiece as the anode and the titanium plate as the cathode, place it in an electrolytic cell containing electrolyte and soak for 12 minutes. After soaking, electrolyze for 5 minutes to obtain the electrolyzed workpiece. The electrolyte is prepared by mixing concentrated phosphoric acid, concentrated sulfuric acid and water in a mass ratio of 64:18:18, with a concentration of 85 wt% for concentrated phosphoric acid and 98 wt% for concentrated sulfuric acid. The electrolysis voltage is 10 V and the electrolysis temperature is 80 °C.
[0083] S3. The workpiece after electrolysis is baked using an electric heating fan with a power of 1200W. The distance between the electric heating fan and the workpiece is controlled to be about 30cm, causing the nickel-platinum plating to peel off. The workpiece is baked until the surface temperature reaches 220±10℃ and held for 8 minutes. At this time, the peeled area accounts for about 76% of the total plating area. Then, while it is still hot, the workpiece is ultrasonically treated with an ultrasonic scalpel at a frequency of 20kHz to remove the nickel-platinum plating, resulting in a workpiece with a plating removal rate of about 78%. The removed plating is collected for the extraction of nickel-platinum.
[0084] S4. Repeat steps S1 to S3 once for the workpiece with a coating removal rate of about 78% in step S3, to obtain a workpiece with complete coating removal.
[0085] S5. The workpiece with the coating completely removed is cleaned with pure water, dried, and then weighed. The mass of the workpiece is 463.82g, the substrate loss is 6.49g, and the loss rate is 1.38%.
[0086] S6. The cleaned workpiece in step S5 is first sandblasted with corundum, and then sandblasted with glass beads and glass sand at a mass ratio of 1:1. After sandblasting, it is cleaned with pure water to obtain the regenerated workpiece.
[0087] Example 5 S1. Take a stainless steel workpiece with a nickel-platinum coating. The workpiece weighs 668.14g. The supplier provides data: the stainless steel substrate weighs 469.87g, that is, the coating weighs 198.27g, and the average coating thickness is 25μm. Spray a 2.5% sodium chromate solution on the non-coating area and the damaged area of the nickel-platinum coated stainless steel workpiece. After standing and drying for 30 minutes, the pretreated workpiece is obtained.
[0088] S2. Using the pretreated workpiece as the anode and the titanium plate as the cathode, the workpiece is placed in an electrolytic cell containing electrolyte and immersed for 8 minutes. After immersion, electrolysis is performed for 8 minutes to obtain the electrolyzed workpiece. The electrolyte is prepared by mixing concentrated phosphoric acid, concentrated sulfuric acid, and water in a mass ratio of 66:17:17, with a concentration of 84 wt% for concentrated phosphoric acid and 97 wt% for concentrated sulfuric acid. The electrolysis voltage is 15 V and the electrolysis temperature is 65 °C.
[0089] S3. The workpiece after electrolysis is baked using an electric heating fan with a power of 800W. The distance between the electric heating fan and the workpiece is controlled to be about 20cm, causing the nickel-platinum plating to peel off. The workpiece is baked until the surface temperature reaches 230±10℃ and held for 5 minutes. At this time, the peeled area accounts for about 78% of the total plating area. Then, while it is still hot, the workpiece is ultrasonically treated with an ultrasonic scalpel at a frequency of 30kHz, causing the nickel-platinum plating to fall off, resulting in a workpiece with a plating removal rate of about 77%. The peeled plating is collected for the extraction of nickel-platinum.
[0090] S4. Repeat steps S1 to S3 once for the workpiece with a coating removal rate of about 77% in step S3, to obtain a workpiece with complete coating removal.
[0091] S5. The workpiece with the coating completely removed is cleaned with pure water, dried, and weighed. The mass of the workpiece is 463.06g, the substrate loss is 6.81g, and the loss rate is 1.45%.
[0092] S6. The cleaned workpiece in step S5 is first sandblasted with corundum, and then sandblasted with glass beads and glass sand at a mass ratio of 1:1. After sandblasting, it is cleaned with pure water to obtain the regenerated workpiece.
[0093] The above are merely preferred embodiments of the present invention and are not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of the present invention.
Claims
1. A method for removing a nickel platinum plating layer, characterized by, Includes the following steps: S1. Spray corrosion inhibitor solution onto the non-plated area and the damaged area of the workpiece, and after standing and drying, the treated workpiece is obtained. S2. The treated workpiece is used as the anode and the titanium plate is used as the cathode. The workpiece is placed in an electrolytic cell containing electrolyte and immersed. After immersion, electrolysis is performed to obtain the electrolyzed workpiece. The composition of the electrolyte is: the mass ratio of concentrated phosphoric acid, concentrated sulfuric acid and water is (60~70):(15~20):(15~20). S3. The workpiece after electrolysis is baked to cause the nickel-platinum coating to peel off. Then, the nickel-platinum coating is peeled off by ultrasonication and the coating is collected to obtain a workpiece with the coating partially or completely removed. S4. Repeat steps S1 to S3 for the workpiece where the plating layer was partially removed in step S3, until the nickel-platinum plating layer is completely removed.
2. The method for removing a nickel platinum plating layer according to claim 1, characterized by, In step S1, the substrate of the workpiece is stainless steel.
3. The method for removing nickel-platinum plating according to claim 1, characterized in that, In step S1, the corrosion inhibitor is sodium chromate, and the mass concentration of the corrosion inhibitor solution is 1.5~2.5%; And / or, in step S1, the time for standing drying is 30 to 40 minutes.
4. The method for removing a nickel platinum plating layer according to claim 1, wherein In step S2, the mass concentration of phosphoric acid is 83-85 wt%; the concentration of concentrated sulfuric acid is 96-98 wt%.
5. The method for removing nickel-platinum plating according to claim 1, characterized in that, In step S2, the soaking time is 8-12 minutes; And / or, in step S2, the electrolysis voltage is 10-15V, the electrolysis temperature is 65-80℃, and the electrolysis time is 5-8min.
6. The method for removing a nickel platinum plating layer according to claim 1, wherein In step S3, the baking is carried out using an electric heating fan; wherein: the power of the electric heating fan is 800~1200W, and the distance from the coating layer is 20~30cm; the workpiece surface temperature is baked to 200~230℃, and the workpiece is kept at this temperature for 5~10 minutes.
7. The method for removing a nickel platinum plating layer according to claim 1, wherein In step S3, an ultrasonic scalpel is used to ultrasonically peel off the nickel-platinum coating, with the ultrasonic scalpel frequency being 20–30 kHz.
8. The method for removing a nickel platinum plating layer according to claim 1, wherein In step S3, nickel and platinum metals are recovered from the collected coating.
9. The method for removing nickel-platinum plating according to claim 1, characterized in that, In steps S3 and S4, the workpiece with all the coating removed is cleaned, then sandblasted, and finally cleaned again to obtain a regenerated workpiece.
10. The method for removing nickel-platinum plating according to claim 9, characterized in that, The specific process of the sandblasting treatment is as follows: first, corundum is used for sandblasting treatment, and then glass beads and glass sand with a mass ratio of (1~2):(1~2) are used for sandblasting treatment.