A processing method for electrochemically polishing an ellipsoidal superconducting cavity using a profiling cathode
By optimizing the electrolyte flow field through the use of a contoured cathode and a fluid-guided structure, the problems of uneven electric field distribution and uneven material removal in the electrochemical polishing of ellipsoidal superconducting cavities were solved, achieving high-quality polishing and improved radio frequency performance of the superconducting cavity.
Patent Information
- Application Number
- CN202611538326.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-24
AI Technical Summary
In the existing electrochemical polishing process of ellipsoidal superconducting cavities, the gap between the traditional cylindrical straight rod cathode and the inner wall of the cavity is inconsistent, resulting in disordered electric field distribution, electrolyte retention in the equatorial region, high grain steps, and rough surface, which affects the radio frequency performance and quality factor of the superconducting cavity.
The cathode is a contoured cathode, including a cathode shaft, an electrode retainer, and a contoured electrode. The electrolyte flow field is optimized through a fluid guiding structure. The electrode retainer enables coaxial positioning and detachable fixation. The contoured electrode replicates the curvature of the cavity to establish a uniform electric field and flow field, suppressing preferential etching of grains, promptly removing electrolysis products, and eliminating dead zones.
The axial and circumferential polishing uniformity of the ellipsoidal superconducting cavity was achieved, the grain step height was reduced, the 2K low-temperature acceleration gradient was improved, the surface finish and radio frequency performance were improved, and the problems of uneven electric field distribution and uneven material removal were solved.
Smart Images

Figure CN123153148A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of superconducting materials technology, and in particular to a method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode. Background Technology
[0002] Superconducting cavities are the core components of superconducting accelerators, used to construct microwave resonant cavities to accelerate charged particles. Ellipsoidal superconducting cavities, due to their geometric properties, are widely used in high-energy physics, nuclear physics, and free-electron lasers. The radio frequency (RF) performance of ellipsoidal superconducting cavities is highly dependent on the quality of their internal surface processing. Electrochemical polishing is the mainstream internal surface finishing process for niobium-based ellipsoidal superconducting cavities. The cathode's structural design directly affects the surface morphology of the cavity after polishing and the final RF performance of the superconducting cavity.
[0003] Existing electrochemical polishing processes for ellipsoidal superconducting cavities mostly employ standard cylindrical straight rod cathodes. Ellipsoidal superconducting cavities have a complex curved surface configuration with a large diameter at the equator and small diameters at the non-equatorial ends. The gap between the standard straight rod cathode and the cavity inner wall varies significantly along the cavity axis, making it difficult to match the electric field distribution to the curved contour of the cavity. This structure introduces several problems: insufficient electric field concentration in the equatorial region leads to preferential etching of grain boundaries and specific crystal orientations, with grain step heights reaching up to 32 μm at weld seams, resulting in a rough surface in the equatorial region; simultaneously, the electric field intensity is too high in the non-equatorial regions, leading to excessively fast polishing rates and insufficient material removal in the equatorial region, resulting in uneven material removal along the cavity axis.
[0004] The high-grain steps and rough surface of the cavity after polishing can induce local magnetic field enhancement, which in turn can cause thermal quenching of the superconducting cavity. Grain boundary steps can also become channels for impurity adsorption and hydrogen diffusion, exacerbating the risk of hydrogen poisoning and hydrogen embrittlement in the niobium matrix. This leads to a decrease in the quality factor Q and acceleration gradient Eacc of the superconducting cavity, making it difficult to meet the performance requirements of high-energy, high-current radio frequency superconducting accelerators.
[0005] Existing technologies employ methods such as wrapping raw material tape around the non-equatorial ends to attempt to improve polishing uniformity. However, this approach increases acid pickling time, further amplifies the risk of hydrogen diffusion, and fails to fundamentally address the issues of high grain steps and poor surface roughness in the equatorial region. It cannot simultaneously achieve surface smoothness, grain etching uniformity, and superconducting cavity RF performance. Therefore, there is an urgent need to develop a new electrochemical polishing solution to overcome these technical shortcomings. Summary of the Invention
[0006] Based on the above analysis, the present invention aims to provide a method for electrochemical polishing of ellipsoidal superconducting cavities using a contoured cathode. This method addresses the problems encountered in the prior art when polishing ellipsoidal niobium superconducting cavities with a conventional cylindrical cathode. These problems include inconsistent gaps between the cathode and the inner wall of the cavity along the axial and circumferential directions, disordered electric field distribution, easy retention of electrolyte and accumulation of electrolytic products in the equatorial region, resulting in high grain steps and poor polishing smoothness in the equatorial weld. Ultimately, this leads to a low low-temperature radio frequency acceleration gradient in the superconducting cavity and an inability to simultaneously achieve surface smoothness, grain etching uniformity, and radio frequency performance of the superconducting cavity.
[0007] On one hand, the present invention discloses a contoured cathode, comprising: a cathode shaft, an electrode retaining ring, and a contoured electrode; The contoured electrode is fixedly mounted on the cathode shaft by an electrode retainer; the curved surface of the contoured electrode replicates the inner curvature profile of the ellipsoidal superconducting cavity. The cathode shaft is used for electrical conduction and overall support and positioning, and the cathode shaft is coaxially arranged with the ellipsoidal superconducting cavity. A fluid guiding structure is provided on the surface of the conforming electrode along a line connecting one end of the short axis of the conforming electrode to the other end of the short axis of the conforming electrode, or a fluid guiding structure is provided along a line connecting one end of the long axis of the conforming electrode to the other end of the long axis of the conforming electrode. The fluid guiding structure is provided with through holes connecting the inside and outside of the conformal electrode, so that the electrolyte can flow in and out of the conformal electrode and optimize the flow field distribution in the cavity.
[0008] Preferably, the equatorial plane is defined as the direction perpendicular to the electrolyte inflow of the shaped cathode, and the two ends of the shaped cathode opposite to the equatorial plane are defined as the south pole and the north pole. The lines connecting the south pole and the north pole on the surface of the shaped electrode where the fluid guiding structure is located are uniformly arranged on the surface of the shaped electrode, dividing the surface of the shaped electrode into equal parts.
[0009] Preferably, the equatorial plane is used as the projection plane, and the angle between any two adjacent lines connecting the North and South Poles is 18±5° on the projection plane.
[0010] Preferably, the fluid guiding structure has a guiding groove as a through hole at one end of the conformal electrode facing the direction of electrolyte inflow, and a micropore array as through holes in the other directions.
[0011] Preferably, the guide channel is an approximately rectangular long channel with a length-to-width ratio of 3 to 4:1.
[0012] Preferably, the micropore array is an array of circular pores with the same diameter, wherein the diameter of the micropores is 5±2mm.
[0013] On the other hand, the present invention also discloses a method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode, comprising: S1. The conformal cathode is installed into the ellipsoidal superconducting cavity and coaxially aligned, so that the conformal cathode and the inner wall of the ellipsoidal superconducting cavity maintain a set polishing gap; the conformal cathode includes a cathode shaft, an electrode retaining ring and a conformal electrode, the conformal electrode surface replicates the curvature profile of the inner cavity of the ellipsoidal superconducting cavity, and the conformal electrode is provided with a fluid guiding structure, the fluid guiding structure including a through hole connecting the inside and outside of the conformal electrode. S2. Introduce electrolyte and establish electrolyte circulation; S3. Apply a voltage between the conformal cathode and the ellipsoidal superconducting cavity serving as the anode for electrochemical polishing; S4. After polishing is complete, disconnect the power, stop the electrolyte circulation, and remove the conformal cathode.
[0014] Preferably, in step S1, the contour electrode and the inner wall of the superconducting cavity maintain a polishing gap of 10-12 mm.
[0015] Preferably, in step S3, the polishing voltage is 10~20V, and / or the current density is 8~32mA / cm. 2, And / or, continue polishing for 100~160 minutes.
[0016] Preferably, the electrolyte flow rate in step S2 is 2~12 L / min.
[0017] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: 1. This invention employs a conformal cathode composed of a cathode shaft, electrode retaining rings, a conformal electrode, and a fluid guiding structure with through holes. The cathode shaft enables conductive transmission and coaxial positioning support, while the electrode retaining rings allow for detachable locking and secure fixation of the conformal electrode, ensuring reliable conductivity and adaptability to minute deformations. A uniform polished gap is formed between the conformal electrode, which replicates the curvature of an ellipsoidal superconducting cavity, and the cavity's inner wall. Combined with the fluid guiding structure with through holes arranged along the long or short axis and penetrating the inside and outside of the conformal electrode, bidirectional electrolyte exchange is achieved, synergistically coordinating electric field control and flow field guidance. This ensures the coaxiality of the cathode assembly and prevents scratches from impacts to the cavity. It also enables the components to be detachable and replaceable, ensuring conductivity. The connection is stable; the balanced polishing electric field distribution suppresses preferential etching of grains, reduces the grain step height, and improves the uniformity of material removal along the cavity axis; at the same time, it effectively diverts the electrolyte and removes electrolytic products, eliminating dead corners where electrolyte stagnates in high curvature areas. The combined effect of the electric field and the flow field improves the overall electrochemical polishing uniformity and surface processing quality of the ellipsoidal superconducting cavity; thus solving the problems of uneven electric field distribution caused by the mismatch between the traditional standard straight rod cathode and the curved surface contour of the ellipsoidal cavity, preferential etching of grains in the equatorial region, high grain steps, and inconsistent material removal along the cavity axis, as well as the defects of electrolyte stagnation and reaction product accumulation in high curvature areas such as the equator during the polishing process, resulting in poor polishing uniformity.
[0018] 2. This invention features a rectangular elongated channel with an aspect ratio of 3-4:1 at the electrolyte inflow end of the conformal electrode, controlling the channel width to be 5±2mm and the length to be 18±3mm. The remaining area is configured with a micro-pore array of equal diameter circular holes, with a micro-pore diameter of 5±2mm. Simultaneously, the spacing between adjacent micro-pores and between micro-pores and the channel is uniformly set to 5±2mm. The large-flow channel facilitates the main liquid inflow and slag discharge, while the micro-pore array achieves full-area liquid dispersion. Through the coordinated configuration of parameters such as size, aspect ratio, and spacing, a combined fluid guiding structure adapted to the ellipsoidal cavity surface is constructed, complementing the uniform electric field of the conformal cathode. The large flow cross-section provided by the channel reduces the inflow resistance, enabling rapid introduction of a large flow rate of electrolyte into the polishing area and smooth discharge of electrolytic solid dissolved products. The micro-pore array uniformly distributes the electrolyte across the entire polishing surface, continuously updating the polishing interface. The uniform spacing between the channel and the micro-pores ensures a smooth flow transition without abrupt changes in flow velocity. The stable flow field and the uniform electric field of the conformal cathode work together to suppress preferential etching of grains, reduce the grain step height, and achieve uniform axial and circumferential polishing of the ellipsoidal superconducting cavity. The grain step height is 14~17μm, which improves the axial and circumferential polishing flatness of the cavity (cavity flatness, the transition area from the equator to the non-equatorial ends is ≤25μm). The 2K low-temperature acceleration gradient is significantly improved to 26~31MV / m. At the same time, it takes into account the mechanical structural rigidity and effective conductive area of the conformal electrode substrate, and avoids the deformation of the cathode due to fluid impact. This solves the problems of insufficient flow cross-section at the liquid inlet of the single microporous structure, slow electrolyte replenishment, and easy accumulation and blockage of electrolytic solid products. It avoids the electrolyte exchange blind zone and electrolyte stagnation in the equatorial region caused by unreasonable size and spacing of the flow guide openings. It also solves the technical defects of the prior art, such as excessive local electrolyte flow rate causing over-etching of the cavity, mismatch between flow field and electric field leading to high polishing grain steps, and poor polishing circumferential and axial uniformity.
[0019] 3. This invention employs a conformal cathode with a conformal electrode and fluid-guided through-holes. During assembly, coaxial alignment is achieved, maintaining a pre-set polishing gap between the cathode and the inner wall of the superconducting cavity. Electrochemical polishing is performed under electrolyte circulation conditions. The conformal electrode replicates the curvature of the cavity's inner surface to obtain a uniform electric field. Simultaneously, the through-holes in the fluid-guided structure allow electrolyte to flow across the conformal electrode, achieving a synergistic effect between the electric and flow fields. This results in a uniform electric field distribution during polishing, suppressing preferential grain etching and reducing grain step height. It can promptly remove electrolytic reaction products, eliminate dead zones where electrolyte remains in the cavity, and improve the polishing uniformity of axial and circumferential material removal in the ellipsoidal superconducting cavity. This solves the technical problems of uneven electric field distribution caused by uneven cathode-cavity gap in existing straight cathode solutions, preferential etching of grains in the equatorial region, high grain steps, easy retention of electrolyte and accumulation of electrolytic products in high curvature positions such as the equator of the ellipsoidal cavity, and uneven axial and circumferential polishing removal in the superconducting cavity. It effectively balances surface finish, grain etching uniformity, and radio frequency performance of the superconducting cavity.
[0020] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0021] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0022] Figure 1 This is a schematic diagram of an ellipsoidal superconducting cavity in a specific embodiment of the present invention; Figure 2 This is a schematic diagram of the conformal cathode installed inside an ellipsoidal superconducting cavity in a specific embodiment of the present invention; Figure 3 This is a schematic diagram of the conformal cathode structure in a specific embodiment of the present invention; Figure 4 This is a schematic diagram of the conformal electrode structure in a specific embodiment of the present invention; Figure 5 This is a schematic diagram of the retaining ring structure in a specific embodiment of the present invention.
[0023] 1-Superconducting cavity; 4-Contouring cathode; 401 - Contouring electrode; 4011 - Micropore; 4012 - Flow channel; 501-Clasp; 601 - Cathode shaft. Detailed Implementation
[0024] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0025] In a first aspect, the present invention discloses a contoured cathode, such as... Figures 1-5 As shown, it includes: a cathode shaft, an electrode retaining ring, and a contoured electrode; The contoured electrode is fixedly mounted on the cathode shaft by an electrode retainer; the curved surface of the contoured electrode replicates the inner curvature profile of the ellipsoidal superconducting cavity. The cathode shaft is used for electrical conduction and overall support and positioning, and the cathode shaft is coaxially arranged with the ellipsoidal superconducting cavity. A fluid guiding structure is provided on the surface of the conforming electrode along a line connecting one end of the short axis of the conforming electrode to the other end of the short axis of the conforming electrode, or a fluid guiding structure is provided along a line connecting one end of the long axis of the conforming electrode to the other end of the long axis of the conforming electrode. The fluid guiding structure is provided with through holes connecting the inside and outside of the conformal electrode, so that the electrolyte can flow in and out of the conformal electrode and optimize the flow field distribution in the cavity.
[0026] During implementation, the cathode shaft is placed inside the ellipsoidal superconducting cavity, and the two are coaxially arranged; the electrolyte enters the ellipsoidal superconducting cavity from one side of the major axis / minor axis and flows out from the other side of the corresponding opening; the ellipsoidal superconducting cavity and the cathode shaft are connected to the positive and negative terminals of an external power supply, respectively, and the electrolyte is used to electrochemically polish the inner cavity of the ellipsoidal superconducting cavity; The cathode shaft serves as a conductive carrier, transferring the cathode potential from the external power source to the conformal electrode. On the other hand, it acts as a main support component, supporting the electrode retainer and the conformal electrode. During assembly, it ensures that the whole structure is coaxial with the ellipsoidal superconducting cavity, controls the relative position of the cathode and the cavity, and avoids uneven gaps and scratches on the inner wall caused by assembly eccentricity. The electrode retainer ring enables detachable locking and fixation between the contour electrode and the cathode shaft; it ensures reliable electrical connection between the conductive components and the cathode shaft, and can also accommodate the slight displacement caused by cavity deformation, maintaining the installation posture of the contour electrode, and facilitating the disassembly, assembly, and replacement of contour electrodes of different specifications. The contour electrode is the core working body of the cathode. Its curved surface replicates the curvature of the ellipsoidal superconducting cavity. During the polishing process, it forms a uniform gap with the inner wall of the cavity to match the contour of the cavity surface, improve the electric field distribution during polishing, reduce local current density differences, suppress preferential etching of grains, reduce grain step height, and improve the uniformity of axial material removal in the cavity. The through-holes of the fluid-guided structure connect the inside and outside of the conformal electrode, allowing the electrolyte to flow and exchange between the inner side of the conformal electrode and the polishing gap of the superconducting cavity through the through-holes. Whether arranged along the long axis or the short axis, the electrolyte can be directionally guided, and the electrolytic reaction products can be carried away in time. This eliminates dead zones where the electrolyte stagnates in high curvature areas such as the equator, optimizes the flow field inside the cavity, and further enhances the polishing uniformity in conjunction with the electric field.
[0027] Compared with existing technologies, this invention employs a conformal cathode composed of a cathode shaft, electrode retaining rings, conformal electrodes, and a fluid guiding structure with through holes. The cathode shaft enables conductive transmission and coaxial positioning support, while the electrode retaining rings allow for detachable locking and secure fixation of the conformal electrodes, ensuring reliable conductivity and adaptability to minute deformations. The conformal electrodes, replicating the curvature of an ellipsoidal superconducting cavity, form a uniform polished gap with the cavity's inner wall. Combined with the through-hole fluid guiding structure arranged along the long or short axis and penetrating the inside and outside of the conformal electrodes, bidirectional electrolyte exchange is achieved, synergistically coordinating electric field control and flow field guidance. This ensures the coaxiality of the cathode assembly, preventing scratches and impacts to the cavity, and allows for the detachable replacement of components. The conductive connection is stable; the balanced polishing electric field distribution suppresses preferential etching of grains, reduces the grain step height, and improves the uniformity of material removal along the cavity axis; at the same time, it effectively diverts the electrolyte, removes electrolytic products, and eliminates dead zones where electrolyte stagnation occurs in high curvature areas. The combined effect of the electric field and the flow field improves the overall electrochemical polishing uniformity and surface processing quality of the ellipsoidal superconducting cavity; thus solving the problems of uneven electric field distribution caused by the mismatch between the traditional standard straight rod cathode and the curved surface contour of the ellipsoidal cavity, preferential etching of grains in the equatorial region, high grain steps, and inconsistent material removal along the cavity axis, as well as the defects of electrolyte stagnation and reaction product accumulation in high curvature areas such as the equator during the polishing process, resulting in poor polishing uniformity.
[0028] Preferably, the equatorial plane is defined as the direction perpendicular to the electrolyte inflow of the shaped cathode, and the two ends of the shaped cathode opposite to the equatorial plane are defined as the south pole and the north pole. The lines connecting the south pole and the north pole on the surface of the shaped electrode where the fluid guiding structure is located are uniformly arranged on the surface of the shaped electrode, dividing the surface of the shaped electrode into equal parts.
[0029] More preferably, the equatorial plane is used as the projection plane, and the angle between any two adjacent lines connecting the North and South Poles is 18±5° on the projection plane.
[0030] It should be noted that the angle between adjacent connecting lines projected onto the equatorial plane is set to 18±5°: If the angle is too large, the spacing between the flow-guiding structures will be too large, creating dead zones for electrolyte stagnation; if the angle is too small, the openings will be too densely arranged, easily causing excessively high local flow velocities, while simultaneously weakening the strength of the contoured electrode structure and reducing the effective conductive area. This angle range allows for a uniform circumferential distribution of the flow-guiding structure, full-domain renewal of the electrolyte at the polishing interface, matching the electric field distribution in the equatorial region of the ellipsoidal cavity, balancing flow field effects, conductivity, and structural stiffness, and improving polishing uniformity.
[0031] Preferably, the fluid guiding structure has a guiding groove as a through hole at one end of the conformal electrode facing the direction of electrolyte inflow, and a micropore array as through holes in the other directions.
[0032] It should be noted that a flow channel is set at the electrolyte inlet end. The flow cross-section of the channel is larger, which can reduce the flow resistance of the electrolyte into the polishing gap, so that the electrolyte can be quickly and in large flow rate introduced into the polishing operation area between the conformal electrode and the inner wall of the superconducting cavity, avoiding insufficient flow at the inlet end; at the same time, it can quickly guide the large volume of electrolytic dissolution products and prevent the products from accumulating and blocking the flow channel on the inlet side.
[0033] Except for the liquid inlet end, the remaining area adopts a micropore array: the micropores have smaller diameters, more openings, and higher distribution density. On the one hand, the electrolyte can be dispersed and sprayed to the high curvature polishing area such as the equator, so that the electrolyte is more evenly distributed in the circumferential direction throughout the cavity, avoiding local over-etching caused by excessive local flow velocity; on the other hand, the micropore array can finely divide the electrolysis products, continuously renew the fresh electrolyte at the polishing interface, and eliminate the dead corners where electrolyte stagnates in the equatorial region.
[0034] The flow channel works in conjunction with the micropore array: the inlet channel is responsible for high-flow-rate electrolyte introduction and slag discharge in the main channel; the micropore array in the remaining areas is responsible for distributing the electrolyte and updating the polishing interface across the entire area. This balances high-flow-rate electrolyte introduction with uniform flow field across the entire area, ensuring sufficient electrolyte supply without excessive local flow velocity differences. It achieves synergy between the flow field and the uniform electric field provided by the contoured cathode, further suppressing preferential grain etching, reducing grain step height, and improving the overall polishing uniformity of the ellipsoidal superconducting cavity.
[0035] Specifically, the guide channel can be an approximately rectangular long channel with a length-to-width ratio of 3 to 4:1, a width of 5±2mm, and a length of 18±3mm.
[0036] Specifically, the micropore array can be a circular array of the same diameter, with a micropore diameter of 5±2mm, and the spacing between adjacent micropores and the spacing between adjacent micropores and guide grooves is 5±2mm.
[0037] It should be noted that the guide channel is designed with a rectangular long channel shape of 3~4:1, which extends along the curved surface to ensure that the liquid inlet has a large flow cross-sectional area, reduce the flow resistance of the electrolyte into the polishing gap, ensure that a large flow of electrolyte is quickly introduced into the polishing area, and facilitate the smooth discharge of solid dissolved products generated by electrolysis, making it less prone to clogging. If the tank width is too small (less than 3mm), the flow cross section is insufficient, the liquid inlet flow rate is limited, the electrolyte supply on the inlet side is insufficient, and product accumulation is likely to occur; if the tank width is too large (greater than 7mm), it will reduce the area of the conformal electrode substrate too much, reducing the structural strength and effective conductive area.
[0038] The length of the guiding groove is controlled at 18±3mm to match the size of the liquid-facing curved surface of the ellipsoidal electrode. If the length is too short, the guiding coverage will be insufficient; if it is too long, it will excessively encroach on the substrate and affect the cathode rigidity.
[0039] The length-to-width ratio of the flow channel is limited to 3~4:1 to ensure that the flow is weak along the curved surface (or easily blocked by electrolytic debris).
[0040] If the micropore diameter is too small (less than 3 mm), the pores are easily blocked by electrolytic debris, reducing the electrolyte exchange capacity; if the diameter is too large (greater than 7 mm), the opening ratio is too high, resulting in a loss of conductive area and causing excessively high local electrolyte jet velocity, leading to local over-etching of the cavity.
[0041] If the spacing between micropores and between micropores and conductive channels is too large, the pore positions will be sparse, and there will be a dead zone for electrolyte exchange on the polished curved surface. Electrolyte will easily stagnate in the equatorial region. If the spacing is too small, the openings will be too dense, and the substrate structure will be weakened by a large number of openings. The conformal electrode will be easily deformed by fluid impact, which will destroy the polishing gap set by the cathode-cavity. At the same time, the effective conductive area will decrease, resulting in abnormal local current density.
[0042] In addition, the above parameters work together: the large-section rectangular guide channel at the liquid-facing end serves as the main liquid inlet and slag outlet; the array of circular micropores in the remaining areas disperses the liquid, continuously updating the electrolyte at the polishing interface across the entire polished surface; a uniform spacing of 5±2mm ensures a smooth flow field transition, avoiding abrupt changes in flow velocity at the junction of the channel and the micropores. The flow field, combined with the uniform electric field provided by the contoured cathode, reduces preferential grain etching, lowers the grain step height, and improves the axial and circumferential polishing uniformity of the ellipsoidal superconducting cavity.
[0043] Compared with existing technologies, this invention features a rectangular elongated channel with an aspect ratio of 3-4:1 at the electrolyte inflow end of the conformal electrode, controlling the channel width to be 5±2mm and the length to be 18±3mm. The remaining area is configured with a micropore array of equal diameter circular holes, each with a diameter of 5±2mm. Simultaneously, the spacing between adjacent micropores and between micropores and the channel is uniformly set to 5±2mm. The large-flow channel facilitates main liquid inflow and slag discharge, while the micropore array achieves full-area liquid dispersion. Through the coordinated configuration of size, aspect ratio, and spacing parameters, a combined fluid guiding structure adapted to the ellipsoidal cavity surface is constructed, complementing the uniform electric field of the conformal cathode. The large flow cross-section provided by the channel reduces the inflow resistance, enabling rapid introduction of a large flow rate of electrolyte into the polishing area and smooth discharge of electrolytically dissolved solids. The micropore array uniformly distributes the electrolyte across the entire polishing surface, continuously updating the polishing interface. The uniform spacing between the channel and the micropores ensures a smooth flow transition with no velocity. The stable flow field and the uniform electric field of the conformal cathode work together to suppress preferential etching of the grains, reduce the grain step height, and achieve uniform axial and circumferential polishing of the ellipsoidal superconducting cavity. The grain step height is 14~17μm, which improves the axial and circumferential polishing flatness of the cavity (cavity flatness, the transition area from the equator to the non-equatorial ends is ≤25μm). The 2K low-temperature acceleration gradient is significantly improved to 26~31MV / m. At the same time, it takes into account the mechanical structural rigidity and effective conductive area of the conformal electrode substrate, and avoids the deformation of the cathode due to fluid impact. This solves the problems of insufficient flow cross section at the liquid inlet of the single microporous structure, slow electrolyte replenishment, and easy accumulation and blockage of electrolytic solid products. It avoids the electrolyte exchange blind zone and electrolyte stagnation in the equatorial region caused by unreasonable size and spacing of the flow guide openings. It also solves the technical defects of the existing technology, such as excessive local electrolyte flow rate causing over-etching of the cavity, mismatch between flow field and electric field leading to high polishing grain steps, and poor polishing circumferential and axial uniformity.
[0044] Specifically, the electrode retainer has a cross-shaped protrusion perpendicular to the cathode axis, and the contour electrode has cross-shaped grooves at both ends parallel to the cathode axis. The cross-shaped protrusion and the cross-shaped groove match and engage, so that the contour electrode is fixedly assembled on the cathode axis by the electrode retainer.
[0045] Secondly, this invention discloses a method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode, such as... Figure 1-5 As shown, it includes: S1. The conformal cathode is installed into the ellipsoidal superconducting cavity and coaxially aligned, so that the conformal cathode and the inner wall of the ellipsoidal superconducting cavity maintain a set polishing gap; the conformal cathode includes a cathode shaft, an electrode retaining ring and a conformal electrode, the conformal electrode surface replicates the curvature profile of the inner cavity of the ellipsoidal superconducting cavity, and the conformal electrode is provided with a fluid guiding structure, the fluid guiding structure including a through hole connecting the inside and outside of the conformal electrode. S2. Introduce electrolyte and establish electrolyte circulation; S3. Apply a voltage between the conformal cathode and the ellipsoidal superconducting cavity serving as the anode for electrochemical polishing; S4. After polishing is complete, disconnect the power, stop the electrolyte circulation, and remove the conformal cathode.
[0046] During implementation, the cathode shaft is fixed to the conformal electrode by an electrode retainer to ensure overall coaxiality. The conformal electrode, which replicates the curvature of the inner cavity, forms a uniform polishing gap with the inner wall of the cavity, improving the polishing electric field distribution. During electrolyte circulation, the electrolyte can flow and exchange inside and outside the conformal electrode through the through holes of the fluid guiding structure, promptly carrying away electrolytic reaction products, eliminating electrolyte stagnation dead zones, and achieving electric field-flow field synergy. During electropolishing, the preferential etching effect of grains is suppressed, the grain step height is reduced, and the polishing uniformity of the ellipsoidal superconducting cavity in the axial and circumferential directions is improved. After polishing, the power is turned off, the liquid is stopped, and the cathode is removed, completing the electrochemical polishing process of the superconducting cavity.
[0047] Compared with existing technologies, this invention employs a conformal cathode with a conformal electrode and fluid-guided through-holes. During assembly, coaxial alignment is achieved, maintaining a pre-set polishing gap between the cathode and the inner wall of the superconducting cavity. Electrochemical polishing is performed under electrolyte circulation conditions. The conformal electrode replicates the curvature of the cavity's inner surface to obtain a uniform electric field. Simultaneously, the through-holes in the fluid-guided structure allow the electrolyte to flow across the conformal electrode, achieving a synergistic effect between the electric and fluid fields. This results in a uniform electric field distribution during polishing, suppressing preferential grain etching and reducing grain step height. It can promptly remove electrolytic reaction products, eliminate dead zones where electrolyte remains in the cavity, and improve the polishing uniformity of axial and circumferential material removal in ellipsoidal superconducting cavities. Furthermore, it solves the technical problems of uneven electric field distribution caused by uneven cathode-cavity gap in existing straight-bar cathode schemes, preferential etching of grains in the equatorial region, high grain steps, easy retention of electrolyte and accumulation of electrolytic products in high curvature positions such as the equator of ellipsoidal cavities, and uneven axial and circumferential polishing removal in superconducting cavities. It effectively balances surface finish, grain etching uniformity, and radio frequency performance of superconducting cavities.
[0048] Specifically, in step S1, a coaxial alignment mechanism is used for alignment adjustment to control the coaxial tolerance between the cathode shaft and the superconducting cavity axis to be ≤ ±0.05mm.
[0049] Specifically, in step S1, the contour electrode and the inner wall of the superconducting cavity maintain a polishing gap of 10-12 mm; the contour machining deviation of the contour electrode is ≤ ±0.05 mm.
[0050] It should be noted that the coaxial tolerance between the cathode axis and the superconducting cavity axis is controlled to be ≤±0.05mm. The purpose is to ensure the consistency of the gap between the circumferential electrode and the inner wall of the cavity. If the coaxial tolerance is too large, the cathode will become eccentric, which will cause the circumferential polishing gap to be of different sizes, the electric field distribution to be distorted, and local preferential etching of grains to occur. At the same time, the cathode component is also prone to scratching and damaging the inner surface of the superconducting cavity.
[0051] A polishing gap of 10-12 mm is maintained between the contoured electrode and the inner wall of the superconducting cavity. This gap is a key control condition for the electric field strength and polishing removal rate: if the gap is too small, the electric field strength is too high, which can easily lead to arcing and local over-etching; if the gap is too large, the electric field strength is insufficient, the material removal efficiency is low, and the polishing in the equatorial region is insufficient. The machining deviation of the contoured electrode is limited to ≤±0.05 mm to ensure that the cathode surface accurately replicates the curvature of the ellipsoidal superconducting cavity, avoids additional gap fluctuations introduced by the cathode's own contour error, ensures uniform electric field throughout the cavity, and suppresses the grain step effect.
[0052] The three parameters work together to ensure a uniform electric field during the polishing process from three dimensions: assembly coaxiality accuracy, working gap, and cathode machining accuracy, providing a structural basis for subsequent flow field optimization.
[0053] Specifically, in step S2, the electrolyte can be a mixed acid electrolyte of hydrofluoric acid and sulfuric acid. This electrolyte is commonly used for electrochemical polishing of niobium superconducting cavities, and the volume ratio of each component is hydrofluoric acid (HF): sulfuric acid (H2SO4) = 1:7~10.
[0054] It should be noted that this mixed electrolyte can achieve controllable anodic dissolution of the niobium substrate. Sulfuric acid serves as a carrier liquid and enhances the conductivity of the solution, while hydrofluoric acid is used to dissolve the niobium oxide film generated during the polishing process, ensuring continuous electrochemical polishing. By controlling the ratio within the above range, both the polishing removal rate and surface quality can be balanced, reducing the risk of over-corrosion and pitting.
[0055] Specifically, in step S2, the electrolyte, driven by a circulating pump, flows through the fluid guiding structure of the conformal cathode at a flow rate of 2~12L / min. The electrolyte passes through the guiding groove and micropores and is continuously exchanged between the inner side of the conformal electrode and the polishing gap, which promptly removes the electrolytic dissolution products of niobium, refreshes the fresh electrolyte at the polishing interface, eliminates dead zones of electrolyte stagnation in high curvature areas such as the equator, and works in conjunction with the uniform electric field to reduce the height of the grain step and improve the uniformity of polishing. The electrolyte flow rate can be 2L / min, 5L / min, 8L / min or 12L / min.
[0056] It should be noted that if the flow rate is too low, such as below 2L / min, the electrolyte circulation and renewal capacity is insufficient, the electrolytic products cannot be carried away in time, and electrolyte stagnation and accumulation are likely to occur in high curvature areas such as the equator. The polishing interface will not receive a continuous supply of fresh electrolyte, which will aggravate the preferential etching phenomenon of grains, increase the height of grain steps, and worsen the polishing uniformity. When the flow rate is too high, such as above 12 L / min, the fluid impact is significantly enhanced. Excessive liquid flow impact force will cause micro-deformation of the conformal electrode, destroying the 10-12 mm polishing gap. At the same time, excessive flow rate will cause inconsistent local scouring intensity, leading to local over-etching of the cavity and increasing the load on the system piping. Within this range, the electrolyte can fully complete the exchange of media inside and outside the conformal electrode with the help of the fluid guiding structure, promptly discharge the electrolysis products, and eliminate the polishing dead zone; it can also avoid the deformation of the cathode structure caused by fluid impact, ensure the stability of the polishing gap and electric field state, realize the synergy of the flow field and electric field, and ensure the axial and circumferential polishing quality of the ellipsoidal superconducting cavity.
[0057] Specifically, in step S3, the polishing voltage is 10~20V, which can be 10V, 14V, 17V, or 20V; the current density is 8~32mA / cm. 2 It can be 8mA / cm 2 16mA / cm 2 24mA / cm 2 Or 32mA / cm 2 The polishing time is 100-160 minutes, which can be 100 minutes, 120 minutes, 140 minutes or 160 minutes.
[0058] It should be noted that the polishing voltage, current density, and polishing time were selected within the above ranges for the following reasons: The polishing voltage determines the electric field strength within the polishing zone. When the voltage is below 10V, the electric field strength is insufficient, resulting in a low anodic dissolution rate of the niobium matrix, inadequate material removal, and difficulty in effectively eliminating grain boundary steps. When the voltage is above 20V, the current density surges, easily leading to localized arcing and bubble aggregation, causing localized over-corrosion and introducing new surface defects. Therefore, a stable anodic dissolution rate is selected within a specific range to match the uniform electric field formed by the contoured cathode.
[0059] Current density and voltage work together to control the material removal rate; current density is below 8 mA / cm². 2 The polishing reaction is slow, resulting in low processing efficiency; the current density is higher than 32 mA / cm². 2 If the anodic reaction is too vigorous, a large number of bubbles will be released, which will disrupt the flow field within the polishing gap, causing surface pitting and uneven grain etching. A specific range can stably control the uniform anodic dissolution of niobium material.
[0060] Polishing time controls the total material removal. If the time is less than 100 minutes, the total material removal is insufficient, and existing surface defects and weld grain steps cannot be fully removed. If the time exceeds 160 minutes, over-polishing increases the risk of intergranular corrosion and also increases the time for hydrogen diffusion in the niobium matrix, raising the risk of hydrogen embrittlement. Selecting a suitable time interval allows for control of the total material removal while adequately removing surface grain steps, reducing the risk of hydrogen diffusion, and enabling high-quality polishing of the ellipsoidal superconducting cavity through the coordinated use of electric and flow fields.
[0061] Within this range, the polishing voltage, current density, and polishing time work in concert to precisely control the anodic dissolution rate and total material removal of the niobium matrix, based on the uniform electric field constructed by the conformal cathode and the stable flow field formed by the fluid guiding structure. Within this parameter combination range, a stable electrochemical polishing reaction is maintained, suppressing abnormal phenomena such as severe gas evolution and arc discharge, avoiding localized over-etching or pitting defects in the cavity; at the same time, sufficient material removal is ensured, effectively reducing grain steps in the weld seam and equatorial region. Simultaneously, electrolyte circulation promptly removes reaction products, shortening the hydrogen enrichment time in the niobium matrix and reducing the probability of hydrogen embrittlement. Through the combined control of voltage, current density, and polishing time, synchronous and uniform axial and circumferential material removal is achieved in the ellipsoidal superconducting cavity, resulting in a high-quality inner cavity surface with low grain steps and improved low-temperature radio frequency performance of the superconducting cavity.
[0062] To more clearly describe the present invention, the following embodiments and comparative examples are provided: Example 1 This embodiment discloses a contour-following cathode, comprising: 25mm diameter cathode shaft, electrode retaining ring, and contoured electrode; The conformal electrode is fixedly mounted on the cathode shaft by an electrode retainer; the curved surface of the conformal electrode replicates the inner curvature profile of the ellipsoidal superconducting cavity; the electrode retainer has a cross protrusion perpendicular to the cathode shaft axis, and the conformal electrode has a cross groove at both ends parallel to the cathode shaft axis. The cross protrusion and the cross groove match and engage so that the conformal electrode is fixedly mounted on the cathode shaft by the electrode retainer. The cathode shaft is used for conductivity and overall support and positioning, and the cathode shaft is coaxially positioned with the ellipsoidal superconducting cavity. A fluid guiding structure is provided on the surface of the conforming electrode along a line connecting one end of the short axis of the conforming electrode to the other end of the short axis of the conforming electrode. The fluid guiding structure has through holes connecting the inside and outside of the contour electrode.
[0063] The lines connecting the North and South Poles on the surface of the conformal electrode where the fluid guiding structure is located are evenly distributed on the surface of the conformal electrode, dividing the surface of the conformal electrode into equal parts; with the equatorial plane as the projection plane, the angle between any two adjacent lines connecting the North and South Poles on the projection plane is 18±5°.
[0064] The fluid guiding structure has a flow channel at one end of the conformal electrode facing the direction of electrolyte inflow, and micropore arrays in the other directions.
[0065] The guide channel is an approximately rectangular long channel with a short side arc, and the length-to-width ratio satisfies 18:3. The guide channel is 5mm wide and 18mm long.
[0066] The micropore array can be a circular array of the same diameter, with a micropore diameter of 5mm, and the spacing between adjacent micropores and the spacing between adjacent micropores and guide grooves is 5mm.
[0067] The machining deviation of the contour of the conformal electrode is ≤ ±0.05mm.
[0068] This embodiment discloses a method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode, including: S1. The above-mentioned conformal cathode is installed into the ellipsoidal superconducting cavity and coaxially aligned, so that the conformal cathode and the inner wall of the ellipsoidal superconducting cavity maintain a polishing gap of 10 mm; the coaxiality tolerance between the cathode axis and the superconducting cavity axis is controlled to be ≤ ±0.05 mm; the major axis of the ellipsoidal superconducting cavity is 150 mm and the minor axis is 100 mm. Based on the 10 mm polishing gap between the conformal cathode and the inner wall of the ellipsoidal superconducting cavity, the size of the conformal cathode can be uniquely determined. S2. Introduce electrolyte and establish electrolyte circulation; the fluid guide structure flows through the shaped cathode at a flow rate of 10 L / min; the electrolyte is a mixed acid electrolyte of hydrofluoric acid and sulfuric acid, and the volume ratio of each component is hydrofluoric acid (HF): sulfuric acid (H2SO4) = 1:9; S3. Electrochemical polishing is performed by applying a voltage between the conformal cathode and the ellipsoidal superconducting cavity serving as the anode; the polishing voltage is 15V; the current density is 20mA / cm². 2 Polish continuously for 120 minutes; S4. After polishing is complete, disconnect the power, stop the electrolyte circulation, and remove the conformal cathode.
[0069] After polishing in Example 1, the ellipsoidal niobium superconducting cavity was tested using the following standards or methods: Grain step height: Using a white light interferometer (WLI), and following the general method for testing the surface morphology of superconducting niobium cavities, multiple samples were taken at the transition regions at both the equator and non-equator ends of the cavity to measure the grain boundary step height; this characterizes the degree of grain boundary etching after polishing.
[0070] Cavity flatness: A 3D contour scanner / laser contour meter is used to continuously scan along the cavity axis (from the equator to both ends) to obtain the contour of the inner wall of the cavity. The maximum contour deviation of the inner wall contour relative to the theoretical ellipsoidal surface is calculated to reflect the overall geometric flatness of the cavity after polishing.
[0071] 2K Vertical Test Acceleration Gradient: Following the Superconducting Radio Frequency Niobium Cavity Vertical Test (SRF cavity verticaltest) standard, vertical radio frequency tests were conducted in a liquid helium 2K cryogenic environment, gradually increasing the radio frequency power and measuring the acceleration gradient of the cavity; this is used to characterize the radio frequency performance of the superconducting cavity.
[0072] Test results: Grain step height is 14~15μm; cavity flatness (transition area from the equator to the non-equatorial ends) ≤22μm; 2K vertical test acceleration gradient is 28.5~31MV / m.
[0073] Example 2 This embodiment discloses a contoured cathode and a method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode, which differs from Embodiment 1 in that: Contouring cathode: The equatorial plane of the contoured cathode perpendicular to the direction of electrolyte inflow is used as the projection plane, and the angle between the lines connecting the two ends of any two adjacent contoured electrodes on the projection plane is 13°.
[0074] The fluid guiding structure has a flow channel at one end of the conformal electrode facing the direction of electrolyte inflow, and micropore arrays in the other directions.
[0075] The guide channel is an approximately rectangular long channel with a short side arc, and the length-to-width ratio satisfies 3:1. The guide channel is 3mm wide and 9mm long.
[0076] The micropore array can be a circular array of the same diameter, with a micropore diameter of 3mm, and the spacing between adjacent micropores and the spacing between adjacent micropores and guide grooves is 3mm.
[0077] The machining deviation of the contour of the conformal electrode is ≤ ±0.05mm.
[0078] Electrochemical polishing method for ellipsoidal superconducting cavities using contoured cathodes: The conformal cathode maintains a polishing gap of 12 mm with the inner wall of the ellipsoidal superconducting cavity; the size of the ellipsoidal superconducting cavity is the same as in Example 1. The size of the conformal cathode can be uniquely determined based on the 10 mm polishing gap between the conformal cathode and the inner wall of the ellipsoidal superconducting cavity. A fluid guiding structure that flows through a contoured cathode at a flow rate of 5 L / min; the volume ratio of each component of the electrolyte is hydrofluoric acid (HF): sulfuric acid (H2SO4) = 1:7; Electrochemical polishing was performed by applying a voltage between a conformal cathode and an ellipsoidal superconducting cavity serving as the anode; the polishing voltage was 12V; and the current density was 12mA / cm². 2 Polish continuously for 100 minutes.
[0079] The ellipsoidal superconducting cavity after electrochemical polishing was tested using the same method as in Example 1. The test results are as follows: The grain step height is 16~17μm; the cavity flatness (transition area from the equator to the non-equatorial ends) is ≤25μm; the 2K vertical test acceleration gradient is 26~28MV / m.
[0080] Example 3 This embodiment discloses a contoured cathode and a method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode, which differs from Embodiment 1 in that: Contouring cathode: The equatorial plane of the contoured cathode perpendicular to the direction of electrolyte inflow is used as the projection plane, and the angle between the lines connecting the two ends of any two adjacent contoured electrodes on the projection plane is 23°.
[0081] The fluid guiding structure has a flow channel at one end of the conformal electrode facing the direction of electrolyte inflow, and micropore arrays in the other directions.
[0082] The guide channel is an approximately rectangular long channel with a short side arc, and the length-to-width ratio satisfies 4:1. The guide channel is 7mm wide and 21mm long.
[0083] The micropore array can be a circular array of the same diameter, with a micropore diameter of 7mm, and the spacing between adjacent micropores and the spacing between adjacent micropores and guide grooves is 7mm.
[0084] The machining deviation of the contour of the conformal electrode is ≤ ±0.05mm.
[0085] Electrochemical polishing method for ellipsoidal superconducting cavities using contoured cathodes: The conformal cathode maintains a 10mm polishing gap with the inner wall of the ellipsoidal superconducting cavity; the ellipsoidal superconducting cavity has a major axis of 160mm and a minor axis of 110mm. The size of the conformal cathode can be uniquely determined based on the 10mm polishing gap between the conformal cathode and the inner wall of the ellipsoidal superconducting cavity. A fluid guiding structure that flows through a contoured cathode at a flow rate of 12 L / min; the volume ratio of each component of the electrolyte is hydrofluoric acid (HF): sulfuric acid (H2SO4) = 1:10; Electrochemical polishing was performed by applying a voltage between a contoured cathode and an ellipsoidal superconducting cavity serving as the anode; the polishing voltage was 20V; and the current density was 32mA / cm². 2 Polish continuously for 160 minutes.
[0086] The ellipsoidal superconducting cavity after electrochemical polishing was tested using the same method as in Example 1. The test results are as follows: The grain step height is 15~16μm; the cavity flatness (transition area from the equator to the non-equatorial ends) is ≤24μm; the 2K vertical test acceleration gradient is 27~29MV / m.
[0087] Comparative Example 1 This comparative example discloses a method for electrochemical polishing of an ellipsoidal superconducting cavity using a standard optical rod cathode, which differs from Example 1 in that: Cathode: A cylindrical optical rod cathode with a diameter of 25mm is adopted. It has no contoured curved surface, no fluid guiding structure, no through holes, guiding grooves and micro-pore arrays. It is a smooth cylindrical optical rod. The rest is the same as in Example 1.
[0088] The ellipsoidal superconducting cavity after electrochemical polishing was tested using the same method as in Example 1. The test results are as follows: The grain step height is 32μm (equatorial weld position); the cavity flatness (transition area from the equatorial to the non-equatorial ends) is ≥87μm, with over-removal in the bundle tube region and insufficient removal in the equatorial region; the 2K vertical test acceleration gradient is 18~21MV / m.
[0089] Combining the detection results of Examples 1-3 and Comparative Example 1, it can be seen that: Comparative Example 1 uses a traditional smooth cylindrical cathode, which lacks contoured curved surfaces and fluid guiding structures. During polishing, the gap between the cathode and the inner wall of the cavity varies significantly along the axial and circumferential directions, resulting in uneven electric field distribution. Electrolyte tends to stagnate and electrolysis products accumulate in the equatorial region. After polishing, the grain step height reaches as high as 32 μm, the cavity flatness deviation is large, the acceleration gradient is only 18~21 MV / m, and the polishing performance is poor.
[0090] Examples 1-3 all employ the conformal cathode with fluid-guiding structure of this invention. The cathode surface replicates the inner contour of the ellipsoidal superconducting cavity. Combined with the liquid-facing end guide channel and the micro-pore array combination flow-guiding structure in the remaining areas, a uniform and stable electric field and flow field can be constructed. This can effectively reduce the grain step height (14-17μm), improve the axial and circumferential polishing flatness of the cavity (cavity flatness, the transition area from the equator to the non-equator ends is ≤25μm), and significantly increase the 2K low-temperature acceleration gradient to 26-31MV / m. The polishing effect is significantly better than that of the traditional bare rod cathode scheme.
[0091] Example 1 selects the preferred process parameters within the parameter range of the present invention, which has the best synergistic effect of flow field and electric field, the lowest grain step height, the best cavity flatness, and the highest acceleration gradient in 2K vertical test (maximum 31MV / m). Examples 2 and 3 select the boundary conditions of the parameter range. The polishing performance is slightly lower than that of Example 1, but still far superior to the comparative example 1 of the prior art, proving that high-quality electrochemical polishing of ellipsoidal niobium superconducting cavity can be achieved within the parameter range of the present invention.
[0092] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A contour-following cathode, characterized in that, include: Includes: cathode shaft, electrode retaining ring, and conformal electrode; The contoured electrode is fixedly mounted on the cathode shaft by an electrode retainer; the curved surface of the contoured electrode replicates the inner curvature profile of the ellipsoidal superconducting cavity. The cathode shaft is used for electrical conduction and overall support and positioning, and the cathode shaft is coaxially arranged with the ellipsoidal superconducting cavity. A fluid guiding structure is provided on the surface of the conforming electrode along a line connecting one end of the short axis of the conforming electrode to the other end of the short axis of the conforming electrode, or a fluid guiding structure is provided along a line connecting one end of the long axis of the conforming electrode to the other end of the long axis of the conforming electrode. The fluid guiding structure is provided with through holes connecting the inside and outside of the conformal electrode, so that the electrolyte can flow in and out of the conformal electrode and optimize the flow field distribution in the cavity.
2. The conformal cathode according to claim 1, characterized in that, With the direction of electrolyte inflow perpendicular to the shaped cathode as the equatorial plane, and the two ends of the shaped cathode opposite to the equatorial plane as the south and north poles, the lines connecting the south and north poles on the surface of the shaped electrode where the fluid guiding structure is located are evenly arranged on the surface of the shaped electrode, dividing the surface of the shaped electrode into equal parts.
3. The conformal cathode according to claim 2, characterized in that, With the equatorial plane as the projection plane, the angle between any two adjacent lines connecting the North and South Poles is 18±5° on the projection plane.
4. The conformal cathode according to claim 1, characterized in that, The fluid guiding structure has a guiding groove as a through hole at one end of the conformal electrode facing the direction of electrolyte inflow, and a micropore array as through holes in the other directions.
5. The conformal cathode according to claim 4, characterized in that, The guide channel is an approximately rectangular long channel with a length-to-width ratio of 3 to 4:
1.
6. The conformal cathode according to claim 4, characterized in that, The micropore array is an array of circular pores of the same diameter, wherein the diameter of the micropores is 5±2mm.
7. A method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode, characterized in that, Using the conformal cathode according to any one of claims 1-6, comprising: S1. The conformal cathode is installed into the ellipsoidal superconducting cavity and coaxially aligned, so that the conformal cathode and the inner wall of the ellipsoidal superconducting cavity maintain a set polishing gap; the conformal cathode includes a cathode shaft, an electrode retaining ring and a conformal electrode, the conformal electrode surface replicates the curvature profile of the inner cavity of the ellipsoidal superconducting cavity, and the conformal electrode is provided with a fluid guiding structure, the fluid guiding structure including a through hole connecting the inside and outside of the conformal electrode. S2. Introduce electrolyte and establish electrolyte circulation; S3. Apply a voltage between the conformal cathode and the ellipsoidal superconducting cavity serving as the anode for electrochemical polishing; S4. After polishing is complete, disconnect the power, stop the electrolyte circulation, and remove the conformal cathode.
8. The method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode according to claim 7, characterized in that, In step S1, the contour electrode and the inner wall of the superconducting cavity maintain a polishing gap of 10-12 mm.
9. The method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode according to claim 7, characterized in that, In step S3, the polishing voltage is 10~20V, and / or the current density is 8~32mA / cm. 2, And / or, continue polishing for 100~160 minutes.
10. The method for electrochemical polishing of an ellipsoidal superconducting cavity using a contoured cathode according to claim 7, characterized in that, In step S2, the electrolyte flow rate is 2~12 L / min.