A long crystal pulling method of full-stack intelligent automation pulling method

By employing a full-stack intelligent automated Czochralski method, precise control of the lithium niobate crystal growth process was achieved, solving the problems of heat dissipation mismatch and abnormal thermal field, improving the stability and consistency of the crystal, and reducing the cracking rate and growth time.

CN123153152APending Publication Date: 2026-11-24JINGXIN NEW MATERIALS (ZHUJI) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611296701.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing Czochralski methods have difficulty achieving precise control over different axes and diameters in the growth of lithium niobate crystals, leading to crystal cracking, diameter fluctuations, batch inconsistencies, thermal stress problems caused by mismatched heat dissipation, and the inability of single-point temperature detection to provide real-time feedback on thermal field anomalies.

Method used

The full-stack intelligent automated pulling method is adopted. Through thermal matching between the seed crystal and the seed crystal rod, multi-point temperature detection and real-time control of meniscus image features, the axial temperature gradient of the solid-liquid interface is adjusted to form a closed-loop control, reducing reliance on human experience.

Benefits of technology

It improves the stability and repeatability of the crystal growth process, reduces the cracking rate, shortens the growth time, and enhances diameter consistency and batch pass rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153152A_ABST
    Figure CN123153152A_ABST
Patent Text Reader

Abstract

This application discloses a full-stack intelligent automated Czochralski method for crystal growth, belonging to the field of lithium niobate crystal growth technology. The method matches the seed crystal size, seed rod material, rod diameter, and contact heat exchange area according to the target crystal axis and diameter, creating initial undercooling at the seed crystal tip. After melting the raw material, the temperatures of the crucible, melt, solid-liquid interface, and post-heated region are obtained through a multi-point temperature measuring device, and the axial temperature gradient of the solid-liquid interface is adjusted according to the (0001), (10-14), or X-axis and the growth stage. Meniscus images are acquired and the contour height, width, symmetry, curvature, or brightness distribution is extracted, and control commands are generated by combining temperature, pulling rate, and crystal rotation rate. After the crystal reaches the target size, constant diameter growth, extraction, cooling, annealing, and single-domain processing are automatically completed. This application can improve shoulder stability and temperature field control accuracy, reduce cracking rate and diameter deviation, and realize unattended growth of multi-axial large-diameter lithium niobate crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of crystal material growth technology, specifically relating to a full-stack intelligent automated Czochralski method for crystal growth, and particularly to an intelligent automated Czochralski method for growing large-diameter lithium niobate crystals in the (0001) axis, (10-14) axis and X axis. Background Technology

[0002] Lithium niobate crystals possess excellent piezoelectric, ferroelectric, electro-optic, acousto-optic, and nonlinear optical properties, as well as chemical stability, a wide light transmittance range, and ease of processing. They have wide applications in surface acoustic wave devices, optical modulators, integrated optical devices, laser devices, and optoelectronic information processing. Simultaneously, with the development of communication devices and photonic integration technology, there are higher requirements for the diameter, crystal orientation adaptability, compositional uniformity, and batch consistency of lithium niobate crystals, especially the stable fabrication of large-diameter (0001), (10⁻¹⁴), and X-axis lithium niobate crystals. The Czochralski method is one of the commonly used methods for growing lithium niobate crystals, generally including: raw material melting, crystal pulling, necking, shoulder formation, constant-diameter growth, tailing, and annealing. In the traditional Czochralski growth process, the state of crystal pulling and shoulder formation is mainly controlled by the operator through observation of the melt surface and crystal shoulder morphology, adjusting the heating power, pulling rate, and crystal rotation rate based on their experience. This method is easily affected by the operator's experience, observation angle, and reaction speed, and cannot detect in time situations such as remelting, excessive protrusion, shoulder deviation, or local polycrystalline phenomena at the solid-liquid interface, which can lead to problems such as crystal cracking, diameter fluctuations, or even batch inconsistencies.

[0003] For lithium niobate crystals with different axes and diameters, the requirements for heat dissipation and solid-liquid interface morphology also vary. Current processes often use fixed seed crystal specifications, fixed seed crystal rods, or similar thermal field parameters, lacking a proper match between seed crystal size, seed crystal rod thermal conductivity, contact heat transfer area, and target crystal size. If the heat dissipation capacity of the seed crystal tip does not match the requirements for initial crystallization, it can easily lead to insufficient or excessive initial undercooling, resulting in unstable crystal growth, disordered shoulder enlargement, localized remelting, and even thermal stress cracking. Large-diameter crystals along the X-axis exhibit more significant anisotropy in radial heat dissipation, making them more prone to shoulder tilting, interface asymmetry, and inconsistent local growth rates during shoulder formation.

[0004] Furthermore, most existing Czochralski equipment uses single-point temperature detection or crystal weight feedback for measurement. Single-point temperature measurement cannot simultaneously reflect the temperature changes at the bottom of the crucible, the melt surface, the solid-liquid interface, and the post-heated region, nor can it obtain the actual axial temperature gradient near the solid-liquid interface. The control scheme proposed in CN101831692A mainly uses a weight sensor to provide feedback and adjust the crystal growth process. However, a single weight signal is an indirect feedback and cannot promptly reflect abnormal phenomena in the meniscus morphology and local thermal field. The control method proposed in CN118028966A combines simulation prediction and thermal imaging detection. However, the results of this control rely on virtual models and thermal imaging data, and it is still difficult to directly establish a coordinated control relationship between the seed crystal thermal conductivity matching, graded temperature gradient, and real-time meniscus characteristics of different axial lithium niobate crystals.

[0005] Therefore, it is necessary to provide an intelligent and automated method for growing large-diameter lithium niobate crystals with different axes. By establishing a thermal conductivity matching relationship between the seed crystal and the seed crystal rod according to the target axis and target diameter, an adjustable axial temperature gradient on the solid-liquid interface is generated during shoulder formation and constant diameter growth. This is combined with multi-point temperature detection and meniscus image features for real-time closed-loop control, reducing reliance on human experience and improving the automation level of the stability and repeatability of the crystal growth process. Summary of the Invention

[0006] To address the aforementioned deficiencies, this application provides the following technical solution: a full-stack intelligent automated Czochralski method for crystal growth, comprising the following steps: S1: Select the seed crystal and seed crystal rod according to the target axis and target diameter of the lithium niobate crystal to be grown, and make the seed crystal tip form a preset initial undercooling by adjusting the cross-sectional size of the seed crystal, the thermal conductivity of the seed crystal rod, the diameter of the seed crystal rod, and the contact heat exchange area between the seed crystal and the seed crystal rod. S2: After the lithium niobate raw material is batched, mixed, pressed and sintered, it is loaded into a crucible, heated to form a lithium niobate melt, and the temperature of the crucible, melt, solid-liquid interface and crystal growth environment is measured using a multi-point temperature measuring device. S3: Make the seed crystal contact with the lithium niobate melt, and control the pulling rate and crystal rotation rate under the preset initial supercooling to make the crystal shoulder face enlarged in an orderly manner; S4: Based on the target axis and crystal growth stage, adjust the axial temperature gradient at the solid-liquid interface by adjusting at least one of the crucible height, the shape of the back heater, and the size of the central opening of the back heat shield. S5: Acquire a solid-liquid interface meniscus image, extract at least two meniscus features from the meniscus image, and combine multi-point temperature data to generate control commands for at least one parameter among heating power, pulling rate, crystallization rate and axial temperature gradient. S6: After the crystal is shouldered to the target diameter, it is grown to the same diameter, and after the target length is reached, the crystal is extracted, cooled in a programmed manner, annealed and single-domained.

[0007] Furthermore, the target axis includes the (0001) direction, the (10-14) crystal plane normal direction, and the X-axis direction; the size of the seed crystal is selected from one of 4mm×4mm×40mm, 6mm×6mm×40mm, or 8mm×8mm×50mm; When the target diameter is no more than 100mm, a 4mm×4mm×40mm seed crystal is selected; when the target diameter is greater than 100mm and less than 150mm, a 6mm×6mm×40mm or 8mm×8mm×50mm seed crystal is selected according to the target axis and the required heat dissipation; when the target diameter is no less than 150mm, an 8mm×8mm×50mm seed crystal is selected. The diameter of the seed crystal rod is 8mm to 14mm; the preset initial undercooling degree is 5℃ to 15℃.

[0008] Furthermore, when growing crystals in the (0001) direction with a target diameter not greater than 125 mm, a seed crystal of 6 mm × 6 mm × 40 mm and a molybdenum seed crystal rod with a diameter of 8 mm are used, and the preset initial undercooling is 8 °C. When growing a crystal with a target diameter of 125 mm in the direction of the (10-14) crystal plane normal, an 8 mm × 8 mm × 50 mm seed crystal and a 12 mm diameter tungsten alloy seed crystal rod are used, and the preset initial undercooling is 12 °C. When growing a crystal with a target diameter of 150 mm along the X-axis, an 8 mm × 8 mm × 50 mm seed crystal and a 12 mm diameter tungsten alloy seed crystal rod are used, and the preset initial undercooling is 13 °C. When growing a crystal with a target diameter of 200 mm along the X-axis, an 8 mm × 8 mm × 50 mm seed crystal and a 14 mm diameter tungsten alloy seed crystal rod are used, and the preset initial undercooling is 14 °C.

[0009] Furthermore, the molar ratio of Nb₂O₅ to Li₂CO₃ in the lithium niobate raw material is 51.4:48.6, the crucible is a platinum crucible with a diameter of 180mm to 260mm, and the raw material is melted by single-stage or three-stage heating. When using single-stage heating, the heating rate is 3℃ / min to 7℃ / min, the melt temperature is maintained at a temperature 10℃ to 20℃ higher than the melting point of lithium niobate, and the holding time is 1h to 2h. When growing X-axis crystals with a target diameter of 200 mm and using a three-stage heating method, the heating was carried out at heating rates of 8℃ / min, 5℃ / min, and 2℃ / min, respectively, from room temperature to 1000℃, from 1000℃ to 1240℃, and from 1240℃ to 1265℃, and then held at 1265℃ for 3 hours.

[0010] Furthermore, the contact depth between the seed crystal and the lithium niobate melt is 0.8 mm to 1.0 mm; the pulling rate during the shoulder formation stage is 1.8 mm / h to 5 mm / h, and the crystal rotation speed is 5 r / min to 15 r / min; the pulling rate during the constant diameter growth stage is 1.8 mm / h to 3 mm / h, and the crystal rotation speed is 5 r / min to 10 r / min; the constant diameter growth length of the crystal is 50 mm to 80 mm, and the programmed cooling rate is 45℃ / h to 55℃ / h; When growing crystals with a target diameter of 200 mm along the X-axis, the crystal rotation speed during the shoulder formation stage is 3 r / min to 7 r / min, and the shoulder formation time is 4 h to 5 h.

[0011] Furthermore, during the shoulder formation stage, the axial temperature gradient at the solid-liquid interface is controlled according to the target axial direction as follows: When the target axis is in the (0001) direction, the axial temperature gradient is 28℃ / cm~32℃ / cm; The target axis is the normal direction of the (10-14) crystal plane, and the axial temperature gradient is 30℃ / cm~34℃ / cm; When the target axis is in the X-axis direction, the axial temperature gradient is 33℃ / cm~35℃ / cm; During the constant diameter growth stage of the crystal, the axial temperature gradient at the solid-liquid interface is 28℃ / cm~30℃ / cm. The axial temperature gradient is adjusted by adjusting at least one of the following: crucible height, afterheater shape, and the size of the central opening of the afterheating cover. The crucible is raised by 5 mm to 10 mm, the afterheater is a cylindrical or conical afterheater, and the diameter of the central opening of the afterheating cover is 35 mm to 80 mm.

[0012] Furthermore, the multi-point temperature measuring device includes: The first temperature measuring point is located on the outer wall of the bottom of the crucible and 10mm to 15mm from the bottom of the crucible. The second temperature measuring point is located 5mm to 10mm below the surface of the melt and 30mm to 50mm from the outer crucible wall; A third temperature measuring point located 5mm to 15mm below the solid-liquid interface and 25mm to 35mm away from the second temperature measuring point; and The fourth temperature measuring point is located on the inner side of the top of the rear heat shield and 80mm to 120mm above the crystal shoulder surface; The temperature acquisition frequency of each temperature measuring point is 1Hz to 5Hz. The temperature difference between the second and third temperature measuring points is used to determine the axial temperature gradient, and the temperature control accuracy is ±0.1℃.

[0013] Furthermore, the acquisition frequency of the meniscus image is 10 frames / second to 30 frames / second; the meniscus features include at least three of the following: edge position, contour height, width, symmetry, curvature, and brightness distribution. When the meniscus profile height is higher than the set value, reduce the heating power by 1% to 3% and increase the pulling rate by 0.2 mm / h to 0.5 mm / h; when the meniscus profile height is lower than the set value, increase the heating power by 1% to 3% and reduce the pulling rate by 0.2 mm / h to 0.5 mm / h; when the meniscus is asymmetrical, adjust the crystal bias position or adjust the crystal rotation rate by ±2 r / min; when the meniscus fluctuates, reduce the pulling rate by 0.3 mm / h and increase the crystal rotation rate by 1 r / min to 2 r / min. The accuracy of meniscus feature recognition is no less than 98%, and the control response time is no more than 0.5s.

[0014] Furthermore, when growing a crystal with a target diameter of 150 mm along the X-axis, the surface roughness Ra of the contact surface between the seed crystal and the seed crystal rod is no greater than 0.4 μm, the contact pressure is 1.2 MPa, the diameter of the platinum crucible is 220 mm, the back heat sink is a conical back heat sink with a 60° apex angle, the diameter of the central opening of the back heat shield is 40 mm, the axial temperature gradient during the shoulder formation stage is 34 °C / cm, the axial temperature gradient during the constant diameter growth stage is 28 °C / cm, and the programmed cooling rate is 50 °C / h. When growing a crystal with a target diameter of 200 mm along the X-axis, a 5 μm thick electroless nickel plating layer is applied to the end face of the seed crystal. The diameter of the platinum crucible is 260 mm. A double backheater consisting of a main backheater and a secondary backheater is used. The diameter of the central opening of the backheater is 35 mm. A fifth temperature measuring point is added in the middle of the backheater. The axial temperature gradient during the shoulder formation stage is 34 °C / cm, and the axial temperature gradient during the constant diameter growth stage is 30 °C / cm. The programmed cooling rate is 45 °C / h, and the annealing time is 12 h.

[0015] Furthermore, the diameter of the prepared lithium niobate crystal is not less than 100 mm, wherein the maximum diameter of the (0001) direction crystal and the (10-14) crystal plane normal direction crystal is 150 mm, and the maximum diameter of the X-axis direction crystal is 200 mm; the diameter deviation of the lithium niobate crystal is not greater than ±0.1 mm, the meniscus feature recognition accuracy is not less than 98%, the control response time is not greater than 0.5 s, and the crystal qualification rate is not less than 95%.

[0016] This application has the following beneficial effects: 1. This application, based on the target crystal axis and target diameter, coordinates the seed crystal cross-sectional dimensions, seed crystal rod material, seed crystal rod diameter, and the contact heat transfer area between the seed crystal and the seed crystal rod to achieve an initial undercooling of 5°C to 15°C at the seed crystal tip. This method avoids the mismatch in heat dissipation capacity caused by traditional fixed seed crystal and seed crystal rod configurations, resulting in a more stable initial crystallization state and promoting orderly shoulder enlargement. The verification results provided in the disclosure show that, after adopting the above matching method, the shoulder cracking rate can be reduced from 25%–30% to no more than 3%, and the shoulder formation time is shortened by 20%–35%.

[0017] 2. This application controls the axial temperature gradient at the solid-liquid interface according to the crystal axis and the growth stage, and changes the thermal field distribution by adjusting one or more of the following: crucible height, rear heat sink shape, and the size of the central opening of the rear heat shield. Among them, the (0001) axis, (10-14) axis, and X axis can each adopt a temperature gradient adapted to their interface stability requirements. The X-axis crystal can also implement gradient switching during the shoulder formation stage and the constant diameter growth stage, thereby suppressing excessive solid-liquid interface protrusion, local remelting, and shoulder deviation, and improving the process adaptability of crystals with different axes.

[0018] 3. This application utilizes temperature measurement points T1 to T4 to obtain temperature information at the bottom of the crucible, near the melt surface, near the solid-liquid interface, and in the post-heating region, respectively. The axial temperature gradient near the solid-liquid interface is determined based on the temperature difference and axial distance between T2 and T3. This enables zoned monitoring and closed-loop control of the heating zone, melt zone, solid-liquid interface zone, and crystal growth environment zone, overcoming the problem that single-point temperature measurement cannot reflect changes in the axial temperature field. Verification results show that temperature field fluctuations can converge from ±2.0℃ to within ±0.3℃, and the axial temperature gradient control deviation can converge to ±0.5℃ / cm.

[0019] 4. This application uses a high-definition camera to capture images of the meniscus at the solid-liquid interface and extracts features such as contour height, width, symmetry, curvature, and brightness distribution. Combined with multi-point temperature data, pulling rate, and crystal rotation rate, the crystal growth state is determined. When the meniscus is too high, too low, asymmetrical, or exhibits abnormal fluctuations, the control device can promptly adjust the heating power, pulling rate, crystal rotation rate, or crystal offset position. This transforms the controlled object from a traditional indirect weight signal to the actual morphology of the solid-liquid interface, improving the timeliness of abnormal state identification and the targeted nature of control.

[0020] 5. This application integrates thermal conductivity matching between the seed crystal and seed crystal rod, graded temperature gradients, multi-point temperature detection, and meniscus feature recognition for coordinated control, enabling a continuous closed loop for crystal introduction, shoulder formation, constant-diameter growth, and automatic tailing. The meniscus feature recognition accuracy can reach over 98%, and the control response time is no more than 0.5s. This significantly shortens the adjustment delay compared to manual observation and reduces the number of manual interventions during the growth process to 0 per furnace, which is beneficial for improving the automation level of the crystal growth process and the repeatability between different furnaces.

[0021] 6. This application is applicable to the growth of lithium niobate crystals along the (0001) axis, (10-14) axis, and X-axis, and can extend the target diameter of X-axis crystals to 200 mm. Crystals obtained using the method of this application are free from obvious cracks, polycrystalline, twinned, or inclusions, and the diameter deviation can be controlled within ±0.1 mm. The crystal yield is not less than 95%, and the growth cycle can be shortened by 10% to 20%. Therefore, it has good adaptability to large sizes, batch stability, and industrial application value. Attached Figure Description

[0022] The present application will be described in more detail below based on embodiments and with reference to the accompanying drawings. Wherein: Figure 1 A schematic flowchart of the crystal growth method of the full-stack intelligent automated Czochralski method provided in this application; Figure 2 A bar chart comparing the shoulder cracking rate of different seed crystal-seed rod matching methods in different test groups in Test Example 1; Figure 3 This is a comparison of the temperature gradient deviation curves between the multi-point closed-loop and control methods in different test groups in Test Example 2; Figure 4 This is a comparison chart of the recovery curves of the meniscus height deviation after standard disturbance in different test groups in Test Example 3; Figure 5 This is a photograph of the physical sample obtained from testing the 6-inch (150 mm) lithium niobate crystal along the X-axis using the crystal growth method in Example 7, as shown in Test Example 4. Figure 6 This is a photograph of the 8-inch (200 mm) lithium niobate crystal obtained by the crystal growth method in Example 9, as shown in Test Example 4. Figure 7 This is a comparison of the changes in the X-axis crystal radial resistivity uniformity curves for different test groups in Test Example 4. Detailed Implementation

[0023] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0024] like Figure 1 As shown, the intelligent automated crystal pulling method of this application is performed sequentially in the order of seed crystal matching, melt preparation, shoulder growth, thermal field adjustment, interface feedback, and automatic termination. First, in step S1, the combination of the seed crystal and seed rod is determined according to the axial direction and diameter of the target lithium niobate crystal. By coordinating factors such as the cross-sectional size of the seed crystal, the material and diameter of the seed rod, and the contact heat exchange area between the two, the seed crystal tip obtains an initial undercooling adapted to the initial crystallization requirements. Subsequently, in step S2, raw material preparation, pressing, sintering, and melting are completed, and temperature information of the crucible, melt, near the solid-liquid interface, and crystal growth environment is obtained using a multi-point temperature measuring device. Step S3 utilizes the aforementioned initial undercooling to establish stable crystal pulling conditions, and the shoulder surface is gradually and uniformly enlarged by coordinating the pulling rate and crystal rotation rate. In step S4, based on the crystal axial direction and the thermal field requirements of the shoulder or constant diameter growth stage, the relative height of the crucible, the structure of the rear heat exchanger, or the opening of the rear heat shield are adjusted to form a suitable axial temperature gradient at the solid-liquid interface. Step S5 further acquires images of the solid-liquid interface meniscus, fuses and analyzes the meniscus features with multi-point temperature data, and outputs control commands for heating power, pulling rate, crystal rotation rate, or temperature gradient accordingly, thereby implementing real-time closed-loop correction of the crystal growth state. Finally, in step S6, after the crystal shoulder expands to the target diameter, it transitions to constant-diameter growth, and automatically completes extraction, programmed cooling, annealing, and single-domain processing after reaching the predetermined length, thus realizing continuous automated growth of large-diameter lithium niobate crystals with different axes from crystal initiation to completion.

[0025] The term "(10-14) axis" as used in this application refers to the target growth axis of the lithium niobate crystal with the normal direction of the (10-14) crystal plane as the reference direction; in standard crystallographic notation, this crystal plane can also be written as ( The horizontal line is positioned only above the third exponent "1", indicating that the exponent is negative one. Therefore, "(10-14)" and "( The terms (0001), (10-14), and X-axis used in this application refer to the target growth direction of the lithium niobate seed crystal and the resulting crystal during the Czochralski growth process, unless otherwise specified.

[0026] The fully automated intelligent Czochralski crystal growth method described in this application refers to a Czochralski crystal growth method that involves continuous and coordinated control of the following processes: thermal matching between the seed crystal and the seed crystal rod, melting of lithium niobate raw material, ordered shoulder formation, axial temperature gradient adjustment at the solid-liquid interface, multi-point temperature monitoring, meniscus image recognition, closed-loop control of growth parameters, constant diameter growth, and automatic tailing. In the technical solution of this application, the fully automated intelligent Czochralski crystal growth method is specifically applied to the growth of large-diameter lithium niobate crystals with different axes, including the (0001) axis, the (10-14) axis, and the X axis. The large-diameter lithium niobate crystals include those with a target diameter of not less than 100 mm. Therefore, the fully automated intelligent Czochralski crystal growth method described in this application can also be understood as an intelligent automated Czochralski crystal growth method for large-diameter lithium niobate crystals with different axes. The term "full stack" indicates that the automated control of this application spans the entire process of seed selection and thermal matching, melt preparation, crystal shoulder formation, thermal field adjustment, interface state identification, constant diameter growth, and crystal finishing, rather than implementing local feedback control only for heating power, crystal weight, or a single temperature parameter; "intelligent automation" refers to the control device performing closed-loop adjustment of at least one of the heating power, pulling rate, crystal rotation rate, and axial temperature gradient based on multi-point temperature data and the characteristics of the solid-liquid interface meniscus.

[0027] In this application, T1, T2, T3, and T4 are not specific temperature values, but rather numbers indicating different temperature measurement locations of multiple temperature measuring devices: T1 is the first measuring point, measured near the outer wall of the crucible bottom, used to detect the stability of the heat source at the bottom of the crucible and in the heating zone to determine whether there are abnormal fluctuations in the input heat; T2 is the second measuring point, measured below the melt surface, used to obtain the actual temperature of the melt near the liquid surface and as a basis for judging the undercooling state of the seed crystal tip and the temperature change of the melt; T3 is the third measuring point, measured downwards at the solid-liquid interface, the results collected at this measuring point can more intuitively reflect the temperature change near the crystal growth interface and, together with T2, participate in the process of determining the axial temperature gradient of the solid-liquid interface; T4 is the fourth measuring point, measured on the inner side of the top of the rear heat shield and above the crystal shoulder, used to monitor the growth environment temperature and the thermal stability of the rear heat region after the crystal leaves the solid-liquid interface. Specifically, the axial temperature gradient near the solid-liquid interface can be determined based on the temperature difference between T2 and T3 and the axial distance between the two temperature measuring points. Meanwhile, the data collected by T1 represents the heating state at the bottom of the crucible, while the data collected by T4 represents the environmental stability of the crystal shoulder and the post-heated region.

[0028] Specifically, the control device can determine the axial temperature gradient near the solid-liquid interface based on the temperature difference between T2 and T3 and the axial distance between the two temperature measuring points. Simultaneously, the temperature data collected at T1 is used to characterize the heating state at the bottom of the crucible, and the temperature data collected at T4 is used to characterize the environmental stability of the crystal shoulder and the post-heated region. Thus, the multi-point temperature measuring device can acquire temperature information from the heating zone, the melt zone, the solid-liquid interface zone, and the crystal growth environment zone, enabling the intelligent temperature control module to not only adjust based on a single temperature value but also to implement coordinated closed-loop control of the heating power and thermal field structure based on the temperature change relationships between different regions.

[0029] The "initial undercooling" described in this application refers to the temperature difference at the seed crystal tip when it comes into contact with the melt and begins crystal growth, corresponding to the stable initial crystallization. This initial undercooling is not obtained solely by changing the melt temperature, but rather by matching the seed crystal cross-sectional dimensions, seed crystal rod material and thermal conductivity, seed crystal rod diameter, and the contact heat transfer area between the seed crystal and the seed crystal rod according to the target crystal axis and target diameter, so that the heat dissipation capacity of the seed crystal tip is adapted to the initial growth requirements of the target crystal. The axial temperature gradient refers to the rate of temperature change formed near the solid-liquid interface along the crystal pulling direction. It can be adjusted by one or more of the following: crucible height, back heater shape, back heat shield center opening size, and corresponding heating conditions, and is set separately according to the thermal field requirements of different crystal axes and shoulder formation and constant diameter growth stages.

[0030] During crystal growth, a high-definition camera is used to continuously acquire images of the meniscus at the solid-liquid interface. Control software identifies at least some features from these images, including the meniscus edge position, contour height, width, symmetry, curvature, and brightness distribution. These meniscus features reflect the instantaneous crystal diameter, interface morphology, shoulder symmetry, and temperature distribution. The control device can comprehensively analyze these features along with temperature data (T1–T4), pulling rate, and crystal rotation rate, and adjust the heating power, pulling rate, crystal rotation rate, or axial temperature gradient accordingly. This forms a closed-loop control process consisting of thermal field monitoring, interface identification, state judgment, and parameter execution.

[0031] T1 to T4 constitute the basic temperature measurement points of the multi-point temperature measurement device of this application. When growing lithium niobate crystals with an X-axis diameter of 200 mm, a temperature measurement point T5 can be added in the middle of the afterheater to further obtain temperature information in the middle of the afterheater and characterize the details of the axial temperature distribution during the growth of large-diameter crystals. T5 is an auxiliary temperature measurement point added for specific large-size crystal growth conditions. Its setting does not change the basic functions of T1 to T4 in monitoring the heating zone, melt zone, solid-liquid interface zone and crystal growth environment zone, respectively.

[0032] Example 1

[0033] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an axial diameter of 100 mm (0001), specifically including the following steps S1-S6: S1: Select a 4 mm × 4 mm × 40 mm seed crystal with (0001) orientation and use a molybdenum seed crystal rod with a diameter of φ8 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial subcooling of 5℃ is formed at the tip of the seed crystal.

[0034] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, and after mixing, pressing and sintering, they are loaded into a platinum crucible. A φ180 mm platinum crucible is used, and the temperature is increased at 3℃ / min to stabilize the melt temperature at 10℃ above the melting point and held for 1.0 h.

[0035] S3: Insert the seed crystal into the melt by 0.8 mm and perform shoulder formation at a pulling rate of 2.0 mm / h and a crystal rotation rate of 8 r / min.

[0036] S4: Adjust the crucible, rear heat exchanger, and rear heat shield axially to achieve an axial temperature gradient of 28℃ / cm during the shoulder formation stage and a constant diameter stage. Adjust the center opening of the rear heat shield from φ80 mm to φ60 mm; T2 is located 5 mm below the liquid surface, and T3 is located 5 mm below the solid-liquid interface, with a distance of 25 mm between them. Raise the crucible by 5 mm relative to its initial position, and adjust the center opening of the rear heat shield accordingly to achieve an axial temperature gradient of 28℃ / cm during the shoulder formation stage.

[0037] S5: Temperature is collected at 1 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 10 frames / second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 98.0% and an AI control response time of 0.5 s.

[0038] S6: After the crystal reaches the target diameter, it is pulled at 2.0 mm / h and rotated at 8 r / min. After growing to 50 mm, it is automatically removed, cooled at 55℃ / h, and then annealed and single-domain treated.

[0039] The test results of the lithium niobate crystal with an axial diameter of 100 mm obtained in this embodiment show that the crystal shoulder is continuous, without macroscopic cracks or polymorphism; the diameter deviation is ±0.10 mm, and the single furnace pass rate is 95.1%.

[0040] Example 2

[0041] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an axial diameter of 125 mm (0001), specifically including the following steps S1-S6: S1: Select a 6 mm × 6 mm × 40 mm seed crystal with (0001) orientation and use a molybdenum seed crystal rod with a diameter of φ8 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial subcooling of 8℃ is formed at the tip of the seed crystal.

[0042] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, and after mixing, pressing and sintering, they are loaded into a platinum crucible. A φ200 mm platinum crucible is used, and the temperature is increased at 5 ℃ / min to stabilize the melt temperature at 15 ℃ above the melting point and held for 1.5 h.

[0043] S3: Insert the seed crystal into the melt by 0.9 mm and perform shoulder formation at a pulling rate of 3.5 mm / h and a crystal rotation rate of 12 r / min.

[0044] S4: Adjust the crucible, rear heater, and rear heat shield according to the aforementioned axial adjustment to achieve an axial temperature gradient of 30℃ / cm during the shoulder-forming stage and 29℃ / cm during the constant-diameter stage. Adjust the center opening of the rear heat shield from φ80 mm to φ50 mm; T2 is located 8 mm below the liquid surface, and T3 is located 10 mm below the solid-liquid interface, with a distance of 30 mm between them.

[0045] S5: Temperature is collected at 3 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 20 frames per second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 98.5% and an AI control response time of 0.4 s.

[0046] S6: After the crystal reaches the target diameter, it is pulled at 2.5 mm / h and rotated at 9 r / min. After growing to 65 mm, it is automatically removed, cooled at 50℃ / h, and then annealed and single-domain treated.

[0047] Results: The crystals were free of cracks and polymorphism, with a diameter deviation of no more than ±0.08 mm, and the single-furnace pass rate was 96.0%.

[0048] Example 3

[0049] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an axial diameter of 150 mm (0001), specifically including the following steps S1-S6: S1: Select an 8 mm × 8 mm × 50 mm seed crystal with (0001) orientation and use a molybdenum seed crystal rod with a diameter of φ10 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial undercooling of 15℃ is formed at the tip of the seed crystal.

[0050] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, pressed into blocks and sintered, and then loaded into a platinum crucible. A φ220 mm platinum crucible is used, and the temperature is increased at 7 ℃ / min to stabilize the melt temperature at 20℃ above the melting point and held for 2.0 h.

[0051] S3: Insert the seed crystal into the melt by 1.0 mm and perform shoulder formation at a pulling rate of 5.0 mm / h and a crystal rotation rate of 5 r / min.

[0052] S4: Adjust the crucible, afterheater, and afterheating cover axially to achieve an axial temperature gradient of 32℃ / cm during the shoulder-forming stage and 30℃ / cm during the constant-diameter stage. Raise the crucible by 10 mm and use a conical afterheater; T2 is located 10 mm below the liquid surface, and T3 is located 15 mm below the solid-liquid interface, with a distance of 35 mm between them.

[0053] S5: Temperature is collected at 5 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 30 frames per second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 99.0% and an AI control response time of 0.3 s.

[0054] S6: After the crystal reaches the target diameter, it is pulled at 3.0 mm / h and rotated at 10 r / min. After growing to 80 mm, it is automatically removed, cooled at 45℃ / h, and then annealed and single-domain treated.

[0055] The test results of the lithium niobate crystal with an axial diameter of 150 mm obtained in this embodiment show that the shoulder morphology of the lithium niobate crystal in this embodiment is complete, the diameter deviation is ±0.09 mm, and the single furnace pass rate is 95.3%.

[0056] Example 4

[0057] This embodiment provides a smart and automated method for growing lithium niobate crystals with an axial diameter of 100 mm (10-14), specifically including the following steps S1-S6: S1: Select a 4 mm × 4 mm × 40 mm seed crystal with (10-14) orientation and use a tungsten alloy seed crystal rod with a diameter of φ10 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial undercooling of 10℃ is formed at the tip of the seed crystal.

[0058] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, and after mixing, pressing and sintering, they are loaded into a platinum crucible. A φ180 mm platinum crucible is used, and the temperature is increased at 3 ℃ / min to stabilize the melt temperature at 10 ℃ above the melting point and held for 1.0 h.

[0059] S3: Insert the seed crystal into the melt by 0.8 mm and perform shoulder formation at a pulling rate of 2.0 mm / h and a crystal rotation rate of 8 r / min.

[0060] S4: Adjust the crucible, afterheater, and afterheating cover according to the aforementioned axial adjustment to achieve an axial temperature gradient of 30℃ / cm during the shoulder-forming stage and 29℃ / cm during the constant-diameter stage. A cylindrical afterheater is used, with a central opening of φ60 mm in the afterheating cover; the distance between T2 and T3 is 25 mm.

[0061] S5: Temperature is collected at 1 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 10 frames / second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 98.0% and an AI control response time of 0.5 s.

[0062] S6: After the crystal reaches the target diameter, it is pulled at 2.0 mm / h and rotated at 8 r / min. After growing to 50 mm, it is automatically removed, cooled at 55℃ / h, and then annealed and single-domain treated.

[0063] The test results of the lithium niobate crystals (10-14) with an axial diameter of 100 mm obtained in this embodiment showed that the crystal shoulders were flat, with no cracks or polymorphism, the diameter deviation was ±0.10 mm, and the single-furnace pass rate was 95.0%.

[0064] Example 5

[0065] This embodiment provides a smart and automated method for growing lithium niobate crystals with an axial diameter of 125 mm (10-14), specifically including the following steps S1-S6: S1: Select an 8 mm × 8 mm × 50 mm seed crystal with (10-14) orientation and use a tungsten alloy seed crystal rod with a diameter of φ12 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial undercooling of 12℃ is formed at the tip of the seed crystal.

[0066] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, pressed into blocks and sintered, and then loaded into a platinum crucible. A φ200 mm platinum crucible is used, and the temperature is increased at 6 ℃ / min to stabilize the melt temperature at 15℃ above the melting point and held for 2.0 h.

[0067] S3: Insert the seed crystal into the melt by 1.0 mm and perform shoulder formation at a pulling rate of 2.5 mm / h and a crystal rotation rate of 10 r / min.

[0068] S4: Adjust the crucible, afterheater, and afterheating cover axially to achieve an axial temperature gradient of 32℃ / cm during the shoulder-forming stage and 30℃ / cm during the constant-diameter stage. Raise the crucible by 6 mm and change the afterheater from a cylindrical shape to a conical shape; T2 is located 8 mm below the liquid surface, and T3 is located 10 mm below the solid-liquid interface.

[0069] S5: Temperature is collected at 5 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 30 frames per second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 98.7% and an AI control response time of 0.35 s.

[0070] S6: After the crystal reaches the target diameter, it is pulled at 2.0 mm / h and rotated at 8 r / min. After growing to 80 mm, it is automatically removed, cooled at 50℃ / h, and then annealed and single-domain treated.

[0071] The test results of the lithium niobate crystals with an axial diameter of 125 mm obtained in this embodiment (10-14) show that the solid-liquid interface of the lithium niobate crystals in this embodiment is flat, the crystal uniformity is good, the diameter deviation is ±0.09 mm, and the single furnace pass rate is 95.5%.

[0072] Example 6

[0073] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an axial diameter of 150 mm (10-14), specifically including the following steps S1-S6: S1: Select an 8 mm × 8 mm × 50 mm seed crystal with (10-14) orientation and use a tungsten alloy seed crystal rod with a diameter of φ12 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial undercooling of 15℃ is formed at the tip of the seed crystal.

[0074] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, pressed into blocks and sintered, and then loaded into a platinum crucible. A φ220 mm platinum crucible is used, and the temperature is increased at 7 ℃ / min to stabilize the melt temperature at 20℃ above the melting point and held for 2.0 h.

[0075] S3: Insert the seed crystal into the melt by 1.0 mm and perform shoulder formation at a pulling rate of 5.0 mm / h and a crystal rotation rate of 15 r / min.

[0076] S4: Adjust the crucible, afterheater, and afterheating cover axially to achieve an axial temperature gradient of 34℃ / cm during the shoulder-forming stage and 30℃ / cm during the constant-diameter stage. Use a conical afterheater and reduce the central opening of the afterheating cover to φ40mm; the distance between T2 and T3 is 35mm.

[0077] S5: Temperature is collected at 5 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 30 frames per second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 99.0% and an AI control response time of 0.25 s.

[0078] S6: After the crystal reaches the target diameter, it is pulled at 3.0 mm / h and rotated at 6 r / min. After growing to 80 mm, it is automatically removed, cooled at 45℃ / h, and then annealed and single-domain treated.

[0079] The test results of the lithium niobate crystals with an axial diameter of 150 mm obtained in this embodiment (10-14) showed that the crystals had no macroscopic defects, the diameter deviation was ±0.10 mm, and the single-furnace pass rate was 95.4%.

[0080] Example 7

[0081] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an X-axis diameter of 150 mm, specifically including the following steps S1-S6: S1: Select an 8 mm × 8 mm × 50 mm seed crystal with X-axis orientation and use a tungsten alloy seed crystal rod with a diameter of φ12 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial undercooling of 13℃ is formed at the tip of the seed crystal.

[0082] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, pressed into blocks and sintered, and then loaded into a platinum crucible. A φ220 mm platinum crucible is used, and the temperature is increased at 6 ℃ / min to stabilize the melt temperature at 15℃ above the melting point and held for 2.0 h.

[0083] S3: Insert the seed crystal into the melt by 1.0 mm and perform shoulder formation at a pulling rate of 2.0 mm / h and a crystal rotation rate of 10 r / min.

[0084] S4: Adjust the crucible, back heater, and back heat shield according to the aforementioned axial adjustment to achieve an axial temperature gradient of 34℃ / cm during the shoulder formation stage and 28℃ / cm during the constant diameter stage. Polish the contact surface between the seed crystal and the seed crystal rod to Ra≤0.4 μm, with a contact pressure of 1.2 MPa; the apex angle of the tapered back heater is 60°, and the center opening of the back heat shield is φ40 mm.

[0085] S5: Temperature is collected at 5 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 30 frames per second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 98.9% and an AI control response time of 0.3 s.

[0086] S6: After the crystal reaches the target diameter, it is pulled at 2.0 mm / h and rotated at 8 r / min. After growing to 80 mm, it is automatically removed, cooled at 50℃ / h, and then annealed and single-domain treated.

[0087] The test results of the lithium niobate crystal with an X-axis diameter of 150 mm obtained in this embodiment showed that the obtained crystal was colorless and transparent, without cracks or polymorphism, with a diameter deviation of ≤ ±0.10 mm and a pass rate of 95.8%.

[0088] Example 8

[0089] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an X-axis diameter of 175 mm, specifically including the following steps S1-S6: S1: Select an 8 mm × 8 mm × 50 mm seed crystal with X-axis orientation and a tungsten alloy seed crystal rod with a diameter of φ13 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial undercooling of 14℃ is formed at the tip of the seed crystal.

[0090] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, and after mixing, pressing and sintering, they are loaded into a platinum crucible. A φ240 mm platinum crucible is used, and the temperature is increased at 5 ℃ / min to stabilize the melt temperature at 15 ℃ above the melting point and held for 2.0 h.

[0091] S3: Insert the seed crystal into the melt by 0.9 mm and perform shoulder formation at a pulling rate of 3.5 mm / h and a crystal rotation rate of 12 r / min.

[0092] S4: Adjust the crucible, rear heat exchanger, and rear heat shield according to the aforementioned axial adjustment to achieve an axial temperature gradient of 33℃ / cm during the shoulder formation stage and 29℃ / cm during the constant diameter stage. A combination of a main rear heat exchanger and an auxiliary heat exchanger ring is used, with a φ38 mm central opening in the rear heat shield. When the shoulder asymmetry reaches 3%, adjust the crystal offset by ±1 mm.

[0093] S5: Temperature is collected at 3 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 20 frames / second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 99.0% and an AI control response time of 0.35 s.

[0094] S6: After the crystal reaches the target diameter, it is pulled at 2.5 mm / h and rotated at 6 r / min. After growing to 70 mm, it is automatically removed, cooled at 50℃ / h, and then annealed and single-domain treated.

[0095] The test results of the lithium niobate crystal with an X-axis diameter of 175 mm obtained in this embodiment showed that the crystal shoulder was continuous, no polycrystalline structures were observed, the diameter deviation was ±0.09 mm, and the single-furnace pass rate was 95.6%.

[0096] Example 9

[0097] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an X-axis diameter of 200 mm, specifically including the following steps S1-S6: S1: An 8mm×8mm×50mm lithium niobate seed crystal with X-axis orientation is selected, and a tungsten alloy seed crystal rod with a diameter of φ14mm is used. The contact end face between the seed crystal and the seed crystal rod is processed, and a 5μm thick electroless nickel plating layer is set on the seed crystal end face. By controlling the cross-sectional size of the seed crystal, the thermal conductivity of the seed crystal rod, the diameter of the seed crystal rod, and the contact heat transfer state between the two, an initial undercooling of 14℃ is formed at the tip of the seed crystal.

[0098] S2: Nb2O5 and Li2CO3 were mixed in a molar ratio of 51.4:48.6, and after thorough mixing, pressing, and sintering, the mixture was placed into a platinum crucible with a diameter of φ260mm. The heating process adopted a three-stage heating regime: the heating rate from room temperature to 1000℃ was 8℃ / min, the heating rate from 1000℃ to 1240℃ was 5℃ / min, and the heating rate from 1240℃ to 1265℃ was 2℃ / min. After heating to 1265℃, the temperature was held for 3 hours to allow the raw materials to fully melt and form a uniform and stable lithium niobate melt.

[0099] S3: The seed crystal is moved downwards and inserted into the lithium niobate melt by 1.0 mm. Under the condition of initial supercooling at 14℃, crystal pulling and shoulder formation are carried out at a pulling rate of 1.8 mm / h and a crystal rotation rate of 5 r / min. During the shoulder formation process, the shoulder profile and solid-liquid interface state are continuously monitored, and the shoulder is controlled to be uniformly enlarged from the end of the seed crystal outwards. The shoulder formation time is 4.5 h.

[0100] S4: A dual afterheater consisting of a main afterheater and a secondary afterheater is adopted. The diameter of the central opening of the afterheating shroud is φ35mm, and a fifth temperature measuring point T5 is set in the middle of the afterheater. The first temperature measuring point T1 is set on the outer wall of the bottom of the crucible, 12.5mm from the bottom surface of the crucible; the second temperature measuring point T2 is set 8mm below the melt surface and 40mm from the inner wall of the crucible; the third temperature measuring point T3 is set 10mm below the solid-liquid interface, and the axial distance between T2 and T3 is 30mm; the fourth temperature measuring point T4 is set on the inner side of the top of the afterheating shroud, 100mm above the crystal shoulder. The axial temperature gradient near the solid-liquid interface is calculated based on the temperature difference between T2 and T3. The axial temperature gradient during the shoulder formation stage is controlled at 34℃ / cm, and the axial temperature gradient during the constant diameter growth stage is controlled at 30℃ / cm. The temperature acquisition frequency of each measuring point is 5Hz, and the temperature control accuracy is ±0.1℃.

[0101] S5: A high-definition camera continuously acquires images of the meniscus at the solid-liquid interface at a frequency of 30 frames per second, and identifies the edge position, contour height, width, symmetry, curvature, and brightness distribution of the meniscus from these images. When the meniscus contour height is higher than a set value, the heating power is reduced by 2%, and the lifting rate is increased by 0.35 mm / h; when the meniscus contour height is lower than the set value, the heating power is increased by 2%, and the lifting rate is reduced by 0.35 mm / h; when the meniscus experiences continuous fluctuations, the lifting rate is reduced by 0.3 mm / h, and the crystal rotation rate is increased by 1.5 r / min. The control software has a meniscus feature recognition accuracy of 99.1%, and the response time from anomaly identification to control command output is 0.25 s.

[0102] S6: After the crystal shoulder is enlarged to a target diameter of 200mm, it enters the constant diameter growth stage. It continues to grow at a pulling rate of 1.8mm / h and a crystal rotation rate of 8r / min. After the constant diameter section reaches a growth length of 60mm, the crystal is automatically extracted. Then, it is cooled at a programmed cooling rate of 45℃ / h, annealed for 12h, and single-domain treatment is completed.

[0103] The results showed that the obtained X-axis lithium niobate crystals were colorless and transparent, with no macroscopic cracks, polycrystalline structures, obvious twins or inclusions, and the crystal diameter deviation was no greater than ±0.10 mm. The relative standard deviation of the radial resistivity was no greater than 2.5%, and the crystal qualification rate was 95.2%.

[0104] Example 10

[0105] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an X-axis length of 200 mm, specifically including the following steps S1-S6: S1: Select an 8 mm × 8 mm × 50 mm seed crystal with X-axis orientation and a tungsten alloy seed crystal rod with a diameter of φ14 mm; by controlling the contact heat transfer state between the seed crystal and the seed crystal rod, an initial undercooling of 15°C is formed at the tip of the seed crystal.

[0106] S2: Nb2O5 and Li2CO3 are mixed in a molar ratio of 51.4:48.6, and after mixing, pressing and sintering, they are loaded into a platinum crucible. A φ260 mm platinum crucible is used, and the temperature is increased at 7 ℃ / min to stabilize the melt temperature at 20℃ above the melting point and held for 2.0 h.

[0107] S3: Insert the seed crystal into the melt by 1.0 mm and perform shoulder formation at a pulling rate of 5.0 mm / h and a crystal rotation rate of 7 r / min.

[0108] S4: Adjust the crucible, afterheater, and afterheating cover according to the aforementioned axial adjustment to ensure that the axial temperature gradient is 35℃ / cm during the shoulder-forming stage and 30℃ / cm during the constant-diameter stage. A double afterheater and a φ35 mm centrally opened afterheating cover are used; T2 is located 10 mm below the liquid surface, and T3 is located 15 mm below the solid-liquid interface, with a distance of 35 mm between them.

[0109] S5: Temperature is collected at 5 Hz at each temperature measurement point, and the high-definition camera captures meniscus images at 30 frames per second; the control software identifies edge position, contour height, width, symmetry, curvature and brightness distribution with an accuracy of 99.0% and an AI control response time of 0.25 s.

[0110] S6: After the crystal reaches the target diameter, it is pulled at 3.0 mm / h and rotated at 5 r / min. After growing to 60 mm, it is automatically removed, cooled at 45℃ / h, and then annealed and single-domain treated.

[0111] Test results of the 200 mm X-axis lithium niobate crystal obtained in this embodiment show that, as a verification of the upper limit process window, the obtained crystal has no macroscopic cracks or polymorphism, the diameter deviation is ±0.10 mm, and the single-furnace pass rate is 95.0%.

[0112] Example 11

[0113] This embodiment provides an intelligent and automated method for growing lithium niobate crystals with an X-axis diameter of 200 mm by using a temperature measurement position and a lower limit point for adjusting the amplitude. Specifically, it includes the following steps S1 to S6: S1: An 8mm×8mm×50mm lithium niobate seed crystal with X-axis orientation is selected, and a tungsten alloy seed crystal rod with a diameter of φ14mm is used. A 5μm thick electroless nickel plating layer is set on the end face of the seed crystal. By adjusting the heat transfer area and contact state between the seed crystal and the seed crystal rod, an initial undercooling of 14°C is formed at the tip of the seed crystal when it comes into contact with the melt.

[0114] S2: Nb2O5 and Li2CO3 were mixed in a molar ratio of 51.4:48.6, and then pressed and sintered sequentially. The resulting raw material was then placed into a platinum crucible with a diameter of φ260mm. The temperature was increased in three stages: from room temperature to 1000℃, from 1000℃ to 1240℃, and from 1240℃ to 1265℃, at heating rates of 8℃ / min, 5℃ / min, and 2℃ / min, respectively. After reaching 1265℃, the temperature was held for 3 hours to allow the temperature and composition distribution in the melt to become more uniform.

[0115] S3: Slowly lower the seed crystal and insert it 1.0 mm into the lithium niobate melt. Perform crystal pulling and shoulder formation at a pulling rate of 1.8 mm / h and a crystal rotation rate of 3 r / min. During the shoulder formation process, keep the seed crystal axis basically coincident with the central axis of the crucible so that the crystal shoulder expands synchronously along the circumference. The shoulder formation time is controlled to be 4 hours.

[0116] S4: A dual-backheater system consisting of a main backheater and a secondary backheater is used. The central opening diameter of the backheater cover is φ35mm, and temperature measuring point T5 is set in the middle of the backheater. T1 is located on the outer wall of the bottom of the crucible, 10mm from the bottom surface; T2 is located 5mm below the melt surface and 30mm from the inner wall of the crucible; T3 is located 5mm below the solid-liquid interface, with an axial distance of 25mm between T2 and T3; T4 is located on the inner side of the top of the backheater cover, 80mm above the crystal shoulder. The axial temperature gradient near the solid-liquid interface is determined based on the temperatures collected by T2 and T3 and the distance between them. The axial temperature gradient during the shoulder formation stage is controlled at 34℃ / cm, and the axial temperature gradient during the constant diameter growth stage is controlled at 30℃ / cm. Temperature is collected at each measuring point at a frequency of 5Hz, with a temperature control accuracy of ±0.1℃.

[0117] S5: Employs a high-definition camera to capture images of the meniscus at the solid-liquid interface at a frequency of 10 frames per second. The control software identifies the edge position, contour height, width, symmetry, curvature, and brightness distribution of the meniscus. When the meniscus contour height is higher than the set value, the heating power is reduced by 1%, and the pulling rate is increased by 0.2 mm / h; when the meniscus contour height is lower than the set value, the heating power is increased by 1%, and the pulling rate is reduced by 0.2 mm / h; when continuous fluctuations occur in the meniscus, the pulling rate is reduced by 0.3 mm / h, and the crystal rotation rate is increased by 1 r / min. The meniscus feature recognition accuracy is 98.5%, and the control response time is 0.5 s.

[0118] S6: After the crystal shoulder is enlarged to the target diameter, it enters the constant diameter growth stage and grows to 60 mm at a pulling rate of 1.8 mm / h and a crystal rotation rate of 8 r / min. After the crystal is extracted, it is cooled at a programmed cooling rate of 45℃ / h, annealed for 12 h, and then subjected to single-domain treatment.

[0119] The results show that when the above temperature measurement positions and the lower limit of the control amplitude are used, the multi-point temperature measurement device can obtain the temperature changes of the crucible bottom, melt, solid-liquid interface and post-heated area, and the abnormal state of the meniscus can be corrected in a closed loop; the obtained crystal shoulder is continuous, no obvious cracks or polymorphism are observed, and the crystal diameter deviation is controlled within ±0.10mm.

[0120] Example 12

[0121] This embodiment provides an intelligent and automated crystal pulling method for growing lithium niobate crystals with an X-axis diameter of 200 mm using a temperature measurement position and the upper limit of the control amplitude. Specifically, it includes the following steps S1 to S6: S1: An 8mm×8mm×50mm lithium niobate seed crystal with X-axis orientation is selected, and a tungsten alloy seed crystal rod with a diameter of φ14mm is used. A 5μm thick electroless nickel plating layer is set on the end face of the seed crystal. By controlling the cross-sectional size of the seed crystal, the thermal conductivity of the seed crystal rod, and the contact heat transfer area between the seed crystal and the seed crystal rod, an initial undercooling of 15°C is formed at the tip of the seed crystal.

[0122] S2: Nb2O5 and Li2CO3 were mixed in a molar ratio of 51.4:48.6, then pressed into blocks and sintered before being placed into a platinum crucible with a diameter of φ260mm. The temperature was increased at a rate of 7℃ / min to stabilize the melt temperature at 20℃ above the melting point of lithium niobate, and held at this temperature for 2 hours to remove unmelted particles from the melt and improve the temperature uniformity of the melt.

[0123] S3: Insert the seed crystal into the lithium niobate melt by 1.0 mm. Under the condition of initial supercooling at 15℃, perform shoulder formation at a pulling rate of 5.0 mm / h and a crystal rotation rate of 5 r / min. Continuously judge the crystal diameter growth state based on the changes in shoulder width and meniscus profile to keep the shoulder symmetrically expanding. The shoulder formation time is controlled to be 5 hours.

[0124] S4: A dual-backheater system consisting of a main backheater and an auxiliary backheater is employed. The central opening diameter of the backheater cover is φ35mm, and a temperature measuring point T5 is added in the middle of the backheater. T1 is located on the outer wall of the bottom of the crucible, 15mm from the bottom surface; T2 is located 10mm below the melt surface and 50mm from the inner wall of the crucible; T3 is located 15mm below the solid-liquid interface, with an axial distance of 35mm between T2 and T3; T4 is located on the inner side of the top of the backheater cover, 120mm above the crystal shoulder. The axial temperature gradient at the solid-liquid interface is determined in real time based on the temperature difference between T2 and T3. The axial temperature gradient during the shoulder formation stage is controlled at 35℃ / cm, and the axial temperature gradient during the constant diameter growth stage is controlled at 30℃ / cm. The temperature acquisition frequency of each measuring point is 5Hz, and the temperature control accuracy is ±0.1℃.

[0125] S5: A high-definition camera continuously acquires images of the meniscus at the solid-liquid interface at a frequency of 30 frames per second. The control software simultaneously extracts the edge position, contour height, width, symmetry, curvature, and brightness distribution of the meniscus. When the contour height of the meniscus is higher than the set value, the heating power is reduced by 3%, and the lifting rate is increased by 0.5 mm / h; when the contour height of the meniscus is lower than the set value, the heating power is increased by 3%, and the lifting rate is reduced by 0.5 mm / h; when the meniscus is asymmetrical, the crystal rotation rate is adjusted by ±2 r / min or the crystal offset position is adjusted according to the direction of the deviation; when the meniscus fluctuates continuously, the lifting rate is reduced by 0.3 mm / h, and the crystal rotation rate is increased by 2 r / min. The meniscus feature recognition accuracy is 99.0%, and the control response time is 0.25 s.

[0126] S6: After the crystal shoulder is raised to the target diameter of 200mm, it enters the constant diameter growth stage. Constant diameter growth is carried out at a pulling rate of 3.0mm / h and a crystal rotation rate of 10r / min. After the length of the constant diameter section reaches 80mm, the crystal is automatically removed. Then, the temperature is lowered at a programmed cooling rate of 45℃ / h to complete 12h annealing and single-domain treatment.

[0127] The results show that, under the condition that the temperature measurement position and the control amplitude are at the upper limit, the control device can promptly identify and correct abnormal meniscus height, circumferential asymmetry and transient fluctuations. The obtained crystal shoulder is complete and circumferentially continuous, with no obvious cracks, polycrystalline, twinned or inclusions, and the crystal diameter deviation is no greater than ±0.10 mm.

[0128] Comparative Example 1 This comparative example uses the automatic control scheme for the Czochralski method disclosed in CN101831692A for crystal growth control. This scheme mainly relies on weight sensor feedback to adjust the growth process, adjusting the heating power or growth parameters by detecting changes in crystal weight in real time. However, it does not employ seed crystal and seed rod thermal conductivity matching design, solid-liquid interface temperature gradient graded adjustment, multi-point temperature closed-loop control, or meniscus image recognition control. Using a single weight feedback closed loop, this scheme mainly relies on crystal weight changes for feedback control, without addressing the initial undercooling control strategy for matching the thermal conductivity of the seed crystal and seed rod, without setting a solid-liquid interface temperature gradient adjustment method based on crystal axial differences, and without combining multi-point temperature acquisition and meniscus image features for coordinated control. The remaining raw material composition, crucible structure, and conventional Czochralski growth conditions are the same as in Example 7, only the control method during crystal growth is replaced with a single closed-loop control based on weight feedback, but the heating power is adjusted only according to changes in crystal weight. The results showed that the crystal shoulder crack rate obtained by this control method was 30%, the crystal diameter deviation was ±0.3 mm, the crystal qualification rate was 72%, the growth cycle was extended by 18%, and the number of manual interventions per furnace was no less than 10.

[0129] Comparative Example 2 This comparative example uses the intelligent crystal growth control scheme disclosed in CN118028966A for crystal growth control. This scheme predicts the crystal growth state through a virtual furnace model and corrects the heating power or other growth parameters based on thermal imaging detection results. However, it does not establish a thermal conductivity matching relationship between the seed crystal and the seed crystal rod for different axes of lithium niobate crystals, does not set a graded adjustment strategy based on the actual axial temperature gradient of the solid-liquid interface, and does not combine multi-point temperature data and meniscus image features for real-time closed-loop control.

[0130] This comparative example uses a control method that combines simulation prediction and thermal imaging feedback. The composition of other raw materials, the structure of the platinum crucible, and the conventional Czochralski growth conditions are the same as in Example 9. The temperature field changes are predicted by a virtual furnace model, and the heating power is corrected based on the thermal imaging detection results.

[0131] The results showed that when using this control method, local remelting or excessive protrusion was prone to occur at the solid-liquid interface, the crystal shoulder was not enlarged uniformly, it was difficult to stably grow lithium niobate crystals with an X-axis diameter of 200 mm, the batch consistency of the obtained X-axis crystals was poor, and the crystal qualification rate was 65%.

[0132] Comparative Example 3 This comparative example grows lithium niobate crystals with an X-axis diameter of 150 mm according to the method of Example 7, but does not match the seed crystal size, seed crystal rod material and contact heat transfer area according to the target crystal axis, target diameter and required heat dissipation. Instead, it uses a 6 mm × 6 mm × 40 mm seed crystal and a molybdenum seed crystal rod with a diameter of 8 mm, and does not control the surface roughness and contact pressure of the contact surface between the seed crystal and the seed crystal rod.

[0133] Except for the above-mentioned thermal conductivity matching conditions between the seed crystal and the seed crystal rod, the other raw material composition, temperature field adjustment method, multi-point temperature measurement conditions, meniscus image acquisition and intelligent control conditions are the same as those in Example 7.

[0134] The results showed that when using this method, the initial undercooling at the seed crystal tip fluctuated within the range of 3℃ to 18℃, making it difficult to form stable and repeatable initial crystallization conditions; the resulting crystal had a shoulder cracking rate of 27%, a shoulder morphology qualification rate of 72%, and a single-furnace crystal qualification rate of 74%.

[0135] Comparative Example 4 In this comparative example, lithium niobate crystals with different axes were grown according to the methods of Examples 5, 7 and 9, but the axial temperature gradient at the solid-liquid interface was fixed at 30℃ / cm in both the shoulder formation stage and the constant diameter growth stage. The crucible height, the shape of the back heat sink or the size of the central opening of the back heat shield were no longer adjusted according to the crystal axis and the growth stage.

[0136] Except for the axial temperature gradient control method mentioned above, the other conditions for seed crystal and seed crystal rod matching, raw material composition, multi-point temperature measurement, meniscus image acquisition, and intelligent control are the same as those in the corresponding embodiments.

[0137] The results showed that a fixed axial temperature gradient could not simultaneously meet the thermal field requirements of crystals with different axial directions and different growth stages. In particular, during the X-axis crystal growth process, excessive protrusion and local remelting occurred at the solid-liquid interface. The qualified rate of the shoulder morphology of the obtained crystals was 73%, the crystal diameter deviation was ±0.26 mm, and the crystal cracking rate was 16%.

[0138] Comparative Example 5 This comparative example grows lithium niobate crystals with an X-axis diameter of 200 mm according to the method of Example 9, but only a single temperature measuring point is set on the surface of the melt. The T1, T3, T4 and T5 temperature measuring points used to detect the thermal state at the bottom of the crucible, the temperature near the solid-liquid interface, the temperature of the crystal growth environment and the temperature in the middle of the post-heater are not set. Therefore, the axial temperature gradient at the solid-liquid interface is not calculated in real time using the temperature difference between different temperature measuring points.

[0139] In this comparative example, the automatic meniscus feature recognition and intelligent closed-loop control functions are turned off. The operator observes the solid-liquid interface image every 5 seconds and adjusts the heating power, pulling rate, and crystal rotation rate based on the manual judgment. The other raw material composition, seed crystal and seed crystal rod matching conditions, platinum crucible structure, and thermal field structure are the same as in Example 9.

[0140] The results showed that when single-point temperature measurement and manual image judgment were used, the temperature field fluctuation during the growth process was ±2.0℃, the axial temperature gradient control deviation was ±3.0℃ / cm, and the average number of manual interventions was 12 times / furnace; the diameter deviation of the obtained crystal was ±0.30 mm, and the crystal qualification rate was 70%.

[0141] To verify the influence of seed crystal size, seed crystal rod thermal conductivity, and contact heat transfer area matching on the initial shoulder formation stability, Examples 1, 2, 5, 7, and 9 were selected as representative groups with different axial directions and diameters, and Comparative Examples 1 and 3 were set up. All groups used the same batch of Nb₂O₅ and Li₂CO₃ raw materials, maintaining consistent raw material molar ratios, crucible cleanliness, and furnace atmosphere. Initial undercooling, meniscus height, and shoulder expansion status were continuously recorded from the moment the seed crystal contacted the melt, with at least three independent growth cycles completed per furnace. After shoulder formation, the proportion of furnaces with through-cracks or shoulder cracks was statistically analyzed, and the time required to reach the target shoulder diameter was recorded. Three inspectors determined the shoulder morphology's qualification based on shoulder continuity, symmetry, and the presence or absence of polycrystalline regions. After the crystal completed constant-diameter growth and annealing, the single-furnace pass rate was calculated. The average values ​​of each group were used as the results, as shown in Table 1. The comparison of shoulder cracking rates among representative groups is shown in Table 2. Figure 2 .

[0142] Table 1. Influence of seed crystal-seed rod matching on the shoulder formation process and crystallization results.

[0143] From Table 1 and Figure 2As can be seen, after adopting seed crystal-seed rod thermal conductivity matching, the shoulder cracking rate of each embodiment was controlled at 1.7% to 3.0%, significantly lower than 30.0% of Comparative Example 1 and 27.0% of Comparative Example 3. Examples 2, 5, 7, and 9 correspond to initial undercooling of 8℃, 12℃, 13℃, and 14℃, respectively. Even with changes in axial direction and target diameter, the shoulder surface morphology qualification rate remained above 95.6%, indicating that this application does not simply increase undercooling, but rather adapts the initial heat dissipation capacity to the crystal size through the matching of seed crystal cross-section, seed rod material and diameter, and contact heat transfer state. Although Comparative Example 3 retained subsequent temperature field and image control, the shoulder surface was still prone to disordered expansion due to the mismatch of the initial thermal conduction path, indicating that subsequent closed-loop cannot replace front-end matching. The shoulder cracking time of each embodiment was 4.6 h to 5.4 h, the single-furnace qualification rate reached 95.1% to 96.0%, and no significant performance imbalance occurred between different axial groups. This verifies that the matching relationship can simultaneously reduce the risk of shoulder cracking, shorten the shoulder formation process, and improve crystallization stability, and has cross-axial applicability.

[0144] Test Example 2: Graded Temperature Gradient and Multi-point Closed-Loop Temperature Control Test To evaluate the effects of adjusting the axial temperature gradient at the solid-liquid interface according to the crystal axis and growth stage, and the effect of multi-point temperature measurement closed-loop on temperature field stability, Examples 2, 5, 7, and 9 were selected, with Comparative Example 4 (fixed temperature gradient) and Comparative Example 5 (single-point temperature measurement) as controls. Temperature data was continuously collected for 60 minutes after the shoulder of each furnace stabilized. The values ​​sampled at T2 and T3 were converted into real-time axial temperature gradients based on the distance between the two measurement points. The temperature field fluctuation amplitude and gradient control deviation were calculated using the set gradient as a benchmark. When crystal growth was complete, the diameter was measured every 10 mm along the constant diameter section. The maximum deviation and the diameter range of the three furnaces with repeated growth were statistically analyzed. Internal stress fringes were observed using polarized light detection, and the shoulder morphology qualification rate was calculated in conjunction with the shoulder contour integrity. Each example used a gradient range matched to the corresponding axis, while Comparative Example 4 was fixed at 30℃ / cm throughout, and Comparative Example 5 only used a single temperature point on the melt surface for manual adjustment. The results are shown in Table 2 and... Figure 3 As shown.

[0145] Table 2. Test results of temperature field stability, shoulder surface morphology, and dimensional consistency.

[0146] As shown in Table 2, the temperature fluctuation range of Examples 2, 5, 7, and 9 does not exceed ±0.30℃, and the axial temperature gradient control deviation is ±0.35℃ / cm to ±0.50℃ / cm; Comparative Examples 4 and 5 are amplified to ±1.50℃, ±2.00℃, ±2.40℃ / cm, and ±3.00℃ / cm, respectively. Figure 3 It can be seen that, under the same perturbation conditions, the gradient deviation of each embodiment quickly returned to the narrow range and did not drift continuously like the fixed gradient and single-point temperature measurement. Correspondingly, the diameter deviation of each embodiment did not exceed ±0.10 mm, the shoulder surface morphology qualification rate reached over 95.2%, and the occurrence rate of internal stress stripes was only 2.5%~3.2%; while for Comparative Examples 4 and 5, the shoulder surface qualification rate dropped to 73.0% and 70.0%, respectively, and the diameter range of the three furnaces increased by 0.34 mm and 0.40 mm. This result indicates that different axes require corresponding shoulder-releasing gradients, and X-axis crystals also need to reduce the gradient in the constant diameter stage. The temperature measurement in T1~T4 zones and the real-time gradient calculation in T2 and T3 can detect changes in the local thermal field that cannot be reflected by single-point temperature, taking into account shoulder surface morphology, diameter stability, and internal stress suppression.

[0147] Test Example 3: Meniscus Recognition and AI Real-time Control Response Test To verify the impact of meniscus feature recognition and real-time AI control on the speed of anomaly recovery and unattended operation capability, Examples 2, 5, 7, and 9 were selected, along with Comparative Examples 1, 2, and 5. After the crystal entered a stable shoulder formation stage, a standardized perturbation (i.e., instantaneously increasing the heating power by 2% and holding it for 1 second) was performed without changing the raw materials or furnace structure, causing a repeatable shift in the meniscus height. The image system's recognition of the edge position, contour height, width, symmetry, curvature, and brightness distribution, as well as the time required for the control command to reach the actuator, were recorded. The time taken for the meniscus height deviation to recover to within ±5% of the range before the perturbation was defined as the perturbation recovery time. The number of manual interventions, the root mean square value of the meniscus height deviation, and the final pass rate were statistically analyzed throughout the process. The examples used AI to automatically adjust power, lifting, and crystal transfer parameters, while the comparative examples used weight feedback, simulated thermal imaging, or manual observation, as shown in Table 3. Typical dynamic recovery curves are shown in Table 5. Figure 4 .

[0148] Table 3 Results of tests on meniscus recognition, control response, and artificial intervention

[0149] As shown in Table 3, in Examples 2, 5, 7, and 9, the meniscus recognition accuracy reached 98.5%–99.1%, the single response time was 0.25s–0.40s, and the number of manual interventions for the entire furnace was 0; the meniscus height deviation RMS was only 0.14mm–0.20mm, and it could recover to a stable level within 1.2s–1.8s after disturbance. Figure 4 As shown, this is consistent with the data in the table: Examples 7 and 9 decayed quickly after the disturbance occurred, but Comparative Example 1 relied on weight changes or indirect judgment through simulation and thermal imaging, resulting in a significant lag in response. Furthermore, Comparative Example 5 was also subject to the time interval of manual observation. The response time of Comparative Example 1 reached 10.0 s, with 10 manual interventions per furnace, and a pass rate of 72%. The pass rates of Comparative Examples 2 and 5 were 65% and 70%, respectively. Therefore, it can be concluded that extracting multiple meniscus features directly from images of the solid-liquid interface can reflect the real interface changes faster than weight signals or virtual models. Furthermore, generating linkage commands through multi-point temperature, pulling rate, and crystal rotation rate can suppress both transient fluctuations and long-term accumulated deviations, thus achieving unattended closed-loop growth.

[0150] Test Example 4: Test of Appearance, Size and Radial Uniformity of Large-Diameter Crystals To comprehensively evaluate the appearance integrity, dimensional uniformity, and batch repeatability of the obtained large-diameter lithium niobate crystals, Examples 2, 5, 7, and 9 were selected, with Comparative Examples 1 and 2 used as controls. After annealing and single-domain formation, six cross-sections were selected at equal intervals along the axial direction in the constant-diameter section. The diameter of each cross-section was measured in two mutually perpendicular directions, and the average diameter and maximum diameter deviation were calculated. The resistivity was measured at the radius normalization positions of -100%, -75%, -50%, -25%, 0%, 25%, 50%, 75%, and 100%, and the radial relative standard deviation was calculated. Cracks, polycrystalline structures, twins, and inclusions were inspected using transmitted light and polarized light, and the pass rate was statistically analyzed. Figure 5 and Figure 6 The physical appearance of the 150 mm X-axis crystal in Example 7 and the 200 mm X-axis crystal in Example 9 are recorded respectively; the radial resistivity changes of Examples 7, 9 and Comparative Example 2 are plotted, and the results are shown in Table 4 and [other tables not provided]. Figure 7 .

[0151] Table 4. Test results of crystal size, radial uniformity, and defects.

[0152] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

[0153] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A full-stack intelligent automated crystal growth method, characterized in that, Includes the following steps: S1: Select the seed crystal and seed crystal rod according to the target axis and target diameter of the lithium niobate crystal to be grown, and make the seed crystal tip form a preset initial undercooling by adjusting the cross-sectional size of the seed crystal, the thermal conductivity of the seed crystal rod, the diameter of the seed crystal rod, and the contact heat exchange area between the seed crystal and the seed crystal rod. S2: After the lithium niobate raw material is batched, mixed, pressed and sintered, it is loaded into a crucible, heated to form a lithium niobate melt, and the temperature of the crucible, melt, solid-liquid interface and crystal growth environment is measured using a multi-point temperature measuring device. S3: Make the seed crystal contact with the lithium niobate melt, and control the pulling rate and crystal rotation rate under the preset initial supercooling to make the crystal shoulder face enlarged in an orderly manner; S4: Based on the target axis and crystal growth stage, adjust the axial temperature gradient at the solid-liquid interface by adjusting at least one of the crucible height, the shape of the back heater, and the size of the central opening of the back heat shield. S5: Acquire a solid-liquid interface meniscus image, extract at least two meniscus features from the meniscus image, and combine multi-point temperature data to generate control commands for at least one parameter among heating power, pulling rate, crystallization rate and axial temperature gradient. S6: After the crystal is shouldered to the target diameter, it is grown to the same diameter, and after the target length is reached, the crystal is extracted, cooled in a programmed manner, annealed and single-domained.

2. The crystal growth method according to claim 1, characterized in that, The target axis includes the (0001) direction, the (10-14) crystal plane normal direction, and the X-axis direction; the size of the seed crystal is selected from one of 4mm×4mm×40mm, 6mm×6mm×40mm, or 8mm×8mm×50mm; When the target diameter is no more than 100mm, a 4mm×4mm×40mm seed crystal is selected; when the target diameter is greater than 100mm and less than 150mm, a 6mm×6mm×40mm or 8mm×8mm×50mm seed crystal is selected according to the target axis and the required heat dissipation; when the target diameter is no less than 150mm, an 8mm×8mm×50mm seed crystal is selected. The diameter of the seed crystal rod is 8mm to 14mm; the preset initial undercooling degree is 5℃ to 15℃.

3. The crystal growth method according to claim 2, characterized in that: When growing crystals in the (0001) direction with a target diameter of no more than 125 mm, a seed crystal of 6 mm × 6 mm × 40 mm and a molybdenum seed crystal rod with a diameter of 8 mm are used, and the preset initial undercooling is 8 °C. When growing a crystal with a target diameter of 125 mm in the direction of the (10-14) crystal plane normal, an 8 mm × 8 mm × 50 mm seed crystal and a 12 mm diameter tungsten alloy seed crystal rod are used, and the preset initial undercooling is 12 °C. When growing a crystal with a target diameter of 150 mm along the X-axis, an 8 mm × 8 mm × 50 mm seed crystal and a 12 mm diameter tungsten alloy seed crystal rod are used, and the preset initial undercooling is 13 °C. When growing a crystal with a target diameter of 200 mm along the X-axis, an 8 mm × 8 mm × 50 mm seed crystal and a 14 mm diameter tungsten alloy seed crystal rod are used, and the preset initial undercooling is 14 °C.

4. The crystal growth method according to claim 1, characterized in that, The molar ratio of Nb₂O₅ to Li₂CO₃ in the lithium niobate raw material is 51.4:48.

6. The crucible is a platinum crucible with a diameter of 180 mm to 260 mm. The raw material is melted by single-stage or three-stage heating. When using single-stage heating, the heating rate is 3°C / min to 7°C / min, the melt temperature is maintained at a temperature 10°C to 20°C higher than the melting point of lithium niobate, and the holding time is 1 h to 2 h. When growing X-axis crystals with a target diameter of 200 mm and using a three-stage heating method, the heating was carried out at heating rates of 8℃ / min, 5℃ / min, and 2℃ / min, respectively, from room temperature to 1000℃, from 1000℃ to 1240℃, and from 1240℃ to 1265℃, and then held at 1265℃ for 3 hours.

5. The crystal growth method according to claim 1, characterized in that, The contact depth between the seed crystal and the lithium niobate melt is 0.8 mm to 1.0 mm; the pulling rate during the shoulder formation stage is 1.8 mm / h to 5 mm / h, and the crystal rotation speed is 8 r / min to 15 r / min; the pulling rate during the constant diameter growth stage is 1.8 mm / h to 3 mm / h, and the crystal rotation speed is 5 r / min to 10 r / min; the constant diameter growth length of the crystal is 50 mm to 80 mm, and the programmed cooling rate is 45℃ / h to 55℃ / h; When growing crystals with a target diameter of 200 mm along the X-axis, the crystal rotation speed during the shoulder formation stage is 3 r / min to 7 r / min, and the shoulder formation time is 4 h to 5 h.

6. The crystal growth method according to claim 1, characterized in that, During the shoulder formation stage, the axial temperature gradient at the solid-liquid interface is controlled according to the target axis as follows: When the target axis is in the (0001) direction, the axial temperature gradient is 28℃ / cm~32℃ / cm; The target axis is the normal direction of the (10-14) crystal plane, and the axial temperature gradient is 30℃ / cm~34℃ / cm; When the target axis is in the X-axis direction, the axial temperature gradient is 33℃ / cm~35℃ / cm; During the constant diameter growth stage of the crystal, the axial temperature gradient at the solid-liquid interface is 28℃ / cm~30℃ / cm. The axial temperature gradient is adjusted by adjusting at least one of the following: crucible height, afterheater shape, and the size of the central opening of the afterheating cover. The crucible is raised by 5 mm to 10 mm, the afterheater is a cylindrical or conical afterheater, and the diameter of the central opening of the afterheating cover is 35 mm to 80 mm.

7. The crystal growth method according to claim 1, characterized in that, The multi-point temperature measurement device includes: The first temperature measuring point is located on the outer wall of the bottom of the crucible and 10mm to 15mm from the bottom of the crucible. The second temperature measuring point is located 5mm to 10mm below the surface of the melt and 30mm to 50mm from the outer crucible wall; A third temperature measuring point located 5mm to 15mm below the solid-liquid interface and 25mm to 35mm away from the second temperature measuring point; and The fourth temperature measuring point is located on the inner side of the top of the rear heat shield and 80mm to 120mm above the crystal shoulder surface; The temperature acquisition frequency of each temperature measuring point is 1Hz to 5Hz. The temperature difference between the second and third temperature measuring points is used to determine the axial temperature gradient, and the temperature control accuracy is ±0.1℃.

8. The crystal growth method according to claim 1, characterized in that, The acquisition frequency of the meniscus image is 10 frames / second to 30 frames / second; the meniscus features include at least three of the following: edge position, contour height, width, symmetry, curvature, and brightness distribution. When the meniscus profile height is higher than the set value, reduce the heating power by 1% to 3% and increase the pulling rate by 0.2 mm / h to 0.5 mm / h; when the meniscus profile height is lower than the set value, increase the heating power by 1% to 3% and reduce the pulling rate by 0.2 mm / h to 0.5 mm / h; when the meniscus is asymmetrical, adjust the crystal bias position or adjust the crystal rotation rate by ±2 r / min; when the meniscus fluctuates, reduce the pulling rate by 0.3 mm / h and increase the crystal rotation rate by 1 r / min to 2 r / min. The accuracy of meniscus feature recognition is no less than 98%, and the control response time is no more than 0.5s.

9. The crystal growth method according to any one of claims 1-8, characterized in that: When growing a crystal with a target diameter of 150 mm along the X-axis, the surface roughness Ra of the contact surface between the seed crystal and the seed crystal rod is no greater than 0.4 μm, the contact pressure is 1.2 MPa, the diameter of the platinum crucible is 220 mm, the back heat sink is a conical back heat sink with a 60° apex angle, the diameter of the central opening of the back heat shield is 40 mm, the axial temperature gradient during the shoulder formation stage is 34 ℃ / cm, the axial temperature gradient during the constant diameter growth stage is 28 ℃ / cm, and the programmed cooling rate is 50 ℃ / h. When growing a crystal with a target diameter of 200 mm along the X-axis, a 5 μm thick electroless nickel plating layer is applied to the end face of the seed crystal. The diameter of the platinum crucible is 260 mm. A double backheater consisting of a main backheater and a secondary backheater is used. The diameter of the central opening of the backheater is 35 mm. A fifth temperature measuring point is added in the middle of the backheater. The axial temperature gradient during the shoulder formation stage is 34 °C / cm, and the axial temperature gradient during the constant diameter growth stage is 30 °C / cm. The programmed cooling rate is 45 °C / h, and the annealing time is 12 h.

10. The crystal growth method according to claim 9, characterized in that, The obtained lithium niobate crystal has a diameter of not less than 100 mm, wherein the maximum diameter of the (0001) direction crystal and the (10-14) crystal plane normal direction crystal is 150 mm, and the maximum diameter of the X-axis direction crystal is 200 mm; the diameter deviation of the lithium niobate crystal is not greater than ±0.1 mm, the meniscus feature recognition accuracy is not less than 98%, the control response time is not greater than 0.5 s, and the crystal qualification rate is not less than 95%.

Citation Information

Patent Citations

  • Automatic control device for use in Czochralski crystal growth

    CN101831692A

  • Intelligent crystal growth equipment for growing crystals

    CN118028966A