Flow guide tube and method for producing the same
By using a flow guide made of integral tantalum carbide material, combined with a porous tantalum carbide substrate and a dense, non-porous outer shell, the problem of stress release and interface reaction in silicon carbide single crystal growth caused by graphite flow guides is solved. This achieves a reduction in crystal edge defects and an improvement in structural stability, making it suitable for silicon carbide single crystal growth.
Patent Information
- Application Number
- CN202611529773.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-24
AI Technical Summary
Existing graphite guide tubes cannot effectively release crystal edge stress during silicon carbide single crystal growth, and are prone to interfacial reactions with the crystal growth atmosphere, resulting in crystal edge defects and warping, which affects production yield and accuracy.
The flow guide tube is made entirely of tantalum carbide, including a porous tantalum carbide substrate and a dense non-porous tantalum carbide shell. It is prepared by two-stage chemical vapor deposition to form an internally porous and externally dense structure, which buffers the stress at the crystal edge and isolates thermal field impurities.
It effectively reduces dislocation density and residual stress at crystal edges, improves wafer warping, enhances crystal crystal quality and structural stability of the flow guide tube, and is suitable for long-cycle industrial production.
Smart Images

Figure CN123153159A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a flow guide tube and its preparation method, belonging to the technical field of flow guide tube preparation for silicon carbide single crystal growth. Background Technology
[0002] The sources of stress in silicon carbide substrates are complex, mainly including intrinsic stress formed during crystal growth, stress introduced by substrate machining, and stress induced during epitaxial growth. These stresses can interfere with the epitaxial growth process through various mechanisms. Among them, the intrinsic stress of the crystal, in addition to the stress accumulation caused by various defects inside the crystal, is also caused by crystal defects such as impurities that are prone to occur in the area where the crystal edge contacts the flow guide tube during crystal growth, thus inducing stress. At the same time, the flow guide tube exerts radial compression on the crystal edge and restricts the free radial growth of the crystal, which also introduces stress at the crystal edge.
[0003] Existing research indicates that stress in silicon carbide single crystals tends to concentrate in the wafer edge region, easily causing macroscopic deformation of the wafer, typically manifested as increased wafer warpage. Significant wafer warpage can adversely affect subsequent semiconductor manufacturing processes such as photolithography and thin-film deposition, reducing process alignment accuracy and on-wafer process uniformity. In severe cases, it can even cause the wafer to break during equipment transport, reducing production yield.
[0004] The existing silicon carbide crystal growth thermal field generally uses graphite guide tubes. Graphite is prone to interfacial reaction with the crystal growth atmosphere, which further aggravates the generation of impurities and crack defects at the crystal edge. In addition, the graphite guide tube is a rigid structure, which cannot buffer or release the growth stress at the crystal edge, making it difficult to effectively solve the problem of stress concentration at the crystal edge.
[0005] To address the interfacial reaction problem in graphite guide tubes, existing technologies include an improved approach of applying a tantalum carbide coating to the surface of the graphite guide tube substrate. However, due to the significant differences in thermal expansion coefficients and interfacial bonding properties between graphite and tantalum carbide, the tantalum carbide coating is prone to cracking, peeling, and flaking under high-temperature and thermal cycling conditions. This not only shortens the service life of the guide tube but also causes secondary contamination of the crystals by the flaking coating debris, introducing new defects and stresses.
[0006] In summary, existing graphite guide tubes and graphite substrates with tantalum carbide coatings are both unable to effectively release the growth stress at the crystal edges and avoid contamination caused by interfacial reactions during crystal growth. There is an urgent need for a guide tube and its preparation method that can release the stress at the crystal edges, isolate thermal impurities, and have a stable and reliable structure. Summary of the Invention
[0007] To address the problems existing in the prior art, the present invention provides a flow guide tube and its preparation method. This method can effectively suppress the introduction of impurities at the crystal edge, and at the same time, it does not restrict radial growth during the crystal growth process, thus effectively releasing the stress at the crystal edge.
[0008] To achieve the above objectives, the present invention employs a flow guide tube, the entire flow guide tube being constructed of tantalum carbide. The flow guide tube includes a porous tantalum carbide substrate and a dense, non-porous tantalum carbide shell covering the outer surface of the porous tantalum carbide substrate. The porous tantalum carbide substrate has a porous structure to reduce crystal edge stress. The dense, non-porous tantalum carbide shell is used to seal the exterior of the flow guide tube and prevent interfacial reactions with the crystal growth atmosphere.
[0009] Preferably, the thickness of the dense, non-porous tantalum carbide shell is 40 μm to 100 μm.
[0010] Preferably, the guide tube is suitable for the thermal field of silicon carbide single crystal growth.
[0011] A second aspect of the present invention also provides a method for preparing the aforementioned guide tube, comprising the following steps: S1. Preparation of graphite preform: Using porous graphite as the substrate, a porous graphite preform with the same external dimensions as the target tantalum carbide guide tube is prepared by machining. S2. Graphite container coating treatment: The inner wall of the graphite container is coated with tantalum carbide to prepare a modified graphite container with a dense tantalum carbide coating on the inner wall. S3. First stage chemical vapor deposition: The porous graphite preform is placed in a modified graphite container, and a mixed reaction gas composed of TaCl5, H2 and inert gas is introduced to carry out a chemical vapor deposition reaction, so that the porous graphite preform is completely reacted and transformed into a porous tantalum carbide matrix. S4. Second stage chemical vapor deposition: The porous tantalum carbide substrate is placed in a modified graphite container, and a mixed reaction gas consisting of TaCl5, CH4, H2 and inert gas is introduced to carry out a chemical vapor deposition reaction, forming a dense and non-porous tantalum carbide shell on the outer surface of the porous tantalum carbide substrate, thus obtaining a tantalum carbide guide tube with a porous interior and a dense and non-porous exterior.
[0012] As a preferred embodiment, the specific process of step S2 includes: The graphite container is placed in the reaction furnace and a vacuum leak test is performed; tantalum oxide powder is laid at the bottom of the graphite container; the temperature is raised to 2100℃~2300℃, the pressure inside the furnace is controlled at 3mbar~10mbar, and the reaction is held for 10h~20h, so that the tantalum oxide is heated and vaporized and reacts with the inner wall of the graphite container to form a dense tantalum carbide coating on the inner wall of the graphite container.
[0013] Preferably, the tantalum oxide powder is laid at a height 10 mm to 20 mm lower than the top height of the target coating.
[0014] Preferably, in step S3, the process parameters for the first stage of chemical vapor deposition are: the molar ratio of TaCl5, H2, and inert gas is 1:(20-40):(20-60), the reaction temperature is 1500℃~1800℃, the reaction pressure is 3mbar~10mbar, and the reaction time is 5h~20h.
[0015] Preferably, in step S4, the process parameters for the second stage of chemical vapor deposition are: the molar ratio of TaCl5, CH4, H2, and inert gas is 1:(1-5):(20-40):(20-60), the reaction temperature is 1200℃~1600℃, the reaction pressure is 5mbar~15mbar, and the reaction time is 5h~10h.
[0016] Preferably, after the first and second stages of chemical vapor deposition reaction are completed, cooling annealing is performed: the temperature is kept constant, the pressure is increased to 100 mbar to 500 mbar within 1 to 3 hours, then the temperature is reduced in stages for annealing, and finally the temperature is naturally cooled to room temperature.
[0017] Preferably, the segmented cooling annealing includes: cooling to 1000-1200℃ for 6-12 hours and holding for 3-5 hours; then cooling to 400-600℃ for another 6-12 hours and holding for 3-5 hours.
[0018] Compared with the prior art, the beneficial effects of the present invention are: 1. Existing graphite flow guides are rigid structures that rigidly confine and compress the edges of silicon carbide crystals during crystal growth, restricting radial free growth and causing continuous accumulation of lattice distortion. This ultimately leads to excessively high edge stress and excessive wafer warpage. This invention employs a porous tantalum carbide substrate, enabling the flow guide body to adapt to micro-deformation and buffering capabilities. It can accommodate radial growth deformation during crystal growth, effectively releasing accumulated growth stress at the crystal edges, preventing stress accumulation, reducing residual stress at the silicon carbide crystal edges and overall average stress, improving macroscopic wafer warpage, and ensuring the process accuracy and yield of subsequent precision processes such as photolithography and thin film deposition.
[0019] 2. Traditional graphite flow guides are prone to interfacial reactions with the crystal growth atmosphere at high temperatures, resulting in edge defects such as erosion pits, impurities, and microcracks. These defect areas are prone to stress concentration, severely affecting substrate quality. The flow guide of this invention is made entirely of tantalum carbide, which exhibits excellent high-temperature chemical stability and does not react with the silicon carbide crystal growth system. Simultaneously, the outer layer is a dense, non-porous tantalum carbide shell, effectively isolating free impurities and particles within the thermal field. This suppresses the nucleation and growth of crystal edge defects from the source, significantly reducing the density of basal dislocations and edge dislocations at the crystal edges, and improving the overall crystallization quality of silicon carbide single crystals.
[0020] 3. Existing improved flow guides generally adopt a heterogeneous structure of "graphite matrix and tantalum carbide coating". Due to the significant difference in the thermal expansion coefficients and interfacial bonding performance of the two materials, the coating is prone to cracking, peeling, and detachment under high-temperature thermal cycling conditions. This not only shortens the service life of the flow guide, but the detached debris can also cause secondary contamination of the crystal, introducing new defects and stresses. This invention adopts an integral tantalum carbide structure, without the interface of heterogeneous materials. The overall thermal properties are uniform and consistent, eliminating the risk of delamination, detachment, and cracking under high-temperature conditions. The structural stability and service life are superior to traditional heterogeneous coated flow guides, making it suitable for long-cycle, multi-batch industrial mass production needs.
[0021] 4. The stepwise chemical vapor deposition (CVD) process of this invention first achieves complete replacement of the porous graphite preform through a first-stage CVD, forming a porous tantalum carbide substrate with porous structure functionality. Then, in the second stage, a carbon source is introduced to selectively deposit a dense, non-porous outer shell on the outer surface, achieving a differentiated functional structure of internal porous pressure relief and external dense impurity isolation. This process path can control the morphology and performance of the internal porous structure and the external dense layer of the flow guide tube. It exhibits good process repeatability and high product consistency, enabling stable and large-scale fabrication of tantalum carbide flow guide tubes with both excellent stress relief and impurity isolation properties. It solves the technical bottleneck of traditional processes that cannot integrate the fabrication of dual-layer functional structures, possessing significant engineering application and industrialization value. Attached Figure Description
[0022] Figure 1 This is a schematic diagram of the sidewall of a silicon carbide crystal prepared using a tantalum carbide guide tube in Embodiment 1 of the present invention; Figure 2 A schematic diagram of the sidewall of a silicon carbide crystal prepared using a traditional graphite guide tube for comparison. Figure 3 This is a dislocation test diagram of the silicon carbide crystal in Embodiment 1 of the present invention; Figure 4 This is a diagram showing dislocation testing of a comparative silicon carbide crystal. Figure 5 This is a test diagram of the overall stress distribution of silicon carbide crystal in Embodiment 1 of the present invention; Figure 6 This is a test diagram showing the overall stress distribution of a silicon carbide crystal as a comparative example. Figure 7 This is a schematic diagram of the tantalum carbide guide tube according to Embodiment 1 of the present invention; Figure 8 This is a schematic diagram of the assembly of the tantalum carbide guide tube in a thermal field according to Embodiment 1 of the present invention; Figure 9 This is a schematic diagram illustrating the principle of tantalum carbide guide tube for reducing crystal stress in Embodiment 1 of the present invention. In the figure: 1. Dense, non-porous tantalum carbide shell; 2. Porous tantalum carbide substrate. Detailed Implementation
[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below. However, it should be understood that the specific embodiments described herein are merely illustrative and are not intended to limit the scope of the invention.
[0024] Example 1
[0025] This embodiment prepares a tantalum carbide guide tube to reduce the stress of silicon carbide crystals. The guide tube is cylindrical and is made entirely of tantalum carbide material. It consists of an internal porous tantalum carbide substrate 2 and a dense non-porous tantalum carbide shell 1 covering its outer surface. The shell thickness is 60μm and is adapted to the thermal field of silicon carbide single crystal growth in PVT method.
[0026] The specific preparation steps are as follows: S1. Preparation of graphite preform: Using porous graphite as the substrate, a porous graphite preform with the same shape and size as the target tantalum carbide guide tube is prepared by machining. S2. Graphite Container Coating Treatment: Place the graphite container into the reaction furnace and perform vacuum leak testing to ensure the furnace body is airtight and leak-free; lay tantalum oxide powder at the bottom of the graphite container, with the powder layer height 15mm lower than the top height of the target coating; raise the temperature to 2200℃, control the furnace pressure at 6mbar, and maintain the temperature for 15 hours; after the tantalum oxide is heated and vaporized, it reacts fully with the inner wall of the graphite container to form a dense and stable tantalum carbide coating on the inner wall of the container, thus obtaining a modified graphite container, which can avoid the adhesion between the preform and the graphite container in subsequent preparation processes; S3. First-stage chemical vapor deposition: A qualified porous graphite preform is placed at the bottom of a modified graphite container and then transferred to a reactor after assembly. A mixed reaction gas of TaCl5, H2, and an inert gas (such as argon) is introduced, with a gas molar ratio of 1:30:40. The reaction temperature is set at 1700℃ and the reaction pressure at 5mbar. The reaction is carried out at a constant temperature for 12 hours to allow the porous graphite preform to completely permeate the reaction and be completely transformed into porous tantalum carbide matrix 2. After the reaction, the temperature is maintained at 1700℃ and the pressure is uniformly increased to 300mbar within 2 hours. Then, the temperature is lowered to 1200℃ and held for 5 hours for 8 hours, and then lowered to 500℃ and held for 5 hours for another 8 hours. Finally, the heating system is turned off and the material is allowed to cool naturally to room temperature. Qualified porous tantalum carbide matrix 2 without uneven color, pores, or cracks is selected. S4. Second-stage chemical vapor deposition: A qualified porous tantalum carbide substrate 2 is placed in a modified graphite container, and a mixed reaction gas of TaCl5, CH4, H2, and inert gas is introduced at a molar ratio of 1:3:30:40. The reaction temperature is set at 1400℃ and the reaction pressure at 10 mbar, and the reaction is carried out at a constant temperature for 8 hours. A dense, non-porous tantalum carbide shell 1 with a thickness of 60 μm is deposited on the outer surface of the porous tantalum carbide substrate 2. The cooling and annealing process is consistent with the first stage, and finally a tantalum carbide guide tube with an internal porous structure and an external dense, non-porous structure is obtained. Its structure is as follows. Figures 7-9 As shown.
[0027] The tantalum carbide flow guide prepared in this embodiment was applied to the PVT method for silicon carbide single crystal growth. Maintaining the same thermal field structure and growth process parameters, only the flow guide was replaced, resulting in silicon carbide crystal A. Testing revealed that crystal A had smooth sidewalls without etch pits; the edge basal dislocation (BPD) density was 57 ea / cm². 2 The edge dislocation (TED) density is 719ea / cm². 2 The crystal edge stress is 4.5–5.5 MPa, the average stress is 2.7 MPa, the crystal edge has few defects and low stress level, and there is no obvious warping deformation.
[0028] Example 2
[0029] The preparation process in this embodiment is basically the same as that in Example 1, except for the chemical vapor deposition parameters, as follows: The first stage of chemical vapor deposition: the molar ratio of TaCl5, H2, and inert gas (such as argon) is 1:20:20, the reaction temperature is 1500℃, the reaction pressure is 3mbar, and the reaction time is 5h; after the reaction is completed, the pressure is increased to 100mbar within 1h, and the subsequent segmented cooling annealing process is the same as in Example 1. The second stage of chemical vapor deposition: the molar ratio of TaCl5, CH4, H2 and inert gas (such as argon) is 1:1:20:20, the reaction temperature is 1200℃, the reaction pressure is 5mbar, and the reaction time is 5h; the resulting dense and non-porous tantalum carbide shell 1 has a thickness of 40μm.
[0030] The tantalum carbide flow guide prepared in this embodiment has a complete structure, free of cracks and surface defects, and exhibits structural stability. The porous substrate possesses excellent porous structure properties, and the dense, non-porous outer shell effectively isolates thermal impurities. When applied to silicon carbide crystal growth, the resulting silicon carbide crystals show no obvious impurities or cracks at the edges, and the edge stress is significantly lower than that of crystals prepared using traditional graphite flow guides. This effectively improves wafer warpage and meets the high-quality production requirements of silicon carbide substrates.
[0031] Example 3
[0032] The preparation process in this embodiment is basically the same as that in Example 1, except for the process parameters, which are as follows: The first stage of chemical vapor deposition: the molar ratio of TaCl5, H2, and inert gas is 1:40:60, the reaction temperature is 1800℃, the reaction pressure is 10mbar, and the reaction time is 20h; after the reaction is completed, the pressure is increased to 500mbar within 3h, and the subsequent segmented cooling annealing process is the same as in Example 1. The second stage of chemical vapor deposition: the molar ratio of TaCl5, CH4, H2 and inert gas was 1:5:40:60, the reaction temperature was 1600℃, the reaction pressure was 15mbar, and the reaction time was 10h; the resulting dense, non-porous tantalum carbide shell 1 had a thickness of 100μm.
[0033] This embodiment can stably prepare a tantalum carbide flow guide with a complete structure and excellent performance. The internal porous structure is uniform and exhibits excellent porous capacity, while the external shell is tightly sealed, resulting in a good external sealing effect. Applied to the PVT silicon carbide crystal growth process, it can effectively release growth stress at crystal edges, suppress edge defect formation, and achieve uniform overall crystal stress and low warpage, making it suitable for industrial mass production conditions.
[0034] Comparative Example This comparative example uses a conventional graphite guide tube from the prior art to replace the tantalum carbide guide tube of the present invention. The remaining thermal field structure, silicon carbide crystal growth process, and environmental parameters are completely consistent with those of Example 1, and silicon carbide crystal B is prepared.
[0035] Morphological and performance testing revealed that the conventional graphite guide tube underwent an interfacial reaction with the crystal growth atmosphere at high temperatures, resulting in crystal B with numerous uniformly eroded graphite pits on its sidewalls and significant edge defects. The basal dislocation (BPD) density at the edge of crystal B reached a high of 391 ea / cm². 2 The edge dislocation (TED) density is as high as 2164 ea / cm.2 The dislocation defects are severely concentrated; the crystal edge stress is 12.1-15.8 MPa, the average stress is 5.5 MPa, the overall stress level is significantly high, the wafer warping deformation is large, which can easily lead to a decrease in the accuracy of subsequent photolithography and thin film deposition processes, and even wafer transport breakage problems.
[0036] in, Figure 1 , Figure 2 The figure is used to compare the appearance defects of the sidewalls of silicon carbide crystals prepared by different guide tubes. As can be seen from the figure, the tantalum carbide guide tube prepared by the present invention can make the sidewalls of the crystal smooth and flat, without erosion pits and micro defects, effectively improving the quality of the crystal edge morphology. Figure 3 , Figure 4 This invention is used to compare the edge dislocation density and defect aggregation of two sets of crystals, and intuitively demonstrates that it can significantly reduce the number of basal plane dislocations and edge dislocations at the edge of silicon carbide crystals, and suppress the aggregation of edge defects. Figure 5 , Figure 6 The edge stress and overall average stress levels of the two sets of crystals were compared to demonstrate that the structure of this invention can effectively release crystal growth stress, reduce residual stress in the crystal, and improve the problem of wafer warping. Finally, a tantalum carbide flow guide with an internally porous and externally dense, non-porous structure was fabricated. Its overall structure, thermal field assembly, and the principle of reducing crystal stress are as follows: Figure 7 , Figure 8 , Figure 9 As shown.
[0037] This invention overcomes the technical bottlenecks of traditional graphite flow guides through a tantalum carbide structure and a two-stage CVD fabrication process. The internal porous structure reduces crystal edge stress, while the external dense, non-porous structure seals the flow guide, preventing interfacial reactions and significantly reducing dislocation density and residual stress at the silicon carbide crystal edges, thus improving wafer warping. Simultaneously, the structure eliminates the risk of delamination and shedding, exhibiting structural stability far superior to traditional products.
[0038] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A flow conductor, characterized in that The entire flow guide tube is made of tantalum carbide material. The flow guide tube includes a porous tantalum carbide substrate (2) and a dense non-porous tantalum carbide shell (1) covering the outer surface of the porous tantalum carbide substrate (2). The porous tantalum carbide substrate (2) has a porous structure to reduce the stress at the crystal edge. The dense non-porous tantalum carbide shell (1) is used to seal the outside of the flow guide tube and prevent it from reacting with the crystal growth atmosphere.
2. The conductor of claim 1, wherein The thickness of the dense, non-porous tantalum carbide shell (1) is 40 μm to 100 μm.
3. The conductor of claim 1, wherein The guide tube is suitable for the thermal field of silicon carbide single crystal growth.
4. A method of manufacturing a flow conductor according to any one of claims 1-3, characterized in that Includes the following steps: S1. Preparation of graphite preform: Using porous graphite as the substrate, a porous graphite preform with the same external dimensions as the target tantalum carbide guide tube is prepared by machining. S2. Graphite container coating treatment: The inner wall of the graphite container is coated with tantalum carbide to prepare a modified graphite container with a dense tantalum carbide coating on the inner wall. S3, First stage chemical vapor deposition: The porous graphite preform is placed in a modified graphite container, and a mixed reaction gas composed of TaCl5, H2 and inert gas is introduced to carry out a chemical vapor deposition reaction, so that the porous graphite preform is completely reacted and transformed into a porous tantalum carbide matrix (2). S4. Second stage chemical vapor deposition: The porous tantalum carbide substrate (2) is placed in a modified graphite container, and a mixed reaction gas composed of TaCl5, CH4, H2 and inert gas is introduced to carry out a chemical vapor deposition reaction. A dense and non-porous tantalum carbide shell (1) is deposited on the outer surface of the porous tantalum carbide substrate (2) to obtain a tantalum carbide guide tube with a porous interior and a dense and non-porous exterior.
5. The method of claim 4, wherein the method further comprises: The specific process of step S2 includes: The graphite container is placed in the reaction furnace and a vacuum leak test is performed; tantalum oxide powder is laid at the bottom of the graphite container; the temperature is raised to 2100℃~2300℃, the pressure inside the furnace is controlled at 3mbar~10mbar, and the reaction is held for 10h~20h, so that the tantalum oxide is heated and vaporized and reacts with the inner wall of the graphite container to form a dense tantalum carbide coating on the inner wall of the graphite container.
6. The method of manufacturing a conductor according to claim 5, wherein The tantalum oxide powder is laid at a height that is 10mm to 20mm lower than the top height of the target coating.
7. The method of manufacturing a conductor according to claim 4, wherein In step S3, the process parameters for the first stage of chemical vapor deposition are as follows: the molar ratio of TaCl5, H2, and inert gas is 1:(20-40):(20-60), the reaction temperature is 1500℃~1800℃, the reaction pressure is 3mbar~10mbar, and the reaction time is 5h~20h.
8. The method of manufacturing a conductor according to claim 4, wherein In step S4, the process parameters for the second stage of chemical vapor deposition are as follows: the molar ratio of TaCl5, CH4, H2, and inert gas is 1:(1-5):(20-40):(20-60), the reaction temperature is 1200℃~1600℃, the reaction pressure is 5mbar~15mbar, and the reaction time is 5h~10h.
9. The method of manufacturing a conductor according to claim 4, wherein After the first and second stages of chemical vapor deposition reaction are completed, cooling annealing is performed: the temperature is kept constant, the pressure is increased to 100 mbar to 500 mbar within 1 to 3 hours, then the temperature is reduced in stages for annealing, and finally the temperature is naturally cooled to room temperature.
10. The method of claim 9, wherein the method further comprises the step of: The segmented cooling annealing process includes: cooling to 1000-1200℃ for 6-12 hours and holding for 3-5 hours; then cooling to 400-600℃ for another 6-12 hours and holding for 3-5 hours.