Method for improving warping of MPCVD super-large discharge area multi-substrate polycrystalline diamond film

By pretreating the substrate stage, working chamber, and multiple substrates, using hydrogen and methane for nucleation, adding argon to regulate plasma distribution, and performing periodic rotation during the growth process, the problem of warpage in polycrystalline diamond films prepared by the MPCVD method was solved, achieving stress balance and warpage control, which is suitable for ultra-large discharge area multi-substrate scenarios.

CN123153166APending Publication Date: 2026-11-24CHENGDU WATERSINE ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611324354.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

When preparing polycrystalline diamond films with ultra-large discharge areas using the MPCVD method, warping problems are severe, especially when multiple substrates are grown simultaneously. Uneven stress distribution leads to varying warping sizes, affecting the processing and performance of the film.

Method used

By pre-treating the substrate stage, working chamber, and multiple substrates, nucleation is achieved using hydrogen and methane, argon is added to regulate the spatial distribution of plasma, and periodic rotation is performed during the diamond film growth process. Each substrate rotates sequentially at a preset angle, so that different directions experience the same growth time at the same position on the substrate stage. Combined with appropriate temperature parameters, isotropic stress distribution is achieved.

Benefits of technology

It effectively controls the warpage of polycrystalline diamond films to within 50μm, solving the problem of severe warpage, reducing stress concentration and geometric distortion, and is suitable for ultra-large discharge area multi-substrate scenarios, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153166A_ABST
    Figure CN123153166A_ABST
Patent Text Reader

Abstract

The application provides a method for improving warping of MPCVD super-large discharge area multi-substrate polycrystalline diamond film, and belongs to the technical field of diamond preparation. The method comprises the following steps: respectively pretreating a substrate table, a working cavity and multiple substrates, placing the substrates on the substrate table and then introducing the substrates into the working cavity; introducing hydrogen and starting microwave heating; introducing hydrogen and methane under preset nucleation conditions to perform diamond nucleation; introducing hydrogen, methane, oxygen and argon under preset growth conditions to perform diamond film growth; periodically rotating each substrate in multiple periods during the growth process, so that different directions of each substrate experience the same growth time at the same position of the substrate table; and cooling after the growth is completed to obtain polycrystalline diamond film. The application realizes isotropic distribution of stress by regulating uniformity of plasma space distribution through argon and combining periodic rotation of the substrates and temperature regulation, and can control warping degree of the super-large discharge area multi-substrate polycrystalline diamond film to be within 50 mu m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of diamond film preparation, and more specifically, to a method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD. Background Technology

[0002] Microwave plasma chemical vapor deposition (MPCVD) is one of the mainstream technologies for preparing high-quality polycrystalline diamond films. MPCVD utilizes microwaves to excite reactive gases to form plasma, depositing diamond films on the substrate surface. It has advantages such as no electrode contamination, high plasma density, and good process controllability, and has been widely used in the preparation of optical-grade and electronic-grade polycrystalline diamond films.

[0003] However, the MPCVD method for preparing polycrystalline diamond films faces a long-standing technical challenge: film warping. MPCVD equipment, limited by its resonant cavity structure, inherently exhibits a strong electric field distribution in the center and weaker at the edges. This non-uniform electric field distribution directly leads to significant radial inhomogeneity in plasma density and substrate surface temperature: the central region has a stronger electric field and higher temperature, resulting in higher stress in the grown diamond film; while the edge region has a weaker electric field and lower temperature, resulting in lower stress in the grown diamond film. This difference between the center and edges is particularly pronounced under conditions of ultra-large discharge areas (on the order of 300 mm in diameter), with stress exhibiting a gradient distribution that gradually increases from the outside to the inside in the radial direction.

[0004] The stress distribution problem becomes even more complex when multiple substrates are grown simultaneously. Because each substrate is positioned differently on the substrate stage, its local electric and temperature fields vary, leading to significant asymmetry in the stress distribution across different substrates and directions. The resulting polycrystalline diamond film exhibits varying degrees of warpage and severe geometric distortion in different directions, greatly impacting subsequent processing and performance. Summary of the Invention

[0005] The purpose of this invention is to provide a method for improving the warpage of polycrystalline diamond films with ultra-large discharge area and multiple substrates in MPCVD. This method can control the warpage of polycrystalline diamond films with ultra-large discharge area and multiple substrates to within 50 μm, effectively solving the technical problem of severe warpage of polycrystalline diamond films.

[0006] This invention is implemented as follows:

[0007] A method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD includes the following steps:

[0008] The substrate stage, working chamber, and multiple substrates are pretreated separately, and the multiple substrates are placed on the substrate stage of the MPCVD equipment and then introduced into the working chamber.

[0009] Hydrogen gas is introduced into the working cavity and microwaves are activated to heat the substrate to a specified temperature;

[0010] Under preset nucleation conditions, hydrogen gas at a first specified flow rate and methane at a first specified concentration are introduced into the working chamber to allow diamond nucleation to occur on the substrate surface.

[0011] Under preset growth conditions, hydrogen gas at a second specified flow rate, methane gas at a second specified concentration, oxygen gas at a third specified flow rate, and argon gas at a fourth specified flow rate are introduced into the working chamber to grow a diamond film on the substrate surface.

[0012] During the diamond film growth process, each substrate is rotated periodically in multiple cycles. In each cycle, the substrate is rotated in sequence at a preset angle so that each substrate experiences the same growth time at the same position on the substrate stage in different directions.

[0013] After growth, the temperature is lowered to obtain a polycrystalline diamond film.

[0014] Furthermore, within each rotation cycle, the substrate rotates sequentially in the same direction according to the initial direction, 180° rotation, 90° rotation, and 180° rotation. After each rotation step, the substrate is grown for the same amount of time under the same growth conditions.

[0015] Furthermore, the total growth time is T, the number of cycles is n, and the substrate grows for the same time t in the initial direction and after each rotation in each rotation cycle, t=(1 / 4)×(T / n), where n is a positive integer, and the substrate direction starts from the initial direction in each new cycle.

[0016] Furthermore, the number of cycles n is 1-3.

[0017] Furthermore, the fourth specified flow rate of argon gas is 500 sccm-1000 sccm.

[0018] Furthermore, the preset nucleation conditions are: power 50kW-60kW, pressure 11kPa-13kPa, substrate temperature 750℃-800℃, nucleation time 10min-60min; the first specified flow rate of hydrogen is 2000sccm-5000sccm, and the first specified concentration of methane is 3%-5%.

[0019] Furthermore, the preset growth conditions are: power 50kW-60kW, pressure 11kPa-13kPa, substrate temperature 750℃-800℃; the second specified flow rate of hydrogen is 2000sccm-5000sccm, the second specified concentration of methane is 1%-3%, and the third specified flow rate of oxygen is 1sccm-10sccm.

[0020] Furthermore, the substrate pretreatment includes: spraying diamond emulsion onto the substrate polishing surface for grinding, rinsing and wiping clean with deionized water after grinding, and then ultrasonically cleaning with anhydrous ethanol and acetone in sequence;

[0021] The pretreatment of the substrate stage and working chamber includes: treating the working surface and heat dissipation surface of the substrate stage until the surface is undamaged and cleaning it; placing the pretreated substrate stage into the working chamber and then etching and cleaning it in a hydrogen and oxygen atmosphere.

[0022] Furthermore, in the periodic rotation, each rotation includes the following steps:

[0023] Shut off all process gases except hydrogen and maintain for 30-60 minutes, then cool to room temperature and break the atmosphere.

[0024] Each substrate is rotated at a preset angle and the substrate surface is ensured to be free of foreign objects. After vacuuming again, hydrogen is introduced to start the microwave, and the power and pressure are increased to the values ​​before growth was stopped. Then, hydrogen and oxygen are introduced to etch for a specified time.

[0025] Furthermore, the specified time is 10-30 minutes; and during the diamond film growth process, the etching time increases with the number of rotations according to a preset time interval.

[0026] The beneficial effects of this invention are:

[0027] This invention improves the process in the following aspects:

[0028] 1. Pre-treatment of the substrate stage, working chamber and multiple substrates can provide a clean and uniform foundation for subsequent diamond film growth, effectively avoiding local stress concentration caused by contaminants or surface defects.

[0029] 2. By introducing hydrogen gas into the working chamber and activating microwaves to heat the substrate to a specified temperature, a stable hydrogen plasma environment can be formed, providing a suitable temperature base and active atmosphere for the nucleation and growth of diamond.

[0030] 3. Under preset nucleation conditions, hydrogen gas at a first specified flow rate and methane at a first specified concentration are introduced to carry out diamond nucleation, which can form a uniform and high-density diamond nucleus layer, laying a good crystal structure foundation for subsequent low-stress growth.

[0031] 4. Under preset growth conditions, hydrogen at a second specified flow rate, methane at a second specified concentration, oxygen at a third specified flow rate, and argon at a fourth specified flow rate are introduced to grow diamond films. The low ionization energy of argon is used to change the spatial distribution of the plasma, so that the plasma remains uniform in a larger spatial range under ultra-large discharge area conditions, thereby improving the plasma density difference between the center and the edge regions. At the same time, the temperature field is indirectly reconstructed by changing the electron temperature and active group concentration in the plasma, effectively reducing the overall stress level caused by the non-uniformity of the electric field and temperature field.

[0032] 5. During the diamond film growth process, each substrate is rotated periodically in multiple cycles, so that different directions of each substrate experience the same growth time at the same position on the substrate stage. This makes the stress accumulation in different directions of the substrate tend to be balanced, and the stress distribution changes from asymmetric to symmetric, effectively avoiding severe geometric distortion caused by stress concentration in one direction. After the growth is completed, the temperature is lowered, which can release the thermal stress accumulated during the growth process at a controllable cooling rate, avoiding the rapid increase of thermal stress caused by excessively fast cooling rate, which could lead to cracking or increased warping of the film.

[0033] After the above improvements, this invention systematically solves the technical problem of warpage of polycrystalline diamond films in multi-substrate MPCVD with ultra-large discharge area by controlling the uniformity of plasma spatial distribution with argon gas, achieving isotropic stress distribution by combining periodic substrate rotation, and combining the synergistic effect of temperature parameters from two dimensions: plasma homogenization and stress direction equalization. It achieves the excellent technical effect of controlling the warpage of polycrystalline diamond films within 50μm. Attached Figure Description

[0034] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained from these drawings without creative effort.

[0035] Figure 1 This is a flowchart of the steps in the method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD, as provided in the application embodiments.

[0036] Figure 2 This is a photograph of the diamond film prepared in Example 1 of the application.

[0037] Figure 3 This is a physical image of the diamond film prepared in Comparative Example 3. Detailed Implementation

[0038] In analyzing existing technologies, the inventors discovered that several technical solutions have been proposed to address the stress and warpage issues of MPCVD diamond films. For example, some solutions alleviate stress by pre-depositing a neutralizing material with a thermal expansion coefficient lower than that of single-crystal silicon on the substrate; others achieve active reconstruction and release of residual stress by repeatedly seeding and growing to form an elastic buffer interface; still others optimize plasma distribution uniformity by improving the substrate stage hardware structure (such as adding annular protrusions) or by adding a rotating mechanism to drive the stage to rotate continuously. However, these solutions all have their limitations: material structure-level solutions increase process complexity and cost; hardware structure improvement solutions are limited by the equipment structure, have limited adjustment space, and cannot solve the stress asymmetry problem caused by the positional differences of each substrate in multi-substrate scenarios. Setting up an independent driving mechanism for each substrate not only significantly increases cost but also makes it inconvenient to process the stage.

[0039] Please refer to Figure 1 This embodiment provides a method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD, comprising the following steps:

[0040] S110. Pre-treatment and import: The substrate stage, working chamber and multiple substrates are pre-treated respectively, and the multiple substrates are placed on the substrate stage of the MPCVD equipment and then imported into the working chamber.

[0041] S120, Heating: Hydrogen gas is introduced into the working chamber and microwaves are started to heat the substrate to the specified temperature.

[0042] S130, Nucleation: Under preset nucleation conditions, hydrogen gas at a first specified flow rate and methane at a first specified concentration are introduced into the working chamber to enable diamond nucleation on the substrate surface.

[0043] S140, Growth: Under preset growth conditions, hydrogen gas at a second specified flow rate, methane gas at a second specified concentration, oxygen gas at a third specified flow rate, and argon gas at a fourth specified flow rate are introduced into the working chamber to grow a diamond film on the substrate surface.

[0044] S150, Periodic Rotation: During the diamond film growth process, each substrate is periodically rotated in multiple cycles. In each cycle, the substrate rotates in a preset angle sequence so that each substrate experiences the same growth time at the same position on the substrate stage in different directions.

[0045] S160, Cooling: After growth is completed, the temperature is lowered to obtain a polycrystalline diamond film.

[0046] By adding argon to improve the uniformity of plasma spatial distribution and by achieving isotropic stress distribution through periodic rotation, the two work synergistically to systematically solve the warping problem of polycrystalline diamond films with ultra-large discharge areas and multiple substrates from two dimensions: plasma homogenization and stress direction equalization. Combined with appropriate temperature and other parameters, the problem can be solved effectively. Moreover, manual rotation does not require a complex structure and will not affect or damage the above equipment. It can solve the warping problem well while maintaining low cost.

[0047] In this embodiment, in step S110, the substrate stage is the core component supporting the substrate, and its surface cleanliness and thermal conductivity uniformity directly affect the temperature distribution on the substrate surface. The cleanliness of the working chamber is related to the stability of the plasma environment and the introduction of impurities during the growth process. By pretreating the substrate stage, working chamber, and substrate respectively, clean and uniform basic conditions can be provided for subsequent diamond film growth, reducing local stress concentration caused by contaminants or surface defects from the source.

[0048] As a preferred example, the substrate pretreatment includes: spraying diamond emulsion onto the substrate polishing surface for grinding, rinsing and wiping clean with deionized water after grinding, and then ultrasonically cleaning with anhydrous ethanol and acetone in sequence.

[0049] Specifically, the substrate pretreatment process is as follows: A P-type single-crystal silicon polished substrate (4 inches in size, 3.5 mm thick) is selected. Diamond emulsion (diamond micropowder W1-W10, prepared at a ratio of 1 ct diamond micropowder to 5 ml-50 ml anhydrous ethanol) is sprayed onto the polished surface of the silicon wafer. A chuck is wrapped with a lint-free cloth, and the substrate is polished by rotating clockwise or counterclockwise for 5-20 minutes. The purpose of polishing is to introduce uniform scratches and defects onto the substrate surface. These scratches and defects serve as preferential sites for diamond nucleation, significantly improving nucleation density and uniformity. After polishing, the substrate is rinsed and wiped clean with deionized water, then ultrasonically cleaned with anhydrous ethanol 1-3 times (5-15 minutes each time), and finally ultrasonically cleaned with acetone 1-3 times (5-15 minutes each time) to thoroughly remove polishing residues and organic contaminants.

[0050] As a preferred example, the pretreatment of the substrate stage and the working chamber includes: treating the working surface and heat dissipation surface of the substrate stage until the surface is undamaged and cleaning it; placing the pretreated substrate stage into the working chamber and then performing etching and cleaning in a hydrogen and oxygen atmosphere.

[0051] Specifically, the pretreatment of the substrate stage involves: using a brushed cloth to treat the working and heat dissipation surfaces of the substrate stage until they are free of damage; then ultrasonically cleaning with anhydrous ethanol 1-2 times (5-15 minutes each time); and finally wiping the working surface with acetone until it is clean and free of foreign matter. Any damage or contaminants on the surface of the substrate stage may lead to poor thermal contact between the substrate and the substrate stage, causing localized temperature anomalies and subsequently stress concentration.

[0052] Specifically, the pretreatment process for the working chamber involves placing the pretreated substrate stage into the working chamber and etching for 1-3 hours under the following conditions: power 50kW-60kW, pressure 11kPa-13kPa, hydrogen flow rate 2000sccm-3000sccm, oxygen flow rate 30sccm-50sccm, and substrate stage temperature 500℃-600℃. The purpose of etching is to use hydrogen-oxygen plasma to clean residual contaminants on the inner wall of the working chamber and the surface of the substrate stage. Simultaneously, it also activates the substrate stage surface to a certain extent, creating a clean and uniform environment for subsequent diamond growth.

[0053] In this embodiment, in step S120, during the MPCVD process, hydrogen is both the main plasma sustaining gas and one of the key reactants for diamond growth. After hydrogen is introduced and microwaves are activated, the hydrogen is excited by the microwaves to form a stable hydrogen plasma. Through the bombardment and heating of the substrate by the plasma, the substrate is uniformly heated to a suitable specified temperature, preparing for subsequent nucleation and growth steps. Preferably, the substrate temperature is raised to above 650°C within 10-30 minutes by introducing hydrogen and activating the microwaves.

[0054] In this embodiment, nucleation in step S130 is a crucial initial stage for diamond film growth. Under appropriate temperature, pressure, and methane concentration conditions, methane decomposes in hydrogen plasma to generate carbon-containing active groups. These active groups adsorb, migrate, and form diamond nuclei on the substrate surface. The nucleation density and uniformity directly affect the crystal quality and stress state of the subsequently grown diamond film. This invention ensures the formation of uniform, high-density diamond nuclei on each substrate surface through preset nucleation conditions (including hydrogen flow rate and methane concentration), laying the foundation for subsequent low-stress growth.

[0055] As a preferred example, the preset nucleation conditions are: power 50kW-60kW, pressure 11kPa-13kPa, substrate temperature 750℃-800℃, nucleation time 10min-60min; the first specified flow rate of hydrogen is 2000sccm-5000sccm, and the first specified concentration of methane is 3%-5%.

[0056] Nucleation conditions directly affect the density, size, and orientation of diamond nuclei, which in turn affect the crystal quality and stress state of the polycrystalline diamond film subsequently grown. Among the aforementioned preset conditions, a power range of 50kW-60kW is suitable for MPCVD equipment with an ultra-large discharge area (300mm diameter), capable of generating plasma with sufficient density and uniformity to ensure uniform nucleation over a large area. A pressure range of 11kPa-13kPa provides good spatial uniformity and stability of the plasma, which is beneficial for achieving uniform nucleation on large-area substrates. A substrate temperature range of 750℃-800℃ is the preferred temperature range for diamond nucleation. Lower temperatures can increase nucleation density, helping to improve film continuity, avoid large-size defects, and reduce thermal mismatch stress; higher temperatures have the opposite effect. A high methane concentration is required during the nucleation stage to provide sufficient carbon source and promote high-density nucleation. A methane concentration of 3%-5% can ensure sufficient nucleation density while avoiding the formation of non-diamond phases due to excessive carbon source. Within a nucleation time range of 10-60 minutes, a uniform and high-density diamond nucleus layer can be formed, laying the foundation for subsequent low-stress growth.

[0057] In this embodiment, step S140 involves introducing hydrogen at a second specified flow rate, methane at a second specified concentration, oxygen at a third specified flow rate, and argon at a fourth specified flow rate into the working chamber under preset growth conditions, thereby enabling diamond film growth on the substrate surface. In the MPCVD process, argon has a low ionization energy. By adding argon to the reaction atmosphere during the growth stage, the spatial distribution characteristics of the plasma can be altered, allowing the plasma to remain uniform over a larger spatial area, thus improving the plasma density difference between the center and edge regions under ultra-large discharge area conditions. Furthermore, the addition of argon can indirectly affect the temperature field distribution and growth rate distribution on the substrate surface by changing the electron temperature and active group concentration in the plasma, playing a role in temperature field reconstruction and effectively reducing the overall stress level caused by uneven electric and temperature fields.

[0058] As a preferred example, the preset growth conditions are: power 50kW-60kW, pressure 11kPa-13kPa, substrate temperature 750℃-800℃; second specified flow rate of hydrogen is 2000sccm-5000sccm, second specified concentration of methane is 1%-3%, and third specified flow rate of oxygen is 1sccm-10sccm.

[0059] Growth conditions are decisive factors in the quality and stress of polycrystalline diamond films. In the aforementioned growth conditions, the power and pressure are maintained within the same range as in the nucleation stage (power 50kW-60kW, pressure 11kPa-13kPa) to ensure the continuity and stability of the plasma state during growth and avoid stress abrupt changes due to sudden changes in power or pressure. The substrate temperature is set to 750℃-800℃, with the growth stage slightly higher than the nucleation stage, which is beneficial for steady-state diamond growth and improved crystal quality. Within this temperature range, the diamond growth rate is moderate, and the crystal defect density is low, which is conducive to obtaining high-quality, low-stress polycrystalline diamond films. The methane concentration is set to 1%-3%, with the growth stage methane concentration lower than the nucleation stage, which is beneficial for preferential diamond crystal growth and improved crystal quality. The lower methane concentration can suppress secondary nucleation and the formation of non-diamond phases, resulting in polycrystalline diamond films with larger grain sizes and higher crystal quality.

[0060] The oxygen flow rate is 1-10 sccm. The addition of oxygen has multiple functions: first, it etches non-diamond phases (such as graphite and amorphous carbon), improving the purity of the diamond film; second, it affects the diamond growth rate and crystal orientation by adjusting the concentration of oxygen-active groups in the plasma; and third, the appropriate amount of oxygen helps reduce stress in the film. Too low an oxygen flow rate (<1 sccm) results in insignificant etching; too high an oxygen flow rate (>10 sccm) may lead to a significant decrease in diamond growth rate or even etching of the diamond.

[0061] In this embodiment, in step S150, the inventors, through in-depth research, recognized that during multi-substrate MPCVD growth, due to differences in electric field strength and temperature at different locations on the substrate stage, different directions of the same substrate, if subjected to different growth times and conditions at different locations on the substrate stage, will result in diamond films deposited in different directions having different microstructures and stress states, ultimately manifesting as macroscopic asymmetric warping. By periodically rotating each substrate during the growth process, each direction of the substrate can undergo the same growth time at various locations on the substrate stage (including locations with strong and weak electric fields). This makes the stress accumulation in different directions of the substrate tend to be balanced, and the stress distribution changes from asymmetric to symmetric, effectively avoiding severe geometric distortion caused by stress concentration in a single direction.

[0062] As a preferred example, in each of the above cycles, the substrate is rotated in the same direction in the order of initial direction, rotation 180°, rotation 90°, and rotation 180°. After each rotation step, the substrate is grown for the same amount of time under the same growth conditions.

[0063] Extensive experiments revealed that the rotation sequence "initial direction → 180° → 90° → 180°" achieves optimal stress equalization. The mechanism lies in the fact that within the plane of the substrate stage, the distribution of electric and temperature fields often differs in the orthogonal directions (0° / 90°) and diagonal directions (45° / 135°). Through the four-step rotation of "initial direction → 180° → 90° → 180°," the substrate grows on the substrate stage at four angles (0°, 180°, 90°, 270°), precisely covering the four orthogonal directions of the substrate plane. Each growth step takes the same amount of time, ensuring that each direction of the substrate experiences exactly the same growth time at each corresponding position on the substrate stage.

[0064] Compared to simpler methods that rotate 90° or 180° per step, the four-step rotation sequence of this invention can more comprehensively cover the spatial distribution characteristics of the substrate's electrostatic and temperature fields. Compared to random or multi-angle rotation, the rotation sequence of this invention has the advantages of simple operation, precise angles, and ease of industrial implementation. From the perspective of stress equalization, this rotation sequence ensures that stress accumulation in different directions of the substrate is completely symmetrical, fundamentally eliminating the root cause of asymmetric warping.

[0065] As a preferred example, the total growth time of the above growth process is T, the number of cycles is n, and the substrate grows for the same time t in the initial direction and after each rotation in each cycle, t=(1 / 4)×(T / n), where n is a positive integer, and the substrate direction starts from the initial direction in each new cycle.

[0066] Understandably, assuming the total growth time is T and there are n cycles, the growth time for each cycle is T / n. In each cycle, the substrate needs to grow once in each of the four directions (initial direction, 180°, 90°, 180°), so the growth time in each direction is (T / n) / 4 = T / (4n).

[0067] The precise time allocation ensures that each substrate undergoes the same growth time at the same location on the substrate stage in different directions, guaranteeing isotropic stress distribution. If the growth times are unequal in each direction, the stress accumulation in different directions will differ, still resulting in asymmetric warping. Furthermore, the substrate orientation starts from the initial orientation in each new cycle, ensuring directional consistency between cycles and avoiding stress accumulation deviations caused by improper cycle transitions.

[0068] As a preferred example, the number of cycles n is 1-3. Understandably, from the theoretical perspective of stress equalization, a larger number of cycles results in more frequent switching of the substrate across different positions on the substrate stage, leading to better stress equalization. However, in actual industrial production, increasing the number of cycles means more frequent shutdowns, vacuuming, substrate rotation, re-vacuuming, and growth resumption. Each rotation operation increases process complexity and operational steps. Theoretically, if each stage can be driven by a motor to achieve continuous uniform rotation of the substrate during growth, the stress in each direction can achieve perfect equilibrium. However, in industrial environments with ultra-large discharge areas (300mm diameter) and high-temperature microwaves (50kW-60kW power), continuous rotation mechanisms face numerous engineering challenges, including sealing reliability, microwave shielding, and independent driving of multiple substrates. Equipment modification costs are high, and long-term operational stability is difficult to guarantee.

[0069] In contrast, the intermittent rotation scheme adopted in this application requires no hardware modification to existing MPCVD equipment and can be implemented solely through process operation, demonstrating significant industrial application value and immediate usability. Considering both warpage reduction and process operability, the inventors determined through extensive experimentation that a cycle number n of 1-3 is optimal. With one cycle (n=1), the substrate only needs to be rotated three times during growth, making operation extremely simple, and warpage can be controlled within 50 μm. When n=2 or 3, the number of rotations increases accordingly, further reducing warpage. Beyond three cycles, the warpage reduction tends to saturate, and the increased number of process steps also increases the potential impact on the stability and consistency of the long-term growth process. Therefore, limiting the cycle number to 1-3 is the optimal choice while ensuring excellent warpage control and balancing process feasibility and ease of operation.

[0070] As a preferred example, the argon flow rate specified in the fourth example is 500 sccm-1000 sccm. If the argon flow rate is too low (e.g., below 500 sccm), its effect on improving the uniformity of plasma spatial distribution is not significant, and it cannot effectively alleviate the difference in plasma density between the center and the edge under ultra-large discharge area conditions; if the argon flow rate is too high (e.g., above 1000 sccm), it will lead to plasma instability and uneven discharge. At the same time, excessively high argon partial pressure will change the proportion of hydrocarbon active groups in the plasma, which may lead to diamond grain refinement or even nano-sized grains, thus degrading the quality of the film.

[0071] Through systematic experiments, the inventors determined that an argon flow rate in the range of 500 sccm-1000 sccm can effectively improve the spatial distribution uniformity of the plasma, achieve temperature field reconstruction, and reduce the overall stress level while ensuring stable plasma discharge.

[0072] More preferably, the effect is better when the argon flow rate is 500sccm-600sccm, as the plasma stability is best within this range and there is no risk of diamond nanoforming.

[0073] As a preferred example, each rotation in the periodic rotation includes the following steps: shutting off the process gases except for hydrogen and maintaining this for 30-60 minutes, cooling to room temperature and then breaking the vacuum; rotating each substrate at a preset angle and ensuring that there are no foreign objects on the substrate surface, re-evacuating the vacuum and then introducing hydrogen to start the microwave, increasing the power and pressure to the values ​​before stopping the growth, and then introducing hydrogen and oxygen for etching for a specified time.

[0074] In actual production, substrate rotation cannot be performed directly under vacuum and high temperature conditions, therefore a complete intermediate operation process is required, the specific process of which is as follows:

[0075] Step 1: Gas Shutdown and Temperature Insulation. Shut down all process gases except hydrogen (including methane, oxygen, argon, etc.), maintaining only a hydrogen atmosphere for 30-60 minutes. The purpose of this operation is to maintain the temperature in a hydrogen atmosphere for a certain period of time after growth stops, releasing some of the thermal stress.

[0076] Step 2: Cooling. The substrate temperature is lowered to room temperature under a hydrogen atmosphere over 3-6 hours at a rate of 3-4°C / min. Slow cooling aims to prevent a rapid increase in thermal stress that could lead to film cracking or increased warping.

[0077] Step 3: Vacuuming and Rotation. After the substrate temperature drops to room temperature, vacuuming (restoring the working chamber from a vacuum state to atmospheric pressure) is performed. Each substrate is rotated at a preset angle, ensuring that there are no foreign objects on the substrate surface. The specific vacuuming operation is as follows: First, the vacuum level of the chamber is evacuated to 10... -3 Below Pa, slowly fill with air to avoid contamination of the substrate surface due to airflow impact.

[0078] Step 4: Re-evacuate and reheat. After rotation, re-evacuate the working chamber to 10°C. -3 Below Pa, hydrogen gas is introduced to start the microwave, and the power and pressure are increased to the values ​​before growth was stopped within 30-60 minutes. This process requires strict control of the heating rate and power ramp-up rate to avoid thermal shock caused by sudden parameter changes.

[0079] Step 5: Etching. Introduce hydrogen (2000 sccm-5000 sccm) and oxygen (10 sccm-30 sccm) and etch for 10-30 minutes. The main purpose of etching is to remove foreign matter that has fallen onto the diamond surface after being removed and repositioned. If this foreign matter is encapsulated in the subsequently grown diamond film, it will become a source of localized stress concentration. As the growth time increases and the grain size continues to increase, the secondary nucleation of the encapsulated foreign matter worsens, exacerbating the stress concentration problem.

[0080] Furthermore, the specified etching time is 10-30 minutes; and during the diamond film growth process, the etching time increases with the number of rotations according to the preset time interval.

[0081] As the growth process progresses, the thickness of the diamond film increases, the grain size gradually enlarges, and the morphology of the film surface also changes. In the early stages of growth, the grain size is small, the film surface is relatively smooth, and foreign objects that fall off are easily etched away; however, in the later stages of growth, the grain size increases significantly, the film surface becomes uneven, and foreign objects easily embed themselves in the gaps between the grains, making removal more difficult.

[0082] Specifically, the etching time can be increased by 5 minutes with each rotation. For example, the first rotation etching takes 10 minutes, the second rotation etching takes 15 minutes, the third rotation etching takes 20 minutes, and so on. This incremental etching time design ensures that foreign matter on the substrate surface can be effectively removed at different growth stages, avoiding local stress concentration and secondary nucleation deterioration caused by foreign matter encapsulation, thereby ensuring the continuity and consistency of stress control throughout the entire growth process.

[0083] In this embodiment of the application, in step S160, after the growth is completed, the temperature is slowly reduced to room temperature by programmed temperature control to avoid the rapid increase in thermal stress caused by the rapid cooling rate, which could lead to cracking or increased warping of the film.

[0084] The polycrystalline diamond film prepared using the method of this invention exhibits a warpage controllable within 50 μm. In contrast, comparative samples prepared using conventional processes (without rotation, without argon gas, or with improper temperature, etc.) generally show warpage exceeding 500 μm, and in severe cases reaching 3000 μm. This invention reduces warpage by more than an order of magnitude. By periodically rotating the substrate, this invention achieves a more balanced stress accumulation in all directions, fundamentally solving the problem of asymmetric stress distribution in multi-substrate MPCVD. Furthermore, the method requires no hardware modification to existing MPCVD equipment; it can be achieved simply by adjusting process parameters (adding argon gas, increasing rotation operation, and adjusting temperature), demonstrating significant industrial application value. It is particularly suitable for multi-substrate scenarios with ultra-large discharge areas (300 mm in diameter), solving the industry challenge of warpage control in this specific scenario and providing a feasible technical solution for the large-scale production of large-size polycrystalline diamond films.

[0085] The present invention will now be clearly and completely described in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are merely a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0086] Example 1

[0087] This embodiment provides a method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD, specifically including the following steps:

[0088] 1. Substrate pretreatment

[0089] A 4-inch, 3.5mm thick P-type monocrystalline silicon substrate was selected. Diamond emulsion was prepared by mixing diamond micropowder (W1-W10) at a ratio of 1 ct to 10 ml of anhydrous ethanol. The diamond emulsion was sprayed onto the polished surface of the silicon wafer, and a suction cup wrapped with a lint-free cloth was used for clockwise grinding for 10 minutes. After grinding, the wafer was rinsed and wiped clean with deionized water, then ultrasonically cleaned twice with anhydrous ethanol (10 minutes each time), and finally ultrasonically cleaned twice with acetone (10 minutes each time).

[0090] 2. Pre-treatment before process

[0091] Substrate stage pretreatment: Use a brushed cloth to treat the working surface and heat dissipation surface of the substrate stage until the surface is undamaged, ultrasonically clean it twice with anhydrous ethanol (10 minutes each time), and then wipe the working surface with acetone until the surface is clean and free of foreign matter.

[0092] Pretreatment of the working chamber: The pretreated substrate stage is placed into the working chamber and etched for 2 hours under the conditions of 55kW power, 12kPa pressure, 2500sccm hydrogen flow rate, 40sccm oxygen flow rate, and 550℃ substrate stage temperature.

[0093] 3. Equipment vacuum inspection

[0094] The working chamber pressure rise rate is ≤1 Pa / h.

[0095] 4. Substrate introduction

[0096] Place the pretreated substrate into the substrate stage, ensuring the substrate surface is free of foreign objects. Place the substrate stage, along with the substrate, into the working chamber, and slowly evacuate the working chamber to 10°C using the vacuum pump. -3 Below Pa.

[0097] 5. Substrate heating

[0098] The microwave was started by introducing hydrogen gas (2500 sccm), and the substrate temperature was raised to 650°C within 20 minutes.

[0099] 6. Nucleation

[0100] Nucleation was performed for 30 minutes under the following conditions: power 55kW, pressure 12kPa, hydrogen flow rate 3500sccm, methane concentration 4%, and substrate temperature 750℃.

[0101] 7. Polycrystalline growth

[0102] Basic growth conditions: power 57kW, pressure 12.5kPa, hydrogen flow rate 3500sccm, methane concentration 2%, oxygen flow rate 5sccm, argon flow rate 550sccm, substrate temperature 780℃, total growth time T=120h.

[0103] In this embodiment, the number of cycles n=2, meaning two complete cycles are performed. The substrate rotation sequence within each cycle is: initial orientation → 180° clockwise rotation → 90° clockwise rotation → 180° clockwise rotation. The growth time for each direction within each cycle is t=(1 / 4)×(T / n)=(1 / 4)×(120 / 2)=15h. The specific operation is as follows:

[0104] First cycle:

[0105] The initial growth direction was 15 hours, and then the operation was carried out in sequence as follows: gas shut-off and heat preservation → cooling → cavitation breaking → rotation 180° → re-vacuuming → heating → etching. The etching time was 15 minutes.

[0106] After rotating 180° clockwise, grow for 15 hours; then follow the same intermediate processing steps, etching for 20 minutes (increasing by 5 minutes for each rotation).

[0107] After rotating 90° clockwise, grow for 15 hours; then follow the same intermediate processing steps, etching for 25 minutes.

[0108] After rotating 180° clockwise, it grows for 15 hours. The first cycle is complete, with a growth time of 60 hours.

[0109] Second cycle: Starting from the initial substrate orientation, repeat the operation of the first cycle (rotation sequence remains initial orientation → 180° → 90° → 180°), with a growth time of 15 hours for each orientation. After the second cycle is completed, the total growth time is 120 hours.

[0110] 8. Cooling

[0111] After growth is complete, all process gases except hydrogen are shut off, and a hydrogen atmosphere is maintained for 40 minutes. Then, the temperature is reduced to room temperature at a rate of 3.5 °C / min for 4.5 hours.

[0112] 9. Results

[0113] The polycrystalline diamond film prepared by the above method has a warpage of 35 μm, as measured by testing. Figure 2 The image shown is a physical picture of the diamond film obtained in this embodiment.

[0114] Example 2

[0115] The only difference between this embodiment and Embodiment 1 is that the argon flow rate is 800 sccm, the number of cycles n=1 (i.e., only one complete cycle is performed, and the growth time in each direction is t=30h), while the other conditions are the same as in Embodiment 1. The warpage of the obtained polycrystalline diamond film was measured to be 48 μm.

[0116] Example 3

[0117] The only difference between this embodiment and Embodiment 1 is that the number of cycles n=3 (i.e., 3 complete cycles are performed, and the growth time in each direction is t=10h), while the other conditions are the same as in Embodiment 1. The warpage of the obtained polycrystalline diamond film was tested to be 22μm.

[0118] To verify the technical effects of the present invention, the following comparative examples are provided:

[0119] Comparative Example 1: The only difference from Example 1 is that the substrate temperature during the growth stage is 850°C. The obtained polycrystalline diamond film exhibits a warpage ≥1000 μm.

[0120] Comparative Example 2: The only difference from Example 1 is that the substrate is not rotated or rotated for an integer number of cycles. The obtained polycrystalline diamond film was tested to have a warpage ≥1000 μm.

[0121] Comparative Example 3: The only difference from Example 1 is the absence of argon gas (argon flow rate was 0 sccm). Testing showed that the obtained polycrystalline diamond film had a warpage ≥500 μm. Figure 3 The image shown is a physical picture of the diamond film obtained in this comparative example.

[0122] Comparative Example 4: The difference from Example 1 is that the substrate temperature is 850°C and the substrate is not rotated. Testing showed that the warpage of the obtained polycrystalline diamond film was ≥2000 μm.

[0123] Comparative Example 5: The difference from Example 1 is that the substrate temperature is 850°C and no argon gas is added. Testing showed that the warpage of the obtained polycrystalline diamond film was ≥1500 μm.

[0124] Comparative Example 6: The difference from Example 1 is that the substrate is not rotated and no argon gas is added. The obtained polycrystalline diamond film exhibits a warpage ≥2000 μm.

[0125] Comparative Example 7: The difference from Example 1 is that the substrate temperature is 850°C, the substrate is not rotated, and no argon gas is added. Testing showed that the warpage of the obtained polycrystalline diamond film was ≥3000 μm.

[0126] The results of the above embodiments and comparative examples fully demonstrate that the synergistic effect of the two core features of periodic substrate rotation and argon gas addition in this invention can significantly reduce the warpage of polycrystalline diamond films, controlling the warpage to within 50 μm, effectively solving the technical problem of severe warpage in polycrystalline diamond films. The low-warpage polycrystalline diamond film prepared using the method of this invention can be applied in fields such as optical windows, heat dissipation substrates for high-power devices, and semiconductor substrates, and has broad industrial application prospects.

[0127] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the invention by those skilled in the art. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the invention should be included within the scope of protection of the invention.

Claims

1. A method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD, characterized in that, Includes the following steps: The substrate stage, working chamber, and multiple substrates are pretreated to provide clean and uniform basic conditions for subsequent diamond film growth, and to avoid local stress concentration caused by contaminants or surface defects. The multiple substrates are placed on the substrate stage of the MPCVD equipment and then introduced into the working cavity; Hydrogen gas is introduced into the working cavity and microwaves are activated to heat the substrate to a specified temperature; Under preset nucleation conditions, hydrogen gas at a first specified flow rate and methane at a first specified concentration are introduced into the working chamber to allow diamond nucleation to occur on the substrate surface. Under preset growth conditions, hydrogen gas at a second specified flow rate, methane gas at a second specified concentration, oxygen gas at a third specified flow rate, and argon gas at a fourth specified flow rate are introduced into the working chamber to grow a diamond film on the substrate surface. During the diamond film growth process, each substrate is rotated periodically in multiple cycles. In each cycle, the substrate is rotated in sequence at a preset angle so that each substrate experiences the same growth time at the same position on the substrate stage in different directions. After growth, the temperature is lowered to obtain a polycrystalline diamond film.

2. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 1, characterized in that, Within each rotation cycle, the substrate rotates in the same direction sequentially in the order of initial direction, 180° rotation, 90° rotation, and 180° rotation. After each rotation step, the substrate is grown for the same amount of time under the same growth conditions.

3. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 2, characterized in that, The total growth time is T, and the number of cycles is n. In each rotation cycle, the substrate grows for the same time t in the initial direction and after each rotation, t = (1 / 4) × (T / n); where n is a positive integer, and the substrate direction starts from the initial direction in each new cycle.

4. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 3, characterized in that, The number of cycles n is 1-3.

5. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 1, characterized in that, The fourth specified flow rate of argon gas is 500 sccm-1000 sccm.

6. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 1, characterized in that, The preset nucleation conditions are: power 50kW-60kW, pressure 11kPa-13kPa, substrate temperature 750℃-800℃, nucleation time 10min-60min; the first specified flow rate of hydrogen is 2000sccm-5000sccm, and the first specified concentration of methane is 3%-5%.

7. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 6, characterized in that, The preset growth conditions are: power 50kW-60kW, pressure 11kPa-13kPa, substrate temperature 750℃-800℃; the second specified flow rate of hydrogen is 2000sccm-5000sccm, the second specified concentration of methane is 1%-3%, and the third specified flow rate of oxygen is 1sccm-10sccm.

8. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 1, characterized in that, The substrate pretreatment includes: spraying diamond emulsion onto the substrate polishing surface for grinding, rinsing and wiping it clean with deionized water after grinding, and then ultrasonically cleaning it with anhydrous ethanol and acetone in sequence. The pretreatment of the substrate stage and working chamber includes: treating the working surface and heat dissipation surface of the substrate stage until the surface is undamaged and cleaning it; placing the pretreated substrate stage into the working chamber and then etching and cleaning it in a hydrogen and oxygen atmosphere.

9. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 1, characterized in that, Each periodic rotation includes the following steps: Shut off all process gases except hydrogen and maintain for 30-60 minutes, then cool to room temperature and break the atmosphere. Each substrate is rotated at a preset angle and the substrate surface is ensured to be free of foreign objects. After vacuuming again, hydrogen is introduced to start the microwave, and the power and pressure are increased to the values ​​before growth was stopped. Then, hydrogen and oxygen are introduced to etch for a specified time.

10. The method for improving the warpage of multi-substrate polycrystalline diamond films with ultra-large discharge area in MPCVD according to claim 9, characterized in that, The specified time is 10-30 minutes; and during the diamond film growth process, the etching time increases with the number of rotations according to a preset time interval.