Silicon core furnace and silicon core drawing method

By employing a differential component design with inner and outer sleeves in the silicon core furnace, and utilizing the difference in thermal expansion coefficients for precise compensation, the problem of inconsistent silicon core growth rates was solved, thereby improving the pulling quality and stability of silicon cores.

CN123153167APending Publication Date: 2026-11-24NINGXIA JINGCHUANG INTELLIGENT EQUIP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611307574.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the process of preparing polycrystalline silicon cores using the Czochralski method, the non-uniformity of the thermal field in the silicon core furnace leads to inconsistent growth rates of each silicon core, and the hard-connected structure causes problems such as core breakage, core bending, or diameter deviation.

Method used

The differential component design employs an inner sleeve and an outer sleeve. The inner sleeve is made of refractory metal, while the outer sleeve is made of high-temperature alloy. By setting the difference in the thermal expansion coefficient of the differential component, precise compensation and stable control of the silicon core growth rate can be achieved.

Benefits of technology

This effectively improves the pulling quality of each silicon core, avoids core breakage and diameter deviation caused by uneven thermal field, and achieves efficient and stable growth of silicon cores.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153167A_ABST
    Figure CN123153167A_ABST
Patent Text Reader

Abstract

This application provides a silicon core furnace and a silicon core pulling method, belonging to the field of silicon core preparation technology, and solves the problem that the pulling quality of each silicon core cannot be guaranteed when pulling simultaneously in the prior art. The silicon core furnace of this application includes: a furnace body, a pulling base, a pulling assembly, and a differential assembly. The furnace body is equipped with a crucible and a heater surrounding the crucible. The pulling base is located at the top of the furnace body and has vertical lifting freedom. The pulling assembly includes a pulling column and grippers. The differential assembly includes an inner sleeve and an outer sleeve. The inner sleeve is made of a material with a first coefficient of thermal expansion, and the outer sleeve is made of a material with a second coefficient of thermal expansion, the second coefficient of thermal expansion being greater than the first coefficient of thermal expansion. This application ensures that the macroscopic pulling force of the pulling base is directly and without hysteresis transmitted to the silicon core by rigidly connecting the inner sleeve and the pulling column, avoiding tension loss due to flexible connections.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of silicon core preparation technology, specifically, it relates to a silicon core furnace and a silicon core pulling method. Background Technology

[0002] In the Czochralski (CZ) method for preparing polycrystalline silicon cores, multi-core simultaneous pulling technology is typically employed to improve production efficiency. However, the thermal field within the silicon core furnace is affected by heater layout, aging of insulation structures, and airflow disturbances, making it difficult to achieve absolutely uniform silicon melt temperature in different areas of the crucible.

[0003] Existing technologies mostly employ a structure where the seed crystal and the pulling mechanism are rigidly connected. When uneven thermal fields cause different growth rates for each silicon core, the rigid connection can result in the faster-growing silicon cores experiencing insufficient stress (or even relaxation), while the slower-growing silicon cores experience stress exceeding the set threshold, which can easily lead to core breakage, bending, or diameter deviation.

[0004] Based on the above, the technical problem of this application is: how to ensure the pulling quality of each silicon core. Summary of the Invention

[0005] The purpose of this application is to address the aforementioned problems in the prior art by proposing a silicon core furnace and a silicon core pulling method, which solves the problem that the pulling quality of each silicon core cannot be guaranteed when pulling simultaneously in the prior art, and effectively improves the pulling quality of each silicon core.

[0006] The objective of this application can be achieved through the following technical solution: A silicon core furnace, comprising: a furnace body, wherein a crucible and a heater surrounding the crucible are disposed within the furnace body; a lifting base, wherein the lifting base is disposed on the top of the furnace body and has a vertical lifting freedom; a lifting assembly, wherein the lifting assembly comprises: a plurality of lifting columns, which are respectively connected below the lifting base; a gripper, wherein the gripper is disposed on the lifting column for gripping a seed crystal; and a differential assembly, wherein the number of differential assemblies is the same as the number of lifting assemblies, the differential assembly comprising: an inner sleeve, wherein the upper end of the inner sleeve is connected to the lifting base, and the lower end of the inner sleeve is rigidly connected to the upper end of the lifting column; and an outer sleeve, wherein the outer sleeve is sleeved outside the inner sleeve, and the lower end of the outer sleeve forms an axial displacement constraint on the lower end of the inner sleeve; wherein the inner sleeve is made of a material having a first coefficient of thermal expansion, and the outer sleeve is made of a material having a second coefficient of thermal expansion, the second coefficient of thermal expansion being greater than the first coefficient of thermal expansion. Understandably, by rigidly connecting the inner sleeve to the lifting column, the macroscopic lifting force of the lifting base is directly and without lag transmitted to the silicon core, avoiding tension runaway caused by flexible connections. By setting a nested structure for the outer sleeve, the thermal expansion of the outer sleeve is limited to the path of action constraining the displacement of the inner sleeve, rather than being superimposed on the lifting stroke, thus structurally avoiding the defect of a single thermal expansion rod exacerbating growth differences. By constraining the axial displacement of the lower end of the outer sleeve, the greater thermal expansion of the outer sleeve is used to offset the thermal expansion of the inner sleeve, converting thermal expansion into a negative feedback fine-tuning force rather than a positive driving force, adapting to the scenario of active movement of the lifting base. By configuring the thermal expansion coefficient of the outer sleeve material to be greater than that of the inner sleeve, a physical basis for differential displacement is provided. The greater the temperature difference, the greater the relative displacement difference, naturally matching the radial temperature field of the central cold and the central outer ring inside the furnace.

[0007] In the aforementioned silicon core furnace, the inner sleeve is made of molybdenum, niobium, tungsten, or their alloys, while the outer sleeve is made of austenitic stainless steel, nickel-chromium-based high-temperature alloys, or cobalt-based high-temperature alloys. The difference between the first and second coefficients of thermal expansion is not less than 10 × 10⁻⁶ / ℃. It is understood that by using an inner sleeve made of a refractory metal, its axial stiffness remains stable below 600℃, preventing high-temperature creep and avoiding deformation of the inner sleeve itself from affecting compensation accuracy. The outer sleeve made of a high-temperature alloy ensures oxidation resistance and no strength reduction under long-term high temperatures, adapting to the long-cycle crystal pulling conditions of the silicon core furnace. The difference in thermal expansion coefficient α between the two is configured to be not less than 10 × 10⁻⁶ / ℃. -6 / ℃: Ensures that within the temperature range of 100℃~600℃, the relative expansion difference between the inner and outer sleeves is sufficient to cover the growth rate difference of 0.1mm / min~0.5mm / min commonly seen in silicon cores, without the need for additional scaling up of the structural dimensions.

[0008] In the aforementioned silicon core furnace, the inner sleeve is made of molybdenum-titanium-zirconium alloy, and its coefficient of thermal expansion is 4.5×10⁻⁶ / ℃ to 5.8×10⁻⁶ / ℃ in the range of 100℃ to 600℃; the outer sleeve is made of 253MA austenitic heat-resistant stainless steel, and its coefficient of thermal expansion is 17.5×10⁻⁶ / ℃ to 19.0×10⁻⁶ / ℃ in the range of 100℃ to 600℃; wherein, the difference between the coefficients of thermal expansion of the inner sleeve and the outer sleeve in the range of 100℃ to 600℃ is 12.5×10⁻⁶ / ℃ to 14.5×10⁻⁶ / ℃. Understandably, by using an inner sleeve made of TZM material, which combines the high melting point and low expansion characteristics of molybdenum with the high-temperature strength enhancement of titanium-zirconium alloy, achieving a tensile strength retention rate of ≥70% at 600℃, it is the most suitable low-cost solution for silicon core furnace conditions among refractory metals. The outer sleeve, made of 253MA material with added cerium and nitrogen, has an oxidation resistance temperature reaching 1150℃, and the difference in thermal expansion coefficient between it and TZM perfectly matches the growth rate difference required by the 30℃~50℃ radial temperature difference in silicon core furnaces, achieving precise compensation without additional adjustments. By configuring a 12.5×10 -6 / ℃~14.5×10 -6 The difference in thermal expansion coefficient α at / ℃ was verified by simulation. Under this difference, a radial temperature difference of 100℃ can produce a differential displacement of 0.125mm / h to 0.145mm / h, which can just offset the growth difference of 0.2mm / min to 0.4mm / min of the multi-silicon core, and the compensation accuracy can reach ±0.05mm / min.

[0009] The aforementioned silicon core furnace also includes a metal sheath, which covers the inner sleeve and / or the outer sleeve on the side facing the furnace. The purity of the metal sheath is not less than 99.95%. It is understood that by using a high-purity metal sheath, the molybdenum / niobium / tungsten material itself is a shallow donor impurity of silicon, and the sheath purity is ≥99.95%, preventing the introduction of deep-energy silicon impurities such as Fe, Cr, Ni, and Ti, thus fundamentally avoiding contamination of the silicon melt by the volatilization of the matrix alloy. By covering the side facing the furnace with the metal sheath, all exposed surfaces in contact with the furnace atmosphere can be fully covered, including the outer cylindrical surface and lower end face of the inner and outer sleeves, eliminating contamination dead zones and achieving a zero-metal contamination crystal pulling environment. The core indicators of the silicon core, such as minority carrier lifetime and resistivity uniformity, can meet semiconductor-grade requirements, adapting to the production needs of polycrystalline silicon reduction carriers.

[0010] In the aforementioned silicon core furnace, the metal sheath is made of molybdenum, niobium, or tungsten. The metal sheath is sealed to the outer wall of the inner sleeve and / or the inner wall of the outer sleeve via vacuum electron beam welding or argon arc welding. The space between the metal sheath and the substrate of the inner / outer sleeve is either vacuum-sealed or filled with alumina powder. It is understood that the vacuum electron beam / argon arc welding seal prevents the sheath from detaching at high temperatures and also prevents base alloy atoms from volatilizing into the furnace through the weld gaps. The vacuum / alumina filling between the metal sheath and the substrate of the inner / outer sleeve eliminates the gap between the sheath and the substrate, preventing residual gas in the gap from expanding due to heat and causing the sheath to bulge or detach at high temperatures. Simultaneously, the alumina powder further improves heat conduction efficiency and prevents localized overheating.

[0011] In the aforementioned silicon core furnace, a sliding mating surface is provided between the inner sleeve and the outer sleeve. This sliding mating surface is coated or laminated with a solid lubricating coating, which is a molybdenum disulfide, graphite, or hexagonal boron nitride coating, with a thickness of 5 μm to 20 μm. It is understood that by providing a solid lubricating coating, good lubrication performance is maintained even at a high temperature of 600℃, with a friction coefficient as low as 0.05 to 0.1, avoiding the stick-slip effect caused by direct metal contact. By limiting the thickness of the solid lubricating coating to 5 μm to 20 μm, lubrication effectiveness is ensured without causing blockage of the sliding gap or restriction of differential displacement due to excessive coating thickness.

[0012] In the aforementioned silicon core furnace, the axial stiffness of the inner sleeve is not less than 1×10⁻⁶. 6 N / m, the axial stiffness of the outer sleeve is not less than 5×10 N / m. 5 N / m. Understandably, the high axial stiffness design ensures that the axial fine-tuning force applied to the outer sleeve only causes nanometer-level elastic deformation of the inner sleeve, without causing macroscopic elongation of the inner sleeve. This prevents the outer sleeve from moving along with the inner sleeve. By designing a stiffness difference between the outer and inner sleeves—with the outer sleeve's stiffness slightly lower than the inner sleeve—the fine-tuning force of the outer sleeve is preferentially applied to the silicon core growth resistance, rather than its own deformation. Force transmission efficiency is ≥99%, ensuring the force transmission accuracy of the differential module, with a compensation error ≤1%. This avoids excessive or insufficient compensation due to insufficient stiffness, improving process stability.

[0013] In the aforementioned silicon core furnace, a water-cooling channel is provided within the lifting base. This water-cooling channel acts on the bottom of the lifting base to cool the top ends of the outer sleeve and the inner sleeve. It is understood that by cooling the connection points at the upper ends of the outer and inner sleeves, the temperature of the connection area between the inner and outer sleeves and the lifting base is controlled below 200℃. This prevents high temperatures from causing a drift in the material's thermal expansion coefficient and creep loosening of the connecting bolts. Directional cooling is achieved, cooling only the upper non-working area without affecting the thermal expansion of the lower working area, ensuring that differential displacement is not disturbed by cooling.

[0014] The aforementioned silicon core furnace also includes multiple acoustic emission sensors. Each acoustic emission sensor is installed inside the lifting base and located on the outer side of the water-cooling channel in the radial direction. The detection end of each acoustic emission sensor acts on the bottom of the lifting base to detect whether the differential component below generates jamming sound waves. The acoustic emission sensors are electrically connected to the drive end of the lifting base. It is understood that placing the acoustic emission sensors on the outer side of the water-cooling channel in the radial direction allows them to be in contact with the outer wall of the water-cooling channel, thereby utilizing the cooling effect of the water-cooling channel to control the operating temperature of the acoustic emission sensors at a lower temperature and avoid high-temperature damage. The acoustic emission sensors can directly pick up the jamming friction sound waves of the differential component and the micro-fracture sound waves before the silicon core breaks, and can feed back signals to the drive end of the lifting base to execute stop or deceleration drive operations.

[0015] Another objective of this application is to provide a silicon core pulling method, applied to the silicon core furnace described in this application, comprising the following steps: starting the heater to form a stable temperature field inside the furnace, and the inner and outer sleeves of each group of differential components undergoing thermal expansion as the temperature rises; driving the lifting base to descend so that the seed crystal contacts the molten metal; The lifting base is controlled to rise at a speed V. Utilizing the difference in thermal elongation of the outer sleeve at different radial positions, an axial fine-tuning force is applied to the inner sleeve through the constraint of the lower end of the outer sleeve, adjusting the growth rate of each silicon core and ensuring that the effective lifting stroke of each lifting column relative to the lifting base is consistent. After growth, the lifting base is raised to detach the silicon core from the liquid surface. Understandably, during the build-up phase, the inner and outer sleeves are allowed to fully thermally expand, putting the differential module into a ready-to-work state, avoiding compensation lag caused by cold start-up. During the crystal pulling phase, the high rigidity of the inner sleeve provides sufficient crystal pulling tension. At this time, the fine-tuning force of the differential module has not yet been fully established, avoiding interference with the necking process. During the equal diameter phase, the differential displacement generated by the radial temperature difference automatically adjusts the growth rate of each silicon core. No manual intervention is required throughout the process, adapting to thermal field fluctuations. In the final stage, the differential module automatically resets during furnace cooling, allowing it to proceed to the next furnace without additional operation.

[0016] Compared with the prior art, this application has the following beneficial effects: This application ensures that the macroscopic lifting force of the lifting base is directly and without hysteresis transmitted to the silicon core by rigidly connecting the inner sleeve and the lifting column, avoiding tension runaway caused by flexible connection; by setting the outer sleeve with a nested structure, the thermal expansion of the outer sleeve is limited to the action path of constraining the displacement of the inner sleeve, rather than being superimposed on the lifting stroke, thus structurally avoiding the defect of a single thermal expansion rod aggravating the growth difference; by constraining the axial displacement of the lower end of the outer sleeve, the thermal expansion of the outer sleeve is offset by the thermal expansion of the inner sleeve, and the thermal expansion is converted into a negative feedback fine adjustment force, rather than a positive driving force, which is suitable for the scenario of active movement of the lifting base; by configuring the thermal expansion coefficient of the outer sleeve material to be greater than that of the inner sleeve thermal expansion system, a physical basis is provided for differential displacement. The greater the temperature difference, the greater the relative displacement difference, which naturally matches the radial temperature field of the center of the furnace being cold and the outer ring being hot. Attached Figure Description

[0017] Figure 1 This is a simplified structural diagram of the silicon core furnace of this application; Figure 2 yes Figure 1 Enlarged structural diagram of region A in the middle; Figure 3 yes Figure 1 Enlarged structural diagram of region B in the middle; Figure 4 This is a schematic flowchart of the silicon core pulling method of this application; 100, Furnace body; 200, Crucible; 300, Heater; 400, Lifting base; 410, Water cooling channel; 420, Acoustic emission sensor; 500, Lifting assembly; 510, Lifting column; 520, Gripper; 600, Differential assembly; 610, Inner sleeve; 620, Outer sleeve; S, Silicon core. Detailed Implementation

[0018] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, specific embodiments of this application are described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.

[0019] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0020] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0021] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "joining," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise expressly limited. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0022] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0023] It should be noted that when an element is referred to as being "fixed to" or "set on" another element, it can be directly on the other element or there may be an intervening element. When an element is considered to be "connected to" another element, it can be directly connected to the other element or there may be an intervening element. The terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only embodiments.

[0024] First, refer to Figure 1 The silicon core furnace of this application includes a furnace body 100, a lifting base 400, a lifting assembly 500, and a differential assembly 600. The furnace body 100 contains a crucible 200 and a heater 300 surrounding the crucible 200. The lifting base 400 is located at the top of the furnace body 100 and has vertical lifting freedom. The lifting assembly 500 includes lifting columns 510 and grippers 520. Multiple lifting columns 510 are connected below the lifting base 400, and the grippers 520 are disposed on the lifting columns 510 for holding the seed crystal. The number of differential assemblies 600 is the same as the number of lifting assemblies 500. See [reference needed]. Figure 2 The differential assembly 600 includes an inner sleeve 610 and an outer sleeve 620. The upper end of the inner sleeve 610 is connected to the lifting base 400, and the lower end of the inner sleeve 610 is rigidly connected to the upper end of the lifting column 510. The outer sleeve 620 is sleeved outside the inner sleeve 610, and the lower end of the outer sleeve 620 forms an axial displacement constraint on the lower end of the inner sleeve 610. The inner sleeve 610 is made of a material with a first coefficient of thermal expansion, and the outer sleeve 620 is made of a material with a second coefficient of thermal expansion, the second coefficient of thermal expansion being greater than the first coefficient of thermal expansion. Understandably, by rigidly connecting the inner sleeve 610 to the lifting column 510, the macroscopic lifting force of the lifting base 400 is directly and without lag transmitted to the silicon core S, avoiding tension loss due to flexible connection; by setting the outer sleeve 620 with a nested structure, the thermal expansion of the outer sleeve 620 is limited to the action path of constraining the displacement of the inner sleeve 610, rather than being superimposed on the lifting stroke, thus structurally avoiding the defect of a single thermal expansion rod aggravating the growth difference; by constraining the axial displacement of the lower end of the outer sleeve 620, the greater thermal expansion of the outer sleeve 620 is used to offset the thermal expansion of the inner sleeve 610, converting thermal expansion into a negative feedback fine-tuning force, rather than a positive driving force, adapting to the scenario of active movement of the lifting base 400; by configuring the thermal expansion coefficient of the material of the outer sleeve 620 to be greater than that of the inner sleeve 610, a physical basis for differential displacement is provided. The greater the temperature difference, the greater the relative displacement difference, naturally matching the radial temperature field of the central cold and the central outer ring inside the furnace body 100.

[0025] In some embodiments, the inner sleeve 610 is made of molybdenum, niobium, tungsten, and their alloys, and the outer sleeve 620 is made of austenitic stainless steel, nickel-chromium-based high-temperature alloy, and cobalt-based high-temperature alloy; the difference between the first coefficient of thermal expansion and the second coefficient of thermal expansion is not less than 10 × 10⁻⁶. -6 / ℃. It is understandable that by setting an inner sleeve 610 made of refractory metal, its axial stiffness is ensured to remain stable below 600℃, preventing high-temperature creep and avoiding deformation of the inner sleeve 610 itself from affecting compensation accuracy. An outer sleeve 620 made of high-temperature alloy material is then used to ensure oxidation resistance and no strength reduction under long-term high temperatures, adapting to the long-cycle crystal pulling conditions of silicon core furnaces. The difference in thermal expansion system α between the two is configured to be no less than 10 × 10⁻⁶. -6 / ℃: Ensures that within the temperature range of 100℃~600℃, the relative expansion difference between the inner and outer sleeves 620 is sufficient to cover the common growth rate difference of 0.1mm / min~0.5mm / min for silicon core S, without the need for additional scaling up of the structural size.

[0026] In some embodiments, the inner sleeve 610 is made of a molybdenum-titanium-zirconium alloy, and the coefficient of thermal expansion of the inner sleeve 610 in the range of 100°C to 600°C is 4.5 × 10⁻⁶. -6 / ℃ to 5.8×10 -6 / ℃; the outer sleeve 620 is made of 253MA austenitic heat-resistant stainless steel, and the coefficient of thermal expansion of the outer sleeve 620 in the range of 100℃ to 600℃ is 17.5×10. -6 / ℃ to 19.0×10 -6 / ℃; wherein, the difference in the coefficient of thermal expansion between the inner sleeve 610 and the outer sleeve 620 within the range of 100℃ to 600℃ is 12.5×10 -6 / ℃ to 14.5×10 -6 / ℃. Understandably, by using an inner sleeve 610 made of TZM material, which combines the high melting point and low expansion characteristics of molybdenum with the high-temperature strength enhancement of titanium-zirconium alloy, achieving a tensile strength retention rate of ≥70% at 600℃, it is the most suitable low-cost solution for silicon core furnace conditions among refractory metals. The outer sleeve 620, made of 253MA material, with added cerium and nitrogen, has an oxidation resistance temperature reaching 1150℃, and the difference in thermal expansion coefficient between it and TZM perfectly matches the growth rate difference required by the silicon core furnace under a radial temperature difference of 30℃~50℃, achieving precise compensation without additional adjustments. By configuring 12.5×10 -6 / ℃~14.5×10 -6 The difference in thermal expansion coefficient α at / ℃ was verified by simulation. Under this difference, a radial temperature difference of 100℃ can produce a differential displacement of 0.125mm / h to 0.145mm / h, which can just offset the growth difference of 0.2mm / min to 0.4mm / min of the multi-silicon core S, and the compensation accuracy can reach ±0.05mm / min.

[0027] In some embodiments, the silicon core furnace of this application further includes a metal sheath, which covers the inner sleeve 610 and / or the outer sleeve 620 on the side facing the furnace interior. The purity of the metal sheath is not less than 99.95%. It is understood that by setting a high-purity metal sheath, the molybdenum / niobium / tungsten material itself belongs to the shallow donor impurities of silicon, and the sheath purity is ≥99.95%, which will not introduce deep-energy impurities of silicon such as Fe, Cr, Ni, and Ti, thus avoiding the volatilization of the matrix alloy and contamination of the silicon melt from the source. By covering the side facing the furnace interior with the metal sheath, all exposed surfaces in contact with the furnace atmosphere can be fully covered, including the outer cylindrical surface and lower end face of the inner and outer sleeves 620, eliminating the dead corners for pollution prevention and achieving a crystal pulling environment with zero metal pollution. The core indicators of silicon core S, such as minority carrier lifetime and resistivity uniformity, can meet the semiconductor-grade requirements, adapting to the production needs of polycrystalline silicon reduction carriers.

[0028] In some embodiments, the metal sheath is made of molybdenum, niobium, or tungsten. The metal sheath is sealed to the outer wall of the inner sleeve 610 and / or the inner wall of the outer sleeve 620 by vacuum electron beam welding or argon arc welding. The space between the metal sheath and the substrate of the inner sleeve 610 / outer sleeve 620 is either vacuum-sealed or filled with alumina powder. It is understood that the vacuum electron beam / argon arc welding seal prevents the sheath from detaching at high temperatures and also prevents base alloy atoms from volatilizing into the furnace through the weld gap. The vacuum / alumina filling between the metal sheath and the substrate of the inner sleeve 610 / outer sleeve 620 eliminates the gap between the sheath and the substrate, preventing residual gas in the gap from expanding due to heat at high temperatures, which could cause the sheath to bulge and detach. Simultaneously, the alumina powder further improves heat conduction efficiency and prevents localized overheating.

[0029] In some embodiments, a sliding mating surface is provided between the inner sleeve 610 and the outer sleeve 620. A solid lubricating coating is coated or laminated onto the sliding mating surface. The solid lubricating coating is a molybdenum disulfide, graphite, or hexagonal boron nitride coating, and its thickness is 5 μm to 20 μm. It is understood that by providing a solid lubricating coating, good lubrication performance is maintained even at a high temperature of 600°C, with a friction coefficient as low as 0.05 to 0.1, avoiding the stick-slip effect caused by direct metal-to-metal contact. By setting the thickness of the solid lubricating coating to 5 μm to 20 μm, lubrication effect is ensured without causing blockage of the sliding gap or restriction of differential displacement due to excessive coating thickness.

[0030] In some embodiments, the axial stiffness of the inner sleeve 610 is not less than 1×10⁻⁶. 6 N / m, the axial stiffness of the 620 outer sleeve is not less than 5×10 N / m. 5N / m. Understandably, the high axial stiffness design ensures that the axial fine-tuning force applied by the outer sleeve 620 only causes nanometer-level elastic deformation of the inner sleeve 610, without causing macroscopic elongation of the inner sleeve 610. This prevents the outer sleeve 620 from moving along with the inner sleeve 610. By designing a stiffness difference between the outer sleeve 620 and the inner sleeve 610, with the outer sleeve 620 having a slightly lower stiffness than the inner sleeve 610, the fine-tuning force of the outer sleeve 620 is preferentially applied to the silicon core S growth resistance, rather than its own deformation. This results in a force transmission efficiency ≥99%, ensuring the force transmission accuracy of the differential module 600, with a compensation error ≤1%. This avoids excessive or insufficient compensation due to insufficient stiffness, improving process stability.

[0031] See Figure 3 In some embodiments, a water-cooling channel 410 is provided inside the lifting base 400. The water-cooling channel 410 acts on the bottom of the lifting base 400 to cool the top of the outer sleeve 620 and the top of the inner sleeve 610. It can be understood that by cooling the connection part at the upper end of the outer sleeve 620 and the inner sleeve 610, the temperature of the connection area between the inner and outer sleeves 620 and the lifting base 400 is controlled below 200°C, avoiding the drift of the material's thermal expansion coefficient and the creep loosening of the connecting bolts caused by high temperature. This achieves directional cooling, cooling only the upper non-working area without affecting the thermal expansion of the lower working area, ensuring that the differential displacement is not disturbed by cooling.

[0032] Continue to refer to Figure 3 In some embodiments, the silicon core furnace of this application further includes multiple acoustic emission sensors 420. Each acoustic emission sensor 420 is installed inside the lifting base 400 and located on the outer side of the water cooling channel 410 in the radial direction. The detection end of each acoustic emission sensor 420 acts on the bottom of the lifting base 400 to detect whether the differential component 600 below generates jamming sound waves. The acoustic emission sensor 420 is electrically connected to the driving end of the lifting base 400. It is understood that by placing the acoustic emission sensor 420 on the outer side of the water cooling channel 410 in the radial direction, it can be in contact with the outer wall of the water cooling channel 410, thereby utilizing the cooling effect of the water cooling channel 410 to control the operating temperature of the acoustic emission sensor 420 at a lower temperature and avoid high-temperature damage. The acoustic emission sensor 420 can directly pick up the jamming friction sound waves of the differential component 600 and the micro-fracture sound waves before the silicon core S breaks, and can feed back signals to the driving end of the lifting base 400 to perform stop driving or deceleration driving operations.

[0033] See Figure 4 The silicon core pulling method of this application, applied to the silicon core furnace of this application, includes the following steps: S100, start the heater 300 to form a stable temperature field inside the furnace body 100, and the inner sleeve 610 and outer sleeve 620 of each differential component 600 will thermally expand as the temperature rises. S200, drive the lifting base 400 to descend, so that the seed crystal contacts the molten metal; S300: Control the lifting base 400 to rise at a speed V. Utilize the difference in thermal elongation of the outer sleeve 620 at different radial positions, apply an axial fine-tuning force to the inner sleeve 610 through the constraint of the lower end of the outer sleeve 620, adjust the growth rate of each silicon core S, and make the effective lifting stroke of each lifting column 510 relative to the lifting base 400 tend to be consistent. After growth (S400), the lifting base 400 is raised to detach the silicon core S from the liquid surface. Understandably, during the build-up phase, the inner and outer sleeves 620 are allowed to fully thermally expand, putting the differential module 600 into a ready-to-work state, avoiding compensation lag caused by cold start-up. During the crystal pulling phase, the high rigidity of the inner sleeve 610 provides sufficient crystal pulling tension. At this time, the fine-tuning force of the differential module 600 has not yet been fully established, avoiding interference with the necking process. During the equal-diameter phase, the differential displacement generated by the radial temperature difference automatically adjusts the growth rate of each silicon core S, requiring no manual intervention throughout the process, adapting to thermal field fluctuations. In the final stage, furnace cooling allows the differential module 600 to automatically reset, allowing it to proceed to the next furnace without additional operation.

[0034] Beneficial effects: This application ensures that the macroscopic lifting force of the lifting base 400 is directly and without lag transmitted to the silicon core S by rigidly connecting the inner sleeve 610 and the lifting column 510, thus avoiding tension loss due to flexible connection. By setting the outer sleeve 620 with a nested structure, the thermal expansion of the outer sleeve 620 is limited to the action path of constraining the displacement of the inner sleeve 610, rather than being superimposed on the lifting stroke, thus structurally avoiding the defect of a single thermal expansion rod aggravating the growth difference. By constraining the axial displacement of the lower end of the outer sleeve 620, the thermal expansion of the outer sleeve 620 is used to offset the thermal expansion of the inner sleeve 610, converting thermal expansion into a negative feedback fine-tuning force instead of a positive driving force, which is suitable for the scenario of active movement of the lifting base 400. By configuring the thermal expansion coefficient of the material of the outer sleeve 620 to be greater than that of the inner sleeve 610, a physical basis for differential displacement is provided. The greater the temperature difference, the greater the relative displacement difference, which naturally matches the radial temperature field of the central cold and the central outer ring inside the furnace body 100.

[0035] The specific embodiments described herein are merely illustrative examples of the spirit of this application. Those skilled in the art to which this application pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of this application or exceeding the scope defined by the appended claims.

Claims

1. A silicon core furnace, comprising a furnace body (100), wherein a crucible (200) is disposed within the furnace body (100) and a heater (300) surrounding the crucible (200); characterized in that, Also includes: A lifting base (400) is provided on the top of the furnace body (100) and has the freedom to lift vertically; A lifting assembly (500), the lifting assembly (500) comprising: Lifting columns (510), wherein there are multiple lifting columns (510) and each is connected to the lower part of the lifting base (400); A gripper (520), the gripper (520) being disposed on the lifting column (510), is used to grip the seed crystal; and A differential assembly (600), the number of which is the same as the number of lifting assemblies (500), the differential assembly (600) comprising: Inner sleeve (610), the upper end of which is connected to the lifting base (400), and the lower end of which is rigidly connected to the upper end of the lifting column (510); An outer sleeve (620) is sleeved outside the inner sleeve (610), and the lower end of the outer sleeve (620) forms an axial displacement constraint on the lower end of the inner sleeve (610). The inner sleeve (610) is made of a material having a first coefficient of thermal expansion, and the outer sleeve (620) is made of a material having a second coefficient of thermal expansion, the second coefficient of thermal expansion being greater than the first coefficient of thermal expansion.

2. The silicon core furnace according to claim 1, characterized in that, The inner sleeve (610) is made of molybdenum, niobium, tungsten, or their alloys, and the outer sleeve (620) is made of austenitic stainless steel, nickel-chromium-based high-temperature alloy, or cobalt-based high-temperature alloy; the difference between the first coefficient of thermal expansion and the second coefficient of thermal expansion is not less than 10 × 10⁻⁶. -6 / ℃.

3. The silicon core furnace according to claim 2, characterized in that, The inner sleeve (610) is made of molybdenum-titanium-zirconium alloy, and the coefficient of thermal expansion of the inner sleeve (610) is 4.5 × 10⁻⁶ in the range of 100°C to 600°C. -6 / ℃ to 5.8×10 -6 / ℃; The outer sleeve (620) is made of 253MA austenitic heat-resistant stainless steel, and the coefficient of thermal expansion of the outer sleeve (620) in the range of 100℃ to 600℃ is 17.5×10⁻⁶. -6 / ℃ to 19.0×10 -6 / ℃; The difference in the coefficients of thermal expansion between the inner sleeve (610) and the outer sleeve (620) within the temperature range of 100°C to 600°C is 12.5 × 10⁻⁶. -6 / ℃ to 14.5×10 -6 / ℃.

4. The silicon core furnace according to claim 1, characterized in that, It also includes a metal sheath, which covers the inner sleeve (610) and / or the outer sleeve (620) on the side facing into the furnace, and the purity of the metal sheath is not less than 99.95%.

5. The silicon core furnace according to claim 4, characterized in that, The metal sheath is made of molybdenum, niobium or tungsten. The metal sheath is sealed to the outer wall of the inner sleeve (610) and / or the inner wall of the outer sleeve (620) by vacuum electron beam welding or argon arc welding. The space between the metal sheath and the substrate of the inner sleeve (610) / outer sleeve (620) is either vacuum or filled with alumina powder.

6. The silicon core furnace according to claim 1, characterized in that, A sliding mating surface is provided between the inner sleeve (610) and the outer sleeve (620). A solid lubricating coating is coated or laminated on the sliding mating surface. The solid lubricating coating is a molybdenum disulfide, graphite, or hexagonal boron nitride coating, and the thickness of the solid lubricating coating is 5μm to 20μm.

7. The silicon core furnace according to claim 1, characterized in that, The axial stiffness of the inner sleeve (610) is not less than 1×10. 6 N / m, the axial stiffness of the outer sleeve (620) is not less than 5×10 N / m. 5 N / m.

8. The silicon core furnace according to claim 1, characterized in that, The lifting base (400) is provided with a water cooling channel (410), which acts on the bottom of the lifting base (400) to cool the top of the outer sleeve (620) and the top of the inner sleeve (610).

9. The silicon core furnace according to claim 8, characterized in that, It also includes multiple acoustic emission sensors (420), each of which is installed inside the lifting base (400) and located on the outer side of the water cooling channel (410) in the radial direction. The detection end of each of the acoustic emission sensors (420) acts on the bottom of the lifting base (400) to detect whether the differential component (600) below generates a jamming sound wave. The acoustic emission sensor (420) is electrically connected to the drive end of the lifting base (400).

10. A method for pulling silicon cores, applied to the silicon core furnace according to any one of claims 1 to 9, characterized in that, Includes the following steps: Start the heater (300) to form a stable temperature field inside the furnace body (100). The inner sleeve (610) and outer sleeve (620) of each differential component (600) undergo thermal expansion as the temperature rises. The driving base (400) is lowered so that the seed crystal contacts the molten metal; The lifting base (400) is controlled to rise at a speed of V. By utilizing the difference in thermal elongation of the outer sleeve (620) at different radial positions, an axial fine-tuning force is applied to the inner sleeve (610) through the constraint of the lower end of the outer sleeve (620), thereby adjusting the growth rate of each silicon core (S) and making the effective lifting stroke of each lifting column (510) relative to the lifting base (400) more consistent. After growth is complete, lift the lifting base (400) to remove the silicon core (S) from the liquid surface.