A multi-source controllable atmosphere annealing method for cadmium zinc telluride / cadmium telluride wafer

By employing independent Cd and Te source cavities and carrier gas flow control during the annealing process of cadmium zinc telluride/cadmium telluride wafers, the problem of inaccurate atmosphere regulation was solved, enabling controllable annealing and performance improvement of the wafers.

CN123153173APending Publication Date: 2026-11-24NORTHWESTERN POLYTECHNICAL UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611508574.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing annealing technologies for cadmium zinc telluride/cadmium telluride wafers, the Cd and Te atmospheres are difficult to adjust independently, resulting in imprecise atmosphere control. Furthermore, the uncontrollable annealing process leaves a damaged layer on the wafer surface, affecting electrical performance and consistency.

Method used

A multi-source controllable annealing method is adopted, in which the Cd source and Te source are set in independent annealing source chambers respectively. Through independent temperature control and carrier gas flow rate adjustment, the Cd and Te atmospheres can be continuously or stagedly controlled, avoiding the need to open the annealing chamber to change the annealing source.

Benefits of technology

It enables controllable adjustment of stoichiometry and defect state of CdZnTe/CdTe wafers, improves the controllability and consistency of the annealing process, reduces the introduction of impurities, and improves electrical properties and surface quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153173A_ABST
    Figure CN123153173A_ABST
Patent Text Reader

Abstract

This invention provides a multi-source controlled atmosphere annealing method for cadmium zinc telluride / cadmium telluride wafers, solving problems such as mutual interference between Cd and Te annealing sources, difficulty in controllable adjustment, and the need to change annealing sources for step-by-step annealing in existing CdZnTe / CdTe wafer annealing methods. This method places the Cd and Te sources in independent annealing source chambers and controls their temperatures independently. By independently adjusting the annealing source temperature, carrier gas flow rate, and gas path on / off state, the Cd atmosphere, Te atmosphere, or Cd / Te mixed atmosphere is transported to the wafer annealing area according to preset conditions. Continuous or staged atmosphere switching is achieved within the same annealing process without opening the furnace to change annealing sources. This invention can control the stoichiometry, point defects, second phase, and processing damage of the wafer, improving its electrical and detection performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor materials technology, specifically relating to a multi-source controlled atmosphere annealing method for cadmium zinc telluride / cadmium telluride wafers, applicable to the preparation and processing of cadmium zinc telluride and cadmium telluride single crystal wafers. Background Technology

[0002] Cadmium zinc telluride (CdZnTe, CZT) and cadmium telluride (CdTe) crystals belong to group II-VI compound semiconductor materials. They have high resistivity, high carrier mobility lifetime product and good room temperature operation characteristics. In recent years, they have gradually become key core materials in fields such as high-performance radiation detectors, medical imaging, high-energy physics and security inspection.

[0003] However, in the actual growth process of compound semiconductor crystals, CdZnTe and CdTe crystals are easily affected by factors such as component volatilization, non-stoichiometry, second-phase formation, and point defects due to limitations in growth technology. Cd, in particular, has a high equilibrium vapor pressure, making it prone to Cd loss during high-temperature crystal growth, leading to defects such as Cd vacancies. Furthermore, Te-rich inclusions or precipitates may form within the crystal, adversely affecting carrier transport and detection performance. The fabrication of detector wafers from ingots typically involves cutting, grinding, and polishing, which can generate residual stress, dislocations, surface defects, and stoichiometric deviations on the wafer surface and near-surface regions, thus affecting subsequent electrode fabrication and device performance. Therefore, heat treatment is usually necessary to adjust the defect state and stoichiometry of CdZnTe / CdTe wafers.

[0004] Current wafer annealing technology mainly employs a vacuum tube sealing method, placing Cd and Te raw materials together with the wafer in a quartz tube. Since Cd and Te have different equilibrium vapor pressures at different temperatures, the vapor pressure environment is controlled by the source temperature to complete the annealing process, thereby achieving electrical property adjustment and second-phase defect control.

[0005] The existing literature, "Two-Step Annealing to Remove Te Secondary-Phase Defects in CdZnTe While Preserving the High Electrical Resistivity," discloses a two-stage annealing method combining Cd and Te atmospheres. First, the CdZnTe crystal is annealed under Cd overpressure conditions to reduce the Te enrichment of the second phase within the crystal. Then, a second annealing is performed in a Te atmosphere to readjust the crystal resistivity and defect compensation state. This literature demonstrates that different Cd / Te atmospheres have different modulating effects on the defects and electrical properties of CdZnTe crystals. However, in this method, the transport process to the wafer is difficult to independently regulate, the atmosphere control is not precise enough, and an uncontrollable atmosphere annealing results in a damage layer of a certain thickness on the wafer surface.

[0006] Chinese patent application CN102168313A discloses a method for vapor-phase annealing modification of cadmium zinc telluride crystals. Existing multi-temperature zone annealing equipment typically places the wafer and annealing source at different locations in a two-stage annealing furnace, controlling the atmosphere through wafer and source temperatures. However, the annealing atmosphere is difficult to controllably adjust during the process. Multiple annealing sources are often located in the same temperature zone, and their vapor generation influences each other, making it difficult to independently adjust the vapor supply of different components by temperature. For processes requiring sequential treatment in Cd, Te, or other atmospheres, some traditional methods require repeated operations at different annealing stages. This not only increases the complexity of the annealing process but also easily introduces impurities such as water and oxygen, affecting the consistency of annealing treatments across different batches.

[0007] Therefore, it is necessary to provide an apparatus and process method that can independently control the Cd source, Te source, and mixed atmosphere annealing, so as to independently and dynamically adjust the Cd and Te atmospheres without opening the annealing chamber or changing the annealing source, thereby achieving controllable adjustment of the stoichiometry and defect state of CdZnTe / CdTe wafers during the annealing process. Summary of the Invention

[0008] To address the problems existing in the background technology, this invention proposes a multi-source controllable annealing method for cadmium zinc telluride / cadmium telluride wafers. This technical solution sets the Cd source and Te source in independent annealing source cavities, each with independent temperature control conditions. Temperature control is used to regulate the generation state of Cd and Te vapors, and the transport state of Cd and Te vapors towards the wafer annealing region is adjusted by controlling the carrier gas flow rate. Simultaneously, an independent temperature control unit is set in the wafer annealing region, making the wafer temperature, Cd source temperature, Te source temperature, and Cd and Te carrier gas flow rates independent of each other. This allows for continuous or phased control of the Cd / Te atmosphere composition during the same annealing process, solving the problems of mutual interference between Cd and Te annealing sources, difficulty in controllable adjustment, and the need to change annealing sources for step-by-step annealing in existing CdZnTe / CdTe wafer annealing processes.

[0009] To achieve the above objectives, the technical solution provided by the present invention is as follows:

[0010] A multi-source controlled atmosphere annealing method for cadmium zinc telluride / cadmium telluride wafers, characterized by comprising the following steps:

[0011] 1) Place the annealing source and the wafer.

[0012] The Cd source and the Te source are placed in separate annealing source cavities, each annealing source cavity is equipped with an independent temperature control unit, and the annealing source cavity is separated from the annealing chamber used to place the wafer.

[0013] The wafer to be annealed is placed in the annealing chamber, the annealing chamber is closed and evacuated, and then a protective atmosphere is introduced to purge the gas and remove residual water and oxygen in the annealing chamber.

[0014] The wafer is a CdZnTe wafer or a CdTe wafer;

[0015] The purity of both the Cd source and the Te source is not less than 99.99%. The gas phase formed by the volatilization of the annealing source during the annealing process directly acts on the wafer surface. If the purity of the annealing source is too low, the metal impurities in it will be transported into the wafer with the gas phase and affect the electrical performance of the wafer. Therefore, the purity of the annealing source needs to be limited.

[0016] 2) Controlled atmosphere annealing

[0017] The wafer is heated to a preset annealing temperature, and the temperature of the wafer annealing area and the temperature of each annealing source cavity are controlled independently.

[0018] Each annealing source cavity is heated and stabilized at its corresponding preset temperature. The flow rate of the carrier gas flowing through each annealing source cavity is set to a preset flow rate. By opening or closing the gas path between each annealing source cavity and the annealing chamber, the atmosphere transported to the wafer annealing area is selected as a single Cd atmosphere, a single Te atmosphere, or a Cd / Te mixed atmosphere. The wafer is then annealed under preset conditions.

[0019] By changing the gas path that is in the open state and the corresponding carrier gas flow rate, the atmosphere transported to the wafer annealing area can be continuously or in stages switched between a single Cd atmosphere, a single Te atmosphere and a Cd / Te mixed atmosphere during the same annealing process. The annealing chamber is not opened and the annealing source is not changed during the switching process.

[0020] 3) Cooling down completes wafer annealing:

[0021] After completing the atmosphere annealing, first lower the temperature of each annealing source cavity, and then lower the wafer temperature according to the cooling procedure under vacuum or inert protective atmosphere. After the wafer temperature drops to the preset temperature, take out the annealed wafer.

[0022] Further, in step 1), the wafer is processed in the following manner:

[0023] S1. Ingot cutting

[0024] The ingot is fixed on the sample stage using paraffin wax or hot melt adhesive, and then cut on a diamond wire cutter to obtain a wafer of the target size.

[0025] S2. Crystal polishing

[0026] The wafers obtained from S1 cutting are polished until there are no visible scratches on the surface, and then mechanical polishing or chemical mechanical polishing is performed using polishing media.

[0027] The polishing medium includes one or more of magnesium oxide, aluminum oxide, and silica sol.

[0028] Furthermore, when processing wafers, after polishing, a chemical etching solution suitable for wafers can be used to remove some of the residual processing damage layer, depending on the damage state of the wafer surface.

[0029] Furthermore, in step 2), when annealing the wafer using a single annealing atmosphere, the specific steps include:

[0030] Individual Cd atmosphere annealing: Adjust the temperature of the annealing source cavity where the Cd source is located and / or the flow rate of the carrier gas flowing through the annealing source cavity to transport the Cd atmosphere to the wafer annealing area and perform Cd atmosphere annealing on the wafer under preset conditions; after the Cd atmosphere annealing is completed, reduce the supply of Cd atmosphere or shut off the gas path where the Cd source is located.

[0031] Te atmosphere annealing: Adjust the temperature of the annealing source cavity where the Te source is located and / or the flow rate of the carrier gas flowing through the annealing source cavity to transport the Te atmosphere to the wafer annealing area, and continue to anneal the wafer in Te atmosphere under preset conditions after annealing in Cd atmosphere.

[0032] The above-mentioned Cd atmosphere annealing and Te atmosphere annealing can be completed continuously in the same annealing device without opening the annealing device cavity, changing the annealing source or reloading the sample. This avoids the process of cooling-opening the furnace-changing the source-re-vacuuming and reduces the introduction of water and oxygen. Among them, Cd atmosphere annealing is used to eliminate Te inclusions, while Te atmosphere annealing is used to regulate electrical properties.

[0033] Further, in step 2), when annealing the wafer using a Cd / Te mixed atmosphere, the gas path of the Cd source is first turned on, and the temperature and flow rate of the carrier gas in the annealing source cavity of the Cd source are independently adjusted to transport the Cd atmosphere to the wafer annealing area. The wafer is then annealed in the Cd atmosphere according to preset conditions. After the Cd source atmosphere annealing is completed, the temperature of the annealing source cavity of the Cd source is lowered to room temperature, the gas path of the Cd source is turned off, and the gas path of the Te source is turned on. The temperature and flow rate of the carrier gas in the annealing source cavity of the Te source are independently adjusted to form a Te atmosphere and transport it to the wafer annealing area. The wafer is then annealed in the Te atmosphere according to preset conditions.

[0034] When annealing in a Cd / Te mixed atmosphere, it is best to anneal in a Cd atmosphere first, followed by a Te atmosphere. That is, first adjust the macroscopic Te inclusion defects, and then adjust the performance by addressing the point defects. Conversely, annealing in a Te atmosphere first will induce Te inclusions, which is not conducive to performance adjustment.

[0035] In addition, multi-stage atmosphere annealing can be performed, that is, stress is first eliminated by inert atmosphere annealing and then electrical properties and macroscopic defects are adjusted by Te source or Cd source annealing.

[0036] Furthermore, in step 1), the vacuuming and protective atmosphere replacement process is repeated at least once to reduce the content of residual water, oxygen and other impurity gases in the annealing chamber.

[0037] The annealing process in step 2) is carried out under vacuum, low-pressure inert atmosphere or flowing inert carrier gas conditions.

[0038] Furthermore, the carrier gas is selected from one or more inert gases among Ar, N2, and He.

[0039] Meanwhile, the present invention also provides a multi-source controllable atmosphere annealing apparatus for cadmium zinc telluride / cadmium telluride wafers, which is characterized by including an inert atmosphere source, a first gas phase transport channel, a second gas phase transport channel, a vacuum atmosphere tube furnace, a cold trap and a mechanical pump.

[0040] The inert atmosphere source is used to provide the flowing carrier gas;

[0041] The first gas phase transport channel and the second gas phase transport channel are independent of each other. The first end of both channels is connected to the inert atmosphere source, and the last end of both channels is connected to the vacuum atmosphere tube furnace.

[0042] Each gas phase transport channel is provided with a first-end needle valve, an annealing source chamber, a flow control unit, and a last-end needle valve in sequence along the direction of carrier gas flow; the two annealing source chambers are used to accommodate Cd source and Te source respectively, and are connected to independent temperature control units respectively;

[0043] The vacuum atmosphere tube furnace is equipped with an annealing rack for placing wafers to be annealed and has an independent temperature control unit; the tail end of the vacuum atmosphere tube furnace is connected to the cold trap through a tail gas path, and a needle valve is installed on the tail gas path.

[0044] The mechanical pump is connected to the cold trap to maintain the vacuum level and recover exhaust gas to prevent contamination of the pump.

[0045] Furthermore, the flow control unit includes one or more of a mass flow controller, a flow meter, and a regulating valve.

[0046] Furthermore, a first pressure gauge is installed on the furnace body of the vacuum atmosphere tube furnace, and a second pressure gauge is installed on the exhaust gas path; the annealing rack is a quartz annealing rack.

[0047] The principle of this invention

[0048] This invention sets up Cd source, Te source and CdZnTe / CdTe wafer in independent control areas, and adjusts the annealing source temperature, carrier gas flow rate and wafer annealing temperature separately to achieve controllable generation, transport and control of Cd annealing atmosphere and Te annealing atmosphere, thereby adjusting the balance of macroscopic defects, stoichiometry and point defects in the wafer.

[0049] Cd and Te have different equilibrium vapor pressures at different temperatures, and the amount of corresponding gas phase produced increases with increasing annealing source temperature. Therefore, by adjusting the Cd source temperature T... Cd and Te source temperature T Te This can alter the generation of Cd and Te atmospheres respectively. The equilibrium vapor pressure of a pure substance can be approximated by an empirical relationship of the Clausius–Clapeyron type as follows:

[0050]

[0051] Among them, P i To correspond to the equilibrium vapor pressure of the annealing source, T i A is the annealing source temperature. i and B iThese are constants related to the thermodynamic properties of the annealing source material. For the same annealing source material, these values ​​are fixed and can be found in well-known physicochemical handbooks or literature in this field. For example, in the reference "VAPOR PRESSURE OF THE METALLIC ELEMENTS", under the two-parameter approximation, the estimated saturated vapor pressure of Cd can be expressed as:

[0052]

[0053] The literature "High Temperature Thermodynamic Properties of ZnTe(s)" experimentally determined the vapor pressure of Te and provided an empirical formula:

[0054]

[0055]

[0056] Meanwhile, the present invention sets up independent carrier gas flow control units in the Cd source and Te source gas paths respectively. The carrier gas carries the Cd or Te atmosphere into the wafer annealing area. Therefore, under the condition of a certain source temperature, the amount of Cd or Te gas transported to the wafer area per unit time can be further adjusted by changing the carrier gas flow rate.

[0057] The actual transport process of Cd and Te vapor phases is simultaneously affected by factors such as annealing source temperature, carrier gas flow rate, system pressure, and gas path structure. Among these factors, the annealing source temperature mainly determines the equilibrium vapor pressure of the Cd or Te source material and its vapor phase generation capacity; the carrier gas flow rate mainly affects the transport rate and supply intensity of the vapor phase from the source region to the wafer annealing region; and system pressure, gas path length, pipe diameter, valve opening, and vapor phase condensation or loss during transport all collectively affect the actual transport efficiency of the vapor phase.

[0058] With other process conditions remaining essentially unchanged, increasing the temperature of the Cd or Te source can increase the equilibrium vapor pressure of the corresponding source material, thereby increasing the amount of Cd or Te atmosphere available for carrier gas transport. Within a certain process range, appropriately increasing the carrier gas flow rate of the corresponding branch can increase the amount of Cd or Te gas phase supplied to the wafer annealing region per unit time. Furthermore, this invention uses control valves installed in the Cd and Te source gas paths to achieve switching between Cd atmosphere, Te atmosphere, or protective atmosphere at different annealing stages.

[0059] Therefore, the annealing source temperature is used to regulate the generation state of the annealing atmosphere, the carrier gas flow rate is used to regulate the transport and supply intensity of the gas phase, and the gas path valve is used to control the switching of different atmospheres and annealing stages. The three work together to achieve controllable adjustment of the atmosphere composition and supply state in the wafer annealing area.

[0060] Advantages of the present invention

[0061] 1. This invention addresses the problem of limited annealing atmosphere control caused by traditional single or multiple annealing sources sharing the same temperature range by controlling the annealing atmosphere through independent Cd and Te sources. The Cd and Te sources are each set with independent temperature and gas path control. The generation state of the Cd and Te gas phases is adjusted by regulating the source temperature, and the transport amount of the corresponding gas phases to the wafer annealing region is adjusted by the carrier gas flow rate. This makes the annealing atmosphere independent of the wafer annealing temperature, providing greater freedom in annealing atmosphere control compared to annealing methods that rely solely on source temperature. This improves the controllability of the Cd and Te atmosphere and the process repeatability during the annealing of CdZnTe / CdTe wafers.

[0062] 2. This invention can be used for single-atmosphere annealing or multi-atmosphere combined annealing, as well as controllable heat treatment under protective or reactive atmosphere conditions. By controlling different atmosphere sources and corresponding gas paths separately, annealing can be achieved in a single Cd atmosphere, a single Te atmosphere, a Cd / Te mixed atmosphere, or a staged atmosphere. Furthermore, protective atmospheres such as Ar, N2, and He, as well as other reactive atmospheres, can be introduced according to process requirements, thereby meeting different heat treatment needs such as stoichiometric adjustment, defect control, surface treatment, and repair of processing damage.

[0063] 3. The present invention features a simple process principle, a continuous and controllable annealing process, and the ability to continuously switch between different atmosphere conditions within the same annealing apparatus. Each atmosphere source is installed in its respective independent annealing source chamber before annealing. By adjusting the source temperature, carrier gas flow rate, and valve status, different atmospheres can be controlled without restarting the furnace or changing the annealing source at different annealing stages. This reduces repetitive operations such as cooling, furnace restarting, and changing annealing sources as in traditional step-by-step annealing, and lowers the risk of impurities such as water and oxygen re-entering the annealing system. Simultaneously, it shortens the process flow and improves the stability and batch consistency of the annealing treatment. Attached Figure Description

[0064] Figure 1 This is a schematic diagram of the structure of the multi-source controllable atmosphere annealing apparatus of the present invention;

[0065] The attached figures are labeled as follows:

[0066] 1-First needle valve at the beginning, 2-First annealing source chamber, 3-First mass flow controller, 4-First needle valve at the end, 5-Second needle valve at the beginning, 6-Second annealing source chamber, 7-Second mass flow controller, 8-Second needle valve at the end, 9-Vacuum atmosphere tube furnace, 10-First pressure gauge, 11-Needle valve, 12-Second pressure gauge, 13-Mechanical pump, 14-Cold trap, 15-Inert atmosphere source, 16-Transition chamber, 17-Annealing chamber;

[0067] Figure 2The images show the observation and statistical results of Te inclusions in the wafer before and after annealing in Example 1, where (a) is before annealing and (b) is after annealing.

[0068] Figure 3 The IV curves of the wafer before and after annealing in Example 2 are shown.

[0069] Figure 4 The carrier mobility lifetime product of the annealed wafer in Example 2 is given, where (a) is before annealing and (b) is after annealing.

[0070] Figure 5 This is the energy dispersive spectroscopy (EDS) spectrum of the annealed wafer from Example 2.

[0071] Figure 6 The images show a comparison of the wafer surface conditions of Comparative Example 1 and Example 1, where (a) is Comparative Example 1 and (b) is Example 1. Detailed Implementation

[0072] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments:

[0073] See Figure 1 This invention relates to a multi-source controllable annealing apparatus for cadmium zinc telluride / cadmium telluride wafers, comprising an inert atmosphere source, a first gas phase transport channel, a second gas phase transport channel, a transition chamber, a vacuum atmosphere tube furnace, a cold trap, and a mechanical pump. The inert atmosphere source provides a flowing carrier gas for the annealing atmosphere. The first and second gas phase transport channels are independent of each other, with their initial ends connected to the inert atmosphere source and their final ends connected to the vacuum atmosphere tube furnace via the transition chamber. Each gas phase transport channel is sequentially equipped with a first-end needle valve, an annealing source chamber, a flow control unit (in this embodiment, a mass flow controller) and a final-end needle valve along the direction of the carrier gas flow. The two annealing source chambers are used to accommodate Cd and Te sources, respectively, and are connected to independent temperature control units. The vacuum atmosphere tube furnace is equipped with an annealing rack for placing the wafers to be annealed and has an independent temperature control unit. Its final end is connected to the cold trap via a tail gas path, and a needle valve is installed on the tail gas path. The mechanical pump is connected to the cold trap. After the wafer is polished, the wafer is placed on an annealing rack (used to hold the wafer) that is compatible with the wafer size, and then placed into the above-mentioned device for annealing.

[0074] This invention regulates the Cd and Te gas phase generation state by adjusting the annealing source temperature and regulates the transport of Cd and Te gas phases to the wafer by adjusting the carrier gas flow rate. At the same time, the wafer annealing area adopts independent temperature control, realizing independent adjustment between wafer temperature, Cd source temperature, Te source temperature and gas phase transport flow rate, reducing the cross-influence between the two annealing sources, eliminating the need to open the furnace and change the annealing source at different annealing stages, and achieving continuous or staged adjustment of single Cd atmosphere, single Te atmosphere and Cd / Te mixed atmosphere in the same annealing process. It is used to control the stoichiometry, point defects, second phase and processing damage of CdZnTe / CdTe wafers, and improve their electrical and detection performance.

[0075] The invention will be further illustrated below with specific examples.

[0076] Example 1

[0077] A controlled annealing method for cadmium zinc telluride / cadmium telluride wafers includes the following steps:

[0078] 1) Fix the CdZnTe ingot onto the sample stage using paraffin wax or hot melt adhesive, and cut it on a diamond wire cutter as required to obtain a wafer with a size of 10 mm × 10 mm × 5 mm.

[0079] 2) Use sandpaper to polish the wafer until there are no visible scratches on the surface, and use magnesium oxide to mechanically polish the CdZnTe material. Then, use acetone, anhydrous ethanol and deionized water to clean the wafer in sequence, and use high-purity N2 to dry it.

[0080] 3) Place a Cd source with a purity of not less than 99.99% in the first annealing source cavity; place the CdZnTe wafer processed in step 2) on a quartz annealing rack that is compatible with the wafer size, and place the annealing rack in the wafer annealing temperature control area of ​​the vacuum atmosphere tube furnace; wherein, the first annealing source cavity and the wafer annealing area are respectively equipped with independent temperature control units.

[0081] 4) Close the Cd source gas path (first gas phase transport channel) and the second gas phase transport channel, and repeat the vacuum-Ar replacement process twice to reduce the content of residual water, oxygen and other impurity gases in the annealing chamber. Add liquid nitrogen to the cold trap to ensure continuous cooling, and collect the exhaust gas to prevent it from entering the vacuum pump.

[0082] 5) Heat the wafer annealing area to the preset temperature of 650℃, independently control the Cd source temperature to 500℃, hold for 2 hours, open the valve on the first gas phase transport channel, and adjust the gas flow valve to adjust the Ar carrier gas flow rate through the first annealing source cavity to 150 sccm, so that the wafer is in a relatively Cd-rich annealing state. Under the above conditions, anneal the CdZnTe wafer in a Cd atmosphere for 60 hours; during this period, the second gas phase transport channel remains closed, and the wafer is in a separate Cd atmosphere annealing environment.

[0083] 6) After annealing, first lower the temperature of the Cd source temperature zone to room temperature, and then lower the CdZnTe wafer from 650 ℃ to room temperature at a rate of 2 ℃ / min under a high-purity Ar protective atmosphere. Then take out the annealed wafer.

[0084] Figure 2 The images and statistics of Te inclusions in the wafer before and after annealing in Example 1 are shown. After annealing, almost all small inclusion phases in the wafer disappeared; it can also be seen from the corresponding inclusion phase size distribution diagram that the number of small inclusion phases smaller than 10 μm in the wafer was greatly reduced after annealing, while the number of large inclusion phases larger than 10 μm in the wafer was only slightly reduced.

[0085] Figure 6 (b) shows the wafer surface after annealing in Example 1. It can be seen that due to the controllable adjustment of the annealing atmosphere, the wafer surface is relatively smooth and there is no rough deposit layer.

[0086] Example 2

[0087] A multi-source controlled annealing method for cadmium zinc telluride / cadmium telluride wafers includes the following steps:

[0088] 1) Fix the CdZnTe ingot onto the sample stage using paraffin wax or hot melt adhesive, and cut it on a diamond wire cutter as required to obtain a wafer with a size of 10 mm × 10 mm × 5 mm.

[0089] 2) Use sandpaper to polish the wafer until there are no visible scratches on the surface, and use magnesium oxide to mechanically polish the CdZnTe material. Then, use acetone, anhydrous ethanol and deionized water to clean the wafer in sequence, and use high-purity N2 to dry it.

[0090] 3) Place a Cd source with a purity of not less than 99.99% in the first annealing source chamber, and place a Te source with a purity of not less than 99.99% in the second annealing source chamber;

[0091] The CdZnTe wafer processed in step 2) is placed on a quartz annealing rack that is compatible with the wafer size, and the annealing rack is placed in the wafer annealing temperature control area of ​​a vacuum atmosphere tube furnace.

[0092] Independent temperature control units are set up for the Cd source cavity, Te source cavity, and wafer annealing area.

[0093] 4) Close the Cd source gas path (first gas phase transport channel) and the Te source gas path (second gas phase transport channel), and repeat the vacuum-Ar replacement process twice to reduce the content of residual water, oxygen and other impurity gases in the annealing chamber.

[0094] 5) Heat the wafer annealing zone to a preset temperature of 650℃, independently control the Cd source temperature to 500℃, hold for 2 hours, open the valve on the first gas phase transport channel, and adjust the gas flow valve to adjust the Ar carrier gas flow rate through the first annealing source chamber to 150 sccm, so that the wafer is in a relatively Cd-rich annealing state. Under the above conditions, anneal the CdZnTe wafer in a Cd atmosphere for 60 hours.

[0095] 6) After the Cd source atmosphere annealing is completed, lower the Cd source temperature to room temperature and close the valve on the first gas phase transport channel. Raise the Te source temperature to 400 ℃, and open the Te source gas valve after the Te source temperature stabilizes. Set the Ar carrier gas flow rate through the second annealing source cavity to 150 sccm. After passing through the Te source cavity, the Ar carrier gas carries the Te gas phase into the wafer annealing area. Continue annealing the CdZnTe wafer treated in step 5) under Te atmosphere conditions for 120 h.

[0096] 7) After annealing, first lower the temperature of the Te source temperature zone to room temperature, and then lower the CdZnTe wafer from 650 ℃ to room temperature at a rate of 2 ℃ / min under a high-purity Ar protective atmosphere. Then take out the annealed wafer.

[0097] Figure 3 The IV curve of the annealed wafer in Example 2 shows the resistivity from 0.63 × 10⁻⁶. 10 The Ω·cm value increased to 2.20 × 10⁻⁶. 10 The efficiency was improved by approximately 3.5 times (Ω·cm). The leakage current at 100 V also decreased significantly from 15.6 nA to 1.37 nA, a reduction of one order of magnitude, reflecting the decrease in the defect density within the crystal (especially Te inclusions and deep-level defects).

[0098] Figure 4 The electron mobility lifetime product of the annealed crystal obtained in Example 2 is 1.18 × 10⁻⁶. -3 cm 2 / V, compared to 8.77×10 in the growth state -4 cm 2 The / V increase of about 35% indicates that the traps encountered by electrons during transport are reduced, and the Te inclusions and related deep-level defects are reduced.

[0099] Figure 5 The energy spectrum of the annealed crystal in Example 2 shows that the full width at half maximum (FWHM) at 59.5 keV is narrower, and the energy resolution is significantly improved, reflecting the improvement in overall electrical and transport properties.

[0100] Comparative Example 1

[0101] In this comparative example, no independent Cd source cavity, no Cd source carrier gas branch, and no independent flow control unit are set up. The Cd source and the wafer are located in the same annealing crucible and the same temperature zone. Specifically:

[0102] 1) Fix the CdZnTe ingot onto the sample stage using paraffin wax or hot melt adhesive, and cut it on a diamond wire cutter as required.

[0103] 2) Use sandpaper to polish the wafer until there are no visible scratches on the surface, and use magnesium oxide to mechanically polish the CdZnTe material. Then, use acetone, anhydrous ethanol and deionized water to clean the wafer in sequence, and use high-purity N2 to dry it.

[0104] 3) Place a pure Cd source with a purity of not less than 99.99% and the CdZnTe wafer processed in step 2) together in the same quartz crucible. The Cd source and CdZnTe wafer are placed alternately to avoid direct contact between the Cd source and the wafer surface. The Cd source is placed at the bottom of the crucible, and the CdZnTe wafer is placed on a quartz support, allowing the Cd vapor phase formed by the volatilization of the Cd source to diffuse inside the crucible and act on the wafer surface.

[0105] 4) Place the quartz crucible containing the Cd source and CdZnTe wafers in a vacuum tube furnace, close the annealing chamber, and use a vacuum pump to evacuate the system to below 10 Pa and maintain this vacuum for 15 min. Then, introduce high-purity Ar into the annealing system for atmosphere replacement. Repeat the vacuum-Ar replacement process twice to reduce the content of residual water, oxygen, and other impurity gases in the annealing chamber.

[0106] 5) The crucible containing the Cd source and the CdZnTe wafer was heated to 650 °C at a rate of 3 °C / min and held at 650 °C for 60 h. During the heating and holding process, the Cd source heated synchronously with the crucible and volatilized inside the crucible to form a Cd atmosphere. The Cd gas phase was transported to the surface of the CdZnTe wafer through natural diffusion and convection inside the crucible, thereby annealing the wafer under Cd atmosphere conditions.

[0107] 6) The CdZnTe wafer was cooled from 650 °C to room temperature at a rate of 2 °C / min under an Ar protective atmosphere.

[0108] Figure 6(a) is a photograph of the surface morphology of the annealed wafer in Comparative Example 1. In this comparative example, the Cd atmosphere is uncontrollable and can only be adjusted by the relationship between vapor pressure and temperature. It can be seen that obvious roughening and deposition / volatilization traces appear on the wafer surface after annealing, indicating that it is difficult to maintain the stable surface state of the wafer under the traditional fixed Cd atmosphere conditions, and a damage layer of a certain thickness will exist on the wafer surface after annealing.

[0109] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the scope of the technology disclosed in the present invention, and such modifications or substitutions should all be covered within the scope of protection of the present invention.

Claims

1. A multi-source controlled atmosphere annealing method for cadmium zinc telluride / cadmium telluride wafers, characterized in that, Includes the following steps: 1) Place the annealing source and the wafer. The Cd source and / or Te source are placed in separate annealing source cavities, each annealing source cavity is equipped with an independent temperature control unit, and the annealing source cavity is separated from the annealing chamber used to place the wafer. The wafer to be annealed is placed in the annealing chamber, the annealing chamber is closed and evacuated, and then a protective atmosphere is introduced for gas purging. The wafer is a CdZnTe wafer or a CdTe wafer; 2) Controlled atmosphere annealing The wafer is heated to a preset annealing temperature, and the temperature of the wafer annealing area and the temperature of each annealing source cavity are controlled independently. Each annealing source cavity is heated and stabilized at its corresponding preset temperature. The flow rate of the carrier gas flowing through each annealing source cavity is set to a preset flow rate. By opening or closing the gas path between each annealing source cavity and the annealing chamber, the atmosphere transported to the wafer annealing area is selected as a single Cd atmosphere, a single Te atmosphere, or a Cd / Te mixed atmosphere. The wafer is then annealed under preset conditions. By changing the gas path in the open state and the corresponding carrier gas flow rate, the atmosphere transported to the wafer annealing area can be continuously or intermittently switched between a single Cd atmosphere, a single Te atmosphere and a Cd / Te mixed atmosphere during the same annealing process. 3) Cooling down completes wafer annealing: After completing the atmosphere annealing, first lower the temperature of each annealing source cavity, and then lower the wafer temperature according to the cooling procedure under vacuum or inert protective atmosphere. After the wafer temperature drops to the preset temperature, take out the annealed wafer.

2. The annealing method according to claim 1, characterized in that: In step 1), the wafer is processed in the following manner: S1. Ingot cutting The ingot is fixed on the sample stage using paraffin wax or hot melt adhesive, and then cut on a diamond wire cutter to obtain a wafer of the target size. S2. Crystal polishing The wafers obtained from S1 cutting are polished until there are no visible scratches on the surface, and then mechanical polishing or chemical mechanical polishing is performed.

3. The annealing method according to claim 2, characterized in that: When processing wafers, after polishing, a chemical etching solution suitable for the wafer is used to remove some of the residual processing damage layer, depending on the damage state of the wafer surface.

4. The annealing method according to claim 1, characterized in that: In step 2), when annealing the wafer using a single annealing atmosphere, the specific steps are as follows: Individual Cd atmosphere annealing: Adjust the temperature of the annealing source cavity where the Cd source is located and / or the flow rate of the carrier gas flowing through the annealing source cavity to transport the Cd atmosphere to the wafer annealing area and perform Cd atmosphere annealing on the wafer under preset conditions; after the Cd atmosphere annealing is completed, reduce the supply of Cd atmosphere or shut off the gas path where the Cd source is located. Separate Te atmosphere annealing: Adjust the temperature of the annealing source cavity where the Te source is located and / or the flow rate of the carrier gas flowing through the annealing source cavity to transport the Te atmosphere to the wafer annealing area, and continue to anneal the wafer in the Te atmosphere under preset conditions.

5. The annealing method according to claim 1, characterized in that: In step 2), when annealing the wafer using a Cd / Te mixed atmosphere, first open the gas path of the Cd source, independently adjust the temperature of the annealing source cavity of the Cd source and the flow rate of the carrier gas, and transport the Cd atmosphere to the wafer annealing area. Anneal the wafer in the Cd atmosphere according to the preset conditions. After the Cd source atmosphere annealing is completed, lower the temperature of the annealing source cavity of the Cd source to room temperature, close the gas path of the Cd source, and then open the gas path of the Te source. Independently adjust the temperature of the annealing source cavity of the Te source and the flow rate of the carrier gas, form a Te atmosphere and transport it to the wafer annealing area. Anneal the wafer in the Te atmosphere according to the preset conditions.

6. The annealing method according to claim 1, characterized in that: In step 1), the vacuuming and protective atmosphere replacement process is repeated at least once to reduce the content of residual water, oxygen and other impurity gases in the annealing chamber. The annealing process in step 2) is carried out under vacuum, low-pressure inert atmosphere or flowing inert carrier gas conditions.

7. The method according to claim 1, characterized in that: The carrier gas is selected from one or more inert gases among Ar, N2, and He.

8. A multi-source controlled atmosphere annealing apparatus for cadmium zinc telluride / cadmium telluride wafers, characterized in that: It includes an inert atmosphere source, a first gas phase transport channel, a second gas phase transport channel, a vacuum atmosphere tube furnace, a cold trap, and a mechanical pump; The inert atmosphere source is used to provide the flowing carrier gas; The first gas phase transport channel and the second gas phase transport channel are independent of each other. The first end of both channels is connected to the inert atmosphere source, and the last end of both channels is connected to the vacuum atmosphere tube furnace. Each gas phase transport channel is provided with a first-end needle valve, an annealing source chamber, a flow control unit, and a last-end needle valve in sequence along the direction of carrier gas flow; the two annealing source chambers are used to accommodate Cd source and Te source respectively, and are connected to independent temperature control units respectively; The vacuum atmosphere tube furnace is equipped with an annealing rack for placing wafers to be annealed and has an independent temperature control unit; the tail end of the vacuum atmosphere tube furnace is connected to the cold trap through a tail gas path, and a needle valve is installed on the tail gas path. The mechanical pump is connected to the cold trap.

9. The multi-source controlled atmosphere annealing apparatus for cadmium zinc telluride / cadmium telluride wafers according to claim 8, characterized in that: The flow control unit includes one or more of a mass flow controller, a flow meter, and a regulating valve.

10. The multi-source controlled atmosphere annealing apparatus for cadmium zinc telluride / cadmium telluride wafers according to claim 8, characterized in that: The vacuum atmosphere tube furnace is equipped with a first pressure gauge on the furnace body and a second pressure gauge on the exhaust gas path; the annealing rack is a quartz annealing rack.

Citation Information

Patent Citations

  • Gas phase annealing modification method for tellurium / zinc / cadmium crystal

    CN102168313A