Rubidium lithium monohydrogen cyanurate electro-optic crystal, its preparation method and use

The solution method for preparing rubidium hydrogen cyanurate-based electro-optic crystals overcomes the limitations of existing electro-optic crystals in terms of laser damage threshold, cost, and size, and realizes a transparent, large-size crystal with high electro-optic coefficient and high laser damage threshold, suitable for electro-optic devices.

CN123153174APending Publication Date: 2026-11-24FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611254565.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing electro-optic crystals have limitations in terms of laser damage threshold, cost, and size, making it difficult to find crystals with excellent overall performance that are easy to grow in large sizes.

Method used

A lithium rubidium hydrogen cyanurate electro-optic crystal (RLHCY) is provided, which is prepared in a glass growth tank by solution method. Large-size transparent crystals are grown by controlling the temperature and seed crystal rotation speed, avoiding the use of precious metal crucibles.

Benefits of technology

A cyanuric acid-rubidium hydrogen lithium electro-optic crystal with high electro-optic coefficient and high laser damage threshold was prepared. It is low in cost and easy to fabricate in large size, making it suitable for electro-optic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153174A_ABST
    Figure CN123153174A_ABST
Patent Text Reader

Abstract

This invention discloses a rubidium hydrogen cyanurate lithium electro-optic crystal, its preparation method, and its applications. The chemical formula of the rubidium hydrogen cyanurate lithium electro-optic crystal is RbLi(HC3N3O3)·2H2O, it belongs to the orthorhombic crystal system, space group Pna21, and its cell parameters are as follows: a =15.682(7)Å, b =3.7453(17)Å, c =12.768(6)Å, α=β=γ=90°, Z=4, unit cell volume is V=749.9Å 3 This invention prepared a lithium rubidium hydrogen cyanurate electro-optic crystal, which (RLHCY crystal) exhibits a high electro-optic coefficient at room temperature (2.2 pm / V) and a high laser damage threshold (4.8 GW / cm). 2 The RLHCY crystal, with its advantages of (1064 nm, 5 ns, 10 Hz), is a colorless and transparent crystal. The preparation method is simple; large-size crystals can be prepared in a glass growth tank using a solution method, eliminating the need for precious metal crucibles such as platinum or iridium, thus offering a significant cost advantage in large-size crystal preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optoelectronic functional crystal materials, and in particular to a cyanuric acid-rubidium hydrogen lithium electro-optic crystal, its preparation method, and its uses. Background Technology

[0002] Electro-optic crystals are crystals that exhibit the electro-optic effect. The electro-optic effect is the phenomenon where the refractive index of a crystal changes with an applied electric field. Various practical electro-optic devices can be fabricated using electro-optic crystals, such as electro-optic modulators, electro-optic Q-switches, and electro-optic deflectors. These devices are widely used in laser and optical modulation fields.

[0003] Currently, commercially available electro-optic crystals mainly include: potassium dideuterium phosphate (DKDP), lithium niobate (LN), rubidium titanium oxy phosphate (RTP), barium metaborate (BBO), and lanthanum gallium silicate (LGS). Each of these crystals has certain limitations: DKDP crystals have a large electro-optic coefficient and a high laser damage threshold, but they are prone to moisture absorption and have high costs; LN crystals have stable physicochemical properties, but a low laser damage threshold; RTP crystals have a large electro-optic coefficient and a high laser damage threshold, but crystal growth is difficult and expensive; BBO crystals have a high laser damage threshold, but a relatively small electro-optic coefficient and a short length in the Z-direction, resulting in a high half-wave voltage when an electric field is applied; LGS crystals have a relatively high laser damage threshold and are easy to fabricate into large-size crystals, but they exhibit optical rotation, increasing the difficulty of device design.

[0004] Therefore, there is a need to find electro-optic crystals with excellent overall performance and ease of growing large-size bulk crystals. From a commercial perspective, there is a particular need for an electro-optic crystal with a high laser damage threshold and low cost of fabricating large-size crystals. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the purpose of this invention is to provide a rubidium hydrogen cyanurate lithium electro-optic crystal, its preparation method and uses.

[0006] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a rubidium hydrogen cyanurate lithium electro-optic crystal, wherein the chemical formula of the rubidium hydrogen cyanurate lithium electro-optic crystal is RbLi(HC3N3O3)·2H2O (abbreviated as RLHCY), it belongs to the orthorhombic crystal system, the space group is Pna21, and the cell parameters are as follows: a =15.682(7)Å, b =3.7453(17)Å, c =12.768(6)Å, α=β=γ=90°, Z=4, unit cell volume is V=749.9Å 3 .

[0007] The electro-optic coefficient of the RLHCY crystal at room temperature is 2.2 pm / V. The RLHCY crystal is a colorless and transparent crystal.

[0008] Secondly, the present invention provides a method for preparing rubidium hydrogen cyanurate lithium electro-optic crystal (solution method), comprising the following steps: Step 1: Mix RbCl, LiOH·H2O, and C3H3N3O3, dissolve them completely in water at 60-70℃, and then cool naturally to room temperature to obtain polycrystalline rubidium hydrogen cyanurate electro-optic crystal; Step 2: Dissolve the polycrystalline lithium rubidium hydrogen cyanurate electro-optic crystal in water at 45~65℃ and keep it at the temperature for 1~5 hours to obtain a lithium rubidium hydrogen cyanurate solution. Step 3: Cool the cyanuric acid-rubidium lithium hydrogen solution to the saturation temperature at a rate of 0.5~1.0℃ / h, introduce a seed crystal on the surface of the cyanuric acid-rubidium lithium hydrogen solution, control the rotation of the seed crystal, and cool to room temperature to obtain the cyanuric acid-rubidium lithium hydrogen electro-optic crystal.

[0009] Optionally, the molar ratio of the raw materials RbCl, LiOH·H2O, and C3H3N3O3 is 1:2:1.

[0010] Optionally, the saturation temperature is 40~55℃.

[0011] Optionally, the seed crystal rotation speed is 6~15 rpm.

[0012] Optionally, after adjusting the seed crystal rotation, the cooling rate is 0.2~1.0℃ / day.

[0013] Thirdly, the present invention provides an application of rubidium hydrogen cyanurate lithium electro-optic crystal in electro-optic devices.

[0014] Fourthly, the present invention provides an electro-optic device, including the aforementioned rubidium hydrogen cyanurate lithium electro-optic crystal.

[0015] Optionally, the electro-optic device is an electro-optic modulator, an electro-optic Q-switch, or an electro-optic deflector.

[0016] It should be noted that the electro-optic modulator is prepared by the following method: polishing the two end faces of the lithium rubidium hydrogen cyanurate electro-optic crystal along the physical Y-axis, depositing conductive films on the two end faces of the lithium rubidium hydrogen cyanurate electro-optic crystal along the physical Z-axis, and then applying an electric field to the conductive films on the two end faces of the lithium rubidium hydrogen cyanurate electro-optic crystal along the physical Z-axis to obtain the electro-optic modulator.

[0017] The electro-optic Q-switch is fabricated by the following method: Crystal 1 and Crystal 2 are provided, which are two identical cyanuric acid-lithium hydrogen electro-optic crystals (used to compensate for natural birefringence). The end faces of Crystal 1 and Crystal 2 along the physical Y-axis are polished, and conductive films are deposited on the end faces of Crystal 1 and Crystal 2 along the physical Z-axis. Crystal 1 and Crystal 2 are connected, wherein the physical Y-axis of Crystal 1 and Crystal 2 are parallel, the physical X-axis of Crystal 1 is parallel to the Z-axis of Crystal 2, and the physical Z-axis of Crystal 1 is parallel to the X-axis of Crystal 2. An electric field is applied to the conductive films on the end faces of Crystal 1 and Crystal 2 along the physical Z-axis to obtain the electro-optic Q-switch.

[0018] The electro-optic deflector is prepared by the following method: the lithium rubidium hydrogen cyanurate electro-optic crystal is prepared into a right-angle prism, the two right-angle faces of the right-angle prism being the physical X-plane and Y-plane of the lithium rubidium hydrogen cyanurate electro-optic crystal, respectively; the inclined surface of the right-angle prism and the right-angle face corresponding to the physical Y-plane of the lithium rubidium hydrogen cyanurate electro-optic crystal are polished; conductive films are deposited on the two sides of the right-angle prism corresponding to the physical Z-plane of the lithium rubidium hydrogen cyanurate electro-optic crystal, respectively; and then an electric field is applied to the conductive films to obtain the electro-optic deflector.

[0019] Beneficial Effects: This invention provides a lithium rubidium hydrogen cyanurate electro-optic crystal, its preparation method, and its applications. The lithium rubidium hydrogen cyanurate electro-optic crystal (RLHCY crystal) prepared by this invention has the advantages of high electro-optic coefficient at room temperature (2.2 pm / V) and high laser damage threshold (4.8 GW / cm² @ (1064 nm, 5 ns, 10 Hz)). The RLHCY crystal is a colorless and transparent crystal. The preparation method is simple; large-size crystals can be prepared in a glass growth tank using a solution method, without the need for precious metal crucibles such as platinum or iridium, thus offering a significant advantage in terms of cost for large-size crystal preparation. Attached Figure Description

[0020] Figure 1 This is a photograph of the RLHCY crystal prepared in Example 3 of the present invention.

[0021] Figure 2 This is a schematic diagram of an electro-optic modulator fabricated using the RLHCY crystal prepared in Example 3 of the present invention.

[0022] Figure 3 This is a schematic diagram of the electro-optic Q-switch fabricated using the RLHCY crystal prepared in Example 3 of the present invention.

[0023] Figure 4 This is a schematic diagram of an electro-optic deflector fabricated using the RLHCY crystal prepared in Example 3 of the present invention. Detailed Implementation

[0024] This invention provides a rubidium hydrogen cyanurate lithium electro-optic crystal, its preparation method, and its uses. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0025] This embodiment provides a rubidium hydrogen cyanurate lithium electro-optic crystal. The chemical formula of the rubidium hydrogen cyanurate lithium electro-optic crystal is RbLi(HC3N3O3)·2H2O (abbreviated as RLHCY), which belongs to the orthorhombic crystal system, space group Pna21, and cell parameters are as follows. a =15.682(7)Å, b =3.7453(17)Å, c =12.768(6)Å, α=β=γ=90°, Z=4, unit cell volume is V=749.9Å 3 .

[0026] It should be noted that the rubidium hydrogen cyanurate lithium electro-optic crystal (RLHCY crystal) described in this embodiment has an electro-optic coefficient of 2.2 pm / V and a laser damage threshold of 4.8 GW / cm at room temperature. 2 It has a wavelength of 1064 nm, 5 ns, and 10 Hz, and is a colorless and transparent crystal. It is foreseeable that it will have good application prospects in electro-optic crystals.

[0027] This embodiment also provides a method for preparing rubidium hydrogen cyanurate lithium electro-optic crystal (solution method), including the following steps: Step 1: Mix RbCl, LiOH·H2O, and C3H3N3O3, dissolve them completely in water at 60-70℃, and then cool naturally to room temperature to obtain polycrystalline rubidium hydrogen cyanurate electro-optic crystal; Step 2: Dissolve the polycrystalline lithium rubidium hydrogen cyanurate electro-optic crystal in water at 45~65℃ and keep it at the temperature for 1~5 hours to obtain a lithium rubidium hydrogen cyanurate solution. Step 3: Cool the cyanuric acid-rubidium lithium hydrogen solution to the saturation temperature at a rate of 0.5~1.0℃ / h, introduce a seed crystal on the surface of the cyanuric acid-rubidium lithium hydrogen solution, control the rotation of the seed crystal, and cool to room temperature to obtain the cyanuric acid-rubidium lithium hydrogen electro-optic crystal.

[0028] It should be noted that this embodiment uses a solution method to prepare the cyanuric acid-rubidium hydrogen lithium electro-optic crystal. The growth container can be a glass growth tank, eliminating the need for precious metal crucibles such as platinum or iridium, thus offering a significant advantage in terms of cost for large-size crystal fabrication. The seed crystal is a small single crystal selected from a polycrystalline cyanuric acid-rubidium hydrogen lithium electro-optic crystal. Furthermore, this embodiment is simple to prepare; first, a polycrystalline cyanuric acid-rubidium hydrogen lithium electro-optic crystal is prepared, then the seed crystal is introduced, and the temperature is lowered to obtain the cyanuric acid-rubidium hydrogen lithium electro-optic crystal, as shown in the figure. Figure 1 As shown, it is large and transparent.

[0029] In some embodiments, the molar ratio of the raw materials RbCl, LiOH·H2O, and C3H3N3O3 is 1:2:1.

[0030] In some embodiments, the saturation temperature is 40~55°C.

[0031] In some implementations, the seed crystal rotation speed is 6 to 15 rpm.

[0032] In some implementations, after adjusting the seed crystal rotation, the cooling rate is 0.2~1.0℃ / day.

[0033] This embodiment also provides an application of rubidium hydrogen cyanurate lithium electro-optic crystal in electro-optic devices.

[0034] This embodiment also provides an electro-optic device, including the aforementioned lithium rubidium hydrogen cyanurate electro-optic crystal.

[0035] In some embodiments, the electro-optic device is an electro-optic modulator, an electro-optic Q-switch, or an electro-optic deflector.

[0036] It should be noted that the electro-optic modulator is prepared by the following method: polishing the two end faces of the lithium rubidium hydrogen cyanurate electro-optic crystal along the physical Y-axis, depositing conductive films on the two end faces of the lithium rubidium hydrogen cyanurate electro-optic crystal along the physical Z-axis, and then applying an electric field to the conductive films on the two end faces of the lithium rubidium hydrogen cyanurate electro-optic crystal along the physical Z-axis to obtain the electro-optic modulator.

[0037] The electro-optic Q-switch is fabricated by the following method: Crystal 1 and Crystal 2 are provided, which are two identical cyanuric acid-lithium hydrogen electro-optic crystals (used to compensate for natural birefringence). The end faces of Crystal 1 and Crystal 2 along the physical Y-axis are polished, and conductive films are deposited on the end faces of Crystal 1 and Crystal 2 along the physical Z-axis. Crystal 1 and Crystal 2 are connected, wherein the physical Y-axis of Crystal 1 and Crystal 2 are parallel, the physical X-axis of Crystal 1 is parallel to the Z-axis of Crystal 2, and the physical Z-axis of Crystal 1 is parallel to the X-axis of Crystal 2. An electric field is applied to the conductive films on the end faces of Crystal 1 and Crystal 2 along the physical Z-axis to obtain the electro-optic Q-switch.

[0038] The electro-optic deflector is prepared by the following method: the lithium rubidium hydrogen cyanurate electro-optic crystal is prepared into a right-angle prism, the two right-angle faces of the right-angle prism being the physical X-plane and Y-plane of the lithium rubidium hydrogen cyanurate electro-optic crystal, respectively; the inclined surface of the right-angle prism and the right-angle face corresponding to the physical Y-plane of the lithium rubidium hydrogen cyanurate electro-optic crystal are polished; conductive films are deposited on the two sides of the right-angle prism corresponding to the physical Z-plane of the lithium rubidium hydrogen cyanurate electro-optic crystal, respectively; and then an electric field is applied to the conductive films to obtain the electro-optic deflector.

[0039] The present invention will be further described below through specific embodiments.

[0040] The RbCl, LiOH·H2O, and C3H3N3O3 used in the following examples are all commercially available raw materials with a purity of not less than 99%.

[0041] Example 1 Weigh out 336.4 g of RbCl raw material, 233.5 g of LiOH·H2O raw material and 358.6 g of C3H3N3O3 raw material in a molar ratio of 1:2:1, and add them sequentially to a growth tank containing 2000 g of ultrapure water. Stir thoroughly at 70°C until completely dissolved, and then cool down to precipitate RLHCY small crystals. The small crystals obtained above were taken out, rinsed with ultrapure water, and then dried in a 90°C oven to obtain polycrystalline rubidium hydrogen cyanurate lithium electro-optic crystal (RLHCY polycrystalline). According to the solubility curve, 302.0 g of RLHCY polycrystal and 1000 g of ultrapure water were weighed and added to the growth tank in sequence. The RLHCY polycrystal was completely dissolved at a temperature of 65°C above the saturation temperature and kept at the temperature for 1 h. The solution was cooled from 65℃ to the saturation temperature of 55℃ at a rate of 1.0℃ / h. A seed crystal was introduced into the solution, the rotation speed of the seed crystal was adjusted to 6 rpm, and the cooling rate was set to 1.0℃ / day. After the solution temperature dropped to room temperature, rubidium hydrogen cyanurate electro-optic crystal (RLHCY crystal) was obtained.

[0042] Example 2 Weigh 285.6 g of RbCl raw material, 198.3 g of LiOH·H2O raw material, and 304.5 g of C3H3N3O3 raw material according to a molar ratio of 1:2:1. Add them sequentially to a growth tank containing 2000 g of ultrapure water and stir thoroughly at 60°C until completely dissolved. Then cool down to precipitate RLHCY small crystals. Take out the small crystals obtained above, rinse them with ultrapure water, and then dry them in a 50°C oven to obtain RLHCY polycrystalline. According to the solubility curve, 302.4 g of RLHCY polycrystal and 1200 g of ultrapure water were weighed and added to the growth tank in sequence. The RLHCY polycrystal was completely dissolved at 50°C, which is above the saturation temperature, and kept at the temperature for 2 h. The solution was cooled to a saturation temperature of 45℃ at a rate of 0.8℃ / h, and a seed crystal was introduced into the solution. The rotation speed of the seed crystal was controlled at 15 rpm, and the cooling rate was 0.5℃ / day. After the solution temperature dropped to room temperature, rubidium hydrogen cyanurate electro-optic crystal (RLHCY crystal) was obtained.

[0043] Example 3 Weigh out 326.7 g of RbCl raw material, 226.8 g of LiOH·H2O raw material and 348.3 g of C3H3N3O3 raw material in a molar ratio of 1:2:1, and add them sequentially to a growth tank containing 2500 g of ultrapure water. Stir thoroughly at 60°C until completely dissolved, and then cool down to precipitate RLHCY small crystals. Take out the small crystals obtained above, rinse them with ultrapure water, and then dry them in a 65°C oven to obtain RLHCY polycrystalline. According to the solubility curve, 378.0 g of RLHCY polycrystal and 1500 g of ultrapure water were weighed and added to the growth tank in sequence. The RLHCY polycrystal was completely dissolved at a temperature of 45°C above the saturation temperature and kept at the temperature for 5 h. The solution was cooled from 45°C to the saturation temperature of 40°C at a rate of 0.5°C / h. A seed crystal was introduced into the solution, and the rotation speed of the seed crystal was controlled at 10 rpm. The cooling rate was set at 0.3°C / day. RLHCY crystals were obtained after the solution temperature dropped to room temperature. This embodiment can obtain crystals such as... Figure 1 A transparent crystal, rubidium hydrogen cyanurate lithium electro-optic crystal (RLHCY crystal).

[0044] Example 4 Weigh 285.6 g of RbCl raw material, 198.3 g of LiOH·H2O raw material, and 304.5 g of C3H3N3O3 raw material according to a molar ratio of 1:2:1. Add them sequentially to a growth tank containing 2000 g of ultrapure water and stir thoroughly at 60°C until completely dissolved. Then cool down to precipitate RLHCY small crystals. Take out the small crystals obtained above, rinse them with ultrapure water, and then dry them in a 70°C oven to obtain RLHCY polycrystalline. According to the solubility curve, 302.4 g of RLHCY polycrystalline material and 1200 g of ultrapure water were weighed and added to the growth tank in sequence. The polycrystalline material was completely dissolved at a temperature of 50°C, which is above the saturation temperature, and kept at a constant temperature for 3 h. The solution was cooled to a saturation temperature of 45℃ at a rate of 1.0℃ / h, and a seed crystal was introduced into the solution. The rotation speed of the seed crystal was controlled at 8 rpm, and the cooling rate was 0.8℃ / day. After the solution temperature dropped to room temperature, rubidium hydrogen cyanurate electro-optic crystal (RLHCY crystal) was obtained.

[0045] Example 5 Weigh out 326.7 g of RbCl raw material, 226.8 g of LiOH·H2O raw material and 348.3 g of C3H3N3O3 raw material in a molar ratio of 1:2:1, and add them sequentially to a growth tank containing 2500 g of ultrapure water. Stir thoroughly at 60°C until completely dissolved, and then cool down to precipitate RLHCY small crystals. Take out the small crystals obtained above, rinse them with ultrapure water, and then dry them in a 60°C oven to obtain RLHCY polycrystalline. According to the solubility curve, 378.0 g of RLHCY polycrystal and 1500 g of ultrapure water were weighed and added to the growth tank in sequence. The RLHCY polycrystal was completely dissolved at a temperature of 45°C above the saturation temperature and kept at the temperature for 4 h. The solution was cooled from 45℃ to the saturation temperature of 40℃ at a rate of 0.5℃ / h. A seed crystal was introduced into the solution, the rotation speed of the seed crystal was adjusted to 12 rpm, and the cooling rate was set to 0.2℃ / day. After the solution temperature dropped to room temperature, rubidium hydrogen cyanurate lithium electro-optic crystal (RLHCY crystal) was obtained.

[0046] The following are application examples: The RLHCY crystal prepared in Example 3 was used to fabricate an electro-optic modulator, such as... Figure 2 As shown.

[0047] Specific steps: Step 1: Process the RLHCY crystal into a cuboid block with dimensions of X = 4 mm, Y = 16 mm, and Z = 4 mm in the X, Y, and Z directions, respectively. Step 2: Polish the two Y-end faces of the crystal and deposit an antireflection coating to reduce reflection. The antireflection coating is usually selected from one or a combination of magnesium fluoride, silicon oxide, tantalum oxide, etc., with a thickness of 50 nm ~ 5 µm. Step 3: Plate gold on the two Z-end faces of the crystal as electrodes, and control the thickness of the gold film to achieve conductivity; Step 4: The laser beam passes along the Y direction of the crystal. Polarizer 1 and polarizer 3 are placed on both sides of the beam passing direction, with their polarization directions perpendicular to each other. The direction of the applied electric field is along the Z direction of the crystal, and the voltage modulation range is 0~3500 volts. This is used to fabricate an electro-optic modulation device.

[0048] The RLHCY crystal prepared in Example 3 was used to fabricate an electro-optic Q-switch, such as... Figure 3 As shown.

[0049] Specific steps: Step 1: Process the RLHCY crystal into two cuboids of the same size, namely crystal 1 and crystal 2. The dimensions of the crystal in the XYZ directions are X = 3 mm, Y = 15 mm, and Z = 3 mm, respectively. Step 2: Polish the Y-end face of the two crystals and deposit an antireflection coating to reduce reflection. The antireflection coating is usually selected from one or a combination of magnesium fluoride, silicon oxide, tantalum oxide, etc., with a thickness of 50 nm ~ 5 µm. Step 3: Plate gold on the Z-end face of the two crystals as electrodes, and control the thickness of the gold film to achieve conductivity. Step 4: Assemble the two crystals on the support. The Y-direction of crystal 1 and crystal 2 is parallel, the X-direction of crystal 1 and the Z-direction of crystal 2 are parallel, the light transmission direction of the laser is along the Y-direction of the crystal, and the direction of the applied electric field is along the Z-direction of the crystal. This will create an electro-optic Q-switch for use in a laser.

[0050] The RLHCY crystal prepared in Example 3 was used to fabricate an electro-optic deflector, such as... Figure 4 As shown.

[0051] Specific steps: Step 1: Process the RLHCY crystal into a right-angle prism with dimensions of X = 5 mm, Y = 5 mm, and Z = 5 mm in the X, Y, and Z directions, respectively. Step 2: Polish the Y-end face of the crystal and the bevel face of the right-angle prism, and deposit an anti-reflection coating to reduce reflection. The anti-reflection coating is usually selected from one or a combination of magnesium fluoride, silicon oxide, tantalum oxide, etc., with a thickness of 50 nm ~ 5 µm. Step 3: Plate gold on the two Z-end faces of the crystal as electrodes, and control the thickness of the gold film to achieve conductivity; Step 4: The laser beam is directed perpendicularly to the Z-direction of the crystal, and the applied electric field is directed along the Z-direction of the crystal. The voltage modulation range is 0~3500 volts. This is used to fabricate an electro-optic deflection device.

[0052] In summary, this invention provides a lithium rubidium hydrogen cyanurate electro-optic crystal, its preparation method, and its applications. This invention yields a lithium rubidium hydrogen cyanurate electro-optic crystal (RLHCY crystal), which possesses advantages such as a high electro-optic coefficient at room temperature (2.2 pm / V) and a high laser damage threshold (4.8 GW / cm² @ (1064 nm, 5 ns, 10 Hz)). The RLHCY crystal is colorless and transparent. The preparation method is simple; large-size crystals can be prepared in a glass growth tank using a solution method, eliminating the need for precious metal crucibles such as platinum or iridium, thus offering a significant cost advantage in large-size crystal preparation.

[0053] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A cyanuric acid-rubidium hydrogen lithium electro-optic crystal, characterized in that, The chemical formula of the cyanuric acid-rubidium hydrogen lithium electro-optic crystal is RbLi(HC3N3O3)·2H2O, it belongs to the orthorhombic crystal system, space group Pna21, and its unit cell parameters are as follows: a =15.682(7)Å, b =3.7453(17)Å, c =12.768(6)Å, α=β=γ=90°, Z=4, unit cell volume is V=749.9Å 3 .

2. The preparation method of the cyanuric acid-rubidium hydrogen lithium electro-optic crystal according to claim 1, characterized in that, Includes the following steps: Step 1: Mix RbCl, LiOH·H2O, and C3H3N3O3, dissolve them completely in water at 60-70℃, and then cool naturally to room temperature to obtain polycrystalline rubidium hydrogen cyanurate electro-optic crystal; Step 2: Dissolve the polycrystalline lithium rubidium hydrogen cyanurate electro-optic crystal in water at 45~65℃ and keep it at the temperature for 1~5 hours to obtain a lithium rubidium hydrogen cyanurate solution. Step 3: Cool the cyanuric acid-rubidium lithium hydrogen solution to the saturation temperature at a rate of 0.5~1.0℃ / h, introduce a seed crystal on the surface of the cyanuric acid-rubidium lithium hydrogen solution, control the rotation of the seed crystal, and cool to room temperature to obtain the cyanuric acid-rubidium lithium hydrogen electro-optic crystal.

3. The method for preparing the cyanuric acid-rubidium hydrogen lithium electro-optic crystal according to claim 2, characterized in that, The molar ratio of the raw materials RbCl, LiOH·H2O, and C3H3N3O3 is 1:2:

1.

4. The method for preparing the cyanuric acid-rubidium hydrogen lithium electro-optic crystal according to claim 2, characterized in that, The saturation temperature is 40~55℃.

5. The method for preparing the cyanuric acid-rubidium hydrogen lithium electro-optic crystal according to claim 2, characterized in that, The seed crystal rotates at a speed of 6~15 rpm.

6. The method for preparing the cyanuric acid-rubidium hydrogen lithium electro-optic crystal according to claim 2, characterized in that, After adjusting the seed crystal rotation, the cooling rate is 0.2~1.0℃ / day.

7. The application of the cyanuric acid-rubidium lithium electro-optic crystal of claim 1 in electro-optic devices.

8. An electro-optical device, characterized in that, Including the cyanuric acid-rubidium hydrogen lithium electro-optic crystal as described in claim 1.

9. An electro-optical device according to claim 8, characterized in that, The electro-optic device is an electro-optic modulator, an electro-optic Q-switch, or an electro-optic deflector.