Single crystal furnace and single crystal silicon rod production method
By integrating heating and cooling functions into the single crystal furnace, the problems of low efficiency and contamination caused by transfer during the annealing process of single crystal silicon rods are solved, realizing an efficient and continuous annealing process and improving the quality and production capacity of single crystal silicon rods.
Patent Information
- Application Number
- CN202611517284.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, monocrystalline silicon rods need to be transferred multiple times during the annealing process, resulting in low annealing efficiency, insufficient production capacity, and susceptibility to secondary contamination, which affects the quality of silicon wafers.
Design a single crystal furnace integrating heating and cooling functions, including a main chamber and a secondary chamber. After the single crystal silicon rod is finished growing, it is directly moved to the induction sleeve heating chamber in the secondary chamber for annealing. Heating is carried out by induction coil and the temperature is controlled by cooling gas, avoiding contamination and repeated heating of the silicon rod during the transfer process.
It enables continuous thermal history control of monocrystalline silicon rods in the furnace, reduces equipment investment and production cycle, improves the efficiency and quality consistency of annealing treatment, and reduces the risk of metal contamination.
Smart Images

Figure CN123153178A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor manufacturing technology, and in particular to a single crystal furnace and a method for producing single crystal silicon rods. Background Technology
[0002] Single-crystal silicon is the fundamental material for semiconductor devices, and its quality directly affects device performance and yield. During the Czochralski process for fabricating single-crystal silicon rods, oxygen from the quartz crucible dissolves into the molten silicon and enters the single-crystal silicon rod. This supersaturated interstitial oxygen forms oxygen precipitate microdefects (BMDs) in subsequent processes. To ensure a clean silicon wafer surface and retain suitable gettering centers within the wafer, annealing is typically required for the single-crystal silicon.
[0003] Current annealing processes typically involve transferring the silicon wafers to a separate annealing furnace after the monocrystalline silicon rods are sliced. This annealing method requires repeated transfers of the silicon wafers, resulting in low annealing efficiency and production capacity, making mass production difficult. Furthermore, the silicon wafers are susceptible to secondary contamination during the transfer process, affecting the quality of the annealed wafers. Summary of the Invention
[0004] This application provides a single crystal furnace and a method for producing single crystal silicon rods to improve the efficiency and quality of annealing treatment of single crystal silicon.
[0005] To achieve the above objectives, according to a first aspect of this application, a single crystal furnace is provided, comprising: The main chamber is used for producing single-crystal silicon rods; The auxiliary chamber is connected to the main chamber, and the single-crystal silicon rod can be moved from the main chamber to the auxiliary chamber. An induction sleeve is disposed in the sub-chamber, and the induction sleeve is provided with a heating cavity that extends along the axial direction, the heating cavity being used to accommodate the single crystal silicon rod; An induction coil is sleeved around the outer periphery of the induction sleeve; the induction coil is used to induce heating in the induction sleeve to increase the temperature of the single crystal silicon rod. A cooling device, at least partially located in the sub-chamber, is capable of introducing cooling gas into the heating chamber.
[0006] Optionally, the induction coil includes at least two coil segments, and the at least two coil segments are arranged along the axial direction; The single crystal furnace also includes a heating power supply, which is electrically connected to at least two of the coil segments.
[0007] Optionally, the cooling device has a first purge port located on the side of the induction sleeve away from the main chamber and facing the heating chamber.
[0008] Optionally, the cooling device has a plurality of first purge ports, which are evenly spaced along the circumference of the induction sleeve.
[0009] Optionally, the induction sleeve has a first opening that communicates with the heating chamber; the cooling device further includes a pipe that passes through the first opening and extends into the heating chamber; the cooling device also has a plurality of second purge ports that are located at one end of the pipe that extends into the heating chamber and are spaced apart circumferentially along the heating chamber.
[0010] Optionally, the single crystal furnace further includes a gas extraction device having a gas extraction port located on the side of the induction sleeve opposite to the first purge port.
[0011] Optionally, the single crystal furnace further includes a heat insulation layer located between the induction coil and the inner wall of the sub-chamber.
[0012] Optionally, the sensing sleeve is a graphite component.
[0013] Optionally, the single crystal furnace further includes at least two temperature probes, which are located inside the heating chamber and arranged at intervals along the axial direction.
[0014] According to a second aspect of this application, a method for producing single-crystal silicon rods is provided, implemented using the aforementioned single-crystal furnace, comprising: Single-crystal silicon rods are formed in the main chamber; The single-crystal silicon rod is moved from the main chamber to the heating chamber of the induction sleeve inside the auxiliary chamber; An alternating current is applied to the induction coil to cause the induction sleeve to heat up, thereby heating the single crystal silicon rod to a preset annealing temperature and holding it at that temperature for a preset time. After the preset heat preservation time, the AC current is stopped from being supplied to the induction coil, and cooling gas is introduced into the heating chamber.
[0015] Optionally, the single-crystal silicon rod rotates at a constant speed about its own axis within the heating chamber.
[0016] Optionally, during the process of introducing the cooling gas, the cooling rate of the single crystal silicon rod is controlled to be between 2°C / min and 5°C / min; After the cooling gas is introduced and the single crystal silicon rod cools down to 600°C, the cooling gas is stopped to allow the single crystal silicon rod to cool naturally to room temperature.
[0017] Optionally, during the process of applying alternating current to the induction coil, the heating rate of the single crystal silicon rod is 5°C / min to 8°C / min; The preset annealing temperature is 900℃ to 1100℃, and the preset duration is 4h to 8h.
[0018] Optionally, it also includes: After the single-crystal silicon rod is moved to the heating chamber and before the single-crystal silicon rod is heated, the main chamber and the secondary chamber are separated, the secondary chamber is evacuated, and inert gas is introduced into the secondary chamber to replace the gas in the secondary chamber.
[0019] Optionally, the gas in the sub-chamber is replaced 2 or 3 times; Each replacement involves evacuating the sub-chamber and introducing the inert gas into the sub-chamber.
[0020] Beneficial effects: In the aforementioned single-crystal furnace, the heating chamber is located within the auxiliary chamber. After the single-crystal silicon rod is fully grown in the furnace, it is lifted into the auxiliary chamber for annealing. From the end of growth until the annealing process is complete, the furnace body does not need to be removed. The single-crystal silicon rod is not exposed to the atmosphere during this process, eliminating the need for loading and unloading the furnace, thus reducing contamination during transfer. Heating and cooling are both integrated within the auxiliary chamber; heating and cooling are completed within the same chamber, resulting in a more continuous thermal history for the single-crystal silicon rod during annealing. Compared to using a separate annealing furnace after slicing, this embodiment eliminates the need for a separate annealing furnace and also eliminates the need for cooling and reheating of the single-crystal silicon rod, shortening the production cycle and reducing equipment investment.
[0021] In the above method, the single-crystal silicon rod remains inside the furnace from the end of growth to the end of annealing, eliminating the need to remove the furnace or expose it to the atmosphere, thus reducing the transfer and handling before and after annealing. The entire single-crystal silicon rod is heated simultaneously within the heating chamber, resulting in a more uniform temperature distribution along both the axial and radial directions, leading to better annealing consistency. Heating, holding, and cooling are all completed within the same heating chamber, ensuring continuous and controllable thermal history. This facilitates the regulation of oxygen precipitation formation according to a preset thermal history, thereby obtaining the desired oxygen precipitate micro-defect density. Compared to using a separate annealing furnace after slicing, this method eliminates the need for a separate annealing furnace and the single-crystal silicon rod undergoing a cooling and reheating process, shortening the production cycle and reducing equipment investment.
[0022] Other features and advantages of this application will be described in detail in the following detailed description section. Attached Figure Description
[0023] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] To gain a more complete understanding of this application and its beneficial effects, the following description will be provided in conjunction with the accompanying drawings, wherein the same reference numerals in the following description denote the same parts.
[0025] Figure 1 This is a schematic diagram of the structure of the single crystal furnace in an embodiment of this application; Figure 2 This is an assembly diagram of components such as the induction sleeve and induction coil in an embodiment of this application; Figure 3 This is a schematic flowchart of the method for producing single-crystal silicon rods in an embodiment of this application; Figure 4 This is a temperature diagram illustrating the annealing process of a conventional diameter single-crystal silicon rod in one embodiment of this application. Figure 5 This is a temperature diagram illustrating the annealing process of a large-diameter single-crystal silicon rod in another embodiment of this application.
[0026] Explanation of reference numerals in the attached figures: 11. Main chamber; 12. Secondary chamber; 13. Throat structure; 14. Isolation valve; 2. Induction sleeve; 21. Heating chamber; 22. First opening; 23. Second opening; 3. Induction coil; 31. Coil segment; 4. Heating power supply; 5. Cooling device; 51. First purge port; 52. Piping; 53. Second purge port; 6. Air extraction device; 61. Air extraction port; 7. Insulation layer; 8. Temperature probe; 9. Single crystal silicon rod. Detailed Implementation
[0027] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the protection scope of this application.
[0028] Taking wafer annealing as an example, after the growth of the single crystal silicon rod 9 in the furnace is completed, the furnace needs to be stopped, cooled and removed. Then, it is processed into silicon wafers through slicing, cleaning and other processes. Subsequently, it is loaded into an independent annealing furnace by a carrier, heated to a high temperature in a hydrogen or argon atmosphere and held at that temperature for a long time. After annealing, it is cooled down and removed from the furnace.
[0029] Annealing is separated from crystal growth and slicing, requiring silicon wafers to undergo multiple transfers. Due to the large number and thinness of the wafers, they easily come into contact with tooling and carriers during loading, transfer, and unloading, and are exposed to the atmosphere. This increases the level of particle and metal contamination on the surface, and the ratio of surface cleanliness to getter sites directly affects device manufacturing yield. After growth is complete, the single-crystal silicon rod is cooled to room temperature, then reheated during annealing. The superposition of these two heating and cooling processes easily introduces new thermal stress. The annealing furnace also requires a separate heating, atmosphere, and temperature control system, resulting in a longer furnace cycle and impacting both production capacity and equipment investment.
[0030] Based on this, the present application provides a single crystal furnace and a method for producing single crystal silicon rods, which enables the single crystal silicon rod 9 to remain in an inert gas environment within the single crystal furnace from the end of growth to the end of annealing, without transfer between furnace bodies, reducing metal contamination on the surface and inside the furnace, while eliminating the need for a separate annealing furnace and repeated heating, shortening the production cycle and reducing equipment investment.
[0031] like Figure 1 , Figure 2 As shown in the illustration, this application provides a single-crystal furnace, including a main chamber 11 and a secondary chamber 12. The secondary chamber 12 is located above the main chamber 11 and communicates with the main chamber 11. The main chamber 11 is used to produce single-crystal silicon rods 9, for example, the main chamber 11 is used to grow single-crystal silicon rods 9 by the Czochralski method. In some embodiments, a throat structure 13 is provided between the main chamber 11 and the secondary chamber 12, and the secondary chamber 12 communicates with the main chamber 11 through the throat structure 13.
[0032] The auxiliary chamber 12 is equipped with an induction sleeve 2. The induction sleeve 2 forms an axial (i.e., Figure 1 , Figure 2 A cavity (vertically) penetrating through the space, referred to in this embodiment as heating cavity 21, is used to accommodate the single crystal silicon rod 9.
[0033] An induction coil 3 is fitted around the outer periphery of the induction sleeve 2. The induction coil 3 is used to induce heating in the induction sleeve 2. Specifically, when alternating current is applied to the induction coil 3, an alternating magnetic field is generated around the induction coil 3. Eddy currents are induced in the induction sleeve 2 in the alternating magnetic field, thus generating heat. The heat is transferred to the monocrystalline silicon rod 9 inside the heating cavity 21 through thermal radiation and thermal conduction. It can be understood that the induction sleeve 2 surrounds the monocrystalline silicon rod 9, and heat is transferred from the periphery of the monocrystalline silicon rod 9 to its interior, resulting in a relatively small radial temperature difference in the monocrystalline silicon rod 9.
[0034] The single crystal furnace also includes a cooling device 5. The cooling device 5 is at least partially located in the sub-chamber 12 and is capable of introducing cooling gas into the heating chamber 21.
[0035] During annealing, after the monocrystalline silicon rod 9 completes its growth in the main chamber 11, it is lifted from bottom to top into the auxiliary chamber 12 and enters the heating chamber 21 of the induction sleeve 2. The monocrystalline silicon rod 9 is placed vertically in the heating chamber 21, maintaining a relatively uniform distance from the inner wall of the induction sleeve 2. Then, alternating current is supplied to the induction coil 3, causing the induction sleeve 2 to heat up. The heat is transferred to the entire monocrystalline silicon rod 9 in the heating chamber 21 through thermal radiation and conduction, raising the temperature of the monocrystalline silicon rod 9 to the preset annealing temperature. This temperature is maintained for a preset time, during which alternating current is continuously supplied to the induction coil 3. After the holding period, the alternating current supply to the induction coil 3 is stopped, and the cooling device 5 introduces cooling gas into the heating chamber 21. The cooling gas carries away the heat from the monocrystalline silicon rod 9, causing it to cool down at a set rate.
[0036] In the aforementioned single-crystal furnace, the heating chamber 21 is located within the sub-chamber 12. After the single-crystal silicon rod 9 completes its growth within the furnace, it is lifted into the sub-chamber 12 for annealing. From the end of growth until the end of annealing, it is not necessary to remove the furnace body. During this process, the single-crystal silicon rod 9 is not exposed to the atmosphere, eliminating the need for handling during loading and unloading, thus reducing contamination during transfer. Heating and cooling are both integrated within the sub-chamber 12; heating and cooling are completed within the same chamber, resulting in a more continuous thermal history for the single-crystal silicon rod 9 during annealing. Compared to using a separate annealing furnace after slicing, this embodiment eliminates the need for a separate annealing furnace and also eliminates the need for cooling and reheating of the single-crystal silicon rod 9, shortening the production cycle and reducing equipment investment.
[0037] In some embodiments, the induction sleeve 2 is a graphite component, meaning the induction sleeve 2 is made of graphite. Graphite has good electrical conductivity and can induce eddy currents and generate heat in an alternating magnetic field. Furthermore, graphite is relatively stable at high temperatures and does not easily volatilize impurities, thus preventing the sleeve itself from introducing impurities into the single-crystal silicon rod 9.
[0038] It is understandable that the induction sleeve 2 can also be made of other materials that can work stably at high temperatures and have electrical conductivity. For example, the induction sleeve 2 can be made of carbon-carbon composite material. Carbon-carbon composite material and graphite are both carbon materials, and they can also generate heat in an alternating magnetic field. They have good thermal shock resistance and are not easy to crack during repeated heating and cooling. Therefore, they are suitable for making sleeves with thin walls.
[0039] Optionally, the single-crystal furnace may also include an insulation layer 7. The insulation layer 7 is located between the induction coil 3 and the inner wall of the sub-chamber 12, and is disposed around the induction coil 3. In some embodiments, the insulation layer 7 is a hard graphite carbon felt with a thickness of 10 cm to 15 cm. The hard graphite carbon felt is resistant to high temperatures, can maintain its shape and heat insulation capacity at the temperature required for annealing, and is made of carbon material, the same as the induction sleeve 2, making it less likely to introduce impurities into the single-crystal silicon rod 9.
[0040] By providing the insulation layer 7, the heat loss from the heating chamber 21 through the wall of the secondary chamber 12 can be reduced, making it easier to maintain the heating chamber 21 at the required annealing temperature during the heating and holding stages. The output power of the heating power supply 4 can also be reduced accordingly. Simultaneously, the insulation layer 7 makes the circumferential heat dissipation within the secondary chamber 12 more uniform, which helps to reduce the circumferential temperature difference in the heating chamber 21. In other embodiments, the insulation layer 7 may not be provided; in this case, the temperature inside the heating chamber 21 can be maintained by increasing the output power of the heating power supply 4.
[0041] like Figure 2 As shown, the induction coil 3 may include at least two coil segments 31, which are arranged along the axial direction of the heating cavity 21 and periodically in the axial direction, that is, the coil segments 31 are arranged sequentially along the axial direction, and the spacing between adjacent coil segments 31 is the same. The single crystal furnace also includes a heating power supply 4, which is electrically connected to the at least two coil segments 31 respectively to supply power to each coil segment 31. In some embodiments, the induction coil 3 is a high-frequency coil with a frequency of 10kHz to 50kHz.
[0042] The single-crystal furnace may also include at least two temperature probes 8, which are located inside the heating chamber 21 and arranged at intervals along the axial direction of the heating chamber 21, for detecting the temperature at different positions along the axial direction within the heating chamber 21. Based on the detected temperature distribution along the axial direction, the power supply of the heating power source 4 to the coil segments 31 at different positions can be adaptively changed, thereby reducing the axial temperature difference and improving the uniformity and quality of annealing.
[0043] The above configuration facilitates zoned temperature adjustment of the heating cavity 21 along its axial direction. The heating power supply 4 supplies power to each coil segment 31, allowing the heating power of each coil segment 31 to be set independently. Temperature probes 8 are spaced apart along the axial direction, reflecting the temperature at different points along the axial direction of the heating cavity 21. Adjusting the power of the corresponding coil segment 31 based on the detection results of each temperature probe 8 can make the temperature at different points along the axial direction of the heating cavity 21 more uniform. It is understood that the temperature distribution along the axial direction of the single-crystal silicon rod 9 is therefore more uniform, and the formation of oxygen precipitates during annealing is also more consistent, which is beneficial for obtaining more uniformly distributed oxygen precipitate micro-defects. Exemplarily, in some embodiments, the temperature deviation of the heating cavity 21 along its axial direction does not exceed ±5°C.
[0044] Continue to refer to Figure 2 As shown, the induction sleeve 2 has a first opening 22 and a second opening 23, both of which are connected to the heating chamber 21. The first opening 22 is located at the end of the induction sleeve 2 that is axially away from the main chamber 11, and the second opening 23 is located at the end of the induction sleeve 2 that is axially close to the main chamber 11.
[0045] The cooling device 5 has a first purge port 51. The first purge port 51 is located on the side of the induction sleeve 2 away from the main chamber 11 and is positioned towards the heating chamber 21. Cooling gas is blown into the heating chamber 21 from the first purge port 51 and the first opening 22 to cool the single crystal silicon rod 9 located in the heating chamber 21.
[0046] The single crystal furnace also includes a gas extraction device 6. The gas extraction device 6 has an extraction port 61, located on the side of the induction sleeve 2 opposite to the first purge port 51, that is, at the end of the induction sleeve 2 where the second opening 23 is located. Cooling gas enters the heating chamber 21 through the first purge port 51 and the first opening 22, then enters the gas extraction device 6 through the second opening 23 and the extraction port 61, and is then discharged from the secondary chamber 12, thus facilitating the continuous input of cooling gas. Optionally, the cooling gas is argon.
[0047] In other words, the first purge port 51 and the exhaust port 61 are located on opposite sides of the induction sleeve 2, forming an airflow path through the heating chamber 21. After entering the heating chamber 21 through the first purge port 51, the cooling gas flows axially along the entire length of the single-crystal silicon rod 9 and then exits through the exhaust port 61. It can be understood that the airflow covers the entire length of the heating chamber 21 axially, resulting in relatively uniform heat exchange conditions and cooling along the entire length of the single-crystal silicon rod 9. Furthermore, the gas after heat exchange is less likely to remain trapped in the secondary chamber 12. The cooling rate of the single-crystal silicon rod 9 can be adjusted by regulating the flow rate of the cooling gas.
[0048] Optionally, the cooling device 5 has multiple first purge ports 51, which are evenly spaced along the circumference of the induction sleeve 2. That is, the multiple first purge ports 51 are distributed around the axis of the induction sleeve 2, with the same spacing between adjacent first purge ports 51, forming a ring-shaped purge port group. After the multiple first purge ports 51 are evenly arranged circumferentially, cooling gas enters the heating chamber 21 from the same height at multiple circumferential locations. The cooling gas conditions at different locations on the single-crystal silicon rod 9 at the same height are relatively similar, resulting in a smaller circumferential temperature difference across the cross-section of the single-crystal silicon rod 9 and reducing the likelihood of overcooling on one side.
[0049] Optionally, the cooling device 5 also has a plurality of second purge ports 53. The cooling device 5 also includes a pipe 52, which passes through the first opening 22 and extends into the heating chamber 21. The plurality of second purge ports 53 are disposed at one end of the pipe 52 that extends into the heating chamber 21 and are spaced apart circumferentially in the heating chamber 21. Cooling gas enters the heating chamber 21 through the pipe 52 and the second purge ports 53. With the plurality of second purge ports 53 located in the heating chamber 21 and spaced apart circumferentially, the cooling gas can enter the heating chamber 21 not only from the first purge port 51, but also from multiple positions circumferentially in the heating chamber 21. Therefore, the middle section of the single crystal silicon rod 9 is also within the coverage of the cooling airflow, which helps to improve the temperature uniformity of the single crystal silicon rod 9 along the axial direction.
[0050] In some embodiments, an isolation valve 14 is provided between the secondary chamber 12 and the main chamber 11. The isolation valve 14 is used to keep the secondary chamber 12 in a connected state or in a disconnected state from the main chamber 11. The isolation valve 14 may be a flap valve. When the isolation valve 14 is in the connected state, the monocrystalline silicon rod 9 can move between the main chamber 11 and the secondary chamber 12 (for example, during the crystal pulling process of producing the monocrystalline silicon rod 9, the main chamber 11 and the secondary chamber 12 are in a connected state); when the isolation valve 14 is in the disconnected state, the secondary chamber 12 becomes a relatively independent cavity, which facilitates the separate atmosphere treatment of the secondary chamber 12.
[0051] like Figure 3 As shown in the embodiments of this application, a method for producing single-crystal silicon rods is also provided. This method is implemented using the above-mentioned single-crystal furnace and includes the following steps.
[0052] Obtain single-crystal silicon rods 9.
[0053] In this embodiment, the single-crystal silicon rod 9 is grown in the main chamber 11 by the Czochralski method, and the grown single-crystal silicon rod 9 is located in the main chamber 11. During the Czochralski process, the main chamber 11 and the auxiliary chamber 12 are in a connected state and are in the same atmosphere.
[0054] The single crystal silicon rod 9 is moved from the main chamber 11 to the heating chamber 21 of the induction sleeve 2 in the auxiliary chamber 12.
[0055] Specifically, the single-crystal silicon rod 9 is lifted from bottom to top into the auxiliary chamber 12 and enters the heating chamber 21. The single-crystal silicon rod 9 is placed vertically in the heating chamber 21, maintaining a relatively uniform distance from the inner wall of the induction sleeve 2.
[0056] An alternating current is applied to the induction coil 3 to cause the induction sleeve 2 to heat up, thereby heating the single crystal silicon rod 9 to a preset annealing temperature and holding it at that temperature for a preset time.
[0057] Specifically, alternating current generates an alternating magnetic field around the induction coil 3. The induction sleeve 2 induces eddy currents in the alternating magnetic field and thus heats up. The heat is transferred to the entire single crystal silicon rod 9 in the heating cavity 21 through thermal radiation and thermal conduction, and the single crystal silicon rod 9 heats up accordingly. After the temperature rises to the preset annealing temperature, alternating current continues to be supplied to the induction coil 3 to keep the single crystal silicon rod 9 at that temperature for a preset time.
[0058] After the preset heat preservation time, the AC current is stopped from being supplied to the induction coil 3, and cooling gas is introduced into the heating chamber 21.
[0059] Specifically, after the heat preservation is completed, the power supply to the induction coil 3 is stopped, the induction sleeve 2 stops heating, and the cooling device 5 introduces cooling gas into the heating chamber 21. The cooling gas carries away the heat from the monocrystalline silicon rod 9, thus cooling the monocrystalline silicon rod 9. Heating and cooling are carried out sequentially, and the AC power supply to the induction coil 3 is stopped before the cooling gas is introduced into the heating chamber 21.
[0060] In the above method, the single-crystal silicon rod 9 remains inside the furnace from the end of growth to the end of annealing, without needing to be removed from the furnace or exposed to the atmosphere, thus reducing the transfer and handling before and after annealing. The entire single-crystal silicon rod 9 is placed in the heating chamber 21 and heated simultaneously, resulting in a relatively uniform temperature distribution along both the axial and radial directions, leading to better annealing consistency. Heating, holding, and cooling are all completed within the same heating chamber 21, ensuring continuous and controllable thermal history. This facilitates the regulation of oxygen precipitation formation according to a preset thermal history, thereby obtaining the desired oxygen precipitate micro-defect density. Compared to using a separate annealing furnace after slicing, this method eliminates the need for a separate annealing furnace and the need for one cooling and reheating cycle of the single-crystal silicon rod 9, shortening the production cycle and reducing equipment investment.
[0061] After the single-crystal silicon rod 9 is moved to the heating chamber 21, and before alternating current is applied to the induction coil 3, the main chamber 11 and the secondary chamber 12 are isolated. The secondary chamber 12 is evacuated, and inert gas is introduced into it to replace the gas inside. Specifically, the gas in the secondary chamber 12 is replaced two or three times. Each replacement includes evacuating the secondary chamber 12 and introducing inert gas, that is, first evacuating the secondary chamber 12 to 15 Torr, then introducing inert gas, repeating this process two to three times to remove oxygen, water vapor, and impurities from the secondary chamber 12. In some embodiments, the inert gas is argon with a purity of not less than 99.99%.
[0062] Alternating current is then applied to the induction coil 3. This alternating current generates an alternating magnetic field around the induction coil 3. Eddy currents are induced in the induction sleeve 2 within this magnetic field, causing it to heat up. This heat is transferred to the entire single-crystal silicon rod 9 within the heating cavity 21 via thermal radiation and conduction, causing the single-crystal silicon rod 9 to heat up. During the heating process, the heating rate of the single-crystal silicon rod 9 is 5°C / min to 8°C / min. For example, a segmented uniform heating method can be used to reduce the temperature difference and thermal stress that might occur inside the single-crystal silicon rod 9 if the heating is too rapid. Within the heating cavity 21, the single-crystal silicon rod 9 rotates uniformly around its own axis, resulting in a more uniform radial temperature distribution across all circumferential directions.
[0063] After the monocrystalline silicon rod 9 is heated to the preset annealing temperature, alternating current continues to be supplied to the induction coil 3, causing the monocrystalline silicon rod 9 to be held at the preset annealing temperature for a preset time. The preset annealing temperature is 900℃ to 1100℃, and the preset time is 4h to 8h. Taking a preset annealing temperature of 900℃ to 1100℃ and a preset time of 4h to 8h as an example, the holding time allows the oxygen after the primary oxygen clusters inside the monocrystalline silicon rod 9 are dissolved to be redistributed, thus regulating the formation of oxygen precipitates. The holding time can be selected according to the specific characteristics of the monocrystalline silicon rod 9. For example, a longer holding time is used for monocrystalline silicon rods 9 with high defect density and large defect size, allowing the internal oxygen precipitate defects to decompose more fully; a shorter holding time is used for monocrystalline silicon rods 9 with low defect density and small defect size, shortening the production cycle while meeting the requirements.
[0064] In some embodiments, the heating rate, annealing temperature, and holding time can be selected according to the specific characteristics of the single-crystal silicon rod 9. For example, as... Figure 4 As shown, for standard diameter single-crystal silicon rods (generally 12 inches or less), the heating rate is 7℃ / min to 8℃ / min, the annealing temperature is 900℃ to 1000℃, and the holding time is 4h to 5h; for larger diameter single-crystal silicon rods (generally 12 inches and above), such as Figure 5 As shown, the heating rate is 5℃ / min to 6℃ / min, the annealing temperature is 1050℃ to 1100℃, and the holding time is 6h to 8h. The corresponding temperature-time curves can be found in [reference needed]. Figure 4 and Figure 5 .
[0065] After the preset heat preservation time, the AC power supply to the induction coil 3 is stopped, and cooling gas is introduced into the heating chamber 21. Specifically, after the heat preservation is completed, the power supply to the induction coil 3 is stopped, the induction sleeve 2 stops heating, and the cooling device 5 introduces cooling gas into the heating chamber 21. The cooling gas carries away the heat from the monocrystalline silicon rod 9, causing the monocrystalline silicon rod 9 to cool down. Heating and cooling are performed sequentially, and the AC power supply to the induction coil 3 is stopped before the cooling gas is introduced into the heating chamber 21. During the process of introducing the cooling gas, the cooling rate of the monocrystalline silicon rod 9 is 2℃ / min to 5℃ / min; after the cooling gas is introduced and the monocrystalline silicon rod 9 cools down to 600℃, the cooling gas supply is stopped, allowing the monocrystalline silicon rod 9 to cool naturally to room temperature. The temperature range of 600℃ to 650℃ is the optimal temperature range for efficient nucleation of interstitial oxygen in silicon. By controlling the cooling rate to 2℃ / min to 5℃ / min and allowing natural cooling after reaching 600℃, the nucleation process during the cooling stage can be relatively controlled, and the thermal stress inside the single crystal silicon rod 9 can be slowly released. The single crystal silicon rod 9 can be removed after its temperature drops below 50℃.
[0066] During the annealing process, the furnace door should not be opened or the equipment parameters adjusted during the heat preservation period to avoid sudden changes in temperature and atmosphere inside the heating chamber 21. During natural cooling, the furnace body can be kept sealed and active heat dissipation can be stopped, allowing the monocrystalline silicon rod 9 to cool with the furnace. After natural cooling is completed, the temperature inside the furnace is roughly equivalent to the room temperature, for example, 20°C to 25°C. At this point, the supply of protective gas to the furnace can be stopped and the monocrystalline silicon rod 9 can be removed.
[0067] In the above method, the secondary chamber 12 is evacuated and replaced with inert gas before annealing. This reduces the amount of oxygen, water vapor, and impurities in the secondary chamber 12, making the single-crystal silicon rod 9 less prone to oxidation at high temperatures and less susceptible to surface contamination. During the heat preservation process, the single-crystal silicon rod 9 rotates around its own axis, resulting in more uniform circumferential heating, which is beneficial for obtaining a more evenly distributed oxygen precipitate micro-defect. The heating rate, annealing temperature, and heat preservation time are set according to the specific conditions of the single-crystal silicon rod 9, which can balance the control effect of oxygen precipitate and production efficiency. The cooling rate is controlled between 2℃ / min and 5℃ / min, and the cooling gas is stopped after cooling to 600℃, and natural cooling is initiated. The nucleation process during the cooling stage is relatively controllable.
[0068] The relationship between annealing temperature, holding time, heating rate, and cooling rate over time can be found in [reference needed]. Figure 4 and Figure 5 . Figure 4 The temperature-time curve of a standard diameter single crystal silicon rod 9 is shown. The heating section corresponds to a heating rate of 7℃ / min to 8℃ / min, the holding section corresponds to an annealing temperature of 900℃ to 1000℃ and a holding time of 4h to 5h, the cooling section corresponds to a cooling rate of 2℃ / min to 5℃ / min, and 600℃ is the switching point where the cooling gas is stopped and natural cooling is switched to. Figure 5 The temperature-time curves of a single-crystal silicon rod 9 with a large diameter and high oxygen content are shown. The heating phase corresponds to a heating rate of 5℃ / min to 6℃ / min, the holding phase corresponds to an annealing temperature of 1050℃ to 1100℃ and a holding time of 6h to 8h, and the cooling phase corresponds to the 600℃ switching point. Figure 4 same.
[0069] In some embodiments, after the above-described annealing treatment, the oxygen precipitate micro-defect density within the single-crystal silicon rod 9 can be controlled to be 1×10⁻⁶. 8 / cm³ to 3×10 9 / cm³. The density of oxygen precipitate micro-defects can be detected by selective etching optical microscopy. For example, a sample taken from a single-crystal silicon rod 9 is first annealed in two stages at 800℃ to 1000℃ to precipitate oxygen. Then, the sample is cleaved and selectively etched with Secco or Wright etching solution. Pit formation is formed at the location of oxygen precipitate micro-defects. Finally, the density of oxygen precipitate micro-defects is obtained by counting and converting the samples using a metallographic microscope.
[0070] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more features. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.
[0071] In the above embodiments, the descriptions of each embodiment have different focuses. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.
[0072] The embodiments, implementation methods, and related technical features of this application can be combined and substituted for each other without conflict.
[0073] The above are merely preferred embodiments of this application and are not intended to limit this application in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of this application without departing from the scope of the technical solution of this application shall still fall within the scope of the technical solution of this application.
Claims
1. A single crystal furnace, characterized in that, include: Main chamber (11), which is used to produce single crystal silicon rods (9); The secondary chamber (12) is connected to the main chamber (11), and the single crystal silicon rod (9) can move from the main chamber (11) to the secondary chamber (12); An induction sleeve (2) is disposed in the sub-chamber (12). The induction sleeve (2) is provided with a heating cavity (21) that runs through the axis. The heating cavity (21) is used to accommodate the single crystal silicon rod (9). An induction coil (3) is sleeved on the outer periphery of the induction sleeve (2); the induction coil (3) is used to cause the induction sleeve (2) to generate heat in the induction, thereby increasing the temperature of the single crystal silicon rod (9); The cooling device (5) is located at least partially in the sub-chamber (12) and is capable of introducing cooling gas into the heating chamber (21).
2. The single crystal furnace according to claim 1, characterized in that, The induction coil (3) includes at least two coil segments (31), and the at least two coil segments (31) are arranged along the axial direction; The single crystal furnace also includes a heating power supply (4), which is electrically connected to at least two of the coil segments (31).
3. The single crystal furnace according to claim 1, characterized in that, The cooling device (5) has a first purge port (51), which is located on the side of the induction sleeve (2) away from the main chamber (11) and is positioned towards the heating chamber (21).
4. The single crystal furnace according to claim 3, characterized in that, The cooling device (5) has a plurality of first purge ports (51), which are evenly spaced along the circumference of the induction sleeve (2).
5. The single crystal furnace according to claim 3, characterized in that, The induction sleeve (2) has a first opening (22) that communicates with the heating chamber (21); the cooling device (5) further includes a pipe (52) that passes through the first opening (22) and extends into the heating chamber (21); the cooling device (5) also has a plurality of second purge ports (53) that are located at one end of the pipe (52) that extends into the heating chamber (21) and are spaced apart along the circumference of the heating chamber (21).
6. The single crystal furnace according to claim 3, characterized in that, The single crystal furnace also includes an air extraction device (6), which has an air extraction port (61) located on the side of the induction sleeve (2) away from the first purge port (51).
7. The single crystal furnace according to claim 1, characterized in that, The single crystal furnace also includes a heat insulation layer (7), which is located between the induction coil (3) and the inner wall of the sub-chamber (12).
8. The single crystal furnace according to claim 1, characterized in that, The sensing sleeve (2) is a graphite part.
9. The single crystal furnace according to any one of claims 1 to 8, characterized in that, The single crystal furnace also includes at least two temperature probes (8), which are located in the heating chamber (21) and are arranged at intervals along the axial direction.
10. A method for producing single-crystal silicon rods, implemented using a single-crystal furnace as described in any one of claims 1 to 9, characterized in that, include: A single-crystal silicon rod (9) is formed in the main chamber (11); The single crystal silicon rod (9) is moved from the main chamber (11) to the heating chamber (21) of the induction sleeve (2) in the auxiliary chamber (12); An alternating current is applied to the induction coil (3) to cause the induction sleeve (2) to heat up, thereby heating the single crystal silicon rod (9) to a preset annealing temperature and holding it at that temperature for a preset time. After the preset time of heat preservation, the AC current is stopped from being supplied to the induction coil (3), and cooling gas is supplied to the heating chamber (21).
11. The method for producing single-crystal silicon rods according to claim 10, characterized in that, In the heating chamber (21), the single crystal silicon rod (9) rotates at a constant speed around its own axis.
12. The method for producing single-crystal silicon rods according to claim 10, characterized in that, During the process of introducing the cooling gas, the cooling rate of the single crystal silicon rod (9) is controlled to be 2℃ / min to 5℃ / min; After the cooling gas is introduced and the single crystal silicon rod (9) cools down to 600°C, the cooling gas is stopped so that the single crystal silicon rod (9) can cool down to room temperature naturally.
13. The method for producing single-crystal silicon rods according to claim 10, characterized in that, During the process of passing alternating current through the induction coil (3), the heating rate of the single crystal silicon rod (9) is 5°C / min to 8°C / min; The preset annealing temperature is 900℃ to 1100℃, and the preset duration is 4h to 8h.
14. The method for producing single-crystal silicon rods according to claim 10, characterized in that, Also includes: After the single crystal silicon rod (9) is moved to the heating chamber (21) and before the single crystal silicon rod (9) is heated, the main chamber (11) and the sub-chamber (12) are separated, the sub-chamber (12) is evacuated, and inert gas is introduced into the sub-chamber (12) to replace the gas in the sub-chamber (12).
15. The method for producing single-crystal silicon rods according to claim 14, characterized in that, The number of gas replacements in the sub-chamber (12) is 2 or 3 times; Each replacement includes evacuating the sub-chamber (12) and introducing the inert gas into the sub-chamber (12).