A coarse denier and low porosity polyester industrial filament and a method for preparing the same
By setting up heating rollers with opposite directions on the stretching heating roller for double-sided symmetrical contact heating and pressure binding, the problems of uneven heating and unstable production of coarse denier, low-pore polyester industrial filaments are solved, achieving highly uniform stretching and highly stable production, and improving the mechanical properties and consistency of the products.
Patent Information
- Application Number
- CN202611675707.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies struggle to achieve both uniform heating and improved mechanical properties while simultaneously enhancing production stability in the production of coarse denier, low-pore polyester industrial filaments. In particular, products with a single filament fineness ≥20D are prone to uneven heating, vibration, and breakage issues on the hot rollers.
By using a combination of a heating roller with opposite directions, the same temperature, and the same surface linear velocity, and a stretching heating roller, double-sided symmetrical contact heating and pressure perpendicular to the surface of the filament bundle are implemented to ensure uniform heat conduction and mechanically bind the filament bundle, thus suppressing single filament jumping.
It achieves highly uniform stretching and stable production of coarse denier, low-pore polyester industrial filaments, improves the consistency of breaking strength, breaking elongation and abrasion resistance, and reduces the abnormal degradation rate of fineness and fuzz.
Smart Images

Figure CN123153183A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polyester industrial filament production technology, and relates to a coarse denier, low-pore polyester industrial filament and its preparation method. Background Technology
[0002] Coarse denier, low-pore polyester industrial filament refers to polyester industrial yarn with a relatively large single filament fineness and a small number of single filaments. In this field, polyester industrial yarn with a total fineness ≥1000D is generally referred to as "coarse denier." Correspondingly, "low-pore" means fewer spinneret holes and fewer single filaments, thus increasing the single filament fineness. This type of industrial yarn has advantages such as high strength, abrasion resistance, and dimensional stability, and is widely used in safety belts, lifting slings, cables, and other fields, forming an important component of abrasion-resistant industrial yarns. Its production process requires no additives; instead, it relies on the extremely high single filament fineness to achieve its abrasion resistance.
[0003] In the existing technology, the production of coarse denier, low-pore polyester industrial filaments mainly suffers from the following problems:
[0004] (1) Uneven heating leads to poor mechanical properties. Due to the large fineness of the monofilament, the side of the monofilament that is in contact with the hot roller is fully heated, while the side that is away from the hot roller is not sufficiently heated because the monofilament is thick and the heating time on the hot roller is short. This results in uneven heating on both sides of the monofilament, which in turn causes uneven stretching. Specifically, this manifests as low breaking strength, large coefficient of variation of breaking strength, large fluctuation of breaking elongation, and high coefficient of variation of breaking elongation.
[0005] (2) Poor production stability. Due to the uneven heating of the relatively thick monofilament, the holding force on the hot roller is uneven, and the monofilament is prone to jumping back and forth on the hot roller, causing phenomena such as fuzz, breakage, and skipping. Especially for products with a monofilament fineness of more than 20D, the skipping problem is more prominent, the spinning condition is extremely unstable, and the physical properties fluctuate greatly. This type of product is basically in a blank state in the market.
[0006] To address the above problems, existing technologies mainly propose two types of solutions from the perspective of improving the heating method.
[0007] One method is non-contact heating. Patent application CN102758287A discloses a yarn heating device that uses a corrugated plate opposite to the guide roller to heat the yarn in a non-contact manner by utilizing multiple spaces defined by the recesses.
[0008] However, non-contact heating (such as infrared heating, heating plates, heating covers, etc.) has inherent drawbacks: poor temperature uniformity, prone to axial or circumferential hot spots, causing localized overheating or underheating, affecting the dyeing uniformity and strength uniformity of the product; low thermal efficiency and high energy consumption, requiring higher heat source temperatures to achieve the heating effect required for the monofilament. Especially for coarse denier, low-pore polyester industrial filaments with a monofilament fineness ≥20D, the above defects are further amplified due to the thicker filaments: the heat transfer depth from the surface to the interior is insufficient, making it more difficult for the core layer to reach the temperature required for stretching; the radial and axial temperature gradients of the monofilament are larger, resulting in poorer heating uniformity; at the same time, the lack of contact constraint between non-contact heating and the monofilament cannot suppress the jumping of the monofilament on the heated roller, exacerbating the problems of filament jumping and breakage. Therefore, non-contact heating cannot guarantee the heating uniformity of this type of product, nor can it solve the problem of monofilament jumping on the heated roller.
[0009] The second method is contact heating. Patent CN214114504U discloses a carbon fiber yarn heating and conveying device, which uses two sets of heating rollers to heat the carbon fiber yarn evenly on both sides. Patent application CN116988174A discloses a method for preparing high-strength, low-elongation polyester industrial yarn, which uses a cross-winding method to heat both sides of the yarn bundle sequentially to improve the uniformity of stretching.
[0010] However, in the above-mentioned contact heating scheme, the two sides of the fiber are not heated at the same time. The fiber will cool down between the two sets of heated rollers. For coarse denier fibers, it is difficult to meet the temperature required for stretching, and the improvement of heating uniformity is limited. At the same time, this scheme also cannot solve the problem of monofilament jumping on the heated rollers.
[0011] In summary, existing technologies still cannot simultaneously meet the requirements of uniform heating, excellent mechanical properties, and stable production for coarse denier, low-pore polyester industrial filaments (especially varieties with a single filament fineness ≥20D), and further improvements are urgently needed. Summary of the Invention
[0012] The purpose of this invention is to solve the problems existing in the prior art and to provide a coarse denier, low-pore polyester industrial filament and its preparation method.
[0013] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0014] A method for preparing coarse denier, low-pore polyester industrial filament includes a stretching process. The stretching process uses stretching hot rollers, and each stretching hot roller is equipped with a heat tracing roller arranged in parallel with it, rotating in the opposite direction, having the same temperature, and having the same surface linear velocity. During the stretching process, the heat tracing roller is used to assist in heating and applying pressure to the filament bundle on the stretching hot roller.
[0015] The principle of this invention is as follows:
[0016] A heat-tracing roller, which is tangentially pressed against the stretching heat roller and rotates in opposite directions at the same temperature and speed, applies double-sided symmetrical contact heating and pressure perpendicular to the surface of the filament bundle (normal direction) to mechanically bind the filament bundle.
[0017] Thermally, polyester is a poor conductor of heat. With traditional single-sided heating, heat is conducted only from one side, resulting in limited heat penetration within a very short residence time. Furthermore, the larger radius of coarse denier fibers causes the temperature on the opposite side to be far below the glass transition temperature, leading to "cold stretching," which produces micropores and voids, resulting in poor mechanical properties. This invention employs double-sided symmetrical contact heating, where heat is conducted symmetrically from both surfaces of the fiber bundle towards the center, with opposite heat flow directions. This doubles the heating rate of the fiber bundle, allowing the entire cross-section to reach above the glass transition temperature within the same residence time. The radial temperature gradient is minimal, achieving uniform softening and ensuring uniform tensile deformation.
[0018] Kinematically, the heating roller and the stretching roller rotate in opposite directions, ensuring that at the point of tangency, the surface linear velocities of both rollers point towards the yarn outlet, jointly propelling the yarn forward. The identical surface linear velocities ensure no relative slippage between the yarn and the roller surfaces, avoiding additional friction or stretching caused by speed differences. Simultaneously, the heating roller does not participate in stretching and does not generate an axial speed gradient; the stretching ratio is precisely controlled by the speed difference between the front and rear stretching rollers, guaranteeing process controllability and reproducibility.
[0019] From a mechanical perspective, coarse-denier, low-pore polyester industrial filaments, due to their thick filaments, few holes, high bending stiffness, and small contact area with the stretching heating roller, resulting in insufficient friction, are prone to radial runout and axial movement during high-speed operation. This leads to fluctuations in heating distance, uneven heating, and even filament breakage. The heating roller presses the filament bundle against the surface of the stretching heating roller through normal pressing, forming a forced clamp, eliminating the free movement space of the filaments, and increasing the friction between the filament bundle and the stretching heating roller. This prevents slippage caused by tension fluctuations, thereby significantly suppressing filament runout and ensuring continuous and stable spinning.
[0020] This invention works synergistically from three dimensions: thermodynamics, kinematics, and mechanics, directly solving the two core problems in existing technologies: "poor mechanical properties due to uneven heating" and "poor production stability," thereby achieving highly uniform stretching and highly stable production of coarse denier, low-pore polyester industrial filaments.
[0021] As a preferred technical solution:
[0022] As described above, in the preparation method of coarse denier low-pore polyester industrial filament, the pressure applied by the heating roller to the filament bundle on the stretching heating roller is monitored in real time during the stretching process, and the position of the heating roller is adjusted in real time so that the absolute value of the relative error of the pressure applied by the heating roller to the filament bundle on the stretching heating roller relative to the set pressure does not exceed 10%, and the relative error = (actual value - set value) / set value × 100%.
[0023] This method can automatically compensate for pressure fluctuations caused by factors such as thermal expansion, wear, and changes in filament specifications, thereby ensuring long-term consistency in filament heating and binding, reducing breakage rates, improving the ease of switching between different product specifications, and providing data support for the fine-tuning of process parameters.
[0024] The method for preparing coarse denier, low-pore polyester industrial filament as described above uses a pressure sensing device to monitor the pressure applied by the heating roller to the filament bundle on the stretching heating roller in real time, and uses an electric displacement device to adjust the position of the heating roller in real time.
[0025] The method for preparing coarse denier, low-pore polyester industrial filament as described above sets the pressure to 0.02-0.2 MPa. This pressure range ensures more effective binding and efficient heat transfer of the coarse denier filament, while also better avoiding damage to the filament bundle or increased frictional damage. This results in more significant effects in reducing breakage rate, improving spinning stability, and enhancing product consistency.
[0026] In the above-described method for preparing coarse denier, low-pore polyester industrial filament, the material and shape of the heating roller are the same as those of the stretching heating roller. The diameter of the heating roller is 1 / 3 to 1 / 2 of the diameter of the stretching heating roller. If the diameter of the heating roller is less than 1 / 3 of the diameter of the stretching heating roller, the rotation speed of the heating roller needs to be significantly increased to ensure the same surface linear velocity, which will aggravate bearing wear, shorten service life, and increase maintenance costs. If the diameter of the heating roller is greater than 1 / 2 of the diameter of the stretching heating roller, it occupies too much space, which is not conducive to compact equipment layout and increases cleaning difficulty. Therefore, controlling the diameter of the heating roller to 1 / 3 to 1 / 2 of the diameter of the stretching heating roller can achieve a good balance between space utilization, equipment cost, and operational stability.
[0027] The method for preparing coarse denier, low-pority polyester industrial filament as described above involves stretching using four hot roller groups, referred to as the first hot roller group, the second hot roller group, the third hot roller group, and the fourth hot roller group. Each hot roller group contains two stretching hot rollers with identical direction, temperature, surface linear velocity, material, shape, and diameter. The first and second hot roller groups are used for gradient preheating, allowing the filament bundle to gradually and uniformly reach above the glass transition temperature, avoiding thermal shock and cold stretching. The third hot roller group undertakes the main stretching, used to achieve high orientation of the molecular chains. The fourth hot roller group is used to further straighten the molecular chains and improve crystallization, reducing the shrinkage rate.
[0028] In the above-described method for preparing coarse denier, low-pore polyester industrial filament, the temperatures of the stretching hot rollers in the first, second, third, and fourth hot roller groups are 80-90℃, 90-100℃, 120-140℃, and 235-245℃, respectively.
[0029] In the above-described method for preparing coarse denier, low-pore polyester industrial filament, the surface linear velocity ratio of the second hot roller group to the stretching hot roller in the first hot roller group is 1.05-1.25, the surface linear velocity ratio of the third hot roller group to the stretching hot roller in the second hot roller group is 3.8-4.2, and the surface linear velocity ratio of the fourth hot roller group to the stretching hot roller in the third hot roller group is 1.3-1.6.
[0030] The preparation method of coarse denier, low-pore polyester industrial filament as described above has the following overall process flow: pre-crystallization of polyester chips → drying → solid phase thickening → melt spinning → cooling and forming → first hot roller group → second hot roller group → third hot roller group → fourth hot roller group → fifth hot roller group → winding. The fifth hot roller group includes two cooling hot rollers with the same direction, temperature, surface linear velocity, material, shape and diameter. The fifth hot roller group is used to cool the filament bundle and adjust the tension so that the filament bundle is wound into shape with appropriate tension after cooling.
[0031] The method for preparing coarse denier, low-pority polyester industrial filament as described above, wherein the intrinsic viscosity of the polyester chips is 0.68 dL / g;
[0032] Pre-crystallization temperature: 130-150℃;
[0033] The drying temperature is 160-175℃, and the moisture content of the dried polyester chips is ≤30ppm.
[0034] The solid-phase thickening temperature is 220-240℃, and the intrinsic viscosity of the polyester chips after solid-phase thickening is 1.12-1.15dL / g. The above temperature range and viscosity index ensure good melt flowability and avoid overheating degradation, thus better realizing the mechanical properties and spinning stability of the product.
[0035] The melt spinning temperature is 285-295℃, which can ensure that the polyester is fully melted and has good fluidity, and avoid thermal degradation or molecular weight reduction due to excessive temperature, thus providing a sufficiently long molecular chain for subsequent high-ratio stretching.
[0036] The cooling and forming process uses side blowing air with a temperature of 20-25℃ and a wind speed of 0.55-0.8m / s, which enables the filaments to cool quickly and evenly, forming a fine and uniform nascent fiber structure. This is beneficial for improving tensile orientation ability and reducing differences in the core-sheath structure.
[0037] The surface linear velocity of the stretching hot rollers in the first hot roller group is 400-600 m / min;
[0038] The temperature of the cooling hot roller in the fifth hot roller group is 120-170℃, and the surface linear velocity of the cooling hot roller in the fifth hot roller group is 20-150 m / min lower than that of the stretching hot roller in the fourth hot roller group.
[0039] With a winding tension of 0.15-0.30 cN / D (centineu / denier, referring to the winding tension borne by a unit denier linear density fiber), it can form a roll with uniform density and smooth unwinding, ensuring the stability of the product throughout the entire process from spinning to downstream processing.
[0040] The present invention also provides a coarse denier, low-porous polyester industrial filament, which is prepared by any of the above methods.
[0041] The specifications of coarse denier, low-pore polyester industrial filament are 2000-3000D / 96F (monofilament fineness ≥20D), with a breaking strength >8.0cN / dtex, breaking elongation 13%-16%, breaking elongation coefficient of variation <10%, dry heat shrinkage (177℃, 10min) ≤8.10%, and abrasion resistance >30,000 cycles. It combines high strength, moderate elongation, excellent uniformity, and thermal dimensional stability, making it particularly suitable for high abrasion and high load-bearing applications such as safety belts, lifting slings, and cables. The fineness abnormality degradation rate is 0.1%-1.15%, and the filament degradation rate is 0.2%-0.62%. The existing equipment can produce a coarse denier, low-porosity monofilament with a fineness of 1500D / 96F. This product has a lot of skipped fibers during production, which causes a 1.0%-2.5% downgrade rate in fineness and a 0.5%-1.5% downgrade rate in fuzz. After using this invention, skipped fibers are basically eliminated, and the downgrade rates in fineness and fuzz are significantly reduced.
[0042] Beneficial effects:
[0043] (1) The present invention sets up a heat tracing roller with opposite direction, the same temperature and the same surface linear velocity on the stretching heat roller to implement double-sided symmetrical contact heating of the filament bundle. The heat is symmetrically conducted from the two surfaces of the filament bundle to the middle, so that the cross section of the filament bundle is uniformly softened and the stretching deformation is uniform and consistent. This effectively solves the problem of poor mechanical properties caused by uneven heating of coarse denier and low porosity polyester industrial filaments on one side.
[0044] (2) The present invention applies pressure perpendicular to the surface of the filament bundle to the stretching hot roller by the heat tracing roller, presses the filament bundle against the surface of the stretching hot roller to form a forced clamp, increases the friction between the filament bundle and the stretching hot roller, suppresses the radial jump and axial movement of the single filament, avoids slippage caused by tension fluctuation, ensures continuous and stable spinning, and reduces the phenomena of filament skipping and breakage. Attached Figure Description
[0045] Figure 1 This is a schematic diagram of the stretching process in the method for preparing coarse denier, low-pore polyester industrial filaments according to the present invention.
[0046] Figure 2This is a schematic diagram of the non-working state of the stretching hot roller and the heat tracing roller of the present invention. The left side is a schematic diagram of the relative positions of the stretching hot roller and the heat tracing roller, and the right side is a schematic diagram of the connection between the stretching hot roller, the heat tracing roller and the electric displacement device and the pressure sensing device (M1 in the figure is the heat tracing roller motor, and M2 is the stretching hot roller motor).
[0047] Figure 3 This is a schematic diagram of the working structure of the stretching hot roller and the heat tracing roller of the present invention. The left side is a schematic diagram of the pressing and fitting of the stretching hot roller and the heat tracing roller, and the right side is a schematic diagram of the connection between the stretching hot roller, the heat tracing roller and the electric displacement device and the pressure sensing device.
[0048] Figures 1-3 In the diagram, 1 is the stretching hot roller a, 2 is the heat tracing roller a, 3 is the stretching hot roller b, 4 is the heat tracing roller b, 5 is the stretching hot roller c, 6 is the heat tracing roller c, 7 is the stretching hot roller d, 8 is the heat tracing roller d, 9 is the cooling hot roller, 10 is the winding machine, 13 is the electric displacement device, and 14 is the pressure sensing device. Detailed Implementation
[0049] The present invention will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0050] The following are the test methods for the relevant performance indicators in each embodiment and comparative example:
[0051] Intrinsic viscosity: The sample was tested according to the capillary viscometer method in GB / T 14190-2017 "Test Method for Fiber Grade Polyester (PET) Chips" 5.1.1, with a solvent temperature of 25℃ and a polyester test solution concentration of 0.05 g / mL.
[0052] Moisture content: The sample was tested according to the gravimetric method in GB / T 14190-2017 "Test Method for Fiber Grade Polyester (PET) Chips" 5.7.1. 20g of sample was taken and heated at 120℃ for 2h.
[0053] Fineness: The sample was tested according to GB / T 14343-2008 "Test Method for Linear Density of Chemical Fiber Filaments", with a pre-tension of 0.05 cN / dtex and a sample length of 10 m.
[0054] Breaking strength, elongation at break, and coefficient of variation of elongation at break: The samples were tested according to GB / T 14344-2022 "Test Method for Tensile Properties of Chemical Fiber Filaments", with a clamping distance of 500 mm and a clamping displacement speed of 500 mm / min.
[0055] Dry heat shrinkage rate: The sample was tested according to FZ / T 50050-2020 "Test method for dry heat shrinkage rate of synthetic fiber industrial filament", with a test temperature of 177℃, a test time of 10min, and a pre-tension of 0.05cN / dtex.
[0056] Abrasion resistance test: Refer to FZ / T 50063-2023, and conduct yarn-to-yarn reciprocating friction test on the sample under a pretension of 0.05cN / dtex.
[0057] The following are the calculation formulas for the relevant performance indicators in each embodiment and comparative example:
[0058] Fineness abnormality downgrade rate = Number of samples downgraded due to fineness exceeding the range × 100% / Total number of samples tested. Referring to the requirements of 5.1 in GB / T16604-2017, the allowable range for fineness deviation of high-strength industrial yarn of superior grade is ±2.0% of the center value. Fineness exceeding this range is judged as fineness exceeding the range downgrade.
[0059] Downgrade rate of fuzzy fibers = number of downgraded samples × 100% / total number of samples in a full roll. Fuzzy fibers refer to defects in the filaments, such as damage that makes them appear fuzzy, or single filaments that are broken and have ends that protrude from the surface of the multifilament. During inspection, the entire surface of the roll must be checked. If the cumulative number of fuzzy fibers in a single roll is greater than 5, it is considered downgraded (according to GB / T 16604-2017).
[0060] The general process for preparing coarse denier, low-pore polyester industrial filaments in various embodiments of the present invention is as follows: Figure 1 As shown, specifically: polyester chips are pre-crystallized, dried, and solid-phase thickening treated in sequence, and then fed into a spinning equipment for melt spinning. The melt is sprayed out through a spinneret to form a filament bundle, which is then cooled and shaped before entering the stretching process.
[0061] The stretching process is sequentially arranged with a first group of hot rollers, a second group of hot rollers, a third group of hot rollers, a fourth group of hot rollers, and a fifth group of hot rollers along the direction of the filament bundle. The first group of hot rollers includes two stretching hot rollers a1 with identical rotation direction, temperature, surface linear velocity, material, shape, and diameter. Each stretching hot roller a1 has a parallel heating roller a2 with identical temperature, surface linear velocity, material, and shape but opposite rotation direction. The second group of hot rollers includes two stretching hot rollers b3 with identical rotation direction, temperature, surface linear velocity, material, shape, and diameter. Each stretching hot roller b3 has a parallel heating roller b4 with identical temperature, surface linear velocity, material, and shape but opposite rotation direction. The third group of hot rollers includes two stretching hot rollers c5 with identical rotation direction, temperature, surface linear velocity, material, shape, and diameter. Each stretching hot roller c5 has a parallel heating roller c5 with identical temperature, surface linear velocity, material, and shape but opposite rotation direction. 6; The fourth hot roller group includes two stretching hot rollers d7 with the same direction of rotation, temperature, surface linear velocity, material, shape and diameter. Each stretching hot roller d7 is paired with a heat tracing roller d8 with the same temperature, surface linear velocity, material and shape but opposite direction of rotation. The fifth hot roller group includes two cooling hot rollers 9 with the same direction of rotation, temperature, surface linear velocity, material, shape and diameter. The diameter of each heat tracing roller is 1 / 3 to 1 / 2 of the diameter of the corresponding stretching hot roller.
[0062] The filament bundle is preheated by the first and second hot roller groups in sequence, stretched by the third hot roller group, and shaped and crystallized by the fourth hot roller group. Then it enters the fifth hot roller group for cooling and tension adjustment, and is finally conveyed to the winding machine 10 for winding and forming.
[0063] In the non-working state, the relative positions and assembly connections of each stretching heating roller and its corresponding heating roller are as follows: Figure 2 As shown; during the stretching process, each hot roller group enters the working state, and the pressing and fitting state and assembly connection relationship between the stretching hot roller and the corresponding heating roller are as follows. Figure 3 As shown, each heat tracing roller is equipped with an electric displacement device 13 and a pressure sensing device 14. During operation, the heat tracing roller and the corresponding stretching heat roller maintain opposite directions, the same temperature, and the same surface linear velocity. The pressure sensing device 14 monitors the pressure applied by the heat tracing roller to the filament bundle on the corresponding stretching heat roller in real time, and the electric displacement device 13 adjusts the position of the heat tracing roller in real time so that the absolute value of the relative error of the applied pressure to the set pressure does not exceed 10%. In this way, the heat tracing roller provides auxiliary heating and applies pressure to the filament bundle on the corresponding stretching heat roller. In conjunction with the stretching heat roller, it achieves double-sided symmetrical contact heating and mechanical restraint, ensuring that the stretching process is uniform and stable. The fifth heat roller group uniformly cools and adjusts the tension of the stretched and shaped filament bundle so that the filament bundle enters the winding process with a suitable tension.
[0064] The raw material and process parameters, as well as the specifications and performance indicators of coarse denier, low-pore polyester industrial filaments in each embodiment, are as follows:
[0065] Example 1
[0066] The raw material and process parameters are set as follows:
[0067] The intrinsic viscosity of the polyester chips is 0.68 dL / g;
[0068] The pre-crystallization temperature is 130℃;
[0069] The drying temperature was 175℃, and the moisture content of the dried polyester chips was 22ppm.
[0070] The solid-phase thickening temperature was 220℃, and the intrinsic viscosity of the polyester chips after solid-phase thickening was 1.12 dL / g.
[0071] The melt spinning temperature is 285℃;
[0072] The cooling and molding process uses side-blowing air, with a side-blowing air temperature of 20℃ and an air velocity of 0.55m / s;
[0073] The temperatures of the stretching hot rollers a, b, c, and d are 80℃, 90℃, 120℃, and 235℃, respectively. The temperature of the cooling hot roller is 120℃. The surface linear velocity of the stretching hot roller a is 600 m / min. The surface linear velocity ratio of the stretching hot roller b to that of the stretching hot roller a is 1.05, the ratio of the surface linear velocity of the stretching hot roller c to that of the stretching hot roller b is 3.81, and the ratio of the surface linear velocity of the stretching hot roller d to that of the stretching hot roller c is 1.6. The surface linear velocity of the cooling hot roller is 20 m / min lower than that of the stretching hot roller d. The diameter of each heating roller is 1 / 3 of the diameter of the corresponding stretching hot roller. The set pressure is 0.02 MPa.
[0074] The winding tension is 0.28 cN / D;
[0075] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0076] The specifications are 2000D / 96F, the breaking strength is 8.45cN / dtex, the breaking elongation is 14.3%, the coefficient of variation of breaking elongation is 5.25%, the dry heat shrinkage rate is 8%, the abrasion resistance is 31,500 cycles, the fineness abnormality degradation rate is 0.11%, and the filament degradation rate is 0.2%.
[0077] Example 2
[0078] The raw material and process parameters are set as follows:
[0079] The intrinsic viscosity of the polyester chips is 0.68 dL / g;
[0080] The pre-crystallization temperature is 135℃;
[0081] The drying temperature was 170℃, and the moisture content of the dried polyester chips was 25ppm.
[0082] The solid-phase thickening temperature was 225℃, and the intrinsic viscosity of the polyester chips after solid-phase thickening was 1.131 dL / g.
[0083] The melt spinning temperature is 288℃;
[0084] The cooling and molding process uses side-blowing air, with a side-blowing air temperature of 22℃ and an air velocity of 0.65m / s.
[0085] The temperatures of the stretching hot rollers a, b, c, and d are 82℃, 94℃, 125℃, and 238℃, respectively. The temperature of the cooling hot roller is 130℃. The surface linear velocity of the stretching hot roller a is 550 m / min. The surface linear velocity ratio of the stretching hot roller b to that of the stretching hot roller a is 1.1, the ratio of the surface linear velocity of the stretching hot roller c to that of the stretching hot roller b is 3.91, and the ratio of the surface linear velocity of the stretching hot roller d to that of the stretching hot roller c is 1.55. The surface linear velocity of the cooling hot roller is 60 m / min lower than that of the stretching hot roller d. The diameter of each heating roller is 1 / 3 of the diameter of the corresponding stretching hot roller. The set pressure is 0.08 MPa.
[0086] The winding tension is 0.25 cN / D;
[0087] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0088] The specifications are 2000D / 96F, the tensile strength is 8.42cN / dtex, the elongation at break is 14.1%, the coefficient of variation of elongation at break is 4.62%, the dry heat shrinkage rate is 7.6%, the abrasion resistance is 32,500 cycles, the fineness abnormality degradation rate is 0.16%, and the filament degradation rate is 0.26%.
[0089] Example 3
[0090] The raw material and process parameters are set as follows:
[0091] The intrinsic viscosity of the polyester chips is 0.68 dL / g;
[0092] The pre-crystallization temperature is 140℃;
[0093] The drying temperature was 165℃, and the moisture content of the dried polyester chips was 25ppm.
[0094] The solid-phase thickening temperature was 230℃, and the intrinsic viscosity of the polyester chips after solid-phase thickening was 1.138 dL / g.
[0095] The melt spinning temperature is 290℃;
[0096] The cooling and molding process uses side-blowing air, with a side-blowing air temperature of 23℃ and an air velocity of 0.75m / s.
[0097] The temperatures of the stretching hot rollers a, b, c, and d are 85℃, 95℃, 130℃, and 240℃, respectively. The temperature of the cooling hot roller is 150℃. The surface linear velocity of the stretching hot roller a is 500 m / min. The surface linear velocity ratio of the stretching hot roller b to that of the stretching hot roller a is 1.15, the ratio of the surface linear velocity of the stretching hot roller c to that of the stretching hot roller b is 4.05, and the ratio of the surface linear velocity of the stretching hot roller d to that of the stretching hot roller c is 1.42. The surface linear velocity of the cooling hot roller is 90 m / min lower than that of the stretching hot roller d. The diameter of each heating roller is 1 / 3 of the diameter of the corresponding stretching hot roller. The set pressure is 0.1 MPa.
[0098] The winding tension is 0.2 cN / D;
[0099] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0100] The specifications are 2500D / 96F, the tensile strength is 8.4cN / dtex, the elongation at break is 14.8%, the coefficient of variation of elongation at break is 5.86%, the dry heat shrinkage rate is 7.2%, the abrasion resistance is 38,000 cycles, the fineness abnormality degradation rate is 0.21%, and the filament degradation rate is 0.35%.
[0101] Example 4
[0102] The raw material and process parameters are set as follows:
[0103] The intrinsic viscosity of the polyester chips is 0.68 dL / g;
[0104] The pre-crystallization temperature is 145℃;
[0105] The drying temperature was 160℃, and the moisture content of the dried polyester chips was 28ppm.
[0106] The solid-phase thickening temperature was 235℃, and the intrinsic viscosity of the polyester chips after solid-phase thickening was 1.145 dL / g.
[0107] The melt spinning temperature is 292℃;
[0108] The cooling and molding process uses side-blowing air, with a side-blowing air temperature of 24℃ and an air velocity of 0.75m / s.
[0109] The temperatures of the stretching hot rollers a, b, c, and d are 88℃, 97℃, 135℃, and 242℃, respectively. The temperature of the cooling hot roller is 160℃. The surface linear velocity of the stretching hot roller a is 450 m / min. The surface linear velocity ratio of the stretching hot roller b to that of the stretching hot roller a is 1.2. The surface linear velocity ratio of the stretching hot roller c to that of the stretching hot roller b is 4.12. The surface linear velocity ratio of the stretching hot roller d to that of the stretching hot roller c is 1.38. The surface linear velocity of the cooling hot roller is 120 m / min lower than that of the stretching hot roller d. The diameter of each heating roller is half the diameter of the corresponding stretching hot roller. The set pressure is 0.15 MPa.
[0110] The winding tension is 0.18 cN / D;
[0111] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0112] The specifications are 3000D / 96F, the tensile strength is 8.38cN / dtex, the elongation at break is 15.5%, the coefficient of variation of elongation at break is 6.23%, the dry heat shrinkage rate is 6.5%, the abrasion resistance is 45,000 cycles, the fineness abnormality degradation rate is 0.25%, and the filament degradation rate is 0.4%.
[0113] Example 5
[0114] The raw material and process parameters are set as follows:
[0115] The intrinsic viscosity of the polyester chips is 0.68 dL / g;
[0116] The pre-crystallization temperature is 150℃;
[0117] The drying temperature was 160℃, and the moisture content of the dried polyester chips was 30ppm.
[0118] The solid-phase thickening temperature was 240℃, and the intrinsic viscosity of the polyester chips after solid-phase thickening was 1.15 dL / g.
[0119] The melt spinning temperature is 295℃;
[0120] The cooling and molding process uses side-blowing air, with a side-blowing air temperature of 25℃ and an air velocity of 0.8m / s;
[0121] The temperatures of the stretching hot rollers a, b, c, and d are 90℃, 100℃, 140℃, and 245℃, respectively. The temperature of the cooling hot roller is 170℃. The surface linear velocity of the stretching hot roller a is 400 m / min. The surface linear velocity ratio of the stretching hot roller b to that of the stretching hot roller a is 1.25, the ratio of the surface linear velocity of the stretching hot roller c to that of the stretching hot roller b is 4.2, and the ratio of the surface linear velocity of the stretching hot roller d to that of the stretching hot roller c is 1.3. The surface linear velocity of the cooling hot roller is 150 m / min lower than that of the stretching hot roller d. The diameter of each heating roller is half the diameter of the corresponding stretching hot roller. The set pressure is 0.2 MPa.
[0122] The winding tension is 0.15 cN / D;
[0123] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0124] The specifications are 3000D / 96F, the tensile strength is 8.35cN / dtex, the elongation at break is 15.8%, the coefficient of variation of elongation at break is 7.25%, the dry heat shrinkage rate is 6.2%, the abrasion resistance is 44,800 cycles, the fineness abnormality degradation rate is 0.28%, and the filament degradation rate is 0.45%.
[0125] Example 6
[0126] The raw material and process parameters are set as follows:
[0127] The only difference from Example 2 is that: real-time pressure control is not performed (during the stretching process, the pressure applied by the heat tracing roller to the filament bundle on the corresponding stretching heat roller is not monitored in real time by the pressure sensing device, nor is the position of the heat tracing roller adjusted in real time by the electric displacement device).
[0128] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0129] The specifications are 2000D / 96F, the tensile strength is 8.35cN / dtex, the elongation at break is 13.6%, the coefficient of variation of elongation at break is 8.42%, the dry heat shrinkage rate is 7.5%, the abrasion resistance is 32,000 cycles, the fineness abnormality degradation rate is 0.52%, and the filament degradation rate is 0.38%.
[0130] Compared to Example 2, Example 6 only eliminated real-time pressure control. Its coefficient of variation for elongation at break significantly increased from 4.62% to 8.42%, the rate of downgrading due to abnormal fineness increased from 0.16% to 0.52%, the rate of downgrading due to fuzzy fibers increased from 0.26% to 0.38%, the breaking strength slightly decreased from 8.42 cN / dtex to 8.35 cN / dtex, and the elongation at break slightly decreased from 14.1% to 14.0%. This is because after eliminating closed-loop control, the pressure applied to the filament bundle by the heating roller cannot remain stable: during periods of low pressure, the filament bundle and the stretching heating roller do not adhere sufficiently, making it difficult to maintain symmetrical heating on both sides. Uneven temperature and stretching of the filament bundle cross-section lead to an increased coefficient of variation and a slight decrease in strength and elongation. Excessive pressure fluctuations can also cause localized damage to the filament bundle. Simultaneously, unstable pressure weakens the forced clamping effect of the heating roller, exacerbating radial runout and axial movement of the single filament, thus increasing the rate of downgrading due to abnormal fineness and the rate of downgrading due to fuzzy fibers.
[0131] Example 7
[0132] The raw material and process parameters are set as follows:
[0133] The only difference from Example 1 is that the pressure is set to 0.01 MPa;
[0134] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0135] The specifications are 2000D / 96F, the tensile strength is 8.42cN / dtex, the tensile elongation at break is 14.3%, the coefficient of variation of tensile elongation at break is 9.65%, the dry heat shrinkage rate is 8.10%, the abrasion resistance is 31,300 cycles, the fineness abnormality degradation rate is 1.15%, and the filament degradation rate is 0.62%.
[0136] Compared to Example 1, Example 7 only reduced the set pressure from 0.02 MPa to 0.01 MPa. The coefficient of variation of elongation at break increased from 5.25% to 9.65%, the rate of downgrading due to abnormal fineness increased from 0.11% to 1.15%, the rate of downgrading due to fuzzy fibers increased from 0.20% to 0.62%, and the dry heat shrinkage rate slightly increased from 8.0% to 8.10%. This is because the set pressure was too low, resulting in insufficient forced clamping effect of the heating rollers. On the one hand, the filament bundle did not fit tightly with the stretching heating rollers and the heating rollers, reducing the double-sided symmetrical heat transfer effect. Uneven heating of the filament bundle cross-section and uneven subsequent stretching increased the coefficient of variation and slightly increased the dry heat shrinkage rate. On the other hand, it could not effectively suppress the radial runout and axial movement of the monofilaments, leading to increased filament skipping on the heating rollers and increasing the rate of downgrading due to abnormal fineness and the rate of downgrading due to fuzzy fibers.
[0137] Comparative Example 1
[0138] The only difference between the preparation method and Example 5 is that there are no heat tracing rollers in each of the hot roller groups;
[0139] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0140] The specifications are 3000D / 96F, the breaking strength is 8.26cN / dtex, the breaking elongation is 16.5%, the breaking elongation coefficient of variation is 11.2%, the abrasion resistance is 41,000 cycles, the fineness abnormality degradation rate is 6.5%, and the filament degradation rate is 2.6%.
[0141] Compared with Example 5, Comparative Example 1 showed an increase in breaking elongation from 15.8% to 16.5%, a rise in the coefficient of variation of breaking elongation from 7.25% to 11.2%, a significant increase in the rate of downgrading due to abnormal fineness from 0.28% to 6.5%, and a significant increase in the rate of downgrading due to fuzz from 0.45% to 2.6%, making it difficult to stably produce qualified products. This is because the 3000D / 96F product has a single filament fineness of 30D. After eliminating the heating roller, the filament bundle is heated only on one side by the stretching heating roller, resulting in uneven heating on both sides, a large temperature gradient across the cross-section, and uneven tensile deformation, which increases the breaking elongation and the coefficient of variation. At the same time, the lack of forced clamping by the heating roller results in insufficient friction between the filament bundle and the stretching heating roller, leading to severe radial and axial runout of the single filament and serious filament skipping, which significantly increases the rate of downgrading due to abnormal fineness and the rate of downgrading due to fuzz.
[0142] Comparative Example 2
[0143] The only difference between the preparation method and Example 5 is that there are no heat-tracing rollers in the third and fourth hot roller groups.
[0144] The specifications and performance indicators of coarse denier, low-pore polyester industrial filaments are as follows:
[0145] The specifications are 3000D / 96F, the breaking strength is 8.29cN / dtex, the breaking elongation is 16.2%, the breaking elongation coefficient of variation is 9.21%, the abrasion resistance is 43,000 cycles, the fineness abnormality degradation rate is 6.3%, and the filament degradation rate is 2.8%.
[0146] Compared with Example 5, Comparative Example 2 showed little difference in breaking strength and elongation at break, but the coefficient of variation of elongation at break increased by 1.96 percentage points, the rate of downgrading due to abnormal fineness increased by 6.02 percentage points, and the rate of downgrading due to fuzzy fibers increased by 2.35 percentage points, both of which showed significant increases. This is because the third hot roller group performs the main stretching function, used to highly orient the molecular chains, while the fourth hot roller group is used to further straighten the molecular chains and improve crystallization; both are core temperature zones in the stretching process. Without the heating rollers in the third and fourth hot roller groups, the filament bundle is heated only by contact with the stretching hot rollers on one side, resulting in a large radial temperature gradient across the cross-section, decreased heating uniformity, and uneven deformation during the main stretching stage, leading to a significant increase in the coefficient of variation of elongation at break. Simultaneously, the lack of forced clamping action from the heating rollers resulted in insufficient friction between the filament bundle and the stretching hot rollers, exacerbating radial and axial movement of the single filaments and significantly increasing filament skipping. Therefore, both the rate of downgrading due to abnormal fineness and the rate of downgrading due to fuzzy fibers increased significantly.
Claims
1. A method for preparing coarse denier, low-pore polyester industrial filament, comprising a stretching process, characterized in that, The stretching process uses stretching hot rollers, and each stretching hot roller is equipped with a heat tracing roller that rotates in the opposite direction, has the same temperature, and the same surface linear velocity. During the stretching process, the heat tracing roller is used to assist in heating and applying pressure to the filament bundle on the stretching hot roller.
2. The method for preparing coarse denier, low-pore polyester industrial filament according to claim 1, characterized in that, During the stretching process, the pressure applied by the heating roller to the filament bundle on the stretching roller is monitored in real time, and the position of the heating roller is adjusted in real time so that the absolute value of the relative error of the pressure applied by the heating roller to the filament bundle on the stretching roller relative to the set pressure does not exceed 10%; the set pressure is 0.02-0.2MPa.
3. The method for preparing coarse denier, low-pore polyester industrial filament according to claim 2, characterized in that, A pressure sensing device is used to monitor the pressure exerted by the heat tracing roller on the filament bundle on the stretching heat roller in real time, and an electric displacement device is used to adjust the position of the heat tracing roller in real time.
4. The method for preparing coarse denier, low-pore polyester industrial filament according to claim 1, characterized in that, The material and shape of the heat tracing roller are the same as those of the stretching heat roller, and the diameter of the heat tracing roller is 1 / 3 to 1 / 2 of the diameter of the stretching heat roller.
5. The method for preparing coarse denier, low-pore polyester industrial filament according to claim 1, characterized in that, The stretching process uses four hot roller groups, which are designated as the first hot roller group, the second hot roller group, the third hot roller group, and the fourth hot roller group. Each hot roller group contains two stretching hot rollers with the same direction of rotation, temperature, surface linear velocity, material, shape, and diameter.
6. The method for preparing coarse denier, low-pore polyester industrial filament according to claim 5, characterized in that, The temperatures of the stretching hot rollers in the first, second, third, and fourth hot roller groups are 80-90℃, 90-100℃, 120-140℃, and 235-245℃, respectively.
7. The method for preparing coarse denier, low-pore polyester industrial filament according to claim 5, characterized in that, The surface linear velocity ratio of the second hot roller group to the stretching hot roller in the first hot roller group is 1.05-1.25, the surface linear velocity ratio of the third hot roller group to the stretching hot roller in the second hot roller group is 3.8-4.2, and the surface linear velocity ratio of the fourth hot roller group to the stretching hot roller in the third hot roller group is 1.3-1.
6.
8. The method for preparing coarse denier, low-pore polyester industrial filament according to claim 5, characterized in that, The overall process flow is as follows: pre-crystallization of polyester chips → drying → solid phase thickening → melt spinning → cooling and molding → first hot roller group → second hot roller group → third hot roller group → fourth hot roller group → fifth hot roller group → winding. The fifth hot roller group includes two cooling hot rollers with the same direction, temperature, surface linear velocity, material, shape and diameter.
9. The method for preparing coarse denier, low-pore polyester industrial filament according to claim 8, characterized in that, The intrinsic viscosity of the polyester chips is 0.68 dL / g; Pre-crystallization temperature: 130-150℃; The drying temperature is 160-175℃, and the moisture content of the dried polyester chips is ≤30ppm. The solid-phase thickening temperature is 220-240℃, and the intrinsic viscosity of the polyester chips after solid-phase thickening is 1.12-1.15 dL / g; The temperature for melt spinning is 285-295℃; Cooling and molding are achieved using side-blowing air, with a side-blowing air temperature of 20-25℃ and an air velocity of 0.55-0.8m / s; The surface linear velocity of the stretching hot rollers in the first hot roller group is 400-600 m / min; The temperature of the cooling hot roller in the fifth hot roller group is 120-170℃, and the surface linear velocity of the cooling hot roller in the fifth hot roller group is 20-150 m / min lower than that of the stretching hot roller in the fourth hot roller group. The winding tension is 0.15-0.30 cN / D.
10. A coarse denier, low-pore polyester industrial filament, characterized in that, It is prepared by any one of the following methods: coarse denier low-pore polyester industrial filament as described in claims 1-9; The specifications of coarse denier, low-pore polyester industrial filament are 2000-3000D / 96F, with a breaking strength >8.0cN / dtex, a breaking elongation of 13%-16%, a breaking elongation coefficient of variation <10%, a dry heat shrinkage rate ≤8.10%, an abrasion resistance of >30,000 cycles, a fineness abnormality degradation rate of 0.1%-1.15%, and a fuzzy filament degradation rate of 0.2%-0.62%.
Citation Information
Patent Citations
Yarn heater
CN102758287A
Preparation method of high-strength low-elongation polyester industrial yarn
CN116988174A
Carbon fiber yarn heating and conveying device
CN214114504U