Polyester staple fiber and method for producing the same
By employing a synergistic approach of vacuum solid-phase thickening, staged stretching, and isolated fluidized heat exchangers, the problem of high thermal shrinkage rate of high molecular weight polyester staple fibers during heat treatment was solved, maintaining high strength and dimensional stability, thus achieving efficient preparation of polyester staple fibers.
Patent Information
- Application Number
- CN202611359691.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-24
Smart Images

Figure CN123153185A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polyester fiber technology, belonging to patent classification number D01F6 / 92, specifically to a polyester staple fiber and its preparation method. Background Technology
[0002] Polyethylene terephthalate (PET) fiber is characterized by good heat resistance, high chemical stability, wide availability of raw materials, and moderate production costs, making it widely used in industrial fabrics, filter materials, reinforcing materials, and heat-resistant nonwoven materials. As application environments increasingly demand higher load-bearing capacity and dimensional stability, polyester staple fibers not only need high breaking strength but also require minimal length change after heating.
[0003] The strength of polyester fibers primarily depends on the polymer chain length, the degree of chain entanglement, and the fiber's axial orientation. Increasing the polyester molecular weight and applying a higher draw ratio to the spun filaments allows more molecular chains to align along the fiber axis, forming oriented crystalline regions, amorphous oriented chains, and tethered chains that bear the load, thereby improving the fiber's breaking strength. However, high draw also stores more elastic strain and residual internal stress within the fiber. When the fiber is subjected to high temperatures during subsequent use, the non-equilibrium molecular chains are prone to shrinkage, leading to significant thermal shrinkage.
[0004] Reducing heat shrinkage typically requires thermal relaxation of the drawn fiber bundle to pre-release some residual internal stress, followed by heat setting to fix the relaxed dimensional state. However, while releasing shrinkage stress, thermal relaxation can also cause some of the amorphous orientation chains and tying chains that bear the load to coil back and deorient, weakening the connection between crystalline regions and resulting in a decrease in fiber strength. Insufficient relaxation makes it difficult to fully reduce residual heat shrinkage; excessive relaxation can destroy the already formed highly oriented load-bearing structure. Therefore, there is a direct process constraint between high-strength structures and low-shrinkage treatment.
[0005] Based on the above, the technical problem that this invention needs to solve is how to fully release the residual stress that causes thermal shrinkage in high molecular weight, highly oriented polyester filaments without changing the main composition of PET homopolymer, while reducing the rewinding and deorientation of amorphous oriented chains and typothetical chains caused by thermal relaxation, thereby reducing the thermal shrinkage rate of polyester staple fibers while maintaining high breaking strength. Summary of the Invention
[0006] The purpose of this invention is to provide a polyester staple fiber and its preparation method to solve the technical problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing polyester staple fiber includes the following steps: Vacuum solid-state thickening of polyethylene terephthalate (PET) polyester chips was performed, followed by melt spinning and graded drawing to obtain drawn fiber bundles. In an isolated fluidized bed heat exchanger, spherical α-alumina ceramic microspheres are aerated with industrial nitrogen gas. The spherical α-alumina ceramic microspheres and the drawn filament bundle are separated by an isolation structure that allows nitrogen gas to pass through while trapping the spherical α-alumina ceramic microspheres. The industrial nitrogen gas, after heat exchange with the spherical α-alumina ceramic microspheres, passes through the unfolded and fixed-length drawn filament bundle to perform pulsed thermal pre-stabilization on the drawn filament bundle. Then, the bundle is cooled while maintaining a constant filament bundle length to obtain a pre-stabilized filament bundle. The pre-stabilized filament bundle is subjected to two-stage, progressively heated, tension-limited thermal relaxation. The bundle is then thermally reshaped to a fixed length according to the length of the bundle after the second stage of thermal relaxation, while the bundle length is kept cool. The cooled filament bundles are cut to obtain polyester staple fibers.
[0008] Preferably, the initial intrinsic viscosity of the polyethylene terephthalate (PET) homopolymer polyester chips is 0.64–0.68 dL / g; the vacuum solid-state viscosity enhancement includes: first treating at 135–145°C and 2–8 kPa for 20–40 min, then treating at 165–175°C and 0.5–2 kPa for 45–75 min, and then performing solid-state polycondensation at 205–215°C and 50–200 Pa until the intrinsic viscosity of the PET homopolymer polyester chips reaches 0.84–0.90 dL / g.
[0009] Preferably, the polyethylene terephthalate (PET) homopolymer polyester chips after vacuum solid-phase thickening are dried at 150–160°C to a moisture content of no more than 30 ppm, and then melt-spun at 278–284°C; the cumulative residence time of the melt at 278°C or above does not exceed 5 min, and the spinning winding speed is 900–1300 m / min.
[0010] Preferably, the staged stretching includes: first stretching 2.95 to 3.05 times in a water bath at 80 to 85°C, and then stretching 1.20 to 1.24 times in superheated steam at 120 to 130°C, with a total stretching ratio of 3.54 to 3.78 times.
[0011] Preferably, the purity of the industrial nitrogen gas is not less than 99.9% and the dew point is not higher than -30℃; the spherical α-alumina ceramic microspheres have a particle size of 150-300μm, a sphericity of not less than 0.90, and an α-Al2O3 content of not less than 99%, and fine powder with a particle size of less than 75μm is pre-screened out; the spherical α-alumina ceramic microspheres form a fluidized bed with a static thickness of 120-200mm, and the apparent velocity of the industrial nitrogen gas is 1.1-1.4 times the minimum fluidization velocity of the fluidized bed.
[0012] Preferably, the isolation structure is a porous sintered metal isolation guide wire channel with a pore size of 20-40 μm disposed in a fluidized bed; the thickness of the drawn wire bundle after unfolding is no more than 2 mm, the temperature when entering the isolation guide wire channel is 105-120°C, the fluidized bed temperature is 182-185°C, the wire bundle tension during pulsed thermal prestabilization is 0.04-0.08 cN / dtex, the processing time is 0.6-1.0 s, and the control endpoint is that the outlet temperature of the drawn wire bundle reaches 178-183°C; after pulsed thermal prestabilization, it is cooled to no higher than 150°C while maintaining the wire bundle length unchanged.
[0013] Preferably, the two-stage progressively heated tension-limited thermal relaxation includes: The first stage of thermal relaxation is carried out at 165–168℃, the outlet linear velocity of the first stage of thermal relaxation is 0.990 times the inlet linear velocity, and the processing time is 8–12 s; Then, a second-stage thermal relaxation is performed at 175–178°C. The exit line velocity of the second-stage thermal relaxation is 0.985 times that of the first-stage thermal relaxation, and the processing time is 6–10 seconds. The cumulative relaxation rate of the two-stage thermal relaxation was 2.485%, and the bundle tension was maintained at 0.005–0.020 cN / dtex during the two-stage thermal relaxation process.
[0014] Preferably, after completing two stages of heat relaxation, the filament bundle is subjected to fixed-length heat re-setting at 198–202°C for 8–12 seconds, based on the exit linear speed of the second stage of heat relaxation and the length of the filament bundle after the second stage of heat relaxation. The ratio of the linear speeds of the front and rear traction rollers of the fixed-length heat re-setting device is 1.000 ± 0.002. After fixed-length heat re-setting, the length of the filament bundle is kept constant, and the filament bundle is cooled to below 70°C before the length constraint is released.
[0015] Preferably, the cooled filament bundle is cut into short polyester fibers with a length of 32 to 51 mm.
[0016] A polyester staple fiber is prepared by the method described above.
[0017] Compared with the prior art, the beneficial effects of the present invention are: 1. Vacuum solid-phase thickening increases the average length and entanglement of PET molecular chains, making it less prone to slippage or direct extraction of molecular chains under stress. Water bath drawing allows the nascent filament bundle to achieve stable necking under relatively uniform heating, reducing local over-drawing; subsequent superheated steam drawing further improves the alignment of molecular chains along the fiber axis and promotes the formation of fine oriented crystalline regions. After the above treatment, more amorphous oriented chains and tying chains capable of transmitting loads are retained between the crystalline regions, allowing external forces to be continuously transmitted along the fiber axis, thus improving the breaking strength of polyester staple fibers.
[0018] 2. Graded and Limited Relaxation: Residual stress within the fiber bundle is released through a gradual heating process. In the lower temperature range, the more mobile amorphous segments first undergo limited shrinkage. In the higher temperature range, the segments with somewhat restricted movement are gradually adjusted, preventing the concentrated release of all internal stress at the same temperature. The cumulative relaxation rate of the two stages is controlled at 2.485%, which releases the main elastic strain that would cause subsequent thermal shrinkage without causing unrestrained and significant shrinkage of the fiber bundle. After relaxation, high-temperature reshaping is performed according to the new shrinkage length to further stabilize the crystalline regions and allow the amorphous regions to regain structural equilibrium under lower internal stress. This length is then maintained and cooled to below 70°C to fix the established structural state, thereby reducing the tendency for the fiber to continue shrinking upon reheating.
[0019] 3. While a highly oriented structure can improve fiber strength, it exists in a non-equilibrium state with high residual stress. Subsequent thermal relaxation, while reducing thermal shrinkage, can cause some of the amorphous oriented chains and ties that bear the load to coil back and deorient, resulting in a loss of strength gained from the previous treatment. To mitigate this effect, this scheme incorporates an isolated fluidized bed heat exchange system composed of industrial nitrogen and spherical α-alumina ceramic microspheres between drawing and thermal relaxation. Industrial nitrogen continuously flows through the microsphere bed, maintaining uniform fluidization of the spherical α-alumina ceramic microspheres and acting as a flowing heat transfer medium to rapidly carry heat from the bed through the unfolded thin fiber bundle. The spherical α-alumina ceramic microspheres, with their large gas-solid contact area, high heat capacity, and good temperature buffering capacity, continuously replenish heat to the nitrogen flowing through the bed, reducing temperature fluctuations caused by changes in nitrogen flow rate and fiber bundle heat. In other words, alumina microspheres are responsible for heat storage, heat homogenization, and stabilizing the thermal field, while industrial nitrogen is responsible for fluidization, heat extraction, heat transfer, and enabling heat to penetrate the fiber bundle. The two complement each other in terms of heat storage and heat transport. After homogenization, the nitrogen acts on the fiber bundle through porous isolation channels, while the alumina microspheres are completely retained and do not directly contact the fibers. Therefore, this synergy is a controllable physical heat transfer coordination, not a chemical reaction between nitrogen, alumina, and PET. When the fiber bundle receives sub-second uniform thermal pulses at a constant length, some uncrystallized oriented chain segments form limited secondary crystalline regions, and the existing microcrystalline boundaries are initially stabilized. Due to the short heating time and the constrained fiber bundle length, the main oriented structure does not have time to undergo significant relaxation. Then, cooling is performed while maintaining the same length, making these limited crystalline regions physical anchors on the molecular chains. After entering the graded relaxation process, the physical anchor points can limit the excessive rewinding of amorphous orientation chains and tethered chains, while the unanchored chain segments can still release residual stress according to a set ratio, thereby reducing the strength loss caused by low shrinkage treatment and ensuring that the strength and dimensional stability of the fiber are maintained. Attached Figure Description
[0020] Figure 1 This is a low-magnification SEM image of the polyester staple fiber prepared in Example 1 of the present invention.
[0021] Figure 2 This is a high-magnification SEM image of the polyester staple fiber prepared in Example 1 of the present invention. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] In the following examples, intrinsic viscosity was determined using the dilute solution capillary method: 0.1250 g of pulverized PET sample was taken each time, and a test solution was prepared with 25.0 mL of a mixed solvent; the mixed solvent was prepared from 60.0 g of phenol and 40.0 g of 1,1,2,2-tetrachloroethane, and the viscosity was measured using a Type 1B Ubbelohde viscometer at 30.0 ± 0.05 °C, and the intrinsic viscosity was calculated according to the Billmeyer relation. The sphericity of the spherical α-alumina ceramic microspheres was the average of the minor axis to major axis ratio of the two-dimensional projection obtained from 100 randomly selected microspheres. The minimum fluidization rate was determined by gradually increasing the nitrogen flow rate and recording the bed pressure drop, with the gas velocity at which the bed pressure drop began to stabilize being taken as the minimum fluidization rate.
[0024] Example 1 A method for preparing polyester staple fiber includes the following steps: 2,000 kg of fiber-grade PET homopolymer chips with an initial intrinsic viscosity of 0.64 dL / g, a residual antimony content of 200 ± 20 mg / kg, and without any intentionally added comonomers were added. These chips were placed in a rotary vacuum reactor with an effective volume of 5 L and a rotation speed of 12 r / min, and treated at 135 °C and 2 kPa for 40 min. The temperature was then increased to 165 °C at a rate of 1.5 °C / min and treated at 0.5 kPa for 75 min. Subsequently, the temperature was increased to 205 °C and solid-state polycondensation was carried out at 50 Pa. No additional catalyst was added during the solid-state polycondensation process. Samples were taken every 60 min through a sealed sampling port, and heating was stopped when the intrinsic viscosity reached 0.84 dL / g.
[0025] The thickened slices were cooled to below 80°C under vacuum, and then subjected to 10 Nm 3 The dehumidified air with a dew point not higher than -40℃ is dried at 150℃ for 8 hours, and the output condition is that the moisture content of the slices is not higher than 30ppm.
[0026] Melt spinning was performed using a spinneret with 144 holes, a hole diameter of 0.25 mm, and a hole length-to-diameter ratio of 2.5. The extruder temperatures in each zone were 270℃, 274℃, and 278℃, respectively, while the spinning box temperature was 278℃. The cumulative residence time of the melt in the zone above 278℃ was 4.0 min. The total discharge rate of the metering pump was 4.20 kg / h, and the spinning winding speed was 900 m / min. The nascent yarn was cooled using a cross-blowing airflow at 22℃ and 0.4 m / s. 0.006 kg of a commercially available heat-resistant PET spinning oil concentrate with an effective ingredient content of 50% was mixed with 0.024 kg of deionized water to prepare 0.030 kg of an oil emulsion with an effective ingredient mass fraction of 10%. This emulsion was then applied entirely via a metering oiling device, ensuring that the effective ingredient content of the oil reached 0.15% of the PET mass.
[0027] Add 10.0 kg of deionized water to the drawing water bath. The nascent filament bundle enters the 80℃ water bath at a speed of 10.000 m / min, with the first-stage drawing roller speed at 29.500 m / min and the first-stage draw ratio at 2.95. Add 3.0 kg of deionized water to the steam generator to produce 120℃ superheated steam at a flow rate of 0.4 kg / h, with the second-stage drawing roller speed at 35.400 m / min, the second-stage draw ratio at 1.20, and the total draw ratio at 3.54.
[0028] The effective fluidization cross-sectional area is 0.005m². 2 The isolated fluidized bed heat exchanger is loaded with 1.260 kg of material with a bulk density of 2.10 g / cm³. 3 Spherical α-alumina ceramic microspheres with a particle size of 150–300 μm, a sphericity of 0.90, and an α-Al₂O₃ content of 99.0% were selected. Fine powder with a particle size less than 75 μm was sieved out to form a 120 mm thick static bed. A porous sintered metal insulating guide wire channel with a pore size of 20 μm was used to separate the microspheres from the fiber bundle.
[0029] The total amount used is 0.30 Nm 3 Industrial nitrogen gas with a purity of 99.9% and a dew point of -30℃, containing 0.20 Nm³ of... 3 Used for system replacement, 0.10 Nm 3 Used for gas replenishment during operation, employing a closed-loop circulation. The minimum fluidization velocity at 182℃ is controlled at 0.045 m / s, and the working gas velocity is set at 0.0495 m / s, which is 1.1 times the minimum fluidization velocity, corresponding to a hot-state circulation flow rate of 0.891 m³ / s. 3 / h.
[0030] The drawn fiber bundles were combined to a bus density of 1200 dtex and fed at a speed of 6,000 m / min, corresponding to a mass flow rate of 0.72 g / min. The fiber bundle thickness was 2.0 mm, the inlet temperature was 105 °C, the fluidized bed temperature was 182 °C, and the constant-length conveying tension was 0.04 cN / dtex. The effective heating length of the isolation guide channel was 0.100 m, the pulsed thermal pre-stabilization time was 1.0 s, and the outlet temperature was controlled in a closed loop at 178 °C. Subsequently, the front and rear rollers were kept at the same speed, and the fiber bundle was cooled to 150 °C with circulating cold nitrogen.
[0031] The pre-stabilized fiber bundle was fed into the first-stage thermal relaxation zone at 165℃ at a speed of 6.000 m / min, with an exit speed of 5.940 m / min, for 12 s, resulting in an effective treatment length of 1.194 m. It was then fed into the second-stage thermal relaxation zone at 175℃, with an exit speed of 5.8509 m / min, for 10 s, resulting in an effective treatment length of 0.983 m. The fiber bundle tension was controlled at 0.005 cN / dtex during both thermal relaxation processes, with a cumulative relaxation rate of 2.485%.
[0032] The filament bundle was re-shaped at 198℃ for 12 seconds at the length after the second stage of heat relaxation, with both the front and rear traction rollers at a speed of 5.8509 m / min, resulting in an effective processing length of 1.170 m. The filament bundle was then cooled to 69℃ while maintaining the same linear speed, and after the length constraint was removed, it was cut into 32 mm polyester staple fibers.
[0033] Example 2 A method for preparing polyester staple fiber includes the following steps: 3,000 kg of fiber-grade PET homopolymer chips with an initial intrinsic viscosity of 0.66 dL / g, a residual antimony content of 200 ± 20 mg / kg, and without any intentionally added comonomers were added. These chips were placed in a 10 L rotary vacuum reactor at 12 r / min and treated at 140 °C and 5 kPa for 30 min. The temperature was then increased to 170 °C at 1.5 °C / min and treated at 1.25 kPa for 60 min. Subsequently, the temperature was increased to 210 °C and solid-state polycondensation was carried out at 125 Pa. Samples were taken every 60 min through a sealed sampling port. Heating was stopped when the intrinsic viscosity reached 0.87 dL / g. No additional catalyst was added during the solid-state polycondensation process.
[0034] The thickened slices were cooled to below 80°C under vacuum, and then subjected to 12 Nm 3 Dehumidified air with a dew point not higher than -40℃ is dried at 155℃ for 7 hours, and the output condition is that the moisture content of the slices is not higher than 30ppm.
[0035] Melt spinning was performed using a spinneret with 144 holes, a hole diameter of 0.25 mm, and a hole length-to-diameter ratio of 2.5. The extruder temperatures in each zone were 272℃, 278℃, and 281℃, respectively, while the spinning box temperature was 281℃. The cumulative residence time of the melt in the zone above 278℃ was 4.5 min. The total discharge rate of the metering pump was 5.13 kg / h, and the spinning winding speed was 1100 m / min. Cooling was achieved using a 22℃, 0.4 m / s cross-blowing airflow. 0.012 kg of a commercially available heat-resistant PET spinning oil concentrate with an effective ingredient content of 50% was mixed with 0.048 kg of deionized water to prepare 0.060 kg of an oil emulsion with an effective ingredient mass fraction of 10%. This emulsion was then applied entirely via a metering oiling device, ensuring that the effective ingredient content of the oil accounted for 0.20% of the PET mass.
[0036] Add 15.0 kg of deionized water to the drawing water bath. The nascent filament bundle enters the 82.5℃ water bath at a speed of 10.000 m / min, the speed of the first-stage drawing roller is 30.000 m / min, and the first-stage draw ratio is 3.00. Add 4.0 kg of deionized water to the steam generator to produce 125℃ superheated steam at a flow rate of 0.6 kg / h, the speed of the second-stage drawing roller is 36.600 m / min, the second-stage draw ratio is 1.22, and the total draw ratio is 3.66.
[0037] The effective fluidization cross-sectional area is 0.005m². 2 The isolated fluidized bed heat exchanger is loaded with 1.680 kg of material with a bulk density of 2.10 g / cm³. 3 Spherical α-alumina ceramic microspheres with a particle size of 150–300 μm, a sphericity of 0.93, and an α-Al₂O₃ content of 99.5% were selected. Fine powder with a particle size less than 75 μm was sieved out to form a 160 mm thick static bed. A porous sintered metal insulating guide wire channel with a pore size of 30 μm was used to separate the microspheres from the fiber bundle.
[0038] The total amount used is 0.40 Nm. 3 Industrial nitrogen gas with a purity of 99.95% and a dew point of -35℃, containing 0.25 Nm³ of... 3 Used for system replacement, 0.15 Nm 3 Used for gas replenishment during operation, employing a closed-loop circulation. The minimum fluidization velocity at 183.5℃ is controlled at 0.045 m / s, and the working gas velocity is set to 0.05625 m / s, which is 1.25 times the minimum fluidization velocity, corresponding to a hot-state circulation flow rate of 1.0125 m³ / s. 3 / h.
[0039] The drawn fiber bundles were combined to a bus density of 2000 dtex and fed at a speed of 8,000 m / min, corresponding to a mass flow rate of 1.60 g / min. The fiber bundle thickness was 1.2 mm, the inlet temperature was 112.5℃, the fluidized bed temperature was 183.5℃, and the constant-length conveying tension was 0.06 cN / dtex. The effective heating length of the isolation guide channel was 0.107 m, the pulsed thermal pre-stabilization time was 0.8 s, and the outlet temperature was controlled in a closed loop at 180.5℃. Subsequently, the fiber bundle was cooled to 145℃ with circulating cold nitrogen while maintaining equal speeds for the front and rear rollers.
[0040] The pre-stabilized fiber bundle was fed into the first-stage thermal relaxation zone at 166.5℃ at a speed of 8.000 m / min, with an exit speed of 7.920 m / min, for 10 s, resulting in an effective treatment length of 1.327 m. It was then fed into the second-stage thermal relaxation zone at 176.5℃, with an exit speed of 7.8012 m / min, for 8 s, resulting in an effective treatment length of 1.048 m. The fiber bundle tension was controlled at 0.0125 cN / dtex during both thermal relaxation processes, with a cumulative relaxation rate of 2.485%.
[0041] The filament bundle was re-shaped at 200℃ for 10 seconds at the length after the second stage of heat relaxation, with the speed of both the front and rear traction rollers at 7.8012 m / min, resulting in an effective processing length of 1.300 m. The filament bundle was then cooled to 65℃ while maintaining the same linear speed, and after the length constraint was removed, it was cut into 38 mm polyester staple fibers.
[0042] Example 3 A method for preparing polyester staple fiber includes the following steps: 5,000 kg of fiber-grade PET homopolymer chips with an initial intrinsic viscosity of 0.68 dL / g, a residual antimony content of 200 ± 20 mg / kg, and without any intentionally added comonomers were added. These chips were placed in a rotary vacuum reactor with an effective volume of 15 L and a rotation speed of 10 r / min, and treated at 145 °C and 8 kPa for 20 min. The temperature was then increased to 175 °C at a rate of 1.5 °C / min and treated at 2 kPa for 45 min. Subsequently, the temperature was increased to 215 °C and solid-state polycondensation was carried out at 200 Pa. Samples were taken every 60 min through a sealed sampling port. Heating was stopped when the intrinsic viscosity reached 0.90 dL / g. No additional catalyst was added during the solid-state polycondensation process.
[0043] The thickened slices were cooled to below 80°C under vacuum, and then subjected to 15 Nm 3 Dehumidified air with a dew point not higher than -40℃ is dried at 160℃ for 6 hours, and the output condition is that the moisture content of the slices is not higher than 30ppm.
[0044] Melt spinning was performed using a spinneret with 144 holes, a hole diameter of 0.25 mm, and a hole length-to-diameter ratio of 2.5. The temperatures of each zone of the extruder were 274℃, 281℃, and 284℃, respectively, while the spinning box temperature was 284℃. The cumulative residence time of the melt in the region above 278℃ was 5.0 min. The total discharge rate of the metering pump was 6.07 kg / h, and the spinning winding speed was 1300 m / min. Cooling was achieved using a 22℃, 0.4 m / s cross-blowing airflow. 0.025 kg of a commercially available heat-resistant PET spinning oil concentrate with an effective ingredient content of 50% was mixed with 0.100 kg of deionized water to prepare 0.125 kg of an oil emulsion with an effective ingredient mass fraction of 10%. This emulsion was then applied entirely through a metering oiling device, ensuring that the effective ingredient content of the oil accounted for 0.25% of the PET mass.
[0045] Add 20.0 kg of deionized water to the drawing water bath. The nascent filament bundle enters the 85℃ water bath at a speed of 10.000 m / min, with the first-stage drawing roller speed at 30.480 m / min and the first-stage draw ratio at 3.048. Add 5.0 kg of deionized water to the steam generator to produce 130℃ superheated steam at a flow rate of 0.8 kg / h. The second-stage drawing roller speed is 37.7952 m / min, the second-stage draw ratio is 1.240, and the total draw ratio is 3.77952.
[0046] The effective fluidization cross-sectional area is 0.005m². 2 The isolated fluidized bed heat exchanger is loaded with 2,100 kg of material with a bulk density of 2.10 g / cm³. 3 Spherical α-alumina ceramic microspheres with a particle size of 150–300 μm, a sphericity of 0.95, and an α-Al₂O₃ content of 99.9% were selected. Fine powder with a particle size of less than 75 μm was sieved out to form a 200 mm thick static bed. A porous sintered metal insulating guide wire channel with a pore size of 40 μm was used to separate the microspheres from the fiber bundle.
[0047] The total amount used is 0.50 Nm. 3 Industrial nitrogen gas with a purity of 99.99% and a dew point of -40℃, containing 0.30 Nm³ of... 3 Used for system replacement, 0.20 Nm 3 Used for gas replenishment during operation, employing a closed-loop circulation. The minimum fluidization velocity at 185℃ is controlled at 0.045 m / s, and the working gas velocity is set at 0.063 m / s, which is 1.4 times the minimum fluidization velocity, corresponding to a hot-state circulation flow rate of 1.134 m³ / s. 3 / h.
[0048] The drawn fiber bundles were combined to a bus density of 1200 dtex and fed at a speed of 10,000 m / min, corresponding to a mass flow rate of 1.20 g / min. The fiber bundle unfolding thickness was 0.5 mm, the inlet temperature was 120 °C, the fluidized bed temperature was 185 °C, and the constant-length conveying tension was 0.08 cN / dtex. The effective heating length of the isolation guide channel was 0.100 m, the pulsed thermal pre-stabilization time was 0.6 s, and the outlet temperature was controlled in a closed loop at 183 °C. Subsequently, while maintaining equal speeds on the front and rear rollers, the fiber bundle was cooled to 140 °C using circulating cold nitrogen.
[0049] The pre-stabilized fiber bundle was fed into the first-stage thermal relaxation zone at 168℃ at a speed of 10.000 m / min, with an exit speed of 9.900 m / min and a treatment time of 8 s, resulting in an effective treatment length of 1.327 m. It was then fed into the second-stage thermal relaxation zone at 178℃, with an exit speed of 9.7515 m / min and a treatment time of 6 s, resulting in an effective treatment length of 0.983 m. The fiber bundle tension was controlled at 0.020 cN / dtex during both thermal relaxation processes, and the cumulative relaxation rate was 2.485%.
[0050] The filament bundle was re-shaped at 202℃ for 8 seconds at the length after the second stage of heat relaxation, with both the front and rear traction rollers at a speed of 9.7515 m / min, resulting in an effective processing length of 1.300 m. The filament bundle was then cooled to 60℃ while maintaining the same linear speed, and after the length constraint was removed, it was cut into 51 mm polyester staple fibers.
[0051] Comparative Example 1: Compared with Example 1, the PET homopolymer chips with an initial intrinsic viscosity of 0.64 dL / g were not subjected to vacuum solid-phase thickening. Instead, they were dried at 150°C to a moisture content of no more than 30 ppm and then directly melt-spun. The other raw materials, dosages and process parameters were the same as in Example 1.
[0052] Comparative Example 2: Compared with Example 1, the isolated fluidized pre-stabilization treatment consisting of industrial nitrogen and spherical α-alumina ceramic microspheres was completely eliminated. The drawn fiber bundle was directly fed into a two-stage thermal relaxation device. All other raw materials, dosages and process parameters were the same as in Example 1.
[0053] Comparative Example 3: Compared with Example 1, spherical α-alumina ceramic microspheres were not loaded into the isolated fluidized heat exchanger. Instead, industrial nitrogen gas at a temperature of 182°C and an apparent flow rate of 0.0495 m / s was used to treat a fixed-length filament bundle for 1.0 s. All other raw materials, dosages, and process parameters were the same as in Example 1.
[0054] Comparative Example 4: Compared with Example 1, 0.30 Nm 3 Industrial nitrogen was replaced with an equal amount of dry air with a dew point of -30°C, and 1.260 kg of spherical α-alumina ceramic microspheres were fluidized at the same apparent flow rate. All other raw materials, dosages, and process parameters were the same as in Example 1.
[0055] Comparative Example 5: Compared with Example 1, the fixed length constraint of the front and rear constant speed rollers was removed during the synergistic prestabilization process of industrial nitrogen and spherical α-alumina ceramic microspheres, allowing the filament bundle to be freely subjected to a 1.0s pulse heat treatment at 182°C and then cooled to 150°C. The remaining raw materials, dosages and process parameters were the same as in Example 1.
[0056] Comparative Example 6: Compared with Example 1, the two-stage limited thermal relaxation at 165°C and 175°C was combined into a single-stage thermal relaxation at 175°C. The inlet roller speed was set to 6.000 m / min, the outlet roller speed was set to 5.8509 m / min, and the processing time was set to 22 s, so that the cumulative relaxation rate was maintained at 2.485%. The remaining raw materials, dosages, and process parameters were the same as in Example 1.
[0057] Comparative Example 7: Compared with Example 1, the fixed-length heat re-setting at 198°C according to the new length after the second stage of heat relaxation was cancelled. The filament bundle that had completed the two stages of heat relaxation was directly cooled to 69°C at 5.8509 m / min and cut. The remaining raw materials, dosages and process parameters were the same as in Example 1.
[0058] Performance testing 1. Linear density test. The test was conducted according to Method A of GB / T 14335—2008 "Test Method for Linear Density of Short Chemical Fibers". Each sample was conditioned for 24 hours in standard atmosphere at (20±2)℃ and (65±4)% relative humidity. Ten bundles of samples were prepared from different locations, each bundle containing 100 single fibers. Slight tension was applied to eliminate the curl without causing fiber elongation. A 20.00 mm length section was cut using a fiber cutter and weighed using an analytical balance with a graduation of 0.01 mg. The linear density of each bundle was calculated using T=10000m / (nL), where T is the linear density (dtex), m is the fiber bundle mass (mg), n is the number of single fibers, and L is the cut length (mm). The result was the arithmetic mean of the ten bundles.
[0059] 2. Tensile property testing. The tensile properties were tested according to GB / T 14337—2022 "Test Method for Tensile Properties of Short Chemical Fibers". Each sample was conditioned for 24 hours at a temperature of (20±2)℃ and a relative humidity of (65±4)%. Tensile strength was measured using an electronic single-fiber tensile tester. The clamping distance was set to 20 mm, the pre-tension per unit linear density was set to 0.15 cN / dtex, and the tensile speed was set to 20 mm / min. Single fibers were randomly selected from different locations on each sample to obtain no fewer than 50 valid results. Breaking strength, elongation at break, load at 10% elongation, and the slope of the initial linear segment of the stress-strain curve were recorded. The breaking strength and the load at 10% elongation were divided by the corresponding single-fiber linear density to obtain the breaking strength and the strength at 10% constant elongation. The initial modulus was calculated based on the initial linear segment of the stress-strain curve. The arithmetic mean of the valid results was taken for each index.
[0060] 3.180℃ Dry Heat Shrinkage Rate Test. The test was conducted according to the basic procedures of GB / T 43015—2023 "Test Method for Dry Heat Shrinkage Rate of Synthetic Short Fibers". Each sample was conditioned for 24 hours at a temperature of (20±2)℃ and a relative humidity of (65±4)%. Thirty-five single fibers were randomly selected and stretched with a unit linear density pre-tension of 0.075 cN / dtex. The length L0 before heat treatment was measured with a measurement accuracy of 0.01 mm. After releasing the pre-tension, the samples were placed in a lateral forced-air drying oven stabilized at (180±1)℃ for 30 minutes. After removal, they were equilibrated in the above-mentioned standard atmosphere for 30 minutes, and then the same pre-tension was applied to measure the length L1 after heat treatment. The dry heat shrinkage rate of a single fiber was calculated as S=(L0-L1) / L0×100%. After removing results due to breakage or clamping abnormalities, at least 30 valid results were retained. The arithmetic mean of the sample results was taken and retained to two decimal places.
[0061] 4. Crystallinity Test. The test was conducted according to GB / T 19466.3—2025 "Differential Scanning Calorimetry (DSC) for Plastics – Part 3: Determination of Melting and Crystallization Temperatures and Enthalpy". The fibers were shredded and mixed thoroughly. 3.0–5.0 mg of the sample was placed in a sealed aluminum crucible. Using an empty aluminum crucible as a reference, the temperature was increased from 25 °C to 300 °C at a rate of 10 °C / min under a nitrogen atmosphere with a flow rate of 50 mL / min. The enthalpy of melting, ΔH, was obtained by integrating the first heating curve. m And the enthalpy of cold crystallization ΔHcc, and according to Xc=(ΔH m The crystallinity is calculated as (-ΔHcc) / 140×100%, where 140J / g is the melting enthalpy of fully crystallized PET; each sample is tested in parallel 3 times, and the result is the arithmetic mean.
[0062] Table 1: The breaking strengths of Examples 1, 2, and 3 were 6.42 cN / dtex, 6.71 cN / dtex, and 6.88 cN / dtex, respectively, and the dry heat shrinkage rates at 180°C were 1.82%, 1.57%, and 1.39%, respectively. With increasing viscosity and draw ratio, the fiber's breaking strength, 10% elongation strength, initial modulus, and crystallinity increased simultaneously, while the elongation at break and dry heat shrinkage decreased accordingly. Example 3 had an initial modulus of 103.7 cN / dtex and a crystallinity of 51.1%, while maintaining an elongation at break of 17.6%, indicating that orientation strengthening and thermal dimensional stabilization could be balanced within the designed process window.
[0063] A comparison of Example 1 with Comparative Examples 2-4 shows that industrial nitrogen and spherical α-alumina ceramic microspheres form a synergistic effect in heat transfer. Industrial nitrogen, as a low-dew-point inert flow medium, can form continuous and dispersed convection channels along the gaps between microspheres and inside the fiber bundle, allowing heat to quickly enter the fiber bundle and maintaining a stable heat treatment atmosphere. The spherical α-alumina ceramic microspheres utilize their heat capacity and thermal conductivity to buffer inlet temperature fluctuations, reducing the temperature difference between the inner and outer layers of the fiber bundle through multi-point heat exchange. Together, they ensure that the fibers are uniformly heated within a short time under a fixed-length constraint, releasing residual stress and stabilizing the crystalline structure while suppressing macroscopic shrinkage. Compared to Comparative Example 2 (omitting this pre-stabilization operation), Comparative Example 3 (using only industrial nitrogen), and Comparative Example 4 (using dry air instead of industrial nitrogen), the fracture strength of Example 1 increased by 0.56 cN / dtex, 0.37 cN / dtex, and 0.21 cN / dtex, respectively, while the dry heat shrinkage rate decreased by 0.36, 0.22, and 0.12 percentage points, respectively. In Comparative Example 5, after the fixed-length constraint was removed, the fiber underwent free shrinkage in this process, and the linear density increased to 1.58 dtex. Although the subsequent dry heat shrinkage rate was 1.58%, the breaking strength and initial modulus decreased to 5.57 cN / dtex and 72.9 cN / dtex, respectively. This indicates that sacrificing shrinkage for free shrinkage weakens the already formed molecular chain orientation. This synergistic system addresses the problems of uneven heating during rapid thermal stabilization and the tendency for dimensional stabilization to come at the cost of orientation strength.
[0064] The remaining comparative results further demonstrate the synergistic effect of each process. Comparative Example 1, which omitted solid-phase thickening, showed a fracture strength of 5.28 cN / dtex, indicating that a higher molecular weight is fundamental for forming an effective load-bearing network. Comparative Example 6, which employed single-segment relaxation treatment, had a fracture strength of 5.96 cN / dtex and a dry heat shrinkage rate of 2.11%, demonstrating that segmented relaxation is more conducive to coordinating orientation retention and residual stress release. Comparative Example 7, which omitted the new length shaping treatment, maintained a fracture strength of 6.34 cN / dtex, but its dry heat shrinkage rate increased to 4.36%, and its crystallinity decreased to 42.6%, indicating that end-point shaping has a direct effect on fixing the structural state after relaxation and reducing subsequent thermal shrinkage.
[0065] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the essence and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing polyester staple fiber, characterized in that, Includes the following steps: Vacuum solid-state thickening of polyethylene terephthalate (PET) polyester chips was performed, followed by melt spinning and graded drawing to obtain drawn fiber bundles. In an isolated fluidized bed heat exchanger, spherical α-alumina ceramic microspheres are aerated with industrial nitrogen gas. The spherical α-alumina ceramic microspheres and the drawn filament bundle are separated by an isolation structure that allows nitrogen gas to pass through while trapping the spherical α-alumina ceramic microspheres. The industrial nitrogen gas, after heat exchange with the spherical α-alumina ceramic microspheres, passes through the unfolded and fixed-length drawn filament bundle to perform pulsed thermal pre-stabilization on the drawn filament bundle. Then, the bundle is cooled while maintaining a constant filament bundle length to obtain a pre-stabilized filament bundle. The pre-stabilized filament bundle is subjected to two-stage, progressively heated, tension-limited thermal relaxation. The bundle is then thermally reshaped to a fixed length according to the length of the bundle after the second stage of thermal relaxation, while the bundle length is kept cool. The cooled filament bundles are cut to obtain polyester staple fibers.
2. The preparation method according to claim 1, characterized in that, The initial intrinsic viscosity of the polyethylene terephthalate (PET) homopolymer polyester chips is 0.64–0.68 dL / g. The vacuum solid-state viscosity enhancement includes: first, treatment at 135–145°C and 2–8 kPa for 20–40 min, then treatment at 165–175°C and 0.5–2 kPa for 45–75 min, followed by solid-state polycondensation at 205–215°C and 50–200 Pa, until the intrinsic viscosity of the PET homopolymer polyester chips reaches 0.84–0.90 dL / g.
3. The preparation method according to claim 2, characterized in that, The polyethylene terephthalate (PET) homopolymer polyester chips after vacuum solid-phase thickening are dried at 150–160°C until the moisture content is no more than 30 ppm, and then melt-spun at 278–284°C. The cumulative residence time of the melt at 278°C or above does not exceed 5 min, and the spinning winding speed is 900–1300 m / min.
4. The preparation method according to claim 3, characterized in that, The staged stretching includes: first stretching 2.95 to 3.05 times in a water bath at 80 to 85°C, and then stretching 1.20 to 1.24 times in superheated steam at 120 to 130°C, with a total stretching ratio of 3.54 to 3.78 times.
5. The preparation method according to claim 1, characterized in that, The purity of the industrial nitrogen gas is not less than 99.9%, and the dew point is not higher than -30℃; the spherical α-alumina ceramic microspheres have a particle size of 150-300μm, a sphericity of not less than 0.90, and an α-Al2O3 content of not less than 99%, and fine powder with a particle size of less than 75μm is pre-screened out; the spherical α-alumina ceramic microspheres form a fluidized bed with a static thickness of 120-200mm, and the apparent velocity of the industrial nitrogen gas is 1.1-1.4 times the minimum fluidization velocity of the fluidized bed.
6. The preparation method according to claim 5, characterized in that, The isolation structure is a porous sintered metal isolation guide wire channel with a pore size of 20-40 μm, set in a fluidized bed; the thickness of the drawn wire bundle after unfolding is no more than 2 mm, the temperature when entering the isolation guide wire channel is 105-120℃, the fluidized bed temperature is 182-185℃, the wire bundle tension during pulsed thermal prestabilization is 0.04-0.08 cN / dtex, the processing time is 0.6-1.0 s, and the control endpoint is that the drawn wire bundle outlet temperature reaches 178-183℃; after pulsed thermal prestabilization, it is cooled to no higher than 150℃ while keeping the wire bundle length unchanged.
7. The preparation method according to claim 1, characterized in that, The two-stage, progressively heated, tension-limited thermal relaxation includes: The first stage of thermal relaxation is carried out at 165–168℃, the outlet linear velocity of the first stage of thermal relaxation is 0.990 times the inlet linear velocity, and the processing time is 8–12 s; Then, a second-stage thermal relaxation is performed at 175–178°C. The exit line velocity of the second-stage thermal relaxation is 0.985 times that of the first-stage thermal relaxation, and the processing time is 6–10 seconds. The cumulative relaxation rate of the two-stage thermal relaxation was 2.485%, and the bundle tension was maintained at 0.005–0.020 cN / dtex during the two-stage thermal relaxation process.
8. The preparation method according to claim 7, characterized in that, After completing two stages of heat relaxation, based on the exit linear speed of the second stage of heat relaxation, the filament bundle is subjected to fixed-length heat re-setting for 8–12 seconds at 198–202°C according to the length of the filament bundle after the second stage of heat relaxation. The ratio of the linear speeds of the front and rear traction rollers of the fixed-length heat re-setting device is 1.000±0.
002. After fixed-length heat re-setting, the length of the filament bundle is kept constant, and the filament bundle is cooled to below 70°C before the length constraint is released.
9. The preparation method according to claim 1, characterized in that, The cooled filament bundles are cut into short polyester fibers with a length of 32–51 mm.
10. A polyester staple fiber, characterized in that, It is prepared by the method described in any one of claims 1-9 above.