Anti-pilling and anti-snagging polyamide fiber and method of making same
By adding nano-silicone powder and polydopamine coating to nylon fibers, combined with specific spinning processes and surface treatments, the problem of insufficient anti-pilling and anti-snagging properties of nylon fibers has been solved, achieving high-performance anti-pilling and anti-snagging effects while maintaining other fiber properties.
Patent Information
- Application Number
- CN202611408443.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-24
Smart Images

Figure CN123153186A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of textile material preparation technology, specifically relating to an anti-pilling and anti-snagging nylon fiber and its preparation method. Background Technology
[0002] As people's living standards continue to improve, the requirements for clothing are no longer limited to warmth and durability, but also include comfort, aesthetics, and functionality. Fabrics are prone to pilling and fuzzing during use, which not only deteriorates the fabric's appearance and feel but also causes wear and tear, reducing its performance.
[0003] Nylon, as a synthetic fiber, has significant advantages: high strength, excellent abrasion resistance, superior elasticity, and lightweight, making it suitable for sportswear, outdoor gear, and clothing with high abrasion resistance requirements; it is also wrinkle-resistant, easy to care for, quick-drying, and does not easily deform. Disadvantages include poor moisture absorption and breathability, a tendency to generate static electricity, potential stuffiness when worn close to the skin, and a tendency to age and yellow with prolonged sun exposure; it is also less environmentally friendly (difficult to degrade). It is often used in functional clothing, but a balance must be struck between comfort and durability.
[0004] Currently, the main methods for modifying the anti-pilling and anti-snagging properties of fiber raw materials are: I. Chemical modification: Starting from the molecular level of the fiber, the physical properties of the fiber are directly changed by adjusting the polymerization or spinning process.
[0005] Reducing fiber strength: This is the most common method. By chemically modifying the fibers to reduce their breaking strength (or hook strength), the small balls formed by friction are more likely to detach or break, rather than becoming more tightly bound.
[0006] Modifying fiber cross-section: Conventional round cross-section fibers are processed into irregular cross-section fibers (such as flat or triangular fibers) using a shaped spinneret. These fibers are more rigid, reducing fiber entanglement and thus improving anti-pilling and anti-snagging properties.
[0007] II. Physical modification: Without changing the chemical composition of the fiber, the microstructure of the fiber surface is changed through post-treatment or spinning process control.
[0008] Fiber surface treatment: During the spinning process, the fiber surface is physically or chemically modified to form a special microstructure.
[0009] Enzymatic hydrolysis: For natural protein fibers (such as wool), treatment with biological enzymes (such as papain) can gently remove the scale layer on their surface that easily causes pilling, without producing harmful byproducts like traditional chlorination treatment, and can also improve dyeing performance. In addition, studies have found that the synergistic effect of polyesterase and cellulase can be used to improve the anti-pilling properties of polyester-cotton blended fabrics.
[0010] III. Composite Structure Design: Combining two or more fibers with different properties in a specific structure to take advantage of each other's strengths and compensate for each other's weaknesses.
[0011] Core-sheath structure: This structure encases easily pilling fibers (such as wool) within the yarn as the core layer, and non-pilling fibers (such as Tencel or profiled polyester fibers) as the sheath layer. This structure utilizes the outer fibers to form a protective layer and is supported by the internal skeleton, reducing fiber migration and slippage, thereby improving anti-pilling performance.
[0012] Wrapped yarn: This involves using filaments (such as polylactic acid filaments) as the core or outer wrapping yarn, which are wrapped with short fibers (such as viscose fibers) during spinning. The strength and cohesion of the filaments can fix the short fibers, reduce their slippage and fuzzing, thereby improving the fabric's abrasion resistance and anti-pilling properties.
[0013] Nylon, despite its good abrasion resistance and high strength, is actually more prone to pilling during friction, and the pills are difficult to detach, making its anti-pilling performance generally inferior to polyester. Achieving anti-pilling properties usually requires blending modified chips, adding anti-pilling agents, or post-treatment. It's important to note that these methods often require a trade-off. For example, reducing fiber strength may reduce pilling but sacrifice fabric durability; while irregularly shaped fibers offer good snag resistance, they may compromise on softness. Therefore, in practical applications, a balance must be found among various properties depending on the intended use of the final product. Summary of the Invention
[0014] In view of the shortcomings and deficiencies of the existing technology, the purpose of this invention is to provide an anti-pilling and anti-snagging nylon fiber and its preparation method, which improves the anti-pilling and anti-snagging performance of nylon while balancing other properties to meet the market demand for specific functional fibers.
[0015] To achieve the objective of this invention, the inventors provide the following technical solution: The present invention firstly provides an anti-pilling and anti-snagging nylon fiber, which is made by melt spinning nylon chips with 3%-10% functional masterbatch based on the weight of nylon chips to obtain nylon filaments, and then applying a polydopamine coating to the surface of the nylon fiber after post-treatment. The functional masterbatch contains 3% to 8% nano silicone powder; the thickness of the polydopamine coating is between 40-50 nm.
[0016] This invention optimizes both the source of fiber raw materials and the spinning process, satisfying the functional requirements of the fiber without compromising its physicochemical properties, thus expanding the application fields of nylon fiber. Adding an appropriate amount of nano-silicone powder effectively improves the mechanical and processing properties of the fiber; the polydopamine coating firmly locks in the nano-silicone powder, further enhancing anti-pilling and anti-snagging properties. Testing shows that the nylon obtained by this invention has an anti-snagging performance of up to level 5, anti-pilling performance ≥ level 4-5, a breaking strength between 4.0-4.5 cN / dtex, and a moisture regain ≤ 4% under standard temperature and humidity conditions (20℃ / 65%RH).
[0017] This invention also provides a method for preparing anti-pilling and anti-snagging nylon fibers, comprising the following steps: (1) Raw material preparation and drying Nylon chips (PA6 or PA66) are used after vacuum drying, with the moisture content controlled below 0.05% to prevent polymer hydrolysis at high temperatures, which would lead to a decline in quality.
[0018] (2) Preparation of functional masterbatch The functional masterbatch is prepared by melt-blending and extruding granulation of 3-8% by weight of nano-silicone powder, 0.5-3% by weight of dispersant, and the balance of nylon chips at a temperature of 210-230℃. First, nano-silicone powder is made into functional masterbatch, and then the functional masterbatch is blended with nylon chips for spinning. This allows the functional masterbatch to be evenly dispersed in the fiber matrix, ensuring that the functional fiber has good spinnability and mechanical properties.
[0019] (3) Melt spinning Functional masterbatch, at a rate of 3%-10% by weight of nylon chips, is melt-blended with nylon chips to obtain a spinning melt. This spinning melt then undergoes melt spinning, cooling and solidification, primary oiling, post-drawing treatment, heat setting, secondary oiling, and winding to produce nylon FDY filament. The melt spinning process involves precise control through two stages of staged drawing. Key process parameters include: first-stage draw ratio 1.05-1.15, second-stage draw ratio 1.25-1.30, first hot roller temperature 65-70℃, second hot roller temperature 140-150℃, winding speed 4500-4600 m / min, and overfeed rate approximately 3-4%. The spinning melt is melt-spun, then cooled and solidified, oiled, and wound to obtain POY precursor yarn. The POY precursor yarn is then placed on a texturing machine and sequentially undergoes two-stage drawing, heat deformation (false twisting), heat setting, cooling, oiling, and winding to finally produce nylon DTY filament. Specifically, the two-stage drawing has a total draw ratio between 1.15 and 1.30, and the first-stage draw ratio is between 1.05 and 1.15. The heat deformation chamber temperature is 160-185℃, the heat setting chamber temperature is 175-195℃, the D / Y ratio is 1.7-1.85, and the processing speed is 650-750 m / min. (4) Post-processing The surface of nylon fiber is micro-etched with formic acid solution, washed and dried. Then, the nylon filament is immersed in dopamine Tris buffer solution and allowed to stand at room temperature for 12-18 hours. The polydopamine coating is deposited on the surface of the nylon fiber by the oxidative self-polymerization reaction of dopamine. After removal, it is washed and dried to obtain the finished nylon filament with anti-pilling and anti-snagging properties.
[0020] Micro-etching the surface of nylon fibers with formic acid solution creates microstructures on the fiber surface, which significantly improves the adhesion of subsequent polydopamine coatings. The PDA coating firmly locks in the nano-silicone powder within the fiber, further enhancing its anti-pilling properties and making it more durable; in addition, the PDA coating enhances the anti-snagging properties of nylon fibers.
[0021] Preferably, in step (1) of this invention, the vacuum drying temperature is 85-100°C and the time is 6-8 hours.
[0022] Preferably, in step (2) of this invention, the volume average diameter (D43) of the nano-silicone powder is 10-20 μm, the active ingredient content is ≥99%, and the organosilicon content is ≥71%. Commercially available products utilize the excellent lubricity of nano-silicone powder to reduce the fiber friction coefficient, enabling the fiber to achieve an anti-pilling grade of 4-5. The name "nano-silicone powder" likely derives from the use of nano-sized raw materials (such as nano-silica) in its production process.
[0023] Preferably, in step (3) of this invention: The spinning assembly uses irregularly shaped spinnerets, such as cross-shaped, trilobal, or grooved irregular shapes. The melting temperature of nylon is 230℃~270℃; The cooling air temperature for cooling and solidification is 10–20℃, and the air velocity is approximately 0.3–0.6 m / s.
[0024] Preferably, in step (4) of this invention, a 10-15% formic acid solution is used, and the micro-etching treatment lasts for 10-20 minutes. The effect of short-duration, low-concentration micro-etching on the mechanical properties of the fiber is almost negligible, but the surface roughness of the fiber is improved after this step, which is more conducive to the adhesion of the coating in the next step.
[0025] Preferably, in step (4) of this invention, a dopamine Tris buffer solution with a concentration of 1-3 g / L and a pH of 8.5 is used. The optimal pH environment for dopamine self-polymerization is around 8.5, and it should be prepared and used immediately.
[0026] Compared with the prior art, the beneficial effects of the present invention are: (1) This invention, through the modification of polyamide polymers and fiber structures, and through a combined process of "adding functional masterbatch containing nano-silicone powder + secondary stretching precision control + micro-etching + polydopamine coating", can endow nylon fibers with dual functions of anti-pilling and anti-snagging. The products tested for anti-pilling and anti-snagging all reach level 4 or above, demonstrating excellent anti-pilling and anti-snagging performance. This invention also solves the problems that may occur when adding functional agents and coatings to nylon fibers, such as fiber embrittlement, reduced mechanical properties, poor air permeability, and deterioration of fabric hand feel, achieving a balance between fabric hand feel and various properties.
[0027] (2) This invention can prepare products with different specifications and functions according to needs, covering FDY / DTY: 20D-100D / 7-96F. The fine denier fibers have a fine total fineness, good strength, and low bending stiffness. After being woven into fabrics, they are transparent, soft, light, and thin, and the fabric surface is smooth and delicate with excellent drape. Application areas include, but are not limited to, clothing fabrics, bedding, socks, underwear, etc.
[0028] (3) The irregular cross-sectional design of the fiber in this invention enhances moisture absorption and breathability. Utilizing the capillary action generated by the micro-grooves on the fiber surface, moisture or sweat is rapidly transferred to the fabric surface and dispersed through wicking, diffusion, and transport, thus achieving the purpose of wicking away moisture and drying quickly. The fabric product is moisture-wicking and perspiration-absorbing, possessing excellent properties such as lightweight, moisture-wicking, quick-drying, coolness, comfort, easy washing, and wrinkle-free operation. The fabric has a soft and delicate feel, does not deform when worn, does not pill, and is resistant to snagging.
[0029] Instruction manual illustrations Figure 1 These are comparative photographs of pilling and fuzzing tests on the yarn fabric of this invention and ordinary nylon fabric (the right image shows ordinary nylon: the sample surface shows obvious pilling and fuzzing, with balls of different sizes and densities covering most of the sample surface; the left image shows the yarn of this invention: the sample surface shows no change, exhibiting better anti-pilling and fuzzing performance). Pilling and fuzzing test: 600 cycles of circular trajectory friction.
[0030] Figure 2 These are comparative photographs of the snag resistance tests of the yarn fabric of this invention and ordinary nylon fabric (the right image shows ordinary nylon: obvious surface snags, with snags of different densities covering most of the sample surface; the left image shows the yarn of this invention: no change on the sample surface, exhibiting better snag resistance, with ≥4 indicating good snag resistance). Snag resistance test: hammer test at 600 rpm. Detailed Implementation
[0031] The present invention will now be described in more detail with reference to the embodiments and accompanying drawings. It should be understood that the implementation of the present invention is not limited to the embodiments described below, and any modifications and / or alterations made to the present invention will fall within the scope of protection of the present invention.
[0032] In this invention, unless otherwise specified, all parts and percentages are by weight, and all equipment and raw materials are commercially available or commonly used in the industry. Unless otherwise specified, the methods used in the embodiments are general techniques in the art.
[0033] Description of main reagents in the examples: Dispersant: Model DYD-9812, Shanghai Deyude Trading Co., Ltd. Nano silicone powder, Guangzhou Weber Technology Co., Ltd., with an average volume diameter (D43) of 10-20 μm, active ingredient content ≥99%, and organosilicon content ≥71%.
[0034] The dopamine Tris buffer in the examples is prepared and used immediately. Taking the preparation of 100 mL of dopamine Tris buffer with a concentration of 2 g / L as an example, the specific operation is as follows: First, prepare the buffer solution: Prepare a Tris-HCl buffer solution with a pH of 8.5 using Tris base and dilute hydrochloric acid; then add dopamine: Weigh 200 mg of dopamine hydrochloride, dissolve it in 100 mL of the above buffer solution, stir well, and use immediately.
[0035] Important: Adjust the pH level before adding dopamine. If you dissolve dopamine in water first and then add Tris to adjust the pH, the dopamine will begin to polymerize prematurely during the pH adjustment process, causing the solution to turn black and the coating effect to deteriorate.
[0036] Example 1 An anti-pilling and anti-snagging nylon fiber is prepared according to the following steps: (1) Raw material preparation and drying Nylon 6 chips were vacuum dried at 90℃ for 6 hours before use, with the moisture content controlled below 0.05%. (2) Preparation of functional masterbatch A functional masterbatch was prepared by melt-blending 5 wt.% nano-silicone powder, 1.5 wt.% dispersant, and 93.5 wt.% nylon 6 chips at approximately 220°C and then extruding and granulating the resulting mixture. (3) Melt spinning 6% of the functional masterbatch, based on the mass of nylon 6 chips, is melt-blended with nylon 6 chips at a temperature of 230-240℃ to obtain a spinning melt. The spinning melt then undergoes melt spinning, cooling and solidification, primary oiling, post-drawing treatment, heat setting, secondary oiling, and winding to produce nylon FDY filaments. The spinning assembly uses cross-shaped spinnerets; the cooling air temperature for cooling and solidification is 20℃, and the air velocity is approximately 0.6 m / s; the melt spinning is precisely controlled through two stages of staged drawing: the first stage draw ratio is 1.08, and the second stage draw ratio is 1.25; the first hot roller temperature is 65℃, the second hot roller temperature is 140℃, the winding speed is approximately 4500 m / min, and the overfeed rate is approximately 3.5%. (4) Post-processing The surface of nylon fiber was micro-etched with a 15% formic acid solution for 10 minutes, washed with deionized water and dried. Then, the nylon FDY filament was immersed in a dopamine Tris buffer solution with a concentration of 2 g / L and a pH of 8.5 and allowed to stand at room temperature for 15 hours to form a polydopamine coating on the surface of the nylon fiber with a thickness of about 50 nm. After removal, it was washed with deionized water and dried to obtain a finished nylon FDY filament with anti-pilling and anti-snagging properties.
[0037] The obtained modified nylon FDY filaments were subjected to various performance tests according to the standard specifications, and the test results are shown in Table 1.
[0038] Example 2 An anti-pilling and anti-snagging nylon fiber is prepared according to the following steps: (1) Raw material preparation and drying Nylon 6 chips were vacuum dried at 85℃ for 8 hours before use, with the moisture content controlled below 0.05%. (2) Preparation of functional masterbatch A functional masterbatch was prepared by melt-blending 3 wt.% nano-silicone powder, 0.5 wt.% dispersant, and 96.5 wt.% nylon chips at approximately 210°C and then extruding and granulating the resulting mixture. (3) Melt spinning 10% of the functional masterbatch, based on the mass of nylon 6 chips, is melt-blended with nylon 6 chips at 260-270℃ to obtain a spinning melt. The melt is then spun, cooled, cured, oiled, and wound to produce POY precursor yarn. The POY precursor yarn is then placed on a texturing machine and sequentially undergoes two-stage drawing, heat deformation (false twisting), heat setting, cooling, oiling, and winding to finally produce nylon DTY filament. The spinning assembly uses cross-shaped spinnerets. The cooling air temperature for curing is 10℃, and the air velocity is approximately 0.3 m / s. The two-stage drawing has a total draw ratio of 1.15, a first-stage draw ratio of 1.05, and a second-stage draw ratio of approximately 1.1. The heat deformation chamber temperature is 165℃, the heat setting chamber temperature is 180℃, the D / Y ratio is 1.8, and the processing speed is 700 m / min. (4) Post-processing The surface of nylon fiber was micro-etched with a 10% formic acid solution for 15 minutes, washed with deionized water and dried. Then, the nylon filament was immersed in a dopamine Tris buffer solution with a concentration of 1 g / L and a pH of 8.5 and allowed to react at room temperature for 18 hours to deposit a polydopamine coating on the surface of the nylon fiber. The polydopamine coating was about 40 nm thick. After removal, it was washed with deionized water and dried to obtain a finished nylon DTY filament with anti-pilling and anti-snagging properties.
[0039] The obtained modified nylon DTY filaments were subjected to various performance tests according to the standard specifications, and the test results are shown in Table 1.
[0040] Example 3 An anti-pilling and anti-snagging nylon fiber is prepared according to the following steps: (1) Raw material preparation and drying Nylon 6 chips were vacuum dried at 100℃ for 6 hours before use, with the moisture content controlled below 0.05%. (2) Preparation of functional masterbatch A functional masterbatch was prepared by melt-blending 8 wt.% nano-silicone powder, 3 wt.% dispersant, and 89 wt.% nylon 6 chips at approximately 230°C and then extruding and granulating the resulting mixture. (3) Melt spinning 3% of the functional masterbatch, based on the mass of nylon 6 chips, is melt-blended with nylon 6 chips at a temperature of 260-270℃ to obtain a spinning melt. The spinning melt then undergoes melt spinning, cooling and solidification, primary oiling, post-drawing treatment, heat setting, secondary oiling, and winding to produce nylon FDY filaments. The spinning assembly uses cross-shaped spinnerets; the cooling air temperature for cooling and solidification is 15℃, and the air velocity is approximately 0.4 m / s; melt spinning is precisely controlled through two stages of graded drawing: the first stage draw ratio is 1.10, and the second stage draw ratio is 1.25; the first hot roller temperature is 70℃, the second hot roller temperature is 150℃, the winding speed is approximately 4600 m / min, and the overfeed rate is approximately 3.3%. (4) Post-processing The surface of nylon fiber was micro-etched with a 12% formic acid solution for 20 minutes, washed with deionized water and dried. Then, the nylon FDY filament was immersed in a dopamine Tris buffer solution with a concentration of 3 g / L and a pH of 8.5 and allowed to stand at room temperature for 12 hours to form a polydopamine coating on the surface of the nylon fiber with a thickness of about 45 nm. After removal, it was washed with deionized water and dried to obtain a finished nylon FDY filament with anti-pilling and anti-snagging properties.
[0041] The obtained modified nylon FDY filaments were subjected to various performance tests according to the standard specifications, and the test results are shown in Table 1.
[0042] Comparative Example 1 (Conventional Process) A nylon FDY filament is prepared according to the following steps: (1) Raw material preparation and drying Nylon 6 chips were vacuum dried at 90℃ for 6 hours before use, with the moisture content controlled below 0.05%. (2) Melt spinning 0.1% of a dispersant based on the mass of nylon 6 chips was melt-blended with nylon 6 chips at a temperature of 230-240℃ to obtain a spinning melt. The spinning melt then underwent melt spinning, cooling and solidification, primary oiling, post-drawing treatment, heat setting, secondary oiling, and winding to produce nylon FDY filaments. The spinning assembly used cross-shaped spinnerets; the cooling air temperature for cooling and solidification was 20℃, and the air velocity was approximately 0.6 m / s; the draw ratio for melt spinning was 1.25; the temperature of the first hot roller was 65℃, the temperature of the second hot roller was 140℃, the winding speed was approximately 4500 m / min, and the overfeed rate was approximately 3.5%. The obtained nylon FDY filaments were subjected to various performance tests according to the standard specifications, and the test results are shown in Table 1.
[0043] Comparative Example 2 An anti-pilling and anti-snagging nylon fiber is prepared according to the following steps: (1) Raw material preparation and drying Nylon 6 chips were vacuum dried at 90℃ for 6 hours before use, with the moisture content controlled below 0.05%. (2) Preparation of functional masterbatch A functional masterbatch was prepared by melt-blending 5 wt.% nano-silicone powder, 1.5 wt.% dispersant, and 93.5 wt.% nylon 6 chips at approximately 220°C and then extruding and granulating the resulting mixture. (3) Melt spinning 6% of the functional masterbatch, based on the mass of nylon 6 chips, is melt-blended with nylon 6 chips at a temperature of 230-240℃ to obtain a spinning melt. The spinning melt then undergoes melt spinning, cooling and solidification, primary oiling, post-drawing treatment, heat setting, secondary oiling, and winding to produce nylon FDY filaments. The spinning assembly uses cross-shaped spinnerets; the cooling air temperature for cooling and solidification is 20℃, and the air velocity is approximately 0.6 m / s; the melt spinning is precisely controlled through two stages of staged drawing: the first stage draw ratio is 1.08, and the second stage draw ratio is 1.25; the first hot roller temperature is 65℃, the second hot roller temperature is 140℃, the winding speed is approximately 4500 m / min, and the overfeed rate is approximately 3.5%. The obtained nylon FDY filaments were subjected to various performance tests according to the standard specifications, and the test results are shown in Table 1.
[0044] Comparative Example 3 Everything else is the same as in Example 1, except for (4) post-processing: Nylon FDY filaments were immersed in a dopamine Tris buffer solution with a concentration of 2 g / L and a pH of 8.5, and allowed to stand at room temperature for 48 hours to form a polydopamine coating on the surface of the nylon fiber with a thickness of about 45 nm. After removal, the nylon FDY filaments were washed with deionized water and dried to obtain a finished nylon FDY filament product with anti-pilling and anti-snagging properties.
[0045] The obtained nylon FDY filaments were subjected to various performance tests according to the standard specifications, and the test results are shown in Table 1.
[0046] Performance testing The tensile strength of the fibers was tested according to GB / T 14344-2008 "Test Method for Tensile Properties of Chemical Fiber Filaments"; the moisture regain of the fibers was tested according to GB / T 6503-2017 "Test Method for Moisture Regain of Chemical Fibers"; the pilling performance was tested according to Chinese National Standard GB / T 4802.1-2008 "Determination of Pilling and Spilling Properties of Textile Fabrics - Part 1: Circular Track Method"; and the snagging performance was tested according to Chinese National Standard GB / T 11047-2008 "Evaluation of Snagging Performance of Textile Fabrics - Hammer Method". The test results are shown in Table 1.
[0047] As shown in Table 1, this invention, by adding functional masterbatch containing nano-silicone powder to modify the polyamide polymer and fiber structure, combined with an optimized "two-stage drafting control + micro-etching + polydopamine coating" process, can endow nylon fibers with dual functions of anti-pilling and anti-snagging. Products tested for both anti-pilling and anti-snagging properties all reached level 4 or higher, demonstrating excellent anti-pilling and anti-snagging performance. Compared with conventional processes, the anti-pilling and anti-snagging performance of this invention can be improved by at least two levels or more, achieving a significant improvement. Adding only nano-silicone powder and using a two-stage drafting process significantly improves anti-pilling and anti-snagging performance, but it falls far short of excellent levels. Post-treatment only involves coating without surface roughening, resulting in a slight advantage in mechanical properties, but a decrease in anti-pilling and anti-snagging performance by one level, especially significantly affecting anti-snagging performance.
Claims
1. An anti-pilling, anti-snagging, nylon fiber characterized in that, The nylon fiber is produced by melt spinning nylon chips with 3%-10% functional masterbatch based on the mass of nylon chips to obtain nylon filaments, and then by post-treatment to attach a polydopamine coating to the surface of the nylon fiber. The functional masterbatch contains 3%-8% nano silicone powder; the thickness of the polydopamine coating is between 40-50 nm.
2. A process for the production of anti-pilling, anti-snagging, polyamide fibers characterized in that, Includes the following steps: (1) Raw material preparation and drying Nylon chips are used after vacuum drying, with the moisture content controlled below 0.05%. (2) Preparation of functional masterbatch The functional masterbatch is prepared by melt-blending and extruding granulation of 3-8% by weight of nano-silicone powder, 0.5-3% by weight of dispersant, and the balance of nylon chips at a temperature of 210-230℃. (3) Melt spinning Functional masterbatch, at a rate of 3%-10% by weight of nylon chips, is melt-blended with nylon chips to obtain a spinning melt. The spinning melt then undergoes melt spinning, cooling and solidification, primary oiling, post-drawing treatment, heat setting, secondary oiling, and winding to produce nylon FDY filament. The melt spinning process is precisely controlled through two stages of staged drawing. Key process parameters include: primary draw ratio 1.05-1.15, secondary draw ratio 1.25-1.30, first hot roller temperature 65-70℃, second hot roller temperature 140-150℃, winding speed 4500-4600 m / min, and overfeed rate 3-4%; or The spinning melt is melt-spun, then cooled and solidified, oiled, and wound to obtain POY precursor yarn. The POY precursor yarn is then placed on a texturing machine and sequentially undergoes two-stage drawing, heat deformation (false twisting), heat setting, cooling, oiling, and winding to finally produce nylon DTY filament. Specifically, the two-stage drawing has a total draw ratio between 1.15 and 1.30, and the first-stage draw ratio is between 1.05 and 1.
15. The heat deformation chamber temperature is 160-185℃, the heat setting chamber temperature is 175-195℃, the D / Y ratio is 1.7-1.85, and the processing speed is 650-750 m / min. (4) Post-processing The surface of nylon fiber is micro-etched with formic acid solution, washed and dried, and then the nylon filament is immersed in dopamine Tris buffer solution and allowed to react at room temperature for 12-18 hours to deposit a polydopamine coating on the surface of the nylon fiber. After removal, it is washed and dried to obtain a finished nylon filament with anti-pilling and anti-snagging properties.
3. A process for the production of anti-pilling anti-snagging nylon fibre as claimed in claim 2, wherein the process is carried out by using a mixture of 2% to 4% of the said polymeric additive and 96% to 98% of the said nylon fibre. In step (1), the vacuum drying temperature is 85-100℃ and the time is 6-8h.
4. A process for the production of anti-pilling and anti-snagging polyamide fibre as claimed in claim 2, wherein the process is characterized by, In step (2), the volume average diameter D43 of the nano silicone powder is 10-20 μm, the active ingredient content is ≥ 99%, and the organosilicon content is ≥ 71%.
5. The method for preparing anti-pilling and anti-snagging nylon fiber according to claim 2, characterized in that, In step (3) mentioned above: The spinning assembly uses irregularly shaped spinnerets; The melting temperature of nylon is 230℃~270℃; The cooling air temperature for cooling and solidification is 10–20℃, and the air velocity is approximately 0.3–0.6 m / s.
6. The method for preparing anti-pilling and anti-snagging nylon fiber according to claim 2, characterized in that, In step (4), formic acid with a concentration of 10-15% is used, and the micro-etching process takes 10-20 minutes.
7. The method for preparing anti-pilling and anti-snagging nylon fiber according to claim 2, characterized in that, In step (4), a dopamine Tris buffer solution with a concentration of 1-3 g / L and a pH of 8.5 is used.