A method for producing high-strength zirconia crystal fibers by high-temperature pressure decomposition

The high-temperature pressure analysis method for preparing zirconia crystal fibers solves the problems of pores and abnormal grain growth caused by densification in traditional methods, and realizes high-strength and high-density zirconia crystal fibers, which are suitable for high-temperature insulation, composite materials and high-temperature filtration materials.

CN123153191APending Publication Date: 2026-11-24SHANDONG LIANGJI TEMPERATURE DOMAIN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611510380.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously achieve high density and fine grain structure in zirconia crystal fibers, resulting in insufficient fiber strength.

Method used

The high-temperature pressure analysis method involves placing zirconium-containing precursor fibers in a pressure vessel and applying a gas pressure of 0.5 to 10 MPa under an oxygen-containing atmosphere for segmented heating treatment, including the thermal decomposition of organic matter and densification crystallization stages. The grain size and density are controlled by utilizing the pressure analysis effect and the densification sintering process.

Benefits of technology

High-density, fine-grained zirconia crystal fibers can be obtained, with a relative density of over 98%, a grain size in the nanometer range, and a tensile strength increase of 1 to 2 times. They are suitable for high-temperature insulation, composite material reinforcement, and high-temperature filtration materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153191A_ABST
    Figure CN123153191A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of high-performance fiber preparation technology, specifically relating to a method for preparing high-strength zirconia crystal fibers through high-temperature pressure desorption. The method involves placing zirconia-containing precursor fibers in a pressure vessel, applying a gas pressure of 0.5–10 MPa in an oxygen-containing atmosphere, and performing segmented heating treatment. First, the temperature is raised to 200–600 °C at a first heating rate of 0.5–5 °C / min to complete the thermal decomposition of organic matter within the fiber. The thermally decomposed gas exhibits a desorption hysteresis effect under pressure. Then, the temperature is raised to 1000–1400 °C at a second heating rate of 1–10 °C / min for densification crystallization, with a holding time of 30–180 min. The container can be evacuated to below 10 Pa before heat treatment. This invention can suppress fiber defects caused by violent gas escape, lower the densification temperature, inhibit grain growth, and achieve a relative density of over 98% in the resulting fibers. The crystals are tetragonal and / or cubic phases, resulting in significantly improved mechanical properties, making it suitable for high-temperature insulation, composite material reinforcement, and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-performance fiber preparation technology, specifically relating to a method for preparing high-strength zirconia crystal fibers by high-temperature pressure analysis. Background Technology

[0002] Zirconia crystal fibers have broad application prospects in aerospace, high-temperature insulation and composite material reinforcement due to their excellent high-temperature stability, corrosion resistance and chemical inertness.

[0003] Traditional methods for preparing high-strength zirconia crystalline fibers typically employ a sol-gel combined with high-temperature calcination process. In this process, when the zirconium-containing precursor fibers are heat-treated at ambient pressure and high temperature, their internal organic components decompose violently, releasing a large amount of gas. This violent gas escape process easily forms penetrating pores and microcracks within the fiber, leading to decreased fiber density and increased internal defects. Simultaneously, to achieve sufficient densification, high sintering temperatures (typically above 1500℃) and long holding times are often required, which in turn promotes abnormal growth of zirconia grains, forming a coarse grain structure. The pores, cracks, and coarse grain structure within the fiber are all key factors contributing to the decline in its mechanical properties (especially tensile strength).

[0004] Therefore, existing technologies cannot simultaneously achieve high fiber density and fine grain structure, thus failing to obtain high-strength, high-integrity zirconia crystal fibers. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing high-strength zirconia crystal fibers through high-temperature pressure analysis. This method aims to solve the technical problems in the prior art, such as defects caused by the violent release of gas inside the fiber due to normal pressure high-temperature treatment, and abnormal grain growth during high-temperature densification, which makes it impossible to achieve both high density and fine grain structure, ultimately resulting in insufficient fiber strength. This invention achieves the technical effect of simultaneously obtaining zirconia crystal fibers with high density, fine grains, and high strength.

[0006] The technical solution of this invention is: A method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption involves placing zirconium-containing precursor fibers in a pressure vessel, applying a gas pressure of 0.5 to 10 MPa in an oxygen-containing atmosphere, and performing segmented heating treatment to transform the zirconium-containing precursor fibers into high-strength zirconia crystal fibers through high-temperature pressure desorption. The segmented heating process includes: heating to a first temperature range at a first heating rate to thermally decompose the organic matter within the fiber, and the gas generated by the thermal decomposition forming a desorption hysteresis effect under the action of applied gas pressure; and then heating to a second temperature range at a second heating rate to densify and crystallize.

[0007] Preferably, the gas pressure is 2 to 8 MPa.

[0008] Preferably, the gas pressure is 4 to 6 MPa.

[0009] Preferably, the first heating rate is 0.5~5 ℃ / min, and the first temperature range is 200~600℃; the second heating rate is 1~10 ℃ / min, and the second temperature range is 1000~1400 ℃.

[0010] Preferably, the oxygen-containing atmosphere is an air atmosphere or a mixture of oxygen and an inert gas.

[0011] Preferably, the temperature is kept warm within the second temperature range for 30 to 180 minutes.

[0012] Preferably, before performing the segmented heating process, the pressure vessel is further subjected to a vacuuming process.

[0013] Preferably, the vacuum level in the vacuuming process is below 10 Pa.

[0014] Preferably, the zirconium-containing precursor fiber is a wet-spun fiber or a solution-impregnated fiber containing zirconium and organic components. The organic components in the zirconium-containing precursor fiber include at least a polymer as a structural agent and / or an organic ligand as a zirconium source support.

[0015] As a preferred option, the high-strength zirconia crystal fibers after densification crystallization treatment can reach a relative density of over 98%, and the crystal structure is tetragonal and / or cubic.

[0016] The core mechanism of this invention is as follows: This invention utilizes external pressure at high temperatures to transform the thermal decomposition process of organic components in zirconium-containing precursor fibers from "violent release at atmospheric pressure" to "pressure-assisted slow release and desorption." In a sealed or pressure-controlled container, high temperature and a predetermined pressure (typically 0.5~10 MPa, in an air or oxygen-containing atmosphere) are simultaneously applied to the zirconium-containing precursor fibers. During the heating process, the organic components inside the fibers decompose to produce gas. However, because the ambient pressure is higher than atmospheric pressure, the driving force for gas nucleation and escape is significantly weakened, creating a desorption hysteresis effect. The decomposed gas is temporarily retained within the precursor matrix in molecular form or in the form of microbubbles, preventing the fibers from developing cracks or through-holes due to violent foaming.

[0017] As the temperature continues to rise and the holding period begins, driven by sustained external pressure and molecular thermal motion, the precursor matrix undergoes viscous flow and plastic deformation. The dispersed supersaturated gases are gradually expelled through slow desorption and short-range diffusion, leaving tiny gaps that are immediately filled and healed by the pressure-assisted densification process. Simultaneously, the applied pressure significantly increases the material migration rate, enabling zirconia particles to achieve sufficient rearrangement and densification sintering at relatively low temperatures. This allows for the acquisition of a sintered body with near-theoretical density before significant grain growth occurs. By adjusting the pressure, heating rate, and holding time, grain boundary migration behavior can be precisely controlled, stably maintaining the tetragonal / cubic zirconia grain size at the nanometer level (typically below 100 nm).

[0018] In summary, this invention integrates "pressure degassing" and "pressure-assisted densification sintering" into a single thermal process, significantly reducing gas discharge defects, lowering the densification temperature, and effectively suppressing grain growth. This ultimately yields high-strength zirconia crystal fibers that possess high density, fine-grained structure, and continuous long fiber morphology. It solves the problems of numerous pores, large grains, and low strength found in existing technologies, while also eliminating the need for sintering aids and maintaining the excellent intrinsic temperature resistance of zirconia.

[0019] The beneficial effects of this invention are as follows: In this invention, during the heating process of the zirconium-containing precursor fiber, the internal solvent and organic additives tend to decompose and volatilize. Upon application of gas pressure, these low-molecular-weight substances are forced into a condensed state or a high-pressure gas dense phase, and are transported from the fiber interior to the surface via molecular diffusion driven by the concentration gradient, and carried away by the gas flow. This process completely avoids the tearing effect on the fiber matrix caused by violent boiling of liquids or instantaneous expansion of gases under normal pressure. Simultaneously, isotropic isostatic pressure continuously acts on the fiber wall, eliminating tensile stress and microcracks caused by volume shrinkage in real time, promoting particle rearrangement and plastic densification. Therefore, the final fiber's relative density can reach over 98%, with an extremely low defect density.

[0020] In this invention, high pressure during the densification process effectively reduces the diffusion coefficient of materials at grain boundaries and surfaces, increasing the activation energy required for grain coarsening and thus strongly inhibiting the growth of zirconia nuclei. This high-pressure densification allows the fibers to form a uniform and dense precursor state before significant grain growth occurs, greatly weakening the driving force for grain growth and enabling the final zirconia fiber grain size to be controlled within 50~200 nm. According to the Hall-Page relation, the nanoscale fine grains endow the fibers with extremely high intrinsic strength, with tensile strength stably reaching 1.5~2.5 GPa, which is 1~2 times higher than that of existing atmospheric pressure calcined fibers.

[0021] In summary, the high-temperature pressure analysis-assisted preparation method provided by this invention fundamentally breaks the contradiction between the traditional method of achieving density through atmospheric pressure calcination and the inherent tendency for growth at low temperatures to result in porous structures. It produces zirconia crystal fibers with high density, fine grains, and high strength using a simple and efficient method, demonstrating outstanding technical effects and promising prospects for industrial applications. Attached Figure Description

[0022] Figure 1 This is a schematic diagram of the method flow of the present invention. Detailed Implementation

[0023] The present invention will be further described below through specific embodiments, but this is not a limitation of the present invention. Those skilled in the art can make various modifications or improvements based on the basic idea of ​​the present invention, but as long as they do not depart from the basic idea of ​​the present invention, they are all within the protection scope of the present invention.

[0024] Figure 1 A method for preparing high-strength zirconia crystal fibers via high-temperature pressure analysis is presented. The precursor fibers are placed in the isothermal zone of a high-temperature atmosphere furnace with pressure control capabilities, and the reaction chamber is sealed. Depending on process requirements, the pressure vessel can be pre-treated by vacuuming, with the vacuum level controlled below 10 Pa to remove residual impurities and provide a clean initial environment for subsequent atmosphere control. After vacuuming, an oxygen-containing atmosphere is introduced, which can be air or a mixture of oxygen and inert gas. When using a mixed atmosphere, the oxygen partial pressure within the furnace can be precisely controlled by adjusting the ratio of oxygen to inert gas, thereby regulating the final zirconia crystal phase composition. After the atmosphere stabilizes, the gas pressure within the system is adjusted to the target range of 0.5–10 MPa. This pressure range is the basic pressure range defined in the claims, balancing equipment cost, operational safety, and process effectiveness. Pressures below 0.5 MPa have limited effect on inhibiting gas escape and promoting densification, while pressures above 10 MPa drastically increase the pressure resistance and sealing requirements of the equipment, leading to a decrease in economic efficiency. Based on performance requirements, a pressure range of 2 to 8 MPa can be further optimized within the basic range. This range can stably suppress the violent decomposition of organic components in the precursor, while significantly promoting the migration and volume diffusion of zirconia grain boundaries, so that the densification process can be completed efficiently before grain growth becomes dominant. For scenarios with higher performance requirements, the pressure range of 4 to 6 MPa can be further optimized to maximize the synergistic effect of pressure desorption and densification.

[0025] After pressure regulation, a segmented heating program is initiated. The entire heating process is divided into two continuous stages, strictly following the heating logic defined in the claims. The first stage involves heating from room temperature to a first temperature range of 200-600℃ at a first heating rate of 0.5-5℃ / min, within which the thermal decomposition of organic matter within the fiber is completed. During the heating process, the organic components inside the precursor gradually decompose to produce gas. Due to the higher ambient pressure than normal pressure, the driving force for gas nucleation and escape is significantly weakened, resulting in a desorption lag effect. The decomposed gas is temporarily retained within the precursor matrix in molecular or microbubble form, preventing cracks or through-holes caused by vigorous foaming. To make the thermal decomposition process smoother and reduce thermal stress accumulation, a more optimal heating rate of 0.5-3℃ / min can be further selected within the range of 0.5-5℃ / min. The slower heating rate provides sufficient reaction time for the organic components, allowing the decomposed gas enough time to complete desorption and diffusion under the pressure field, avoiding a concentrated burst of decomposition reaction due to a rapid temperature increase.

[0026] After the organic matter has undergone sufficient thermal decomposition, the second stage of heating begins. The temperature is increased from the first temperature range to a second temperature range of 1000–1400 °C at a second heating rate of 1–10 °C / min, where densification crystallization occurs. Upon entering the second temperature range, a holding treatment is performed while maintaining the target gas pressure for 30–180 min. During this holding stage, the continuous external pressure and molecular thermal motion jointly drive the precursor matrix to undergo viscous flow and plastic deformation. The previously dispersed supersaturated gas is gradually expelled through slow desorption and short-range diffusion, and the remaining micro-gaps are immediately filled and healed by the pressure-assisted sintering densification process. Simultaneously, the applied pressure significantly increases the material migration rate, allowing zirconia particles to achieve sufficient rearrangement and densification sintering at relatively low temperatures, resulting in a sintered body with near-theoretical density before significant grain growth occurs. To further optimize the balance between grain size and density, an optimal holding temperature of 1200-1400 ℃ can be selected within the range of 1000-1400 ℃, and a holding treatment of corresponding duration can be used to precisely control the final grain size and the degree of sintering neck growth.

[0027] After the heat treatment is completed, the system is cooled to room temperature in the furnace, then the pressure is released and the product is removed, yielding high-strength zirconia crystal fibers. Throughout the heat treatment process, the presence of pressure deeply couples the three processes of thermal decomposition, gas desorption, and densification crystallization in time and space, allowing them to work synergistically.

[0028] The high-strength zirconia crystal fibers prepared by the above process have a relative density of over 98% and a tetragonal and / or cubic crystal structure. These high-strength zirconia crystal fibers can be used in high-temperature insulation materials, as reinforcing phases in composite materials, or in high-temperature filtration materials. Based on their excellent high-temperature resistance, high strength, and low defect rate, they can maintain stable operation for extended periods in extreme environments.

[0029] The core of this invention lies in placing the zirconium-containing precursor fiber in a pressure-controlled device, applying a pressure of 0.5-15 MPa under an oxygen-containing atmosphere, and performing heat treatment. This allows the zirconium-containing precursor fiber to simultaneously undergo thermal decomposition, gas desorption, and densification crystallization to obtain zirconium oxide crystal fiber. The heat treatment includes a heating stage and a holding stage, with the heating rate not exceeding 5°C / min. Specifically, this method fundamentally alters the thermodynamics and kinetics of traditional atmospheric pressure heat treatment by introducing a controllable external pressure field (0.5-15 MPa). During the heating stage, this pressure effectively weakens the driving force for gas molecule nucleation and aggregation, forcing the decomposed gas to dissolve in the precursor matrix in a supersaturated state or form extremely small bubbles. This avoids fiber cracking and the formation of large pores caused by instantaneous gas volume expansion; this is the pressure desorption effect. During the heat preservation stage, the continuous external pressure not only promotes the further slow diffusion and discharge of residual gases, but more importantly, it significantly enhances the migration rate of materials (especially atoms or vacancies at grain boundaries), greatly reducing the activation energy required for the densification sintering of zirconia particles. This allows the fibers to reach a state close to the theoretical density at a relatively low temperature and in a shorter time, while the grains have not yet had sufficient time and kinetic conditions to undergo significant Ostwald ripening and grow, thus achieving the simultaneous attainment of fine grains and high density.

[0030] The present invention will be further described in detail below through several specific embodiments: Example 1: This example uses zirconium-containing precursor fibers prepared by wet spinning, with air as the reaction atmosphere, no vacuum pretreatment, and basic pressure parameters.

[0031] In the precursor preparation stage, zirconium oxychloride aqueous solution and 10% polyvinyl alcohol aqueous solution by mass are mixed at a volume ratio of 4:1. After stirring evenly, the mixture is filtered, degassed under vacuum, and extruded through a spinneret with a pore size of 20 μm into an ethanol coagulation bath to form a continuous zirconium-containing precursor fiber with a fiber diameter of about 15 μm. The organic component is polyvinyl alcohol as a structural agent.

[0032] In the process, precursor fibers are arranged on a sample holder and placed in a high-temperature tube furnace with pressure control. After sealing the chamber, air is directly introduced. Once the atmosphere is replaced, the system pressure is adjusted to 0.5 MPa. A segmented heating program is then initiated. In the first stage, the temperature is increased to 400 °C at a first heating rate of 2 °C / min. At this temperature, the organic matter undergoes thermal decomposition, utilizing pressure to create a desorption hysteresis effect. Subsequently, the temperature is increased to a second temperature range of 1200 °C at a second heating rate of 3 °C / min. This temperature is then held for 90 min to allow for densification and crystallization. After the holding period, the furnace is cooled to room temperature, and the fibers are removed after depressurization.

[0033] Performance characterization results showed that the relative density of the fiber was 98.2% as determined by the Archimedes displacement method, X-ray diffraction analysis showed that the crystal structure was a pure tetragonal phase, the average grain size was calculated to be about 95 nm using the Scherrer formula, and the tensile strength of the single filament was about 1.6 GPa as measured by the tensile test.

[0034] Example 2: In this example, zirconium-containing precursor fibers prepared by solution impregnation were subjected to vacuum pretreatment using a mixed atmosphere of oxygen and argon as the reaction atmosphere and medium pressure parameters.

[0035] In the precursor preparation stage, the porous alumina fiber template was immersed in a 0.5 mol / L zirconium propoxide ethanol solution for 30 min, then removed and dried at 80 °C. The immersion-drying process was repeated 3 times to obtain the fiber loaded with zirconium precursor. The organic component was the propoxide ligand serving as the zirconium source support.

[0036] In the process, precursor fibers are arranged on a sample holder and placed in a hot isostatic pressing furnace. After sealing the cavity, a vacuum is applied, controlling the vacuum level at 8 Pa. After vacuuming, a mixture of oxygen and argon is introduced, with oxygen accounting for 20% of the volume, and the system pressure is adjusted to 2 MPa. A segmented heating program is initiated. In the first stage, the temperature is increased to 300 °C at a first heating rate of 1 °C / min to complete the thermal decomposition and desorption lag process of organic matter. Subsequently, the temperature is increased to a second temperature range of 1300 °C at a second heating rate of 2 °C / min, and held at this temperature for 60 min for densification and crystallization. After holding at this temperature, the furnace is cooled to room temperature, and the fibers are removed after depressurization.

[0037] Performance characterization results show that the fiber has a relative density of 98.5%, a crystal structure in which tetragonal phase and a small amount of cubic phase coexist, an average grain size of about 75 nm, and a tensile strength of about 1.8 GPa.

[0038] Example 3: In this example, zirconium-containing precursor fibers prepared by wet spinning were pretreated under vacuum with air as the reaction atmosphere and medium-high pressure parameters were selected.

[0039] In the precursor preparation stage, zirconium oxychloride aqueous solution and 12% polyvinyl alcohol aqueous solution were mixed at a volume ratio of 3:1. A small amount of citric acid was added as an organic ligand. After stirring evenly, the mixture was filtered and degassed. The resulting zirconium-containing precursor fiber was obtained by wet spinning and drying. The organic components included polyvinyl alcohol as a structural agent and citric acid ligand as a zirconium source carrier.

[0040] In the process, precursor fibers are arranged on a sample holder and placed in a high-temperature tube furnace with pressure control. After sealing the chamber, a vacuum is applied, controlling the vacuum level at 5 Pa. After vacuuming, air is introduced, and the system pressure is adjusted to 4 MPa. A segmented heating program is initiated. In the first stage, the temperature is increased to 500 °C at a first heating rate of 1.5 °C / min to fully complete the thermal decomposition of organic matter, with the decomposition gases slowly released under pressure. Subsequently, the temperature is increased to a second temperature range of 1350 °C at a second heating rate of 5 °C / min, and held at this temperature for 120 min for densification and crystallization. After holding at this temperature, the furnace is cooled to room temperature, and the fibers are removed after depressurization.

[0041] Performance characterization results show that the fiber has a relative density of 98.8%, a crystal structure dominated by tetragonal phase with trace amounts of cubic phase, an average grain size of about 60 nm, and a tensile strength of about 2.1 GPa.

[0042] Example 4: In this example, composite precursor fibers prepared by wet spinning are used. Vacuum pretreatment is performed using a mixed atmosphere of oxygen and argon as the reaction atmosphere, and high pressure is used to optimize the parameters.

[0043] In the precursor preparation stage, zirconium acetylacetonate is dissolved in N,N-dimethylformamide to prepare a solution with a concentration of 0.8 mol / L. Polyacrylonitrile is then added as a structural agent. After stirring and dissolving, a spinning solution is obtained. After filtration and degassing, wet spinning is performed and the solution is dried to obtain zirconium-containing precursor fibers. The organic components include polyacrylonitrile as a structural agent and acetylacetonate ligand as a zirconium source carrier.

[0044] In the process, precursor fibers are arranged on a sample holder and placed in a hot isostatic pressing furnace. After sealing the cavity, a vacuum is applied, controlling the vacuum level at 3 Pa. After vacuuming, a mixture of oxygen and argon is introduced, with oxygen comprising 30% of the volume, and the system pressure is adjusted to 6 MPa. A segmented heating program is initiated. In the first stage, the temperature is increased to 550 °C at a first heating rate of 1 °C / min to complete the cyclization oxidation of polyacrylonitrile and the decomposition of organic ligands. Under pressure, the gas exhibits a desorption hysteresis effect. Subsequently, the temperature is increased to a second temperature range of 1300 °C at a second heating rate of 4 °C / min, and held at this temperature for 150 min for densification and crystallization. After holding at this temperature, the furnace is cooled to room temperature, and the fibers are removed after depressurization.

[0045] Performance characterization results show that the fiber has a relative density of 99.1%, a crystal structure in which tetragonal and cubic phases coexist, an average grain size of about 50 nm, and a tensile strength of about 2.3 GPa.

[0046] Example 5: This example uses zirconium-containing precursor fibers prepared by solution impregnation, with air as the reaction atmosphere, no vacuum pretreatment, and medium-high pressure parameters.

[0047] In the precursor preparation stage, the carbon fiber template was immersed in a 1.0 mol / L zirconium oxychloride aqueous solution for 20 min, then removed and dried at 100 °C. The immersion-drying process was repeated 4 times to obtain fibers loaded with zirconium precursors. The organic components consisted of the carbonaceous components of the carbon fiber itself and a small amount of adsorbed hydrolysis products.

[0048] During the process, precursor fibers are arranged on a sample holder and placed in a high-temperature tube furnace with pressure control. After sealing the chamber, air is directly introduced. Once the atmosphere is replaced, the system pressure is adjusted to 8 MPa. A segmented heating program is then initiated. In the first stage, the temperature is increased to 600 °C at a first heating rate of 3 °C / min to complete the thermal decomposition of the organic components on the carbon fiber surface and the zirconium precursor. Subsequently, the temperature is increased to a second temperature range of 1400 °C at a second heating rate of 8 °C / min, and held at this temperature for 30 min for densification and crystallization. After the holding period, the furnace is cooled to room temperature, and the fibers are removed after depressurization.

[0049] Performance characterization results show that the fiber has a relative density of 98.3%, a predominantly cubic crystal structure, an average grain size of approximately 85 nm, and a tensile strength of approximately 1.7 GPa.

[0050] Example 6: In this example, composite precursor fibers prepared by wet spinning are used. Vacuum pretreatment is performed using a mixed atmosphere of oxygen and argon as the reaction atmosphere and high pressure limiting parameters are used.

[0051] In the precursor preparation stage, zirconium oxychloride and citric acid are mixed in a molar ratio of 1:2 to form an aqueous solution. Polyvinylpyrrolidone is then added as a structural agent. After stirring evenly, the mixture is filtered and degassed. The resulting zirconium-containing precursor fiber is obtained by wet spinning and drying. The organic components include polyvinylpyrrolidone as a structural agent and citric acid ligand as a zirconium source carrier.

[0052] In the process, precursor fibers are arranged on a sample holder and placed in a hot isostatic pressing furnace. After sealing the cavity, a vacuum is applied, controlling the vacuum level at 2 Pa. After vacuuming, a mixture of oxygen and argon is introduced, with oxygen comprising 25% by volume, and the system pressure is adjusted to 10 MPa. A segmented heating program is initiated. In the first stage, the temperature is increased to 200 °C at a first heating rate of 0.5 °C / min, slowly completing the thermal decomposition of the low-boiling-point components in the precursor. The gas desorption process is highly gradual under pressure. Subsequently, the temperature is increased to a second temperature range of 1100 °C at a second heating rate of 1 °C / min, and held at this temperature for 180 min for densification and crystallization. After holding at this temperature, the furnace is cooled to room temperature, and the fibers are removed after depressurization.

[0053] Performance characterization results show that the fiber has a relative density of 98.7%, a pure tetragonal crystal structure, an average grain size of about 40 nm, and a tensile strength of about 2.0 GPa.

[0054] This application also provides an application of the high-strength zirconia crystal fiber, used in high-temperature insulation materials, as a reinforcing phase in composite materials, or as a high-temperature filtration material. Based on its excellent high-temperature resistance (zirconia itself has a high melting point), high strength, and low defect rate, this fiber is ideally suited for extreme environments. As a high-temperature insulation material, its fine-grained structure helps reduce thermal conductivity; as a reinforcing phase in ceramic-based or metal-based composite materials, its high strength and toughness significantly improve the damage resistance of the composite material; as a high-temperature filtration material, its high purity and chemical stability ensure long-term operation in corrosive atmospheres. Through the above technical solutions, the product of this application has clear and broad application value in high-end industrial fields.

[0055] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption, characterized in that: The zirconium-containing precursor fiber is placed in a pressure vessel, and under an oxygen-containing atmosphere, a gas pressure of 0.5 to 10 MPa is applied, and a segmented heating process is performed to transform the zirconium-containing precursor fiber into high-strength zirconium oxide crystal fiber through high-temperature pressure desorption. The segmented heating process includes: heating to a first temperature range at a first heating rate to thermally decompose the organic matter within the fiber, and the gas generated by the thermal decomposition forming a desorption hysteresis effect under the action of applied gas pressure; and then heating to a second temperature range at a second heating rate to densify and crystallize.

2. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption according to claim 1, characterized in that: The gas pressure is 2 to 8 MPa.

3. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption according to claim 1, characterized in that: The gas pressure is 4 to 6 MPa.

4. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption according to claim 1, characterized in that: The first heating rate is 0.5~5 ℃ / min, and the first temperature range is 200~600 ℃; the second heating rate is 1~10 ℃ / min, and the second temperature range is 1000~1400 ℃.

5. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption according to claim 1, characterized in that: The oxygen-containing atmosphere is an air atmosphere or a mixture of oxygen and an inert gas.

6. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure analysis according to claim 1, characterized in that: The temperature is then maintained within the second temperature range for 30 to 180 minutes.

7. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption according to claim 1, characterized in that: Before performing the segmented heating process, the pressure vessel is also evacuated.

8. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption according to claim 7, characterized in that: The vacuum level in the vacuuming process is below 10 Pa.

9. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption according to claim 1, characterized in that: The zirconium-containing precursor fiber is a wet-spun fiber or a solution-impregnated fiber containing zirconium and organic components. The organic components in the zirconium-containing precursor fiber include at least a polymer as a structural agent and / or an organic ligand as a zirconium source support.

10. The method for preparing high-strength zirconia crystal fibers by high-temperature pressure desorption according to any one of claims 1 to 9, characterized in that: The relative density of high-strength zirconia crystal fibers after densification crystallization treatment can reach over 98%, and the crystal structure is tetragonal and / or cubic.