A looped pile fabric and a method of making the same

By optimizing the warp and weft yarn weaving structure of loop pile fabric and adopting curved threading and jacquard finishing processes, the high breakage rate and snagging problems of loop pile fabric during the weaving process were solved, and high-quality fabric production was achieved.

CN123153202APending Publication Date: 2026-11-24JIANGYIN XINGWU WOOL FABRIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610976281.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-02
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing loop pile fabrics have a high breakage rate during the weaving process and are prone to snagging, resulting in surface defects.

Method used

An optimized warp and weft yarn weaving structure is adopted, with the second warp yarn being threaded in a curved shape along the oblique direction to form a loop structure. Combined with jacquard finishing technology, an arched part with alternating odd and even yarns is constructed, which converts longitudinal tension into oblique shear force and reduces yarn breakage rate.

Benefits of technology

It significantly reduces the yarn breakage rate of loop pile fabric, improves the fabric density and hand feel, reduces defects, and improves the yield and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153202A_ABST
    Figure CN123153202A_ABST
Patent Text Reader

Abstract

This invention discloses a loop pile fabric and its preparation method, characterized in that: a first warp yarn (1) and a weft yarn (3) are woven into a plane and an odd-even alternating arched section is constructed on at least one side; a second warp yarn (2) is curvedly threaded through adjacent arched sections along a first oblique direction (10) and a second oblique direction (11), and then looped back along opposite first directions (8) and second directions (9), such as from the first arched section (4) to the second arched section (5), and then back through to the third arched section (6). This structure converts longitudinal tension into oblique shear force, so that the arched sections restrain each other to form a uniform mechanical fulcrum, significantly reducing the yarn breakage rate and snagging defects during weaving, while improving the density of the pile surface and the softness and toughness of the hand.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fabric weaving technology, specifically to a loop pile fabric and its preparation method. Background Technology

[0002] Loop pile fabric, as a textile material with unique texture and function, has shown broad application potential in the fields of clothing, home furnishings, and decoration in recent years. The fabric surface is covered with dense, ring-shaped short fibers, and this special structure gives the fabric an excellent tactile experience and visual appeal.

[0003] The typical structure of loop pile fabric consists of a plain or twill weave base and a top layer of raised loops. Through a specific process, some warp or weft yarns form incomplete loops during weaving, which are then preserved as stable pile after post-processing. Compared to traditional cut pile fabrics, its pile surface exhibits a regular ring distribution, combining a three-dimensional feel with flexibility.

[0004] Traditional loop pile fabrics use bamboo / wood / steel wire rods inserted into the shed, causing the warp yarns to loop and form uncut loops. After the fabric is formed, a cutter cuts the pile warp between the two layers of ground fabric, loosening it to form an independent pile surface. The pile is formed by cutting some of the pile weft floats. Modern loop pile fabric production often uses a double weaving process. The base layer uses high-strength fine denier synthetic fibers or combed cotton yarn to build a stable skeleton, while the pile layer uses an electronic rapier loom with a jacquard device to control the float length and sinking frequency of the pile warp, achieving a uniform pile surface.

[0005] However, existing loop pile fabrics have a high breakage rate during the weaving process, and are particularly prone to snagging, which can cause defects on the pile surface. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a loop pile fabric and its preparation method.

[0007] To achieve the above objectives, the technical solution provided by the present invention is as follows: A loop pile fabric includes a plane formed by a first woven warp and weft yarn, wherein the warp yarn forms an arched portion protruding from the plane on at least one side of the plane, the arched portions being arranged in an alternating odd and even pattern on the plane, and a second warp yarn passes through the arched portion in a curved manner along an oblique direction and sequentially passes through the first arched portion along a first direction between the first arched portion and the second arched portion adjacent in a first oblique direction, passes around the second arched portion and then passes through the second arched portion along a second direction from the side of the second arched portion away from the first arched portion, and then passes back to the third arched portion adjacent to the first arched portion along the second oblique direction; wherein the angle between the first oblique direction and the second oblique direction is <180°, and the first direction is opposite to the second direction.

[0008] As a preferred technical solution, the warp thread passes through the third arch portion from the side closest to the first arch portion.

[0009] As a preferred technical solution, the radial line passes through the third arch portion from the side away from the first arch portion and, with the line connecting the second and third arch portions as the axis, passes through the fourth arch portion which is symmetrically arranged with respect to the first arch portion.

[0010] As a preferred technical solution, the first warp yarn is made of polyester filament or long-staple cotton, and the second warp yarn is made of wool yarn or cashmere yarn; the weft yarn is made of one of polyester filament, long-staple cotton, nylon, and spandex.

[0011] As a preferred technical solution, the first warp yarn has a count of 40-80, the second warp yarn has a count of 20-40, and the weft yarn has a count of 30-60.

[0012] The present invention further provides a method for preparing the above-mentioned fabric, comprising the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a plane, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in warm water at 40-50℃, add 2-5% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform the first shrinking. S3. The initial product, after the first layer of shrinkage is completed, is then napped on a napping machine to obtain the intermediate product. S4. The product is steam-spun twice, and fabric softener is sprayed onto the surface of the product using steam.

[0013] S5. After the second shrinking process is completed, the middle product is processed into the final product of loop pile fabric through jacquard weaving.

[0014] As a preferred technical solution, on a three-dimensional textile machine, the second warp yarn constructs an arched section in a curved path at an angle of 15-30°; the loop height is programmed and controlled within the range of 1.0-3.5mm; during the weaving process, the tension of the first warp yarn needs to be stabilized at 18-25cN, and the tension of the weft yarn is maintained at 12-18cN.

[0015] As a preferred technical solution, the bending angle of the steel wire needle used for napping is 45-60°, the ratio of the forward and reverse napping speeds is 1:(1.5-2), and the napping tension is controlled at 15-20cN.

[0016] As a preferred technical solution, the fabric softener is an organosilicon softener, which is mixed with water at a mass ratio of 1:(10-20) and then heated to a steam state for secondary shrinkage.

[0017] As a preferred technical solution, the jacquard process uses U-shaped or H-shaped loop jacquard needles, and performs three-dimensional loop pile forming on the intermediate product after the second shrinkage at a machine speed of 300-600 rpm; the needle density is set to 80-200 needles / square inch, and the jacquard depth is ≥0.7 times the loop height.

[0018] The advantages and beneficial effects of this invention are as follows: By optimizing the loop pile forming method and weaving process, the curved threading method and jacquard setting of the second warp yarn, the arched portions constructed by the first warp yarn on both sides of the plane are arranged in an alternating odd and even pattern, forming a uniformly distributed mechanical support point. The second warp yarn is threaded along a curved path along the oblique direction, looping back and forth between adjacent arched portions, so that the arched portions restrain each other. Compared with the traditional straight loop pile structure, the curved threading transforms the longitudinal tension into oblique shear force, resulting in a loop pile fabric with excellent quality and feel, a significantly reduced yarn breakage rate, and a significant reduction in defects, ensuring that the loop pile is uniform and dense. Attached Figure Description

[0019] Figure 1 This is one of the structural schematic diagrams of the fabric shown in this invention; Figure 2 This is the second structural schematic diagram of the fabric shown in this invention; In the diagram: 1-first warp yarn, 2-second warp yarn, 3-weft yarn, 4-first arch, 5-second arch, 6-third arch, 7-fourth arch, 8-first direction, 9-second direction, 10-first oblique direction, 11-second oblique direction. Detailed Implementation

[0020] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, the specific embodiments of this application will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, it should be noted that, for ease of description, only the parts relevant to this application are shown in the accompanying drawings, not the entire structure. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this application.

[0021] The terms “comprising” and “having”, and any variations thereof, used in this application are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units is not limited to the steps or units listed, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to such process, method, product, or apparatus.

[0022] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly or implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0023] This invention relates to a loop pile fabric and its preparation method. The fabric optimizes the weaving structure of the first warp yarn 1 and the weft yarn 3. The second warp yarn 2 passes through the arched portion in a curved shape along a diagonal direction, and sequentially passes through the first arched portion 4 along a first direction 8 between the first arched portion 4 and the second arched portion 5 adjacent to the first arched portion 4 along a first diagonal direction 10. After bypassing the second arched portion 5, it passes through the second arched portion 5 along a second direction 9 from the side of the second arched portion 5 away from the first arched portion 4, and then passes back to the third arched portion 6 adjacent to the first arched portion 4 along a second diagonal direction 11. The angle between the first diagonal direction 10 and the second diagonal direction 11 is <180°, and the directions of the first direction 8 and the second direction 9 are opposite. The curved threading method of the second warp yarn 2 and the jacquard finishing process achieve a uniform distribution of the loop pile structure, enhanced mechanical properties, and a significant reduction in yarn breakage rate. The first warp yarn 3 and the weft yarn 3 are woven into a plane, forming an alternating odd-even arched section on at least one side. The second warp yarn is threaded along an oblique, curved path through adjacent arched sections, which include a first arched section 4, a second arched section 5, a third arched section 6, and a fourth arched section 7, and are sequentially looped along the first direction 8 and the second direction 9, forming a mutually restraining three-dimensional looped pile structure. This structure not only improves the fabric's density and hand-feel softness, but also effectively reduces the rate of yarn breakage and snagging defects during weaving, thereby improving the fabric's yield and performance.

[0024] In this invention, the "first warp yarn" refers to the main warp yarn that constitutes the basic planar structure, supporting the skeleton of the overall fabric and ensuring sufficient strength and stability. The "second warp yarn" is a pile yarn that forms a loop structure between the arched sections through a specific curved threading path, thereby constructing the loop pile shape. The "weft yarn" is a transverse yarn interwoven with the warp yarn, which plays a role in fixing the structure and enhancing the overall performance of the fabric during the weaving process. The "arched section" refers to the raised structure formed by the weaving of the first warp yarn and the weft yarn, which is arranged in an odd-even alternating pattern on the fabric surface, forming the basic unit of the loop pile.

[0025] This invention transforms longitudinal tension into oblique shear force, creating mutually restraining mechanical fulcrums between the arched sections. Specifically, the second warp yarn is threaded along an oblique, curved path, passing through the first arched section, around the second arched section, and then exiting through the third arched section, forming a symmetrical structure with the first arched section using the line connecting the second and third arched sections as the axis. This looping method ensures that when the fabric is stretched by external forces, the tension is no longer concentrated in a single direction, but is distributed among multiple arched sections through oblique shear force, thereby improving the fabric's tear resistance and abrasion resistance.

[0026] Furthermore, this invention enhances the overall performance of loop pile fabric by controlling weaving parameters and post-processing techniques. For example, during weaving, the tension of the first warp yarn is controlled at 18-25 cN, and the tension of the weft yarn is maintained at 12-18 cN to ensure the stability and uniformity of the fabric structure. The oblique angle of the curved path of the second warp yarn is controlled at 15°-30°, and the loop height is programmed within the range of 1.0-3.5 mm to ensure the three-dimensionality and density of the loop pile. In the napping process, steel wire needles with a bending angle of 45°-60° are used, the ratio of forward to reverse pile speed is 1:(1.5-2), and the napping tension is controlled at 15-20 cN to improve the smoothness and hand feel of the pile surface. In the post-processing stage, a silicone softener is mixed with water at a mass ratio of 1:(10-20) and heated to a steam state for a second shrinking process, further enhancing the softness and durability of the fabric. The jacquard process uses U-shaped or H-shaped loop jacquard needles, with the machine speed controlled at 300-600 rpm and the needle density set at 80-200 needles / square inch. The jacquard depth is ≥0.7 times the loop height to achieve precise three-dimensional loop jacquard forming.

[0027] As a further explanation, the difference between the loop pile fabric shown in this invention and the prior art is that the prior art's loop pile preparation process mostly adopts a pre-reserved loop pile structure and cut pile yarn. After the fabric production is completed, the loop pile is separated by a cut pile process to achieve the preparation of loop pile. Because the cut pile process destroys the original winding structure of the fibers, the root of the pile after cutting is only fixed by a single warp or weft yarn. Cutting causes the pile to loosen or even fall off, and the loop pile fabric has a high amount of shedding during washing. In contrast, this invention uses a weaving structure in which the second warp yarn passes through the arched part in a curved shape along the oblique direction, and passes through the first arched part in a first direction between the first arched part and the second arched part adjacent to the first oblique direction. After passing around the second arched part, it passes through the second arched part in a second direction from the side of the second arched part away from the first arched part, and then passes back to the third arched part adjacent to the first arched part along the second oblique direction. Through the continuous connection of back-threading and looping, the loop pile can be limited by the second and third arched parts to control the size of the loop pile. In actual production, the diameter of the loop pile structure can be preset by inserting knitting needles. Since the loop pile structure is continuously prepared, there is no need to cut the pile, and uniform loop pile fabric can be obtained by using jacquard technology.

[0028] In this invention, to prevent the loop pile from shrinking after the jacquard is completed, a lining can be glued or sewn onto the non-jacquard side of the loop pile fabric.

[0029] The loop pile fabric of this invention can be widely used in clothing, home decoration, automotive interiors, and other fields, and is especially suitable for the high-end fabric market where high requirements are placed on feel, breathability, and abrasion resistance. Its structural design is reasonable, its manufacturing process is mature, and it has good market application prospects.

[0030]

Example 1

[0031] Its preparation method includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a planar structure, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in 40℃ warm water, add 2% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform a shrinking process. S3. The initial product after the first shrinking process is subjected to napping treatment on a napping machine. The wire needle bend angle is 45°, the ratio of forward to reverse napping speed is 1:1.5, and the napping tension is controlled at 15cN to obtain the intermediate product. S4. The product is shrunk twice with steam, and silicone fabric softener is sprayed onto the surface of the product with steam. The silicone fabric softener is mixed with water at a mass ratio of 1:10 and then heated to a steam state. S5. After the second shrinking is completed, the middle product is processed into the final product of loop pile fabric through jacquard. The jacquard process uses U-shaped loop jacquard needles, the machine speed is controlled at 300 rpm, the needle density is set at 80 needles / square inch, and the jacquard depth is 0.7 times the loop height.

[0032] The loop pile fabric produced in this embodiment has a good hand feel and density, a low yarn breakage rate, and a uniform pile surface, making it suitable for lightweight clothing fabrics.

[0033]

Example 2

[0034] Its preparation method includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a planar structure, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in 45℃ warm water, add 3% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform a shrinking process. S3. The initial product after the first shrinking process is subjected to napping treatment on a napping machine. The wire needle bend angle is 50°, the ratio of forward to reverse napping speed is 1:1.8, and the napping tension is controlled at 18cN to obtain the intermediate product. S4. The product is shrunk twice with steam, and silicone fabric softener is sprayed onto the surface of the product with steam. The silicone fabric softener is mixed with water at a mass ratio of 1:15 and then heated to a steam state. S5. After the second shrinking is completed, the middle product is processed into the final product of loop pile fabric through jacquard. The jacquard process uses H-type loop jacquard needles, the machine speed is controlled at 450 rpm, the needle density is set at 120 needles / square inch, and the jacquard depth is 0.75 times the loop height.

[0035] The loop pile fabric produced in this embodiment has excellent softness and three-dimensionality, making it suitable for use in high-end clothing fabrics.

[0036]

Example 3

[0037] Its preparation method includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a planar structure, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in 48℃ warm water, add 4% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform a shrinking process. S3. The initial product after the first shrinking process is subjected to napping treatment on a napping machine. The wire needle bend angle is 55°, the ratio of forward to reverse napping speed is 1:1.9, and the napping tension is controlled at 19cN to obtain the intermediate product. S4. The product is shrunk twice with steam, and silicone fabric softener is sprayed onto the surface of the product with steam. The silicone fabric softener is mixed with water at a mass ratio of 1:18 and then heated to a steam state. S5. After the second shrinking is completed, the middle product is processed into the final product of loop pile fabric through jacquard. The jacquard process uses U-shaped loop jacquard needles, the machine speed is controlled at 500 rpm, the needle density is set at 160 needles / square inch, and the jacquard depth is 0.8 times the loop height.

[0038] The loop pile fabric produced in this embodiment has a high density and a good hand feel, making it suitable for home decor fabrics.

[0039]

Example 4

[0040] Its preparation method includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a planar structure, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in 50℃ warm water, add 5% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform a shrinking process. S3. The initial product after the first shrinking process is subjected to napping treatment on a napping machine. The wire needle bend angle is 60°, the ratio of forward and reverse napping speed is 1:2, and the napping tension is controlled at 20cN to obtain the intermediate product. S4. The product is shrunk twice with steam, and silicone fabric softener is sprayed onto the surface of the product with steam. The silicone fabric softener is mixed with water at a mass ratio of 1:20 and then heated to a steam state. S5. After the second shrinking is completed, the middle product is processed into the final product of loop pile fabric through jacquard. The jacquard process uses H-type loop jacquard needles, the machine speed is controlled at 600 rpm, the needle density is set at 200 needles / square inch, and the jacquard depth is 0.85 times the loop height.

[0041] The loop pile fabric produced in this embodiment has extremely high density and abrasion resistance, making it suitable for automotive interior fabrics.

[0042]

Example 5

[0043] Its preparation method includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a planar structure, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in 42℃ warm water, add 2.5% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform a shrinking process. S3. The initial product after the first shrinking process is subjected to napping treatment on a napping machine. The wire needle bend angle is 48°, the ratio of forward to reverse napping speed is 1:1.6, and the napping tension is controlled at 16cN to obtain the intermediate product. S4. The product is shrunk twice with steam, and silicone fabric softener is sprayed onto the surface of the product with steam. The silicone fabric softener is mixed with water at a mass ratio of 1:12 and then heated to a steam state. S5. After the second shrinking is completed, the middle product is processed into the final product of loop pile fabric through jacquard. The jacquard process uses U-shaped loop jacquard needles, the machine speed is controlled at 350 rpm, the needle density is set at 100 needles / square inch, and the jacquard depth is 0.72 times the loop height.

[0044] The loop pile fabric produced in this embodiment has good softness and breathability, and is suitable for underwear fabrics.

[0045]

Example 6

[0046] Its preparation method includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a planar structure, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in 47℃ warm water, add 4.5% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform a shrinking process. S3. The initial product after the first shrinking process is subjected to napping treatment on a napping machine. The wire needle bend angle is 58°, the ratio of forward to reverse napping speed is 1:1.95, and the napping tension is controlled at 19.5cN to obtain the intermediate product. S4. The product is shrunk twice with steam, and silicone fabric softener is sprayed onto the surface of the product with steam. The silicone fabric softener is mixed with water at a mass ratio of 1:19 and then heated to a steam state. S5. After the second shrinking is completed, the middle product is processed into the final product of loop pile fabric through jacquard. The jacquard process uses H-type loop jacquard needles, the machine speed is controlled at 580 rpm, the needle density is set at 190 needles / square inch, and the jacquard depth is 0.83 times the loop height.

[0047] The loop pile fabric produced in this embodiment has good abrasion resistance and three-dimensional effect, and is suitable for outdoor sportswear fabrics.

[0048]

Example 7

[0049] Its preparation method includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a planar structure, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in 41℃ warm water, add 2.2% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform the first shrinking process. S3. The initial product after the first shrinking process is subjected to napping treatment on a napping machine. The wire needle bend angle is 46°, the ratio of forward to reverse napping speed is 1:1.55, and the napping tension is controlled at 15.5cN to obtain the intermediate product. S4. The product is shrunk twice with steam, and silicone fabric softener is sprayed onto the surface of the product with steam. The silicone fabric softener is mixed with water at a mass ratio of 1:11 and then heated to a steam state. S5. After the second shrinking is completed, the middle product is processed into the final product of loop pile fabric through jacquard. The jacquard process uses U-shaped loop jacquard needles, the machine speed is controlled at 320 rpm, the needle density is set at 90 needles / square inch, and the jacquard depth is 0.71 times the loop height.

[0050] The loop pile fabric produced in this embodiment has a good hand feel and breathability, and is suitable for infant and toddler clothing fabrics.

[0051]

Example 8

[0052] Its preparation method includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn and the weft yarn are woven into a planar structure, and the second warp yarn is introduced through heddles to obtain the initial product. S2. Place the initial product in 49℃ warm water, add 4.8% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform the first shrinking process. S3. The initial product after the first shrinking process is subjected to napping treatment on a napping machine. The wire needle bend angle is 59°, the ratio of forward to reverse napping speed is 1:1.98, and the napping tension is controlled at 19.8cN to obtain the intermediate product. S4. The product is shrunk twice with steam, and silicone fabric softener is sprayed onto the surface of the product with steam. The silicone fabric softener is mixed with water at a mass ratio of 1:19.5 and then heated to a steam state. S5. After the second shrinking is completed, the middle product is processed into the final product of loop pile fabric through jacquard. The jacquard process uses H-type loop jacquard needles, the machine speed is controlled at 590 rpm, the needle density is set at 195 needles / square inch, and the jacquard depth is 0.84 times the loop height.

[0053] The loop pile fabric produced in this embodiment has extremely high density and abrasion resistance, making it suitable for industrial fabrics with high abrasion resistance requirements.

[0054] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A loop pile fabric, characterized in that: The plan includes a first warp yarn (1) and a weft yarn (3) formed by a woven arrangement. The first warp yarn (1) forms an arched portion protruding from the plan on at least one side of the plan. The arched portions are arranged in an alternating odd and even pattern on the plan. The second warp yarn (2) passes through the arched portion in a curved shape along an oblique direction. It passes through the first arched portion (4) in sequence along a first direction (8) between the first arched portion (4) and the second arched portion (5) adjacent to the first oblique direction (10). After passing around the second arched portion (5), it passes through the second arched portion (5) along a second direction (9) from the side of the second arched portion (5) away from the first arched portion (4) and passes back to the third arched portion (6) adjacent to the first arched portion (4) along a second oblique direction (11). The angle between the first oblique direction (10) and the second oblique direction (11) is <180°. The directions of the first direction (8) and the second direction (9) are opposite.

2. The loop pile fabric according to claim 1, characterized in that: The second warp (2) passes through the third arch (6) from the side near the first arch (4).

3. The loop pile fabric according to claim 1, characterized in that: The second warp (2) passes through the third arch (6) on the side away from the first arch (4), and passes through the fourth arch (7) which is symmetrically arranged with respect to the line connecting the second arch (5) and the third arch (6).

4. The loop pile fabric according to claim 1, characterized in that: The first warp yarn (1) is made of polyester filament or long-staple cotton, and the second warp yarn (2) is made of wool yarn or cashmere yarn; the weft yarn (3) is made of one of polyester filament, long-staple cotton, nylon, or spandex.

5. The loop pile fabric according to claim 1, characterized in that: The first warp yarn (1) has a count of 40-80, the second warp yarn (2) has a count of 20-40, and the weft yarn (3) has a count of 30-60.

6. The loop pile fabric according to claim 1, characterized in that: The height of the arched part is 1.0-3.5mm.

7. The loop pile fabric according to claim 1, characterized in that: The oblique angle of the curved guide path is 15°-30°.

8. A method for preparing the loop pile fabric according to any one of claims 1-7, characterized in that: Includes the following steps: S1. On a three-dimensional textile machine, the first warp yarn (1) and the weft yarn (3) are woven into a plane, and the second warp yarn (2) is introduced through a heald to obtain the initial product; S2. Place the initial product in warm water at 40-50℃, add 2-5% wool shrinking agent by weight of the warm water, and mechanically knead for 20 minutes to perform the first shrinking. S3. The initial product, which has been shrunk in one pass, is napped on a napping machine to obtain the intermediate product; S4. The product is steam-steamed for a second shrinkage, and fabric softener is sprayed onto the surface of the product using steam. S5. After the second shrinking process is completed, the middle product is processed into the final product of loop pile fabric through jacquard weaving.

9. The preparation method according to claim 8, characterized in that: In S1, the second warp yarn (2) constructs an arched section in a curved path at an angle of 15-30°; the loop height is programmed and controlled within the range of 1.0-3.5mm; during the weaving process, the tension of the first warp yarn (1) needs to be stable at 18-25cN, and the tension of the weft yarn (3) is maintained at 12-18cN; in step S3, the bending angle of the steel wire needle used for napping is 45-60°, the ratio of the forward and reverse napping speeds is 1:(1.5-2), and the napping tension is controlled at 15-20cN.

10. The preparation method according to claim 8, characterized in that: In step S4, the fabric softener is an organosilicone softener. The organosilicone softener is mixed with water at a mass ratio of 1:(10-20) and then heated to a steam state for a second shrinking process. In step S5, the jacquard process uses U-shaped or H-shaped loop jacquard needles to perform three-dimensional loop forming on the mid-sized product after the second shrinking process at a machine speed of 300-600 rpm. The needle density is set to 80-200 needles / square inch, and the jacquard depth is ≥0.7 times the loop height.