A cashmere-like super fine denier bionic knitted structure and a weaving method thereof

By incorporating a curled configuration at the end of the dyeing and finishing process, combined with the support and filling fibers, the problems of low survival rate of the curled fibers and messy pile in existing technologies are solved, achieving stable curling and orderly flattening of cashmere-like knitted fabrics.

CN123153205APending Publication Date: 2026-11-24SUZHOU DAYI TEXTILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611325834.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing cashmere-like knitted fabrics have high loosening rate and low curl survival rate after the pile curl is imparted at the fiber or yarn stage and undergoes dyeing and high temperature setting processes; the curling at the fiber level leads to random pile orientation; the ultra-fine denier pile has low bending stiffness and random lying direction; the arc geometry of the cut pile is not utilized; the high temperature setting intuition is contrary to the requirement of maintaining the pile curvature configuration.

Method used

In the final stage of dyeing and finishing, curling is imparted by high-temperature pre-setting before the loops are cut, which allows the pile to relax under constrained conditions. The post-setting temperature is then lowered, and by combining the different configurations of the supporting pile and the filling pile, a stable curled structure is formed using weaving geometry.

Benefits of technology

It improves the survival rate of the curl, makes the down neat and avoids tangling, and achieves orderly lying and stable curling of the down, which conforms to the biomimetic prototype of cashmere.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153205A_ABST
    Figure CN123153205A_ABST
Patent Text Reader

Abstract

This invention discloses a cashmere-inspired ultra-fine denier biomimetic knitting structure and its weaving method, belonging to the field of knitted fabric manufacturing technology. The pile layer consists of ultra-fine denier filling fibers and coarser supporting fibers, mimicking the binary structure of goat hair's guard hair and pile. The filling fibers exhibit a residual curvature in a free state, with two fibers cut from the same sinker arc in opposite directions forming an arched unit. The key to the weaving method lies in shifting the timing of initiating the curl to the final stage of dyeing and finishing: before the loops are cut, a sinker arc is used as a template for high-temperature pre-setting, solidifying the curl into a permanent residual curvature. After loop cutting, a post-setting temperature at a level 35 degrees Celsius lower than the pre-setting temperature is used for finishing. Simulations show that the survival rate of curl initiation at the yarn stage is only 4.2%, and the retention rate at conventional high-temperature post-setting is only 9.6%, while this invention achieves 55.6%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of knitted fabric manufacturing technology, specifically to a cashmere-like ultra-fine denier biomimetic knitted structure and its weaving method. Background Technology

[0002] Cashmere is the finest of all natural fibers, typically 13-16 micrometers in fineness, with a scale density of about 60-70 scales per millimeter. It lacks a medullary layer in the middle of the fiber and is generally 35-45 millimeters in length. The reason cashmere feels superior to sheep's wool and conventional synthetic fibers at the same weight is widely acknowledged in the industry not only because of its fineness, but also because of its high crimp count, crimp rate, and crimp recovery rate. The fiber exhibits a sparse yet deep three-dimensional crimp, with a natural crimp count of about 4-6 crimps per centimeter. This crimp allows the fibers to both bind together and leave gaps, giving the aggregate a soft, supple feel and excellent resilience.

[0003] Using ultra-fine denier synthetic fibers to imitate cashmere has been a long-standing technological approach in the textile industry. Taking polyester as an example, the linear density of ultra-fine denier filaments can reach below 0.5 decibels (corresponding to a diameter of approximately 6.8 micrometers), which is superior to cashmere in terms of fineness. However, the feel of the finished product is still significantly different from cashmere, with the problem mainly concentrated on the issue of "curl." Existing technologies developed for this purpose all focus on the fiber or yarn level, resulting in five defects that remain unresolved to this day.

[0004] Firstly, the crimping occurs too early, meaning most of the crimp doesn't survive to the finished product. Whether using high-elasticity yarn, false-twist textured yarn, or potentially crimped composite fibers, or creating spiral pile using hydrolyzed core yarn plus wrapping yarn followed by hydrolysis to remove the core, the crimp is already solidified during the spinning or yarn processing stage. The fabric then undergoes two high-temperature processes: dyeing and stretching / setting. Polyester experiences significant stress relaxation above its glass transition temperature, while the pile yarn is in a stretched state under tension during these two processes. This relaxation smooths out the solidified crimp. The industry phenomenon that "pile made with high-elasticity yarn collapses after leaving the setting machine" stems from this, but no literature has yet quantified this causal relationship.

[0005] Secondly, the crimping at the fiber level results in a disordered pile. The method of using the difference in shrinkage rates between the two components to cause the pile to bend depends on the random position of the fibers within the yarn. This results in a chaotic pile orientation and uneven luster on the finished pile surface, a phenomenon known in the industry as "aurora spots." Existing technology itself acknowledges the existence of this defect.

[0006] Thirdly, compensating by lengthening or increasing the density of the pile will introduce new problems. The bending stiffness of microfiber decreases with the fourth power of its diameter. A pile with a linear density of 0.5 dtex and a length of 1.0 mm has a critical Euler buckling load of only about 0.77 micronewtons. The longer the pile, the lower this critical load becomes with the reciprocal of the square of its length. The pile will collapse under slight external force, and the collapse direction will be random and the fibers will be intertwined, making it difficult to recover after combing.

[0007] Fourth, although cut pile fabrics can be cut into pile at the sinker arc, the resulting pile is always treated as upright short fibers. The technological contributions of existing cut pile fabrics, compound cut pile fabrics, and various high and low pile fabrics are concentrated in the design of the weave structure, yarn arrangement path, and cutting position. The inherent arc geometry of each pile after cutting is regarded as an object that needs to be "straightened and ironed" in the subsequent finishing process, rather than a resource that can be utilized.

[0008] Fifth, the unresolved objective obstacle lies in the prevailing belief in the field that higher heat-setting temperatures result in stronger setting effects, and that high temperatures are commonly used in the finishing processes of pile fabrics to make the pile stand upright. Based on this intuition, the setting temperature after loop cutting or combing is usually set above 180 degrees Celsius. In pile finishing processes, there are even practices where the initial setting is done at 120-140 degrees Celsius, followed by setting at 210-230 degrees Celsius after combing to make the pile stand upright. In other words, the setting temperature not only doesn't decrease but actually increases significantly, with the explicit purpose of making the pile stand upright. This operation is indeed beneficial for the dimensional stability of the base fabric, but it is devastating to the curvature of the pile: at this point, the pile is no longer subject to any geometric constraints, and the secondary relaxation at high temperatures will only drive it back to a straight line. This intuition is exactly the opposite of the process direction required by this invention, and is the direct reason why similar solutions have not been proposed for so long.

[0009] Therefore, there is a need in the art for a knitting structure and a knitting method thereof that does not rely on the fiber's own crimp and can stably maintain the cashmere-like crimped configuration of ultrafine denier fibers. Summary of the Invention

[0010] The technical problem this invention aims to solve is that: the curl of existing cashmere-like knitted fabrics is entirely imparted at the fiber or yarn stage, requiring stress relaxation through two processes: dyeing and high-temperature setting, resulting in an extremely low curl survival rate; the curling at the fiber level leads to disordered pile orientation; the ultra-fine denier pile has low bending stiffness, and after being loaded, it falls in random directions and becomes entangled; the inherent arc geometry of the pile is not utilized when cutting loops into pile; and the prevailing intuition in the field that "the higher the setting temperature, the stronger the fabric" is contrary to the requirement of maintaining the curled structure of the pile.

[0011] The technical concept of this invention is based on the relationship between the viscoelastic stress relaxation and thermal history sequence of polyester. When polyester is heated above its glass transition temperature, its internal elastic strain gradually transforms into permanent deformation according to a relaxation function; this transformation is irreversible, and the relaxation fraction is determined by both temperature and time. From this, we can derive a conclusion never before addressed in the prior art: whether a curvature can survive to the finished product depends on at which stage of the process chain it is applied, and how many high-temperature processes it must undergo afterward. The earlier the curvature is applied, the more high-temperature relaxation processes it needs to endure, and the lower its survival rate.

[0012] Therefore, this invention shifts the timing of imparting curvature to the end of the dyeing and finishing process, and changes the template for imparting curvature from fiber to weaving geometry: a high-temperature pre-forming is performed while the loops are not yet cut and the filling yarn is being forcibly bent into a sinking arc by the jaws of the sinking plate, so that the bending strain is fully relaxed under the constraint and the curvature of the sinking arc is solidified into the permanent residual curvature of the yarn; after that, the loops are cut, and each filling yarn naturally has a residual curvature of half a sinking arc.

[0013] Most importantly, simply completing the aforementioned pre-forming process is insufficient to preserve this curvature, because the pile is in a free state after loop cutting. If the subsequent setting process still uses high temperatures as intuitively understood in the art, the secondary relaxation will erase the residual curvature that has just been cured. Therefore, this invention further stipulates that the post-setting temperature T2 must be at least 35 degrees Celsius lower than the pre-setting temperature T1 of the loop state. This temperature gradient contradicts the common intuition in the art that "the higher the setting temperature, the stronger the bond," and is the key difference between this invention and conventional practices; both are indispensable.

[0014] The biomimetic prototype of this invention is the binary structure of goat hair: the outer layer of guard hairs is coarse, long, and straight, responsible for supporting the thickness of the entire coat layer; the inner layer of down is fine, short, and curly, responsible for filling the gaps and providing a soft, supple feel. Accordingly, this invention divides the down layer into two groups: supporting hairs and filling hairs. The supporting hairs have a coarser linear density, a longer free length, and maintain an upright configuration, while the filling hairs have an ultra-fine denier linear density, a shorter free length, and residual curvature.

[0015] This invention also reveals a closed geometric relationship that directly locks the process parameters to the biomimetic target. After the loops are cut, each filling hair is exactly a semicircular arc, so its free length L is equal to the product of pi and the residual radius of curvature R. The ratio of R to L is always the reciprocal of pi, i.e., 0.318. Extending this residual curvature into continuous curls, the arc length of a complete curl cycle is twice the product of pi and R. Therefore, the equivalent number of curls C is equal to 1 divided by the arc length of this cycle, which is also equal to 1 divided by 2 times L. Let C fall within the natural curl count range of cashmere, 4~6 curls / cm, and we can inversely calculate that the free length L of the filling hair should be 0.83~1.25 mm. The corresponding loop height h is equal to 2 times L divided by pi, which should be 0.53~0.80 mm. Thus, the process parameter of "how long the plush should be," which was originally determined based on appearance experience, has been converted into a definite quantity that can be directly calculated from the biomimetic target.

[0016] To solve the above-mentioned technical problems, the present invention provides a cashmere-like ultra-fine denier biomimetic knitting structure and its weaving method. The aforementioned cashmere-like ultrafine denier biomimetic knitted structure includes a base fabric layer and a pile layer located on one side of the base fabric layer. The pile layer consists of two sets of pile: filling pile and support pile. The filling pile is an ultrafine denier filament with a monofilament linear density of no more than 0.5 dtex and a free length L of 0.83~1.25 mm. In its free state, it exhibits a residual bending configuration, with a residual radius of curvature R to free length L ratio of 0.28~0.36, corresponding to an equivalent number of curls of 4~6 per centimeter. Two filling piles, cut from the same sinking arc, are fixed at their roots to two adjacent loops in the same loop row. Their residual bending directions are opposite, and their arc convex surfaces face away from each other, forming a pair of arched units. The lateral span of the arched unit is 2R, and the average spacing between adjacent piles in the pile layer is no more than one-twentieth of this lateral span. The support pile is a filament with a monofilament linear density of 2.0~5.0 dtex and a free length of 1.5~2.2 times that of the filling pile. It has an upright structure and accounts for 15% to 35% of the total mass of the pile layer.

[0017] This invention also provides a method for weaving a cashmere-like ultra-fine denier biomimetic knitted structure, comprising: S1, simultaneously feeding ground yarn, filling yarn, and support yarn into the knitting machine on a double-sided circular knitting machine, wherein the filling yarn is formed into loops with a loop height of 0.53~0.80 mm by the sinker jaw pads, and the support yarn loop height is 1.5~2.2 times that of the filling yarn; S2, dyeing at 125~135 degrees Celsius, holding for 30~60 minutes, and then dehydrating and drying; S3, while the loops are not yet cut, pre-forming the loop state at 175~200 degrees Celsius for 30~90 seconds with an overfeed rate of 2%~6%, so that the relaxation fraction of the bending strain of the filling yarn is not less than 0.90; S4, cutting the filling yarn at the apex of the sinker arc with a loop-cutting tool, obtaining a free length L equal to pi and the loop height h. Half of the filling wool is cut from the same sinker arc, and the two filling wools cut from the same sinker arc have opposite residual bending directions; S5, cut the sinker arc of the support yarn and comb the pile layer with a napping machine; S6, set the formed filling wool at 130~160 degrees Celsius for no more than 40 seconds. There are no other heat treatment processes between the pre-setting and post-setting of the loop state except for loop cutting and combing, and the T1-T2 temperature is not less than 35 degrees Celsius, so that the residual curvature retention rate is not less than 50%.

[0018] Furthermore, the loop height can be calculated by inversely using the target equivalent crimp number, which is equal to 1 divided by the product of pi and the equivalent crimp number; the pre-setting temperature can be 185 degrees Celsius for 45 seconds, and the post-setting temperature can be 150 degrees Celsius for 30 seconds; the pre-setting and post-setting can be performed on the same tenter frame, and the temperature setting value is sent to the heating actuator of each drying oven area through its control interface and read back by the fabric temperature measuring device; the support yarn sinker arc can be cut at the offset on both sides of the arc apex to obtain support loops of unequal length.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0020] First, by shifting the timing of instilling curvature from the yarn stage to the final dyeing and finishing stage, the survival rate of curl is increased by an order of magnitude. Numerical simulations show that the existing technical route of instilling curvature at the yarn stage, after dyeing at 130 degrees Celsius for 40 minutes and setting at 180 degrees Celsius for 30 seconds, has a curl survival rate of only 4.2%; while the present invention, with pre-setting in the loop state followed by cooling and setting, achieves a residual curvature retention rate of 55.6%, which is 13.3 times that of the former.

[0021] Second, a temperature gradient rule is presented that contradicts conventional intuition in the field but is supported by simulation. If the post-setting temperature is set to 180 degrees Celsius based on the intuition that "the higher the setting temperature, the stronger the bond," the retention rate drops from 55.6% to 9.6%; however, if only the post-setting temperature is lowered without pre-setting in the loop state, the retention rate is 0%. The two methods must be used in conjunction to form an inseparable technical whole.

[0022] Third, the curvature of the pile is determined by weaving parameters rather than yarn, making it calculable and reproducible. There is a closed relationship between the free length of the filling pile and the equivalent number of curls, C=1 / (2L), which transforms the goal of "making a pile with a number of curls comparable to cashmere" from an experience-dependent objective into a process quantity that can be directly calculated from the pile height.

[0023] Fourth, the direction of the pile's collapse after compression is uniquely determined by the residual curvature, and is no longer random. Through Elastica large deformation simulation, under 16 different random initial defects and compression to 60% of the free height, the orderliness of the collapse direction of the upright pile was only 0.50 (half positive and half negative), while the orderliness of the filling fibers with residual curvature was 1.00 (all 16 cases were in the same direction). The pile surface thus collapses neatly, can be combed back, and avoids aurora spots caused by tangling and cross-linking.

[0024] Fifth, paired, oppositely shaped arched units form a lateral bridging between the pile. The lateral span of the filling pile is 2R, which is 637 micrometers at a free length of 1.0 mm and a pile density of 60 g / m², equivalent to 22.1 times the average spacing between adjacent piles, while the lateral span of the upright pile is zero.

[0025] Sixth, the load-bearing division between the supporting hair and the filling hair is clear, conforming to the biomimetic prototype of goat hair. The Euler buckling critical load of the filling hair with a monofilament linear density of 0.5 dtex and a length of 1.0 mm is 0.773 micronewtons, while that of the supporting hair with a monofilament linear density of 3.0 dtex and a length of 1.8 mm is 8.592 micronewtons, a difference of 11.1 times; when the mass ratio of the supporting hair is 25%, its individual load-bearing capacity reaches 239 Pa. Attached Figure Description

[0026] Figure 1 This is a cross-sectional schematic diagram of the biomimetic cashmere ultrafine denier knitted structure according to an embodiment of the present invention;

[0027] Figure 2 This is a flowchart of the weaving method according to an embodiment of the present invention;

[0028] Figure 3 This is a schematic diagram illustrating the principle of the changes in the filling yarn configuration in the three stages of pre-forming, loop cutting, and post-forming in an embodiment of the present invention.

[0029] Figure 4 This is a simulation result diagram of the residual curvature retention rate and subsequent shaping temperature change in an embodiment of the present invention. Detailed Implementation

[0030] The present invention will be further described below with reference to the accompanying drawings and embodiments. The following embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. The present invention is applicable to various cut-loop pile knitted fabrics woven from synthetic filaments, represented by polyethylene terephthalate, which have distinct glass transition and thermoplastic setting characteristics, and is not limited to the specific machine types, linear densities, and color schemes listed in the embodiments.

[0031] I. Structural Composition

[0032] The cashmere-like ultra-fine denier biomimetic knitting structure in this embodiment is as follows: Figure 1 As shown, it includes a base fabric layer 1, a support layer 2, and a filling layer 3.

[0033] The base fabric layer 1 is a weft-knitted double-sided structure, woven from ground yarn 10 to form the base structure. The roots of the filling pile 3 and the supporting pile 2 are respectively fixed to the base fabric layer 1 by the filling yarn loops woven together with the ground yarn 10. Therefore, the pile and the base fabric are fixed by loops rather than glue or heat-fused adhesive, and the pile strength does not depend on the third component.

[0034] The filling wool 3 is an ultra-fine denier polyethylene terephthalate filament with a monofilament linear density of 0.5 dB. Its diameter, converted from linear density to density, is approximately 6.8 micrometers, which is finer than the 13-16 micrometers of cashmere. The free length L of the filling wool 3 is 1.00 mm. When not subjected to external force, it exhibits a residual curvature configuration with a residual radius of curvature R of 0.318 mm. The ratio of R to L is 0.318, falling within the range of 0.28-0.36 defined in the claims.

[0035] Two filler hairs 3, cut from the same settling arc, are fixed at their roots to two adjacent coils in the same coil row. Their residual bending directions are opposite, and their convex surfaces face away from each other, forming a pair of arched units 4 on the base fabric layer 1. Figure 1 As shown in the dashed box, the lateral span of arched unit 4 is 2R, or 0.637 mm.

[0036] Support hair 2 is a polyethylene terephthalate filament with a monofilament linear density of 3.0 dB and a diameter of approximately 16.6 micrometers, which is on the same fineness scale as the guard hairs in goat hair. The free length of support hair 2 is 1.80 mm, which is 1.8 times the free length of filling hair 3. It has an upright configuration and its mass accounts for 25% of the total mass of the pile layer. The pile layer density in this embodiment is 60 g / m².

[0037] II. Method Implementation

[0038] The weaving method flow of this embodiment is as follows: Figure 2 As shown, it includes steps S1 to S6.

[0039] S1. Weaving. Loop fabric is woven on a double-sided circular knitting machine with a bobbin diameter of 30 inches and a gauge of E28. The ground yarn 10 is made of 83 dtex / 72 ends of low-elastic polyester yarn; the filling yarn is made of 111 dtex / 216 ends of ultra-fine polyester filament with a monofilament linear density of 0.51 dtex; the support yarn is made of 111 dtex / 36 ends of polyester filament with a monofilament linear density of 3.08 dtex. The filling and support yarns are fed in through their respective yarn feeders and formed into loops by the jaws of the sinker 5, with the knitting needles 6 completing the loop formation. The loop height h of the filling yarn is set by the combined height of the jaws of the sinker 5 and the bending depth of the cam; in this embodiment, it is 0.637 mm. The loop height of the support yarn is 1.15 mm, which is 1.8 times the loop height of the filling yarn.

[0040] The value of the loop height h is not determined empirically, but rather derived from the target equivalent curl count. Let L be the free length of the filling wool after the loop is cut. Since half a loop is cut, L is equal to half the product of pi and h. Furthermore, since this segment of wool is exactly a semicircle, its residual radius of curvature R satisfies L equal to the product of pi and R, therefore R is equal to half of h, and the ratio of R to L is always the reciprocal of pi, i.e., 0.318. When this residual curvature is extended into continuous curls, the arc length of a complete curl cycle is twice the product of pi and R. Therefore, the equivalent curl count C is equal to 1 divided by 2 times L, where C is in units per centimeter and L is in centimeters. The natural crimp count of cashmere is 4-6 crimps / cm. Let C fall within this range, then L is 0.83-1.25 mm. Therefore, h is twice L divided by pi, which is 0.53-0.80 mm. In this embodiment, h = 0.637 mm, corresponding to L = 1.00 mm and C = 5.0 crimps / cm.

[0041] S2. Dyeing. After pretreatment to remove oil, the terry cloth is dyed with disperse dyes in a high-temperature, high-pressure overflow dyeing machine at 130 degrees Celsius for 40 minutes. It is then washed, dehydrated, and dried. During this stage, the terry loops remain intact and are not cut.

[0042] S3. Loop Pre-setting. With all loops still attached, the grey fabric is fed into the tenter frame 8. The pre-setting temperature T1 is set to 185 degrees Celsius, the dwell time t1 corresponding to the machine speed is 45 seconds, and the overfeed rate is 4%. At this time, the filling yarn is forcibly bent by the settling arc formed by the settling jaws, with tension on the outside and compression on the inside, and the bending strain is geometrically constrained and locked. At 185 degrees Celsius, the polyester undergoes sufficient stress relaxation, and the bending strain is converted into permanent deformation according to the relaxation function. Numerical simulation shows that the relaxation fraction under this condition is 0.963, meaning that 96.3% of the settling arc curvature is solidified as the permanent residual curvature of the filling yarn.

[0043] The overfeed rate is set at 2% to 6% because: if the overfeed rate is too low, the warp tension will lengthen the settling arc and reduce its curvature, making the actual cured curvature radius greater than the design value; if the overfeed rate is too high, the fabric surface will wrinkle and the width will be unstable. In this example, 4% is used.

[0044] S4. Loop Cutting to Form Pile. Using the loop cutter 7, cut the sinker arc of the filling yarn at its apex. The cut position is at the apex of the arc, ensuring that the two filling piles cut from the same sinker arc are of equal length, both being half the product of pi and h, i.e., 1.00 mm, and that their residual curvature directions are opposite. This is directly determined by the geometric fact that the semicircle is cut from its midpoint, requiring no additional steps, and is thus formed on the base fabric layer 1. Figure 1 The paired arched units 4 are shown.

[0045] S5. Cut and comb the support yarn. Use the loop cutter 7 to cut the sinker arc of the support yarn, and then comb the pile layer with the raising machine 9 to make the support fibers 2 stand upright and the arc-convex surfaces of the filling fibers 3 face outward. Because of its high linear density and high bending stiffness, the support fibers maintain an upright configuration after combing.

[0046] As a further implementation method, the sinker arc of the support yarn can be cut off at an offset point on both sides instead of at the apex of the arc. The offset is 0.10 to 0.20 times the length of the sinker arc, so that the two support hairs cut off are of unequal length, with the ratio of the longer to the shorter hair being 1.2 to 1.8. This creates two levels of support hair in terms of height, further approximating the actual shape of uneven guard hair length in goat wool.

[0047] S6. Post-setting. The changes in the filling yarn configuration during the three stages of pre-setting, loop cutting, and post-setting in the terry state are as follows: Figure 3 As shown. The cut fabric is then fed back into the tenter frame 8, with the setting temperature T2 set at 150 degrees Celsius and the dwell time at 30 seconds. The temperature in this step must meet the requirement that T1-T2 is not less than 35 degrees Celsius; in this embodiment, it is 185-150=35 degrees Celsius.

[0048] This is where the present invention differs from conventional practices and requires special explanation. After the ring is cut, the filler material is freed from the geometric constraints of the settling arc and is in a free state. The residual elastic recovery stress within it will drive it to straighten. If the temperature is still the conventional 180 degrees Celsius, the secondary stress relaxation fraction will reach 0.900, meaning that 90% of the residual curvature that was just cured will be erased again. However, when the temperature is reduced to 150 degrees Celsius and the time is controlled at 30 seconds, the secondary relaxation fraction is only 0.423, and the residual curvature is preserved by 57.7%.

[0049] III. Simulation Verification and Data

[0050] The following data are numerical simulation results, not actual bench test values. The material model and all parameters used in the simulation are as follows to enable those skilled in the art to reproduce the results: the flexural modulus of polyethylene terephthalate is 3.0 GPa, and the density is 1380 kg / m³; stress relaxation is expressed using the tensile index (KWW) form, where the relaxation fraction equals 1 minus a negative exponent term. The exponent of this negative exponent term is the heat treatment time t divided by the characteristic relaxation time, then raised to the power of the shape exponent and prefixed with a negative sign. The shape exponent is 0.35, and the characteristic relaxation time varies with temperature according to the Arrhenius relation. The two parameters of the model were calibrated using two industrial practices: 180°C / 30 seconds corresponds to a relaxation fraction of 0.90, and 120°C / 30 seconds corresponds to a relaxation fraction of 0.10. Based on this calibration, the apparent activation energy is 217.6 kJ / mol, and the pre-exponential factor is 2.313 x 10^-25 seconds. After calibration, the characteristic relaxation times at 180, 150, and 130 degrees Celsius were 2.77 seconds, 166 seconds, and 3569 seconds, respectively. All control groups used the same set of parameters without further parameter tuning.

[0051] Under this model, the relaxation fraction of the pre-shaped loop (geometrically constrained) state is denoted as the first relaxation fraction, and the relaxation fraction of the post-shaped (loop free) state is denoted as the second relaxation fraction. Then, the residual curvature retention rate of the filling wool after loop cutting is equal to the product of the complement of the first relaxation fraction and the second relaxation fraction.

[0052] The results of the three control groups are shown in the table below.

[0053] The control group was the non-control group, i.e. the current process: first cut the loop and then shape it, without pre-shaping the loop state, then shape it at 150 degrees Celsius for 30 seconds, the first relaxation fraction was 0, the second relaxation fraction was 0.423, and the residual curvature retention rate was 0.0%.

[0054] Control group two is one of the conventional methods, which involves incorporating crimp into the yarn using existing technology: crimping is applied during the spinning or yarn processing stage, followed by dyeing at 130°C / 40 minutes and setting at 180°C / 30 seconds. The relaxation fractions for these two processes are 0.581 and 0.900, respectively, resulting in a crimp survival rate of 4.2%. Sensitivity scanning of dyeing conditions for this method shows that within the commonly used dyeing window for polyester—125–135°C and 30–60 minutes—the survival rate consistently remains below 6%.

[0055] Control group three is the second group of the conventional method, which follows the intuitive operation in this field that "the higher the setting temperature, the stronger the bond": the pre-setting temperature for the loop state is 185 degrees Celsius for 45 seconds, but the setting temperature is still 180 degrees Celsius for 30 seconds. The first relaxation fraction is 0.963, the second relaxation fraction is 0.900, and the residual curvature retention rate is 9.6%.

[0056] The present invention uses a pre-setting process of 185 degrees Celsius for 45 seconds followed by a post-setting process of 150 degrees Celsius for 30 seconds, with a first relaxation fraction of 0.963 and a second relaxation fraction of 0.423. The residual curvature retention rate is 55.6%, which is 13.3 times that of the control group.

[0057] Two points are evident from this. First, the two most readily apparent solutions to this problem for those skilled in the art are to incorporate the curling into the yarn and to increase the setting temperature for a stronger hold. The former has a survival rate of only 4.2%, while the latter further reduces the retention rate from 55.6% to 9.6%, which is counterproductive. Second, the two methods of this invention are ineffective when separated: pre-setting only in the looped state without lowering the post-setting temperature results in a retention rate of 9.6%; lowering the post-setting temperature without pre-setting in the looped state results in a retention rate of 0.0%. The two methods must be used in conjunction; this invention is an inseparable technical whole.

[0058] It should be noted that two-stage heat setting is not uncommon in the dyeing and finishing industry. In some processes, the temperature of the later stage can be lower than that of the earlier stage. However, in those cases, the earlier stage heat setting occurs before the fabric has developed pile, or the cooling is due to reasons unrelated to pile morphology, such as the chemical stability of auxiliaries. The temperature difference is usually only around 10 degrees Celsius. The temperature gradient of this invention differs from this in three ways: First, the earlier stage heat setting must occur in a specific state where the loops have not yet been cut and the pile yarn is being forcibly bent by the sinker arc; second, the purpose and criterion for cooling is to ensure that the residual curvature of the pile after loop cutting is not less than 50%; third, the lower limit of the temperature difference derived from this criterion is 35 degrees Celsius, which is much greater than the temperature difference of conventional two-stage heat setting.

[0059] Figure 4The paper presents the variation in residual curvature retention rate under subsequent setting temperatures when the initial setting temperature is fixed at 185 degrees Celsius for 45 seconds and the subsequent setting time is 30 seconds. When the temperature gradient T1-T2 is 65, 55, 45, 35, 25, 15, and 5 degrees Celsius, the retention rates are 86.7%, 79.8%, 69.6%, 55.6%, 39.0%, 22.4%, and 9.6%, respectively. Based on this, it is determined that a retention rate of not less than 50% requires a temperature gradient of not less than 35 degrees Celsius, and a retention rate of not less than 70% requires a temperature gradient of not less than 50 degrees Celsius. The requirement of T1-T2 not being less than 35 degrees Celsius in the claims stems from this.

[0060] The pre-defined process window was also determined by scanning. With the post-forming temperature fixed at 150 degrees Celsius / 30 seconds, a pre-forming temperature of 175 degrees Celsius required more than 45 seconds to achieve 50.8% yield; at 185 degrees Celsius, 15 seconds achieved 51.7%, 45 seconds 55.6%, and further extending to 90 seconds only increased it to 56.9%, showing diminishing returns. Therefore, the claims specify a pre-forming temperature of 175-200 degrees Celsius and a time of 30-90 seconds.

[0061] The orderliness of the pile's collapsing direction was simulated using a planar elastica large deformation model. The pile was discretized into 36 segments, with the angle between each segment and the base fabric normal as variables. The bending energy was calculated as the integral along the arc length of the square of the difference between the curvature and the natural curvature of each segment. Under the equality constraint of a given tip height, the configuration with minimum energy was found. Sixteen different random initial defects were taken for each type of pile. When compressed to 60% of their respective free height, the tip lateral deviation of the upright pile was positive in 4 cases and negative in 12 cases, with an directional orderliness (absolute value of the average lateral deviation sign) of 0.50; the filling pile with residual curvature was positive in 16 cases and negative in 0 cases, with an directional orderliness of 1.00. This indicates that the collapsing direction of the upright pile is determined by uncontrollable random initial defects, while the collapsing direction of the filling pile with residual curvature is uniquely determined by its residual curvature.

[0062] The Euler buckling critical load of the pile is calculated using the formula for a slender compression bar with one end fixed and the other free. The filler pile with a monofilament linear density of 0.5 dtex and a free length of 1.0 mm has a load of 0.773 micronewtons, while the support pile with a monofilament linear density of 3.0 dtex and a free length of 1.8 mm has a load of 8.592 micronewtons, a difference of 11.1 times. At a pile layer density of 60 g / m², the individual load-bearing capacity of the support pile with a mass percentage of 5%, 10%, 15%, 20%, 25%, 30%, 40%, and 50% are 48, 95, 143, 191, 239, 286, 382, ​​and 477 Pa, respectively. The claims limit the support pile mass percentage to 15%~35%, with the lower limit ensuring a support pile load-bearing capacity of no less than 143 Pa, and the upper limit preventing the overall fineness from being sacrificed due to excessive coarse denier fibers. Since the Euler buckling critical load is proportional to the square of the linear density and inversely proportional to the square of the free length, within the range of 2.0 to 5.0 dtex of linear density and 1.5 to 2.2 times the length specified in this invention, the ratio of the critical load of the support pile to the filling pile varies between 3.3 and 44.4. The 3.0 dtex and 1.8 times used in this embodiment correspond to 11.1. This ratio is not included as an independent limiting condition in the claims to avoid redundant constraints with the limitations on linear density and length.

[0063] The calculation of lateral bridging is based on the pile surface density and the geometry of the arched unit. When the pile surface density is 60 g / m² and the free length of the filling pile is 0.83, 1.00, and 1.25 mm, the pile surface density is 1.45 x 10⁹, 1.20 x 10⁹, and 9.60 x 10⁸ per m², respectively, with average spacing of 26.3, 28.9, and 32.3 μm, respectively. The lateral span 2R of the arched unit is 528, 637, and 796 μm, respectively, which is 20.1, 22.1, and 24.7 times the average spacing; the lateral span of the upright pile is always zero.

[0064] It should be noted that this invention, verified by simulation, does not advocate increasing the thermal resistance or insulation performance of the pile layer. Simulations show that the thickness of the pile layer under body pressure is mainly determined by the fineness and free length of the supporting fibers, and is essentially unrelated to whether the filling fibers have residual curvature. At the same fineness, the pile with residual curvature has a slightly smaller thickness because its free height is the chord length, which is slightly smaller than the arc length of the upright pile. The effect of this invention lies in maintaining the curled configuration, the orderliness of the collapsing direction, and the lateral bridging, rather than insulation. Similarly, this invention does not advocate that the pile collapses due to its own weight. Based on the self-weight buckling calculation of a slender pressure bar, the critical self-weight buckling length of a 0.5 dtex single-filament pile is approximately 17 mm, which is much larger than the 0.83~1.25 mm involved in this invention. Self-weight is not the cause of collapse; collapse is caused by external load.

[0065] IV. Actuators and Control Interfaces

[0066] In this embodiment, both pre-setting and post-setting are performed on the same tenter frame 8. The tenter frame 8 has multiple independently temperature-controlled oven zones, each equipped with an electric heating actuator and a circulating fan. Temperature setpoints T1 and T2 are sent to the heating actuators of each oven zone via the control interface of the tenter frame 8. The fabric temperature measuring device reads back the actual temperature in real time and feeds it back to the control interface. When the deviation between the read value and the set value exceeds 3 degrees Celsius, the control interface adjusts the heating power of the corresponding oven zone until the deviation decreases. The dwell time t1 and the post-setting time are jointly determined by the speed of the tenter frame 8 and the effective length of the oven, with the speed set via its frequency converter control interface. The overfeed rate is determined by the ratio of the linear velocities of the feed roller and the output roller, and is set via the overfeed control interface.

[0067] The loop height h is determined by the sinker 5 and the knitting needle 6: the jaw height of the sinker 5 determines the geometric upper limit of the sinker arc, and the bending depth of the looping triangle is set by the triangle adjustment mechanism of the circular knitting machine. Together, they determine the actual loop height. The cutting position is determined by the loop cutting cutter 7: its blade height relative to the fabric surface is set by the screw fine-tuning mechanism of the cutter holder, and the arc apex cutting and offset cutting are determined by this height. The combing of the pile layer is completed by the raising machine 9, and its needle roller speed and fabric tension are set by the control panel of the raising machine 9.

[0068] The machine models, yarn specifications, temperatures, and times described in the above embodiments are merely examples, and those skilled in the art can adjust them within the scope of this invention based on specific equipment conditions. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this invention should be included within the protection scope of this invention.

Claims

1. A cashmere-like ultra-fine denier biomimetic knitted structure, comprising a base fabric layer and a pile layer located on one side of the base fabric layer, characterized in that: The pile layer consists of two sets of pile: filling pile and support pile. The filling pile is made of ultra-fine denier filament with a monofilament linear density of no more than 0.5 dtex and a free length L of 0.83~1.25 mm. In a free state without external force, it exhibits a residual bending configuration, with a residual radius of curvature R to free length L ratio of 0.28~0.36, corresponding to an equivalent crimp number of 4~6 crimps / cm. Two filling piles, cut from the same sinking arc, are fixed at their roots to two adjacent coils in the same coil row, with their residual bending directions opposite and their arc convex surfaces facing away from each other, forming a paired arched unit. The lateral span of the arched unit is 2R, and the average spacing between adjacent piles within the pile layer is no greater than one-twentieth of this lateral span, allowing the filling pile of the same arched unit to span multiple adjacent piles. The support pile has a monofilament linear density of 2.0~5.

0. The filaments of the filler have a free length of 1.5 to 2.2 times that of the filler fibers. They are upright in the free state and their mass accounts for 15% to 35% of the total mass of the pile layer. When the pile layer is unloaded after being compressed, the recovery direction of the residual bending configuration of the filler fibers is uniquely determined by the residual bending configuration. There are no filler fibers in the pile layer that have had their residual bending removed by subsequent heat treatment and have returned to an upright configuration.

2. The cashmere-like ultra-fine denier biomimetic knitted structure according to claim 1, characterized in that, The free length L of the filling hair is equal to the product of pi and its residual radius of curvature R, and the equivalent curl number C is equal to 1 divided by 2 times the free length L, where C is in units per centimeter and L is in centimeters.

3. The cashmere-like ultra-fine denier biomimetic knitted structure according to claim 1, characterized in that, The lateral span is 20 to 25 times the average spacing between adjacent fibers in the pile layer; the filler fibers have a monofilament linear density of 0.5 dtex and a free length of 1.00 mm, the support fibers have a monofilament linear density of 3.0 dtex and a free length of 1.80 mm, and the ratio of their Euler buckling critical loads is 11.

1.

4. The cashmere-like ultra-fine denier biomimetic knitted structure according to claim 1, characterized in that, The base fabric layer is a weft-knitted double-sided structure, and the roots of the filling fibers and the supporting fibers are respectively fixed by the filling yarn loops woven together with the ground yarn; the areal density of the pile layer is 40~90 g / m².

5. The cashmere-like ultra-fine denier biomimetic knitted structure according to any one of claims 1 to 4, characterized in that, Both the filling fibers and the supporting fibers are made of polyethylene terephthalate filaments, and the ratio of the linear density of the supporting fibers to the linear density of the filling fibers is 4 to 10.

6. A method for weaving a cashmere-inspired ultrafine denier biomimetic knitted structure, used to obtain the cashmere-inspired ultrafine denier biomimetic knitted structure as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1. On a double-sided circular knitting machine, ground yarn, filling yarn, and support yarn are fed in simultaneously for weaving. The filling yarn is an ultra-fine denier filament with a monofilament linear density of no more than 0.5 dtex, which is formed into loops by sinker pads. The loop height h is set to 0.53~0.80 mm. The support yarn is a filament with a monofilament linear density of 2.0~5.0 dtex, and its loop height is set to 1.5~2.2 times that of the filling yarn loop height, resulting in a terry fabric. S2. After pretreatment, the terry fabric is dyed at 125~135 degrees Celsius for 30~60 minutes, followed by dehydration and drying. S3. While all loops are still intact, the terry fabric is pre-shaped in a loop state at a pre-shaped temperature T1 of 175~200 degrees Celsius for 30~90 minutes. S1. With an overfeed rate of 2%~6%, the filling yarn undergoes stress relaxation under the forced bending configuration of the sinker arc, and its bending strain relaxation fraction is not less than 0.90, thereby solidifying the curvature of the sinker arc into the permanent residual curvature of the filling yarn; S4. The sinker arc of the filling yarn is cut off at its apex with a loop cutter, forming a filling pile with a free length L equal to half the product of pi and the pile height h, falling within the range of 0.83~1.25 mm, and the residual bending directions of the two filling piles cut from the same sinker arc are opposite; S5. The sinker arc of the support yarn is cut off with a loop cutter, and the pile layer is combed by a raising machine, so that the free length of the support pile is 1.5~2.2 times the free length of the filling pile. S6. Perform post-setting on the fabric after loop cutting. The post-setting is the heat setting applied to the formed filling fibers after loop cutting. No other heat treatment process is set between the loop-state pre-setting and the post-setting except for loop cutting and combing. The post-setting temperature T2 is 130~160 degrees Celsius and meets the requirement that T1-T2 is not less than 35 degrees Celsius, and the time is not more than 40 seconds. The secondary stress relaxation fraction of the filling fibers in the free state is not higher than 0.45, and the residual curvature retention rate of the filling fibers after loop cutting is not less than 50%.

7. The weaving method according to claim 6, characterized in that, The height h of the loops mentioned in step S1 is calculated by inversely from the target equivalent number of curls C. h is equal to 1 divided by the product of pi and C, where C is 4~6 curls / cm, C is in units of curls / cm, and h is in units of centimeters.

8. The weaving method according to claim 6, characterized in that, In step S3, the pre-setting temperature T1 is set to 185 degrees Celsius and the time t1 is set to 45 seconds; in step S6, the post-setting temperature T2 is set to 150 degrees Celsius and the time is set to 30 seconds, and T1-T2 is 35 degrees Celsius.

9. The weaving method according to claim 6, characterized in that, Steps S3 and S6 are both performed on the same tenter frame. The temperature setpoint of the tenter frame is sent to the heating actuator of each drying oven area through its control interface, and the actual temperature is read back by the fabric temperature measuring device. When the deviation between the read value and the set value exceeds 3 degrees Celsius, the heating power is adjusted by the control interface.

10. The weaving method according to claim 6, characterized in that, In step S5, the sinking arc of the support yarn is cut at the offset on both sides of the arc apex, and the offset is 0.10 to 0.20 times the arc length of the sinking arc, so that the two support yarns cut off are of different lengths, with the ratio of the longer one to the shorter one being 1.2 to 1.8.