Highly moisture-permeable and warm lyocell-based blended raised fabric and method of making the same
By using a specific blending process of lyocell, wool, acrylic, and spandex, along with physical napping and low-temperature setting, the problem of balancing moisture permeability and warmth retention in single-layer lyocell fiber fabrics has been solved. This process achieves high moisture permeability and warmth retention while suppressing fibrillation and pilling, thus improving the overall performance of the fabric.
Patent Information
- Application Number
- CN202611638656.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies struggle to achieve a synergistic improvement in both moisture permeability and warmth retention in lyocell fiber fabrics within a single-layer structure, while simultaneously suppressing fibrillation and pilling. Furthermore, most technologies rely on chemical crosslinking or antifibrillation finishing, increasing process complexity and environmental impact.
It uses a blend of four fibers—lyocell, wool, acrylic, and spandex—in a specific ratio, combined with physical napping and low-temperature setting processes. Through Siro compact spinning and double rib knitting processes, it forms an efficient still air layer to enhance warmth retention and maintain a continuous moisture transport channel, avoiding chemical cross-linking finishing.
The single-layer structure achieves a synergistic balance between high thermal resistance and high moisture permeability, significantly suppressing fibrillation, improving anti-pilling performance, and maintaining the softness and wearing comfort of the fabric.
Smart Images

Figure CN123153207A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional textile technology, and in particular relates to a Lyocell blended napped fabric with both high moisture permeability and warmth retention, and its preparation method. Background Technology
[0002] As a fundamental material closely related to human life, textiles have long since transcended their traditional attributes of warmth and decoration, continuously iterating towards multifunctionality, high functionality, and environmental friendliness. Traditional textiles are mostly made by simply weaving natural fibers, resulting in limited functionality and suitability for various scenarios. In contrast, modern functional textiles integrate new material technologies and precision weaving processes, achieving a dual upgrade in both material and function. They are widely used in many fields such as home furnishings, architecture, outdoor products, industry, and clothing, and have become an important development trend in the textile industry.
[0003] The core advantage of breathable and warm functional fabrics is their ability to both lock in heat and wick away sweat, keeping the body dry and warm during cold weather or exercise, without feeling stuffy or cold. This balance of "warmth without sweating" is difficult for ordinary fabrics to achieve simultaneously. It is well known that warmth and breathability are two key performance indicators for evaluating the comfort of textile fabrics, and their performance is constrained by their fabric structure and transmission mechanisms. Improving the warmth of a fabric usually relies on forming a stable, static air layer inside and on the surface of the fabric to increase thermal resistance. However, such structures often reduce moisture diffusion channels and increase resistance to moisture transfer, leading to a decrease in the fabric's breathability. Conversely, if a more open and loose fabric structure is used to ensure good moisture transfer, it is difficult to form an effective heat-locking air layer, thus reducing warmth. Therefore, how to achieve a synergistic improvement in high warmth and high breathability within a single-layer, lightweight structure has long been a technical challenge in the field of functional textile fabrics.
[0004] Lyocell fiber, due to its excellent moisture absorption and wicking properties and skin-friendly characteristics, produces fabrics with good breathability and comfort, and has been widely used in clothing fabrics in recent years. However, pure Lyocell fabrics have low thermal resistance under conventional structures, resulting in insufficient warmth retention. Furthermore, Lyocell fibers are prone to fibrillation under high-humidity friction conditions, leading to pilling and severely affecting the fabric's appearance and lifespan. This usually requires chemical cross-linking or specialized antifibrillation finishing to inhibit these processes, increasing process complexity and environmental impact. In the early stages of development, the applicant attempted to use the highly breathable Lyocell fiber in close-fitting thermal fabrics. While pure Lyocell single-layer knitted fabrics have excellent moisture permeability, their thermal resistance is too low. To improve warmth retention, pure Lyocell double-layer composite knitted fabrics were used (Comparative Example 1), or polyester was introduced to create Lyocell / polyester blended double-layer composite knitted fabrics (Comparative Example 2), but the improvement in thermal resistance remained limited and at a low level. Simultaneously, the double-layer structure reduced the fabric's softness and significantly decreased moisture permeability. Existing technologies disclose some methods for achieving the moisture-permeable and warmth-retaining properties of fabrics through double-layer or triple-layer fabric structures, as detailed below:
[0005] CN116100873A discloses a double-layer lightweight thermal fabric and its manufacturing process, which relates to the field of textile production technology. The fabric includes an outer fabric and an inner fabric. The outer fabric is composed of at least two of aerogel fiber, graphene fiber, hollow fiber, and denier fiber. The inner fabric is composed of a mixture of kapok fiber, cotton fiber, and companion fiber. The companion fiber is selected from one, two, or three of viscose fiber, lyocell fiber, and bamboo fiber, either spun purely or mixed. The fabric is a double-layer plain weave fabric.
[0006] CN121250612A discloses a moisture-permeable and heat-insulating composite fabric and its processing method, which relates to the field of textile technology. The key points of its technical solution are: it includes a base layer 1, a base layer 2 and an intermediate layer woven into an integral shape; the two sides of the moisture-wicking part are interwoven and fixed with the moisture-permeable part 1 and the moisture-permeable part 2 respectively; the moisture-wicking part, the moisture-permeable part 1 and the moisture-permeable part 2 all contain bamboo charcoal fiber; the windproof part 1 and the windproof part 2 are arranged opposite to each other and are supported by the heat-insulating part to form a heat-insulating cavity; the heat-insulating part is composed of a number of warp floats and a number of weft floats and is filled in the heat-insulating cavity.
[0007] The above explorations show that simply increasing thickness or introducing hydrophobic fibers is insufficient to achieve a synergistic effect of warmth and breathability in a single-layer, lightweight structure. While patented technologies employing double or triple-layer structures have improved fabric breathability to some extent and enhanced warmth, the resulting reduction in fabric softness and significantly decreased moisture permeability remains unresolved, and the overall performance in terms of both breathability and warmth is not ideal. In existing technologies, fabrics involving lyocell blends are mostly two- or three-component systems, and improvements in existing technologies often focus on single properties, such as improving warmth and shape retention by adding polyester or acrylic fibers, or inhibiting fibrillation through chemical finishing.
[0008] In other words, existing technologies have not revealed how to utilize the synergistic effects of multiple fibers to simultaneously achieve the following four objectives without any chemical crosslinking or fibrillation treatment: (1) obtaining high thermal resistance in a single-layer structure; (2) maintaining high moisture permeability of lyocell fabrics; (3) significantly improving anti-pilling and anti-fuzzing properties; and (4) effectively inhibiting fibrillation of lyocell fibers. The simultaneous achievement of these objectives involves not only the selection of the blending ratio but also the coordination between fiber characteristics and the preparation process. Developing a lyocell-based blended warm and breathable fabric with simple processing and excellent overall performance has urgent industrial demand and significant technological value. Summary of the Invention
[0009] In view of the shortcomings of the existing technology, the technical problem to be solved by the present invention is to provide a Lyocell blended napped fabric that simultaneously achieves high thermal resistance and high moisture permeability in a single-layer structure fabric by means of physical methods, while effectively suppressing fibrillation, improving anti-pilling performance, and effectively improving the wearing comfort of the fabric, and the preparation method thereof.
[0010] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for preparing a Lyocell blended napped fabric with both high moisture permeability and warmth retention, characterized by comprising the following steps:
[0011] I. Preparation of blended yarn:
[0012] (1) Prepare 40-50 parts of Lyocell fiber, 8-15 parts of wool fiber, and 30-40 parts of acrylic fiber by weight for later use;
[0013] (2) Mix Lyocell fiber, wool fiber and acrylic fiber according to the weight parts, and sequentially process them through opening, carding, drawing, roving and spinning. Use Siro compact spinning process to spin blended yarn with a yarn count of 40-60 English count and a twist of 850-1100 twists / m to obtain a Lyocell / wool / acrylic three-component blended yarn.
[0014] II. Fabric weaving:
[0015] (3) Place the blended yarn obtained in step (2) in an environment with a temperature of 20-25℃ and a relative humidity of 60%-70% and let it stand for 24 hours to balance. This will pre-treat the blended yarn and stabilize its moisture regain at 7%-9%.
[0016] (4) Take 5 to 10 parts by weight of spandex filament for later use;
[0017] (5) The blended yarn and spandex filament pretreated in step (3) are fed into a double rib circular knitting machine at the same time, and the fabric is woven using the double rib knitting process; wherein the spandex filament is fed in separately and participates in loop formation together with the blended yarn, and the fabric weight is 280-290 g / m². 2 ;
[0018] III. Physical finishing:
[0019] (6) The fabric woven in step (5) is pretreated by applying a napping agent working solution through padding.
[0020] (7) Use a wire roller napping machine to nap the fabric. The napping speed is set to 7-9 m / min and the nap height after napping is 0.3-0.5 mm.
[0021] (8) After the napping is completed, immediately send the fabric into the brushing machine and brush it twice with a double-sided soft brush roller to completely remove the loose hairs on the fabric surface. At the same time, straighten the direction of the pile to ensure that the pile is uniformly fluffy.
[0022] IV. Segmented Low-Temperature Shaping and Finishing:
[0023] (9) After brushing, the fabric is pre-conditioned by standing in an environment with a temperature of 25-30℃ and a relative humidity of 65%-70% for 15-20 minutes to stabilize the moisture content of the internal fibers of the fabric at 8%-10%.
[0024] (10) Select a needle plate tenter hot air setting machine to perform tentering and setting treatment on the greige fabric, and then pass through the first preheating zone, the second main setting zone and the third cooling zone in sequence.
[0025] (11) After finishing, the Lyocell blended napped fabric is obtained.
[0026] The above-mentioned method for preparing a lyocell blended fleece fabric with high moisture permeability and warmth includes step (1) with 46 parts lyocell fiber, 10 parts wool fiber, and 36 parts acrylic fiber; and step (4) with 8 parts spandex filament.
[0027] In the above-mentioned method for preparing a Lyocell blended fleece fabric with high moisture permeability and warmth, in step (2), the yarn count of the blended yarn is 50 English count and the twist is 980 twists / meter.
[0028] In the above-mentioned method for preparing Lyocell blended napped fabric with high moisture permeability and warmth, in step (6), the napping agent working solution is an organosilicon microemulsion with a mass fraction of 5-15 g / L, the padding temperature is 40-50℃, and the padding rate is 65%-75%.
[0029] In the above-mentioned method for preparing Lyocell blended napped fabric with high moisture permeability and warmth, in step (7), the needle cloth of the steel wire roller napping machine is 28-32 gauge high elasticity curved angle steel wire needle cloth, the needle cloth density is 450-550 teeth / square centimeter, the napping roller speed is 180-220 r / min, and the speed ratio of the linear velocity of the napping roller surface to the fabric travel speed is 20:1-25:1.
[0030] The above-mentioned method for preparing a Lyocell blended napped fabric with high moisture permeability and warmth, wherein step (7) involves a step-by-step napping process, specifically including the following steps:
[0031] 1) First pass of napping: napping along the longitudinal direction of the fabric surface, adjusting the contact pressure between the napping roller and the fabric to 0.2-0.3MPa, initially pulling out the short fibers on the surface;
[0032] 2) Second light backflushing: Gently pull in the opposite direction at a 30° angle to the first backflushing direction, adjust the contact pressure to 0.15-0.2MPa, and comb through the pile fibers pulled out in the first backflushing to make the pile distribution more even;
[0033] 3) Third round of nap trimming: Gently lift the fabric again along the longitudinal direction of the fabric surface to precisely control the nap height to 0.3-0.5mm, while sweeping away the loose hairs on the fabric surface.
[0034] In the above-mentioned method for preparing Lyocell blended napped fabric with high moisture permeability and warmth, during the stretching and setting process in step (10), the fabric feeding tension is 5-8 N / m, the fabric width is stretched to be 2%-3% larger than the target width of the finished product, and the needle plate penetration depth is 2-3 mm.
[0035] In the above-mentioned method for preparing a Lyocell blended fleece fabric with high moisture permeability and warmth, during the segmented low-temperature setting process in step (10), the temperature of the first preheating zone is set at 90-100℃, and the fabric stays in this zone for 20-30 seconds. The temperature of the second main setting zone is 100-120℃, the setting time is 1-1.5 minutes, and the hot air velocity is 12-15 m / s. In the third cooling zone, the fabric is immediately sent to the air-cooling zone after setting and rapidly cooled in an environment below 30℃ for 30-40 seconds, so that the fiber structure can be rapidly cooled and set, and the fluffy fleece surface can be locked.
[0036] In the above-mentioned method for preparing a Lyocell blended napped fabric that combines high moisture permeability and warmth, the temperature of the second main setting zone is 110℃, the setting time is 1.2min, and the hot air velocity is 13m / s.
[0037] A lyocell blended napped fabric with both high moisture permeability and warmth retention is prepared by the above-described method. The thermal resistance of the fabric is 0.042–0.047 μm. 2• K / W, moisture permeability 4463~4813 g / (m 2 •24h), the pilling and fuzzing level is 4-5.
[0038] The advantages of this invention, which combines a highly breathable and warm lyocell blended napped fabric with its preparation method, are as follows: Addressing the long-standing technical contradiction in the field of close-fitting thermal fabrics—the difficulty in simultaneously achieving warmth and breathability—and the inherent defect of lyocell fibers being prone to fibrillation during wear, this invention proposes a novel technical solution combining a four-fiber blend with physical napping. This invention completely abandons traditional chemical cross-linking and fibrillation treatments, relying solely on the synergistic combination of four fibers—lyocell, wool, acrylic, and spandex—in specific proportions, along with physical napping and low-temperature setting processes. This allows the fabric to achieve a synergistic balance between high thermal resistance and high moisture permeability within a single-layer structure. This combination utilizes the natural crimp of wool and the bulkiness of acrylic to create a highly efficient still air layer through napping, enhancing warmth. Furthermore, the lyocell-based fiber network maintains continuous moisture transport channels, unexpectedly overcoming the problem of significantly reduced moisture permeability caused by the bulky structure of conventional napped fabrics. Meanwhile, this specific fiber combination and physical napping process also significantly inhibits the fibrillation of lyocell, so the fabric does not undergo fibrillation after washing and has excellent anti-pilling and anti-fuzzing properties. Attached Figure Description
[0039] Figure 1 This is a front view of the Lyocell blended napped fabric obtained in Example 1 of the present invention.
[0040] Figure 2 This is a photograph of the back of the Lyocell blended napped fabric obtained in Example 1 of the present invention.
[0041] Figure 3 The image shows the front view of the Lyocell blended napped fabric prepared in Example 1 after three washes.
[0042] Figure 4 The image shows the front view of the Lyocell blended napped fabric prepared in Example 2 after three washes.
[0043] Figure 5 The image shows the front view of the Lyocell blended napped fabric prepared in Example 3 after three washes.
[0044] Figure 6 The frontal SEM image of the pure Lyocell knitted double-layer composite fabric prepared in Comparative Example 1 after three washes.
[0045] Figure 7 The image shows the frontal SEM image of the double-layer composite fabric of Lyocell knitted fabric and Lyocell / polyester interwoven fabric prepared in Comparative Example 2 after washing three times. Detailed Implementation
[0046] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0047] In this invention, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in its actual use or operating state, specifically the drawing directions in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc., are used merely as illustrative purposes and do not impose numerical requirements or establish an order. The term "multiple" means "two or more".
[0048] A method for preparing a Lyocell blended napped fabric that combines high moisture permeability and warmth includes the following steps:
[0049] I. Preparation of blended yarn:
[0050] (1) Prepare 40-50 parts of lyocell fiber, 8-15 parts of wool fiber, and 30-40 parts of acrylic fiber by weight for later use. Lyocell fiber serves as the main component, ensuring the fabric's high moisture permeability and skin-friendly, dry feel. If its content is below the above range, the moisture permeability advantage weakens; if it is above the above range, it will significantly increase the risk of fibrillation and reduce yarn bulk, which is not conducive to the formation of a uniform nap in subsequent napping. Wool fiber provides lasting bulkiness, elasticity, and warmth through its natural crimp structure; when the wool content is below 8%, the above effects are not significant; if it is above 15%, the fabric is prone to felting and shrinkage, and the cost increases. 30%-40% acrylic fiber supplements the volume bulk and is a key component for the formation of a uniform and efficient nap through physical napping. Spandex fiber gives the fabric the necessary elastic recovery and dimensional stability, preventing napping and structural deformation during use. The specific combination of the above four fibers solves the technical difficulty of balancing moisture permeability and warmth in traditional blended napped fabrics, and simultaneously achieves low fibrillation and high anti-pilling and anti-fuzzing grades after washing.
[0051] (2) Lyocell fiber, wool fiber and acrylic fiber are mixed in the weight proportions mentioned above, and then processed in sequence through opening, carding, drawing, roving and spinning. The blended yarn is spun using Siro compact spinning technology. The yarn count is 40-60 English count and the twist is 850-1100 twists / m. The blended yarn of Lyocell / wool / acrylic three components is obtained. The yarn count and twist ensure that the yarn has the necessary strength while retaining a moderately fluffy structure, providing a suitable fiber cohesion and napping foundation for subsequent napping finishing.
[0052] II. Fabric weaving:
[0053] (3) Place the blended yarn obtained in step (2) in an environment with a temperature of 20-25℃ and a relative humidity of 60%-70% and let it stand for 24 hours to balance. This pretreatment of the blended yarn will stabilize the moisture regain of the blended yarn at 7%-9%. The pretreatment can eliminate residual stress inside the yarn and avoid problems such as yarn breakage and uneven tension during weaving.
[0054] (4) Take 5 to 10 parts by weight of spandex filament for later use;
[0055] (5) The blended yarn and spandex filament pretreated in step (3) are fed into a double rib circular knitting machine at the same time, and the fabric is woven using the double rib knitting process; wherein the spandex filament is fed in separately and participates in loop formation together with the blended yarn, and the fabric weight is 280-290 g / m². 2 Spandex filaments provide the fabric with the necessary elastic recovery and dimensional stability, preventing pilling and structural deformation during subsequent use. The double rib knit structure offers excellent extensibility and structural stability, making it suitable for close-fitting wear and providing a uniform loop surface for pilling.
[0056] The specific weaving process is as follows:
[0057] a. Equipment selection
[0058] The equipment uses a double rib knitting machine with a gauge of 24-28G (24-28 needles per inch), which is suitable for knitting 40-60 count fine blended yarns and ensures a fine and uniform loop structure.
[0059] b. Alignment and adjustment of coiling machine parts
[0060] The needle groove of the lower needle cylinder and the needle groove of the upper needle plate of the double rib knitting machine are configured at 90° relative to each other, and the lower needle and the upper needle are arranged with one high heel needle and one low heel needle alternately.
[0061] Strictly calibrate the alignment of the upper and lower needles: the upper high heel needle is aligned with the lower low heel needle, and the upper low heel needle is aligned with the lower high heel needle, so that the two 1+1 rib structures are precisely combined to form a standard double rib structure.
[0062] c. Step-by-step loop knitting control
[0063] Unwinding loop: Use a synchronous start-up method where the lower needle leads the upper needle by 1 to 3 stitches. The lower needle comes out first to hold the fabric, preventing the fabric from flowing out of the cylinder when the lower needle is unwinding, reducing fabric defects, and keeping the tension at a low level.
[0064] Yarn padding: A delayed loop-forming process is adopted, with yarn padding before the needle goes down. The position of the yarn guide is adjusted with the needle going down as the core and also takes into account the yarn padding position of the needle going up. The yarn padding tension is stably controlled at 3.5±0.2cN. The spandex filament is fed separately using an active yarn feeding method, and the yarn feeding tension is independently controlled to ensure that the loop-forming of the blended yarn and the spandex filament is synchronized and the ratio is stable.
[0065] Yarn bending into loops: The yarn bending process is adopted. The lower needle first hooks the yarn to complete the pre-bending, and then the upper needle is raised to distribute part of the yarn to the upper needle. The upper and lower needles complete the final bending at the same time. The loop length uniformity CV value is controlled at ≤2.1% to ensure that there are no sparse or dense lines on the fabric surface.
[0066] Pulling: The pulling mechanism adopts a continuous and uniform pulling mode, and the pulling tension is controlled at 8-12N to ensure that the fabric is smoothly released from the looping area and to avoid loop displacement and loose or tight streaks on the fabric surface.
[0067] d. Precise weight control
[0068] During the weaving process, the row density of the loops is monitored in real time and controlled at 14-16 rows per centimeter, and the warp density is controlled at 12-14 warps per centimeter. The loop length is finely adjusted by adjusting the tension speed, and the weight per square meter of the fabric is precisely locked at 280-290 g / m². 2 .
[0069] After weaving, the greige fabric is naturally relaxed and stacked for 24 hours to eliminate weaving tension. The weight is then re-measured, and the deviation is controlled within ±3-5%. Unqualified greige fabrics are re-woven by adjusting the process.
[0070] e. Quality inspection before unloading
[0071] Inspect the surface of the fabric to confirm that there are no broken yarns, holes, uneven weaves, horizontal stripes, or other weaving defects. The double rib weave has loops on both sides and no missed stitches or misaligned patterns.
[0072] Verify that the width of the greige fabric is controlled between 185 and 190 cm, and that the fabric surface is flat and without curling edges, meeting the quality requirements for double rib greige fabric.
[0073] f. Dyeing and finishing
[0074] The dyeing and finishing process for the above-mentioned greige fabric is as follows: greige fabric preparation → pre-forming → pretreatment → dyeing → finishing. Among these, greige fabric preparation is used to check the quality and measurement of the greige fabric; pre-forming is used to stabilize the greige fabric dimensions; pretreatment is used to remove impurities from the fiber surface; dyeing is used to impart color to the fabric; and finishing is used to improve the hand feel and fabric style.
[0075] It should be noted that no chemical cross-linking or antigenic fiberization treatment is performed during the dyeing and finishing process of this invention, so as to maintain the technical feature of "completely abandoning chemical cross-linking and antigenic fiberization treatment" of this invention, thereby maintaining the high moisture permeability and environmental friendliness of the fabric.
[0076] III. Physical finishing:
[0077] (6) The fabric woven in step (5) is pretreated by applying a raising agent working solution through padding. The raising agent working solution is an organosilicon microemulsion with a mass fraction of 5-15 g / L. The padding temperature is 40-50℃ and the padding rate is 65%-75%. The raising agent can form a uniform lubricating film on the fiber surface, reduce the friction coefficient between fibers and between fibers and the raising needle cloth, facilitate the smooth pulling of fibers during raising without breaking them, reduce shedding and fiber damage, and make the pile surface fuller, more uniform and delicate.
[0078] After pretreatment, the fabric is allowed to relax naturally for 10-15 minutes to eliminate internal stress accumulated during weaving and dyeing, ensuring uniform fabric tension during subsequent napping. It should be noted that the napping agent is a conventional process aid in napping, serving only a physical auxiliary role in lubrication and friction reduction. It does not participate in the chemical cross-linking and modification of the fibers, nor is it an antigen-fibering finishing agent. Therefore, its use does not affect the core technical feature of this invention: "no chemical cross-linking or antigen-fibering treatment."
[0079] The specific process is as follows:
[0080] a. Raising equipment and card cloth configuration
[0081] A steel wire roller raising machine (such as the Italian LAFA raising machine) is selected, using 28-32 gauge high-elasticity curved steel wire needle cloth. The needle cloth density is controlled at 450-550 teeth / cm², which is suitable for the fiber characteristics of Lyocell blended fabrics and reduces shedding caused by excessive raising. The raising roller speed is set to 180-220 r / min, and the speed ratio of the linear velocity of the raising roller surface to the fabric travel speed is controlled at 20:1-25:1 to ensure a gentle and uniform raising force.
[0082] b. Step-by-step napping operation process
[0083] First pass of napping (pulling): Pile the nap along the longitudinal direction of the fabric surface. Adjust the contact pressure between the napping roller and the fabric to 0.2-0.3 MPa to initially pull out the short fibers on the surface and avoid excessive napping in some areas.
[0084] Second light backflushing: Gently pull in the opposite direction of the first backflushing at a 30° angle, adjusting the contact pressure to 0.15-0.2 MPa, and comb through the nap pulled out in the first backflushing to make the nap distribution more even.
[0085] The third round of nap trimming: Gently lift the fabric again along its longitudinal direction to precisely control the nap height within the range of 0.3 to 0.5 mm, while sweeping away any loose fibers to reduce shedding during subsequent use.
[0086] Shearing: Use a shearing machine to remove excessively long loose hairs that exceed the target pile height, so that the pile height is uniform.
[0087] Combing: The nap is combed using a combing machine to straighten the nap direction and improve the fluffiness and uniformity of the nap.
[0088] Heat treatment: The velvet surface is lightly heat-treated using a heat treatment machine to make the velvet surface smooth and stable in shape.
[0089] c. Immediate treatment after napping
[0090] After the napping is completed, the fabric is immediately fed into the brushing machine and brushed twice with soft brush rollers in both directions to thoroughly remove loose hairs from the fabric surface. At the same time, the nap direction is straightened to ensure that the nap fluffiness is consistent.
[0091] (7) A steel wire roller raising machine is used to raise the fabric, which goes through the following processes: raising, shearing, combing, and calendering. The raising speed is set to 7-9 m / min, and the pile height after raising is 0.3-0.5 mm. The steel wire roller raising machine uses 28-32 gauge high-elasticity curved steel wire needle cloth with a needle cloth density of 450-550 teeth / cm². The raising roller speed is 180-220 r / min, and the speed ratio of the linear velocity of the raising roller surface to the fabric travel speed is 20:1-25:1.
[0092] This process can form a uniform, fine, fluffy nap layer on the fabric surface, effectively constructing a stable still air layer to increase thermal resistance. At the same time, it controls the nap density and height to avoid blocking moisture channels, thereby improving warmth retention while maintaining high moisture permeability. No chemical napping agents or bulking agents are applied during the napping process.
[0093] (8) After the napping is completed, immediately send the fabric into the brushing machine and brush it twice with a double-sided soft brush roller to completely remove the loose hairs on the fabric surface. At the same time, straighten the direction of the pile to ensure that the pile is uniformly fluffy.
[0094] IV. Segmented Low-Temperature Shaping and Finishing:
[0095] (9) After brushing, the fabric is pre-conditioned and placed in an environment with a temperature of 25-30℃ and a relative humidity of 65%-70% for 15-20 minutes to stabilize the moisture content of the internal fibers of the fabric at 8%-10%; avoid direct high-temperature setting which will cause the pile to flatten and the hand to become hard.
[0096] (10) A needle-plate tenter type hot air setting machine is used to perform tentering and setting treatment on the greige fabric. During the tentering and setting process, the fabric tension is 5-8 N / meter. A low-tension fabric feeding mode is adopted to avoid excessive stretching that would cause loss of elasticity of the spandex fibers and ensure the high elasticity recovery performance of the fabric in the future. When feeding the fabric, the width of the greige fabric is stretched to 2%-3% larger than the target width of the finished product, and the needle plate penetration depth is 2-3 mm. This ensures that the fabric surface is flat and wrinkle-free without damaging the napped structure of the surface layer. Then, it passes through the first preheating zone, the second main setting zone, and the third cooling zone in sequence; specifically:
[0097] First preheating zone: The temperature is set to 90-100℃. The fabric stays in this zone for 20-30 seconds to allow the fabric to heat up slowly and the fibers to soften gradually, avoiding the rapid collapse of the pile caused by instantaneous high temperature.
[0098] The second main setting zone: the temperature is precisely controlled at 100-120℃, the setting time is strictly controlled at 1-1.5min, the hot air speed is adjusted to 12-15m / s, and a penetrating hot air circulation is adopted to ensure that the fabric is heated evenly on both sides, which not only fixes the nap shape after the napping, but also prevents the wool and spandex fibers from being overheated and deteriorating in performance.
[0099] The third cooling zone: The shaped fabric is immediately sent to the air-cooling zone and rapidly cooled for 30-40 seconds in an environment below 30℃. This allows the fiber structure to cool and set quickly, locking in the fluffy pile and preventing the pile from sticking and flattening due to pressure after leaving the machine.
[0100] After the segmented low-temperature setting process is completed, a post-setting quality inspection is conducted. The fabric width shrinkage rate is checked to ensure dimensional stability meets standards. The pile height is measured, with a drop not exceeding 0.05mm, ensuring the pile remains fluffy and full after setting.
[0101] The segmented low-temperature setting process of the present invention does not add any chemical crosslinking agents or resin finishing agents throughout the entire process. It achieves dimensional stability and fixation of the pile surface shape of the fabric only through this gentle physical heat setting, and avoids damage to the spandex and wool fibers caused by high temperature.
[0102] (11) After finishing, the Lyocell blended napped fabric is obtained. For example... Figure 1 , 2 As shown, the thermal resistance of this fabric is 0.042–0.047 μm. 2 • K / W, moisture permeability 4463~4813 g / (m 2 •24h), the pilling and fuzzing level is 4-5.
[0103] The present application will be specifically described below through specific embodiments. The following embodiments are only some embodiments of the present application and are not intended to limit the present application.
[0104] Example 1
[0105] A method for preparing a Lyocell blended napped fabric that combines high moisture permeability and warmth includes the following steps:
[0106] I. Preparation of blended yarn:
[0107] (1) Prepare 46 parts of Lyocell fiber, 10 parts of wool fiber and 36 parts of acrylic fiber by weight for later use;
[0108] (2) The Lyocell fiber, wool fiber and acrylic fiber are mixed according to the weight parts, and then processed through opening, carding, drawing, roving and spinning processes in sequence. The blended yarn is spun using Siro compact spinning process, with a yarn count of 50 English count and a twist of 980 twists / m, to obtain a Lyocell / wool / acrylic three-component blended yarn.
[0109] II. Fabric Weaving:
[0110] (3) Place the blended yarn obtained in step (2) in an environment with a temperature of 23°C and a relative humidity of 65% for 24 hours to allow it to stand and balance. This will pre-treat the blended yarn and stabilize its moisture regain at 8%.
[0111] (4) Take 8 parts of spandex filament by weight and set aside;
[0112] (5) The blended yarn and spandex filament pretreated in step (3) are fed into a double rib circular knitting machine at the same time, and the fabric is woven using the double rib knitting process; wherein the spandex filament is fed in separately and participates in loop formation together with the blended yarn, and the fabric weight is 285g / m². 2 ;
[0113] III. Physical finishing:
[0114] (6) The fabric woven in step (5) is pretreated by applying a napping agent working solution through padding; the napping agent working solution is an organosilicon microemulsion with a mass fraction of 10 g / L, the padding temperature is 45℃, and the padding rate is 70%;
[0115] (7) A steel wire roller raising machine is used to raise the fabric. The raising speed is set to 8 m / min, and the pile height after raising is 0.4 mm. The steel wire roller raising machine uses No. 30 high-elasticity curved steel wire needle cloth with a needle cloth density of 500 teeth / square centimeter. The raising roller speed is 200 r / min, and the speed ratio of the linear velocity of the raising roller surface to the fabric travel speed is 22:1. The raising process is a step-by-step raising process, which includes the following steps:
[0116] 1) First pass of napping: napping along the longitudinal direction of the fabric surface, adjusting the contact pressure between the napping roller and the fabric to 0.25 MPa, initially pulling out the surface short fibers;
[0117] 2) Second light backflushing: Gently pull in the opposite direction at a 30° angle to the first backflushing direction, adjust the contact pressure to 0.18MPa, and comb through the pile fibers pulled out in the first backflushing to make the pile surface more evenly distributed;
[0118] 3) Third pass of nap trimming: Gently lift the fabric again along the longitudinal direction of the fabric surface to precisely control the nap height at 0.4mm, while sweeping away the loose hairs on the fabric surface.
[0119] (8) After the napping is completed, immediately send the fabric into the brushing machine and brush it twice with a double-sided soft brush roller to completely remove the loose hairs on the fabric surface. At the same time, straighten the direction of the pile to ensure that the pile is uniformly fluffy.
[0120] IV. Segmented Low-Temperature Shaping and Finishing:
[0121] (9) After brushing, the fabric is pre-conditioned by standing in an environment with a temperature of 25-30℃ and a relative humidity of 65%-70% for 15-20 minutes to stabilize the moisture content of the internal fibers of the fabric at 8%-10%.
[0122] (10) Use a needle plate tenter hot air setting machine to perform tentering and setting treatment on the fabric. During the tentering and setting process, the fabric tension is 5-8 N / m. When feeding the fabric, stretch the fabric width to 2%-3% larger than the target width of the finished product. The needle plate penetration depth is 2-3 mm.
[0123] The fabric then passes through the first preheating zone, the second main setting zone, and the third cooling zone in sequence. The temperature in the first preheating zone is set at 95℃, and the fabric stays in this zone for 25 seconds. The temperature in the second main setting zone is 110℃, the setting time is 1.2 minutes, and the hot air velocity is 13 m / s. In the third cooling zone, the fabric is immediately sent to the air-cooling zone after setting and rapidly cooled for 35 seconds in an environment below 30℃, so that the fiber structure can be quickly cooled and set, locking in the fluffy pile.
[0124] (11) After finishing, the Lyocell blended napped fabric is obtained.
[0125] The thermal resistance of the Lyocell blended napped fabric prepared in this embodiment is 0.045m. 2 ·K / W, moisture permeability 4681g / (m 2 •24h), the pilling and fuzzing level is 4-5.
[0126] Example 2
[0127] A method for preparing a Lyocell blended napped fabric that combines high moisture permeability and warmth includes the following steps:
[0128] I. Preparation of blended yarn:
[0129] (1) Prepare 40 parts of Lyocell fiber, 15 parts of wool fiber and 40 parts of acrylic fiber by weight for later use;
[0130] (2) The Lyocell fiber, wool fiber and acrylic fiber are mixed according to the weight parts, and then processed through opening, carding, drawing, roving and spinning in sequence. The blended yarn is spun using Siro compact spinning process, with a yarn count of 40 English count and a twist of 850 twists / m, to obtain a Lyocell / wool / acrylic three-component blended yarn.
[0131] II. Fabric weaving:
[0132] (3) Place the blended yarn obtained in step (2) in an environment with a temperature of 20℃ and a relative humidity of 60% for 24 hours to allow it to stand and balance. This will pre-treat the blended yarn and stabilize its moisture regain at 7%.
[0133] (4) Take 5 parts of spandex filament by weight and set aside;
[0134] (5) The blended yarn and spandex filament pretreated in step (3) are simultaneously fed into a double rib circular knitting machine, and the fabric is woven using a double rib knitting process; wherein the spandex filament is fed separately and participates in loop formation together with the blended yarn, and the fabric weight is 280g / m². 2 ;
[0135] III. Physical finishing:
[0136] (6) The fabric woven in step (5) is pretreated by applying a napping agent working solution through padding; the napping agent working solution is a silicone microemulsion with a mass fraction of 5 g / L, the padding temperature is 50℃, and the padding rate is 75%;
[0137] (7) A steel wire roller raising machine is used to raise the fabric. The raising speed is set to 7 m / min, and the pile height after raising is 0.3 mm. The steel wire roller raising machine uses No. 28 high-elasticity curved steel wire needle cloth with a needle cloth density of 450 teeth / cm². The raising roller speed is 180 r / min, and the speed ratio of the linear velocity of the raising roller surface to the fabric travel speed is 20:1. The raising process is a step-by-step raising process, which includes the following steps:
[0138] 1) First pass of napping: napping along the longitudinal direction of the fabric surface, adjusting the contact pressure between the napping roller and the fabric to 0.2MPa, initially pulling out the surface short fibers;
[0139] 2) Second light backflushing: Gently pull in the opposite direction at a 30° angle to the first backflushing direction, adjust the contact pressure to 0.15MPa, and comb through the pile pulled out in the first backflushing to make the pile distribution more even.
[0140] 3) Third pass of nap trimming: Gently lift the fabric again along the longitudinal direction of the fabric surface to precisely control the nap height to 0.3mm, while sweeping away the loose hairs on the fabric surface.
[0141] (8) After the napping is completed, immediately send the fabric into the brushing machine and brush it twice with a double-sided soft brush roller to completely remove the loose hairs on the fabric surface. At the same time, straighten the direction of the pile to ensure that the pile is uniformly fluffy.
[0142] IV. Segmented Low-Temperature Shaping and Finishing:
[0143] (9) After brushing, the fabric is pre-conditioned by standing in an environment with a temperature of 25-30℃ and a relative humidity of 65%-70% for 15-20 minutes to stabilize the moisture content of the internal fibers of the fabric at 8%-10%.
[0144] (10) Use a needle plate tenter hot air setting machine to perform tentering and setting treatment on the fabric. During the tentering and setting process, the fabric tension is 5-8 N / m. When feeding the fabric, stretch the fabric width to 2%-3% larger than the target width of the finished product. The needle plate penetration depth is 2-3 mm.
[0145] The fabric then passes through the first preheating zone, the second main setting zone, and the third cooling zone in sequence. The temperature in the first preheating zone is set at 90℃, and the fabric stays in this zone for 30 seconds. The temperature in the second main setting zone is 100℃, the setting time is 1.5 minutes, and the hot air velocity is 12 m / s. In the third cooling zone, the fabric is immediately sent to the air-cooling zone after setting and rapidly cooled for 30 seconds in an environment below 30℃, so that the fiber structure can be quickly cooled and set, locking in the fluffy pile.
[0146] (11) After finishing, the Lyocell blended napped fabric is obtained.
[0147] The thermal resistance of the Lyocell blended napped fabric prepared in this embodiment is 0.047m. 2 ·K / W, moisture permeability 4463g / (m 2 •24h), the pilling and fuzzing level is 4-5.
[0148] Example 3
[0149] A method for preparing a Lyocell blended napped fabric that combines high moisture permeability and warmth includes the following steps:
[0150] I. Preparation of blended yarn:
[0151] (1) Prepare 50 parts of Lyocell fiber, 8 parts of wool fiber, and 30 parts of acrylic fiber by weight for later use;
[0152] (2) The Lyocell fiber, wool fiber and acrylic fiber are mixed in the weight proportions mentioned above, and then processed through opening, carding, drawing, roving and spinning processes in sequence. The blended yarn is spun using Siro compact spinning process, with a yarn count of 60 English count and a twist of 1100 twists / m, to obtain a Lyocell / wool / acrylic three-component blended yarn.
[0153] II. Fabric weaving:
[0154] (3) Place the blended yarn obtained in step (2) in an environment with a temperature of 25°C and a relative humidity of 70% and let it stand for 24 hours to balance. This will pre-treat the blended yarn and stabilize its moisture regain at 9%.
[0155] (4) Take 10 parts of spandex filament by weight and set aside;
[0156] (5) The blended yarn and spandex filament pretreated in step (3) are fed into a double rib circular knitting machine at the same time, and the fabric is woven using the double rib knitting process; wherein the spandex filament is fed in separately and participates in loop formation together with the blended yarn, and the fabric weight is 290g / m². 2 ;
[0157] III. Physical finishing:
[0158] (6) The fabric woven in step (5) is pretreated by applying a napping agent working solution through padding; the napping agent working solution is an organosilicon microemulsion with a mass fraction of 15 g / L, the padding temperature is 40℃, and the padding rate is 65%;
[0159] (7) A steel wire roller raising machine is used to raise the fabric. The raising speed is set to 9 m / min, and the pile height after raising is 0.5 mm. The steel wire roller raising machine uses No. 32 high-elasticity curved steel wire needle cloth with a needle cloth density of 550 teeth / square centimeter. The raising roller speed is 220 r / min, and the speed ratio of the linear velocity of the raising roller surface to the fabric travel speed is 25:1. The raising process is a step-by-step raising process, which includes the following steps:
[0160] 1) First pass of napping: napping along the longitudinal direction of the fabric surface, adjusting the contact pressure between the napping roller and the fabric to 0.3MPa, initially pulling out the surface short fibers;
[0161] 2) Second light backflushing: Gently pull in the opposite direction at a 30° angle to the first backflushing direction, adjust the contact pressure to 0.2MPa, and comb through the pile pulled out in the first backflushing to make the pile surface more evenly distributed;
[0162] 3) Third pass of nap trimming: Gently lift the fabric again along the longitudinal direction of the fabric surface to precisely control the nap height to 0.5mm, while sweeping away the loose hairs on the fabric surface.
[0163] (8) After the napping is completed, immediately send the fabric into the brushing machine and brush it twice with a double-sided soft brush roller to completely remove the loose hairs on the fabric surface. At the same time, straighten the direction of the pile to ensure that the pile is uniformly fluffy.
[0164] IV. Segmented Low-Temperature Shaping and Finishing:
[0165] (9) After brushing, the fabric is pre-conditioned by standing in an environment with a temperature of 25-30℃ and a relative humidity of 65%-70% for 15-20 minutes to stabilize the moisture content of the internal fibers of the fabric at 8%-10%.
[0166] (10) Use a needle plate tenter hot air setting machine to perform tentering and setting treatment on the fabric. During the tentering and setting process, the fabric tension is 5-8 N / m. When feeding the fabric, stretch the fabric width to 2%-3% larger than the target width of the finished product. The needle plate penetration depth is 2-3 mm.
[0167] The fabric then passes through the first preheating zone, the second main setting zone, and the third cooling zone in sequence. The temperature in the first preheating zone is set at 100℃, and the fabric stays in this zone for 20 seconds. The temperature in the second main setting zone is 120℃, the setting time is 1 minute, and the hot air velocity is 15 m / s. In the third cooling zone, the fabric is immediately sent to the air-cooling zone after setting and rapidly cooled in an environment below 30℃ for 40 seconds, so that the fiber structure can be quickly cooled and set, locking in the fluffy pile.
[0168] (11) After finishing, the Lyocell blended napped fabric is obtained.
[0169] The thermal resistance of the Lyocell blended napped fabric prepared in this embodiment is 0.042m. 2 ·K / W, moisture permeability 4813g / (m 2 •24h), the pilling and fuzzing level is 4-5.
[0170] Comparative Example 1
[0171] This comparative example is a pure Lyocell knitted double-layer composite fabric, without blending with other fibers or napping treatment, and is directly woven and then regularly shaped.
[0172] Comparative Example 2
[0173] This comparative example is a double-layer composite fabric of lyocell knitted fabric and lyocell / polyester interwoven fabric, which is woven directly without napping treatment and then regularly shaped.
[0174] The performance test results of the Lyocell blended fleece fabric with both high moisture permeability and warmth prepared by this invention are as follows:
[0175] The test methods are as follows: Thermal resistance was determined according to GB / T 11048-2018 using the evaporative hot plate method. Moisture permeability was determined according to GB / T 12704.2-2009 Method A (positive cup method), under constant temperature conditions of 38℃ and 50% relative humidity, with the 24-hour moisture permeability calculated based on the mass loss of the permeability cup per unit time. Pilling and fuzzing were assessed by washing three times using the 4N washing program of a European standard washing machine and then drying, with the grade determined using standard samples. Flavofibrillation was assessed by washing three times using the 4N program in ISO 6330 and then drying, with subjective evaluation based on the fiber morphology observed using a scanning electron microscope. The test results of Examples 1-3 and Comparative Examples 1-2 are shown in Table 1.
[0176] Table 1 Performance test results of the examples and comparative examples
[0177] Sample Name Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 <![CDATA[Thermal resistance (m 2 ·K / W)]]> 0.045 0.047 0.042 0.017 0.019 <![CDATA[Water Vapor Transmission Rate (g / (m 2 ·24h))]]> 4681 4463 4813 5690 4461 pilling level 4-5 4-5 4-5 3-4 4
[0178] As shown in Table 1, the thermal resistance of Examples 1, 2, and 3 of the present invention reached 0.045 μm. 2 ·K / W, 0.047 m 2 ·K / W and 0.042 m 2 • K / W, significantly higher than Comparative Example 1 (0.017 m 2 The results of Example 1 (0.019 m²·K / W) and Comparative Example 2 (0.019 m²·K / W) demonstrate that this fabric achieves significantly improved warmth retention even with a single-layer structure. On the other hand, the moisture permeability of Examples 1, 2, and 3 are 4681 g / (m²·K / W). 2 ·24h), 4463g / (m 2 ·24h) and 4815g / (m 2 (24h), despite having a much higher thermal resistance than the comparative example, it still maintained excellent moisture permeability. Of particular note is its superior performance compared to the double-layer composite fabric with polyester (Comparative Example 2, moisture permeability 4461 g / (m²)). 2 (24h) The embodiments of the present invention demonstrate significantly superior warmth retention while also exhibiting good moisture permeability, highlighting the unique advantages of the four-fiber combination and physical napping structure in enhancing both warmth retention and moisture permeability. This result indicates that the present invention, through the combination of fiber ratio and napping process, significantly improves the thermal resistance of the fabric without sacrificing moisture permeability, instead stabilizing it within a high range.
[0179] like Figure 3-7 As shown, the anti-pilling and anti-fuzzing grades of Examples 1-3 are all 4-5, which is superior to the 3-4 grades of Comparative Example 1 and the 4 grades of Comparative Example 2. Taking Example 1 as an example, the electron microscope images after 3 washes ( Figure 3 The results showed that fibrillation was basically not observed on the fabric surface, while comparative examples 1 and 2 (…) Figure 6 , Figure 7The fibrillation of Lyocell fibers was evident. This further demonstrates the effectiveness of the specific four-fiber ratio and physical napping process of this invention in inhibiting fibrillation.
[0180] It should be noted that those skilled in the art generally believe that lyocell fibers, without chemical crosslinking or antifibrillation finishing, will inevitably undergo severe fibrillation after friction and washing. However, this invention, by completely abandoning chemical crosslinking, achieves significant inhibition of lyocell fibrillation solely through the synergistic effect of a specific four-fiber combination and a physical napping process. Figure 3 Furthermore, the fabric exhibits an anti-pilling rating of 4-5. This finding was unexpected, as pilling processes are generally considered to exacerbate fiber surface damage. Actual wear tests using the fabric as close-fitting thermal underwear revealed consistent positive feedback from participants: the fabric was soft and skin-friendly, provided significant warmth, and exhibited no stuffiness or dampness during exercise or sitting, remaining dry and comfortable even after extended wear. After multiple washes, there was no significant pilling or deformation, demonstrating good durability. This invention features a simple process, eliminates the use of organic solvents and crosslinking agents, is environmentally friendly, and has controllable costs, providing an industrial-scale preparation approach for high-performance close-fitting thermal fabrics that differs from existing chemical modification routes.
[0181] Of course, the above description is not intended to limit the present invention, and the present invention is not limited to the examples given above. Any changes, modifications, additions or substitutions made by those skilled in the art within the scope of the present invention should be protected by the present invention.
Claims
1. A method for preparing a Lyocell blended napped fabric that combines high moisture permeability and warmth retention, characterized in that, Includes the following steps: I. Preparation of blended yarn: (1) Prepare 40-50 parts of Lyocell fiber, 8-15 parts of wool fiber, and 30-40 parts of acrylic fiber by weight for later use; (2) Mix Lyocell fiber, wool fiber and acrylic fiber according to the weight parts, and sequentially process them through opening, carding, drawing, roving and spinning. Use Siro compact spinning process to spin blended yarn with a yarn count of 40-60 English count and a twist of 850-1100 twists / m to obtain a Lyocell / wool / acrylic three-component blended yarn. II. Fabric Weaving: (3) Place the blended yarn obtained in step (2) in an environment with a temperature of 20-25℃ and a relative humidity of 60%-70% and let it stand for 24 hours to balance. This will pre-treat the blended yarn and stabilize its moisture regain at 7%-9%. (4) Take 5 to 10 parts by weight of spandex filament for later use; (5) The blended yarn and spandex filament pretreated in step (3) are fed into a double rib circular knitting machine at the same time, and the fabric is woven using the double rib knitting process; wherein the spandex filament is fed in separately and participates in loop formation together with the blended yarn, and the fabric weight is 280-290 g / m². 2 ; III. Physical finishing: (6) The fabric woven in step (5) is pretreated by applying a napping agent working solution through padding. (7) Use a wire roller napping machine to nap the fabric. The napping speed is set to 7-9 m / min and the nap height after napping is 0.3-0.5 mm. (8) After the napping is completed, immediately send the fabric into the brushing machine and brush it twice with a double-sided soft brush roller to completely remove the loose hairs on the fabric surface. At the same time, straighten the direction of the pile to ensure that the pile is uniformly fluffy. IV. Segmented Low-Temperature Shaping and Finishing: (9) After brushing, the fabric is pre-conditioned by standing in an environment with a temperature of 25-30℃ and a relative humidity of 65%-70% for 15-20 minutes to stabilize the moisture content of the internal fibers of the fabric at 8%-10%. (10) Select a needle plate tenter hot air setting machine to perform tentering and setting treatment on the greige fabric, and then pass through the first preheating zone, the second main setting zone and the third cooling zone in sequence. (11) After finishing, the Lyocell blended napped fabric is obtained.
2. The method for preparing the Lyocell blended napped fabric with high moisture permeability and warmth retention according to claim 1, characterized in that: In step (1), there are 46 parts of lyocell fiber, 10 parts of wool fiber, and 36 parts of acrylic fiber; in step (4), there are 8 parts of spandex filament.
3. The method for preparing the Lyocell blended napped fabric with high moisture permeability and warmth retention according to claim 1, characterized in that: In step (2), the yarn count of the blended yarn is 50 English count and the twist is 980 twists / meter.
4. The method for preparing the Lyocell blended napped fabric with high moisture permeability and warmth as described in claim 1, characterized in that: In step (6), the working solution of the hair-raising agent is an organosilicon microemulsion with a mass fraction of 5-15 g / L, the padding temperature is 40-50℃, and the padding rate is 65%-75%.
5. The method for preparing the Lyocell blended napped fabric with high moisture permeability and warmth retention according to claim 1, characterized in that: In step (7), the needle cloth of the steel wire roller raising machine is 28 to 32 high elasticity curved steel wire needle cloth, the needle cloth density is 450 to 550 teeth / square centimeter, the raising roller speed is 180 to 220 r / min, and the speed ratio of the linear velocity of the raising roller surface to the speed of the fabric surface is 20:1 to 25:
1.
6. The method for preparing the Lyocell blended napped fabric with high moisture permeability and warmth retention according to claim 1, characterized in that: In step (7), the napping finishing is a step-by-step napping process, which specifically includes the following steps: 1) First pass of napping: napping along the longitudinal direction of the fabric surface, adjusting the contact pressure between the napping roller and the fabric to 0.2-0.3MPa, initially pulling out the short fibers on the surface; 2) Second light backflushing: Gently pull in the opposite direction at a 30° angle to the first backflushing direction, adjust the contact pressure to 0.15-0.2MPa, and comb through the pile fibers pulled out in the first backflushing to make the pile distribution more even; 3) Third round of nap trimming: Gently lift the fabric again along the longitudinal direction of the fabric surface to precisely control the nap height to 0.3-0.5mm, while sweeping away the loose hairs on the fabric surface.
7. The method for preparing the Lyocell blended napped fabric with high moisture permeability and warmth as described in claim 1, characterized in that: During the stretching and setting process in step (10), the fabric tension is 5-8 N / meter, and the fabric width is stretched to be 2%-3% larger than the target width of the finished product. The needle plate penetration depth is 2-3 mm.
8. The method for preparing the Lyocell blended napped fabric with high moisture permeability and warmth retention according to claim 1, characterized in that: In the segmented low-temperature setting process of step (10), the temperature of the first preheating zone is set at 90-100℃, and the fabric stays in this zone for 20-30 seconds. The temperature of the second main setting zone is 100-120℃, the setting time is 1-1.5 minutes, and the hot air velocity is 12-15 m / s. In the third cooling zone, the fabric is immediately sent to the air-cooling zone after setting and rapidly cooled in an environment below 30℃ for 30-40 seconds, so that the fiber structure can be rapidly cooled and set, and the fluffy pile surface can be locked.
9. The method for preparing the Lyocell blended napped fabric with high moisture permeability and warmth retention according to claim 8, characterized in that: The temperature of the second main shaping zone is 110℃, the shaping time is 1.2min, and the hot air velocity is 13m / s.
10. A Lyocell blended napped fabric that combines high moisture permeability and warmth, characterized in that: The fabric, prepared by the method according to any one of claims 1-9, has a thermal resistance of 0.042–0.047 μm. 2 • K / W, moisture permeability 4463~4813 g / (m 2 •24h), the pilling and fuzzing level is 4-5.
Citation Information
Patent Citations
Double-layer light warm-keeping fabric and manufacturing process
CN116100873A
Moisture-permeable warm-keeping composite fabric and processing method thereof
CN121250612A