A method for preparing a pet micro / nano cross-scale fiber nonwoven material

By employing piezoelectric jet injection and high-speed airflow stretching technology, the problem of uniform distribution of nanofibers in micron-sized fiber skeletons has been solved, forming stable cross-scale fiber assemblies, improving the filtration performance and flexibility of the material, and adapting to the needs of wide-scale production.

CN123153218APending Publication Date: 2026-11-24HARBIN INST OF TECH AT WEIHAI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611538047.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing methods for preparing composite materials of micron-fibers and nanofibers suffer from problems such as easy agglomeration of nanofibers, difficulty in uniform dispersion, and insufficient bonding strength. Furthermore, it is difficult to achieve continuous and uniform coverage over a wide range, which affects the cross-scale structural stability and performance of the materials.

Method used

By combining piezoelectric jetting technology with high-speed airflow stretching, nanofibers are uniformly distributed in a micron-scale framework through the construction of a micron-fiber web, nanofiber jetting, secondary airflow stretching, and electrostatic embedding. Stable multi-scale fiber assemblies are formed by uniform deposition control in the width direction.

Benefits of technology

This method achieves uniform dispersion of nanofibers in a micron-fiber framework, increases the specific surface area and filtration performance of the material, enhances its flexibility and breathability, adapts to different production needs, and improves production efficiency and material utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153218A_ABST
    Figure CN123153218A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing PET micro / nano-scale cross-scale fiber nonwoven materials. Micron-sized chopped PET fibers are opened and combed to obtain a micron-fiber web. Nanoscale PET fibers are then ejected from the micron-fiber web using a piezoelectric jet to form a nascent PET fiber stream. This nascent PET fiber stream undergoes secondary stretching through high-temperature compressed air, and under the influence of airflow and electrostatic adsorption, it penetrates the interior of the micron-fiber web along its thickness direction, forming an embedded cross-scale fiber assembly. The cross-scale fiber assembly is then hot-pressed to obtain the PET micro / nano-scale cross-scale fiber nonwoven material. This invention enables PET nanofibers to enter the interior of the PET micron-fiber web, forming a non-surface-coated three-dimensional cross-scale embedded structure. It solves the problems of existing nanofiber layers mainly deposited on the surface of micron-based substrates, easy agglomeration of nanofibers, insufficient interfacial bonding stability, and difficulties in large-width continuous fabrication.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nonwoven technology, specifically to a method for preparing PET micro / nano-scale multi-scale fiber nonwoven materials. Background Technology

[0002] With the increasing demands for lightweight, high-efficiency filtration, flexible breathability, and high specific surface area performance in fields such as air purification, water treatment, protective filtration, and functional textiles, nonwoven materials have been widely used in filter media, adsorbent materials, protective fabrics, and environmental remediation materials due to their advantages such as short process flow, strong structural designability, high porosity, and suitability for continuous production. Traditional nonwoven materials are mostly made from micron-sized chopped fibers through processes such as opening, carding, web laying, and reinforcement. Their fiber skeleton has good mechanical support, bulkiness, and breathability. However, due to the large fiber diameter, the specific surface area of ​​fibers per unit mass of material is limited, and the pore size distribution between fibers is relatively wide. Therefore, their ability to retain, adsorb, and interact with fine particulate matter, aerosols, micro-pollutants, or partially dissolved impurities remains insufficient.

[0003] In recent years, nanofiber materials have shown great application potential in air filtration, liquid filtration, adsorption separation, functional protection, and composite textile materials due to their small fiber diameter, large specific surface area, fine pore size, and high surface activity. Introducing nanofibers into traditional microfiber nonwoven materials can maintain the flexibility, strength, and air permeability of the microfiber skeleton while filling fiber pores, increasing interfacial contact area, and improving pore size distribution. This allows for the construction of micro / nanoscale cross-scale fiber structures that serve as both a supporting skeleton and an efficient trapping interface. Such cross-scale structures achieve a good balance between filtration resistance, adsorption efficiency, softness, and material stability, thus becoming an important direction for the development of nonwoven functional materials. However, existing methods for preparing composite microfibers and nanofibers still have certain limitations. On the one hand, nanofibers have small diameters and high surface energy, making them prone to entanglement and aggregation due to van der Waals forces, electrostatic interactions, or solvent residues. This makes it difficult to achieve sufficient dispersion using carding equipment, unlike conventional short microfibers. Furthermore, directly mixing nanofibers and microfibers and then carding them together can easily lead to problems such as nanofiber clumping, uneven distribution, fiber breakage, or equipment blockage. On the other hand, some existing nanofiber deposition methods form a separate nanofiber layer on the surface of a microfiber mesh. The nanofibers mainly cover the surface of the substrate and are difficult to fully penetrate into the interior of the microfiber mesh. This results in insufficient bonding strength between the microfiber skeleton and the nanofiber layer, which can easily lead to nanofiber shedding, interlayer peeling, or filtration performance degradation during subsequent winding, cutting, use, or repeated bending.

[0004] Furthermore, existing nanofiber composite nonwoven materials also have shortcomings in terms of continuous and wide-width preparation. Some processes are limited by spraying range, receiving distance, deposition uniformity, and equipment movement, making it difficult to achieve uniform nanofiber coverage on a wide-width carded web. Even when a nanofiber layer can be formed, problems such as inconsistent deposition amounts across the width, significant structural differences between the central and peripheral regions, and difficulty in stably embedding nanofibers into a micron-fiber framework often exist. These problems not only affect the uniformity and stability of the cross-scale fiber structure but also limit its application in large-scale filtration materials, functional textiles, and environmental remediation materials. Therefore, how to generate nano-scale PET fibers online and uniformly insert them into the micron-fiber framework under airflow stretching, electrostatic action, and aerodynamic guidance, based on the continuous carding formation of a micron-scale PET fiber web, while avoiding nanofiber aggregation and surface accumulation, to form a stable micron / nano-embedded cross-scale fiber aggregate, is a technical problem urgently needing to be solved in this field. In particular, a preparation method is needed that can simultaneously achieve uniform nanofiber dispersion, micron-fiber framework support, and continuous coverage across the width, so that the prepared nonwoven material possesses flexibility, air permeability, and adsorption filtration performance. Summary of the Invention

[0005] To address the aforementioned limitations of existing technologies, the present invention aims to provide a method for preparing PET micro / nano-scale multi-scale fiber nonwoven materials. This invention achieves uniform distribution of nanofibers within a micron-scale framework through micron-fiber web construction, nanofiber jetting, secondary airflow stretching and electrostatic embedding, and controlled uniform deposition along the width direction. This results in a structurally stable and high-performance multi-scale fiber aggregate, solving problems such as the nanofiber layer primarily depositing on the surface of a micron-scale substrate, easy agglomeration of nanofibers, insufficient interfacial bonding stability, and difficulties in continuous fabrication across wide widths.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides a method for preparing PET micro / nano-scale multi-scale fiber nonwoven materials, comprising the following steps: (1) Construction of micron fiber web: PET micron-sized short chopped fibers are opened and combed to form a continuously conveyed micron fiber web; (2) Nanofiber jetting: Piezoelectric jetting is used above the micron fiber web to spray the PET solution through the spinneret to form nano-sized PET fibers, thus forming a PET nascent fiber stream; (3) Secondary stretching and electrostatic embedding of airflow: The nascent PET fibers are stretched twice by high-temperature compressed air to form PET nanofibers with a diameter of 150-220 nm. Under the action of airflow traction and electrostatic adsorption, the PET nanofibers enter the interior of the micron fiber web along the thickness direction to form a cross-scale fiber aggregate with an embedded structure. (4) Uniform deposition control in the width direction: The cross-scale fiber assembly is hot-pressed and shaped to obtain a cross-scale nonwoven material in which nanofibers are distributed on the surface and inside the pores of the PET microfiber skeleton, namely PET micro / nano cross-scale fiber nonwoven material.

[0007] Preferably, in step (1), the diameter of the PET micron-sized short-cut fibers is 10~50 μm and the length is 10~80 mm.

[0008] Preferably, in step (1), the PET solution is prepared by cutting PET slices into micro-slices and then dissolving them in a mixed solvent containing dichloromethane and trifluoroacetic acid to obtain a PET solution; the concentration of the PET solution is 5~15wt%.

[0009] Cut the PET chips into 1-3 mm pieces for easier dissolution. Wash with deionized water to remove surface dust and impurities. Immerse in ethanol or acetone for 10-20 minutes to remove oil and organic contaminants. Vacuum dry at 80-115℃ for 8-12 hours. Dissolve the dried PET chips in a mixed solvent of DCM and TFA (mass ratio 80:20) to obtain a PET solution.

[0010] Preferably, in step (1), the combing parameters are: cylinder speed 350-450 r / min, doffer speed 40-60 r / min; and the density of the micron fiber web is 20-60 g / m³. 2 .

[0011] Preferably, in step (2), the parameters of the piezoelectric jet injection are: piezoelectric driving frequency of 3 to 10 kHz, driving voltage of 100 to 180 V, and reciprocating frequency of 0.5 to 2 Hz.

[0012] Preferably, in step (3), the pressure of the high-temperature compressed air is 0.25–0.40 MPa, and the gas flow rate is 0.25–0.45 m³ / s. 3 / h, at a temperature ranging from room temperature to 120°C.

[0013] Preferably, in step (4), the temperature of the shaping treatment is 50-80°C, the pressure is 0.10-0.20 MPa, and the time is 10-20 s.

[0014] A second aspect of the present invention provides a PET micro / nano cross-scale fiber nonwoven material prepared by a method thereof, the PET micro / nano cross-scale fiber nonwoven material comprising a PET micro fiber skeleton and PET nanofibers embedded within the PET micro fiber skeleton, the PET nanofibers being distributed along the thickness direction of the material in the pores on the surface of the PET micro fiber and between adjacent PET micro fiber.

[0015] Preferably, the width of the PET micro / nano cross-scale fiber nonwoven material is 800~1500 mm, and the surface density variation coefficient in the width direction is not greater than 10%.

[0016] A third aspect of the present invention provides the application of PET micro / nano-scale multi-scale fiber nonwoven materials in the preparation of filter and protective products.

[0017] The beneficial effects of this invention are: (1) Effectively solve the problem of nanofiber agglomeration: Through piezoelectric jet spraying technology and high-speed airflow friction charging effect, nanofibers can be uniformly dispersed in the micron-scale fiber skeleton, avoiding the agglomeration problem caused by the high adsorption of nanofibers in conventional methods.

[0018] (2) Cross-scale fiber structure: By combining micron fibers and nanofibers, a cross-scale fiber aggregate is formed, which has a larger specific surface area, which is conducive to improving the adsorption performance of the fiber and enhancing the filtration and purification capabilities of the material.

[0019] (3) Improve flexibility and breathability: The fiber aggregates prepared by this method have good hand feel, flexibility and breathability while maintaining a high specific surface area, making them suitable for various fields, especially in textiles and environmental governance, where they have broad application prospects.

[0020] (4) Improved production efficiency: Compared with traditional nanofiber preparation methods, the preparation method of the present invention can simultaneously produce micron-sized and nano-sized fibers, and has high throughput production capacity, thus improving production efficiency and material utilization.

[0021] (5) Flexible width control: The reciprocating control system driven by the servo motor can automatically adjust the width as needed, flexibly control the spraying range of nanofibers, and adapt to different production requirements. Attached Figure Description

[0022] Figure 1 Example 1: Schematic diagram of a piezoelectric current composite jet device for nonwoven fabrication of ultrafine PET fibers; Figure 2 : A structural schematic diagram of the feed cylinder, spinneret and piezoelectric-driven reciprocating striker, i.e. a partial cross-sectional schematic diagram of the core generating end; Figure 3 : Schematic diagram of the structure of a Venturi coaxial drawing tube; The following components are shown in the diagram: 1. Material barrel, 2. Spinneret, 3. Piezoelectric driven reciprocating striker, 4. Feeding device, 5. Solenoid valve control unit, 6. Control unit, 7. High-temperature resistant compressed air pipeline, 8. Air preheater unit, 9. Flow regulating valve, 10. Heating unit, 11. Pressure gauge, 12. Safety valve, 13. Venturi coaxial drawing tube, 14. Receiving and web forming unit, 15. Compressed air source, 16. Air pipe connector, 31. Piezoelectric actuator, 32. Piston rod, 131. Central channel, 132. Top flange, 133. Outer sleeve, 134. Annular airflow buffer chamber, 135. Air inlet, 136. Gradient guide surface, 137. Inner annular cone surface, 138. Airflow jet slit, 139. Expansion hood, 140. Bottom outlet end ring; Figure 4 Example 2: Schematic diagram of the overall process of the preparation method; Figure 5 Schematic diagram of the structure of the nonwoven carding machine (a) and the piezoelectric jet spraying system (b); Figure 6 : A schematic diagram of nascent nanofibers being stretched a second time by compressed airflow and entering a micron-fiber web; Figure 7 Schematic diagram of nanofibers embedded in a PET microfiber framework in a multi-scale nonwoven material; Figure 8 (a) Schematic diagram of the reciprocating width control system of the piezoelectric jet injection module; (b) Enlarged view of the linear slide rail section; Figure 9 Electron microscopy images of the PET micro / nano cross-scale fiber nonwoven material prepared in Example 2, (a) scale bar 2 μm, (b) scale bar 1 μm. Detailed Implementation

[0023] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0024] As introduced in the background section, nanofibers, due to their strong adsorption properties, are prone to aggregation and difficult to disperse using traditional carding techniques, which limits their application in practical production. Traditional methods struggle to effectively combine micron- and nanofibers, making it difficult to achieve cross-scale fiber structures, thus affecting material properties. Solving the problems of nanofiber aggregation and dispersion, and effectively combining micron- and nanofibers to form cross-scale fiber structures with good specific surface area, flexibility, and high performance, has become an urgent technical challenge.

[0025] Based on this, the objective of this invention is to provide a method for preparing PET micron / nanoscale multi-scale fiber nonwoven materials. This invention first designs a piezoelectric current composite jet device for the nonwoven fabrication of ultrafine PET fibers, such as... Figures 1-3 As shown. This device uses a servo motor-driven 1.5m linear guide rail, consisting of a synchronous belt and synchronous pulley, to control the reciprocating frequency and achieve full coverage of nanofibers in the width direction of the carding machine. Specifically, it includes: (1) Reciprocating jet control: The reciprocating motion of the jet module is controlled by adjusting the 1.5m linear guide rail driven by the servo motor. This reciprocating motion controls the jet width by adjusting the frequency, thereby ensuring that the nanofibers are evenly distributed over a wide range. The adjustment of the reciprocating frequency ensures full coverage of the fibers in the width direction of the carding machine.

[0026] (2) Spraying module configuration: The nano-PET fiber piezoelectric jet spraying module consists of two sets of identical piezoelectric jet units. Each set of units sprays fibers in a circular spot with a diameter of 30~80mm and a spraying height of 100~350mm. This structure allows for uniform spraying of fibers over a wide area.

[0027] (3) Automated control: The linear guide rail is controlled by a host computer consisting of a PLC and a touch screen unit. The reciprocating distance can be set according to the required width, thereby realizing flexible control of variable width to meet different production needs.

[0028] PET micron-sized short-cut fibers are opened and carded through multiple cylinders using a nonwoven carding machine to form a uniform web structure. Using this device, nano-sized PET fibers (diameter: 80~500nm) are injected into the web by a piezoelectric jet-driven ejector pin. The ejector uses a heated barrel with spinnerets at the bottom, with a diameter of 10~20 microns. The piezoelectric jet-driven ejector pin extrudes the molten PET at high speed, forming nano-sized fibers through the spinnerets. The ejected nano-sized fibers undergo secondary stretching with high-temperature compressed air. After stretching, the fibers are rubbed by a high-speed drying airflow, acquiring an electrostatic charge. The electrostatically charged nanofibers penetrate deep into the micron-sized PET web skeleton through the airflow, forming an embedded, multi-scale fiber aggregate. This structure effectively avoids nanofiber aggregation and ensures uniform fiber dispersion. This method achieves uniform distribution of nanofibers within a micron-scale framework through the synergistic effect of airflow stretching and embedding, thereby obtaining structurally stable and high-performance multi-scale fiber assemblies. The overall process flow is as follows: Figure 4 As shown.

[0029] (1) Construction of micron-fiber mesh: such as Figure 5As shown, the microfiber skeleton was first constructed. Short-cut PET fibers were selected as the microfiber-level raw material, with a fiber diameter of 18–25 μm and a length of 30–40 mm. After opening treatment, the fibers were fed into a nonwoven carding machine and carded multiple times under the conditions of cylinder speed 350–450 r / min and doffer speed 40–60 r / min to fully disperse the fibers and form a uniformly arranged web structure. The resulting microfiber web surface density was controlled at 20–60 g / m². 2 The nanofibers are continuously transported to the subsequent nanofiber spraying area through a conveying device, thereby constructing a stable three-dimensional support framework.

[0030] (2) Nanofiber jetting: Based on the above-mentioned formation of micron fiber web, combined with Figure 5 The piezoelectric jetting system shown is used for the online preparation of nanofibers. Specifically, a PET spinning solution is dissolved in a DCM / TFA solvent to prepare a homogeneous spinning solution with a mass fraction of 5–15 wt%. After heating, stirring, and allowing to stand for degassing, the solution is injected into the jetting device. Under the action of the piezoelectric drive unit, the solution is extruded through micron-sized spinnerets to form a nascent fiber stream. The piezoelectric drive frequency is 3–10 kHz, and the drive voltage is 100–180 V, thereby ensuring the stability and continuity of the jetting process. The jetted nascent nanofibers are guided by gravity and airflow to the lower micron-fiber web region.

[0031] (3) Secondary airflow stretching and electrostatic embedding: such as Figure 6 As shown, the nascent fibers formed by the jetting enter the high-temperature compressed air zone and undergo secondary stretching under the traction of the high-speed airflow. The compressed air pressure is controlled at 0.25–0.40 MPa, and the gas flow rate is 0.25–0.45 m³ / s. 3 The process involves a high-speed airflow at a temperature ranging from room temperature to 120°C. During this process, a tensile force is applied along the fiber axis, causing the nascent fibers to rapidly refine and align, ultimately forming nanofibers with a diameter of approximately 150–220 nm. Simultaneously, due to airflow turbulence and friction between fibers, a certain amount of charge is generated on the nanofiber surface, providing favorable conditions for subsequent intercalation and composite formation.

[0032] like Figure 7 As shown, nanofibers stretched by airflow enter the interior of the microfiber web under the synergistic effect of aerodynamic and electrostatic forces, attaching to the surface of the microfibers or filling the gaps between the fiber pores, thereby forming a stable cross-scale embedded structure. This structure effectively avoids the aggregation of nanofibers during the deposition process, improves their dispersion uniformity in the microfiber framework, and significantly increases the specific surface area and interfacial contact area of ​​the material.

[0033] (4) Uniform deposition control in the width direction: To achieve uniform distribution of nanofibers over a wide width range, such as Figure 8 As shown, this embodiment employs a reciprocating jet control system to laterally regulate the piezoelectric jet module. The jet module is mounted on a linear guide rail and driven by a servo motor to achieve reciprocating motion. The reciprocating frequency is controlled between 0.5 and 2 Hz, and the motion stroke covers the entire web width range. Through this reciprocating scanning method, nanofibers can be uniformly deposited in the width direction, thereby obtaining a multi-scale fiber nonwoven material with a width of up to 1500 mm, while ensuring the structural consistency between the edge and center regions of the material.

[0034] After the nanofiber embedding and composite process, the resulting multi-scale fiber web is transported to a hot-pressing device for structural shaping. Hot-pressing is performed at 50–80°C and 0.10–0.20 MPa for 10–20 seconds to form a stable bond between the nanofibers and microfibers, preventing fiber detachment or structural loosening during subsequent use or processing. Finally, a winding device achieves continuous collection, yielding a finished multi-scale fiber nonwoven material with uniform structure and stable performance.

[0035] To enable those skilled in the art to better understand the technical solution of this application, the technical solution of this application will be described in detail below with reference to specific embodiments.

[0036] The test materials used in the embodiments of this invention are all conventional test materials in the art and can be purchased through commercial channels.

[0037] Example 1: Piezoelectric current composite jet device for nonwoven fabrication of ultrafine PET fibers This invention provides an ultrafine fiber piezoelectric current composite jet device (see...) Figures 1-3 The device includes a feed cylinder 1, a spinneret 2, a piezoelectric driven reciprocating striker 3, a feeding device 4, a solenoid valve control unit 5, a control unit 6, a high-temperature resistant compressed air pipeline 7, an air preheater unit 8, a flow regulating valve 9, a heating unit 10, a pressure gauge 11, a safety valve 12, a venturi coaxial drawing tube 13, and a receiving and forming unit 14.

[0038] The feeding device 4 is a pneumatic raw material tank. In this embodiment, the feeding device 4 is indeed a pneumatic raw material tank, which contains PET solution. Its outlet end is connected to the inlet end of the material cylinder 1 through a pipeline, and is used to continuously feed PET solution into the material cylinder 1. The feeding air pressure is 2 to 5 bar. The pressure gauge 11 is installed on the top of the feeding device 4 to monitor the air pressure inside the feeding device 4 in real time. The safety valve 12 is installed on the top of the feeding device 4 and is located to one side of the pressure gauge 11. When the air pressure inside the feeding device 4 exceeds 12 bar, it automatically releases pressure to prevent the feeding device 4 from being damaged by overpressure, thereby achieving safety protection.

[0039] The material cylinder 1 is a conical structure with a small outlet end at the bottom. Inside, a gradually narrowing flow channel is formed that gradually narrows from top to bottom in the vertical direction. The gradually narrowing flow channel causes the PET fluid to gradually increase in velocity as it flows downward and to be oriented along the axis of the material cylinder 1, which helps to reduce the velocity distribution difference of the fluid at the outlet end.

[0040] The outer wall of the barrel 1 is provided with a heating unit 10, which is a heating sleeve or heating ring arranged around the outer wall of the barrel 1. It has a segmented temperature control function to keep the PET in the barrel 1 in a flowable and extrudable state; the temperature inside the barrel 1 is 200-320 ℃. A spinneret 2 is fixedly installed at the outlet end of the barrel 1, and the spinneret 2 is arranged coaxially with the barrel 1.

[0041] like Figure 2 As shown, the spinneret 2 is a flat plate or plate-shaped flange structure with a micro-orifice array extending along its thickness direction. The micro-orifice array is formed by rows and columns of micro-orifices, with a diameter of 10–50 μm, a number of 200–2000 micro-orifices, and a center-to-center distance of 60–120 μm between adjacent micro-orifices. The micro-orifices are streamlined channel structures with a cross-section that gradually narrows along the flow direction; that is, the inlet diameter of the micro-orifice is larger than the outlet diameter, and the channel wall is a smoothly transitioning curved surface to reduce the flow resistance of the PET fluid within the orifices and improve the stability of the jet. The micro-orifice array on the spinneret 2 can be fabricated using laser micromachining, electrical discharge machining, or MEMS lithography. In this embodiment, the micro-orifice diameter of the spinneret 2 is 20–40 μm, the number of micro-orifices is 500–1500, and the center-to-center distance between adjacent micro-orifices is 70–100 μm.

[0042] The piezoelectrically driven reciprocating striker 3 is vertically arranged above the material cylinder 1 along the axis of the material cylinder 1. It includes a piezoelectric actuator 31 and a piston rod 32 driven by the piezoelectric actuator 31 and extending vertically downward. The lower end of the piston rod 32 passes through the top wall of the material cylinder 1 and extends into the material cylinder 1, that is, the lower end of the piston rod 32 extends into the tapered flow channel of the material cylinder 1.

[0043] The piezoelectric actuator 31 is a multilayer piezoelectric ceramic actuator, and its inherent resonant frequency is not lower than the upper limit of the required operating frequency; the piston rod 32 is made of hard alloy or tungsten material, which has high rigidity and wear resistance.

[0044] Driven by the control unit 6, the piezoelectrically driven reciprocating striker 3 reciprocates at a frequency of 20-100 kHz and an amplitude of 0.05-0.5 mm along the axis of the feed cylinder 1. The lower end of the piston rod 32 periodically impacts and squeezes the PET in the feed cylinder 1, applying periodic impact pressure to the PET, causing the PET to be ejected through the micro-hole array of the spinneret 2 to form a primary jet. The peak value of the impact pressure is greater than the static feeding pressure of the feeding device 4, thereby overcoming the surface tension and viscous resistance of the PET fluid in the micro-holes.

[0045] In this embodiment, the piezoelectrically driven reciprocating striker 3 operates at a frequency of 25–90 kHz and has an amplitude of 0.08–0.40 mm.

[0046] The Venturi coaxial drawing tube 13 is located directly below the spinneret 2 and is coaxial with the spinneret 2. It includes an outer sleeve 133, a tapered reducing tube, and a tapered expanding tube that are coaxially arranged from top to bottom and connected sequentially.

[0047] A central channel 131 is provided in the center of the Venturi coaxial drawing tube 13. The upper end of the central channel 131 is opposite to the micro-orifice array of the spinneret 2. The primary jet ejected from the spinneret 2 moves downward along the central channel 131. The central channel 131 extends through the top flange 132 of the Venturi coaxial drawing tube 13 and into the Venturi coaxial drawing tube 13. The outer sleeve 133 is arranged around the central channel 131, and the outer sleeve 133 and the central channel 131 form an annular airflow buffer chamber 134. The air inlet 135 is opened on the side wall of the outer sleeve 133 and communicates with the annular airflow buffer chamber 134 for introducing compressed air.

[0048] The tapered reducing tube is sequentially connected to the lower end of the outer sleeve 133. Its inner wall includes a gradually narrowing guide surface 136 at the top and an inner ring cone surface 137 at the bottom. The gradually narrowing guide surface 136 is a cone surface that gradually narrows along the airflow direction. The lower end of the central channel 131 is inserted into the tapered reducing tube along the axial direction of the outer sleeve 133.

[0049] An annular acceleration cavity is formed between the outer wall of the central channel 131 and the inner wall of the tapered tube. The diameter of the central channel 131 is larger than the diameter of the small diameter opening of the tapered tube. Therefore, an airflow jet slit 138 for compressed air to flow downward is formed between the inner wall of the tapered tube and the bottom end of the central channel 131.

[0050] The airflow jet slit 138 is an annular slit surrounding the central channel 131, with its centerline forming an angle of 15° to 30° with the axis of the central channel 131. That is, the jet direction of the airflow jet slit 138 converges inward and tilts downward.

[0051] The small-diameter opening of the tapered expanding tube is sealed to the small-diameter opening of the tapered contracting tube. The tapered expanding tube includes an expansion shroud 139 and a bottom outlet end ring 140 disposed at the lower end of the expansion shroud 139. The expansion shroud 139 is independently disposed below the airflow jet slit 138. Its inlet end is connected to the small-diameter opening of the tapered contracting tube, and the opening gradually expands downward, forming a transition flow channel that is isolated from the outside world and has a gradually expanding cross-section. The bottom outlet end ring 140 constitutes the outlet end of the Venturi coaxial drawing tube 13.

[0052] Compressed air enters the annular airflow buffer chamber 134 through the inlet 135, where it is uniformly pressurized circumferentially. It is then accelerated by the tapered guide surface 136, guided by the inner annular cone surface 137, and ejected at high speed from the airflow jet slit 138 at an angle of 15° to 30° with the axis of the central channel 131. A negative pressure and axisymmetric high-speed traction flow field is formed at the outlet of the central channel 131, which performs secondary stretching on the primary jet in the central channel 131, producing the Venturi effect. The stretched ultrafine fiber moves smoothly downward along with the airflow through the expansion guide hood 139 and is discharged from the bottom outlet end ring 140.

[0053] The annular airflow buffer cavity 134, the tapered guide surface 136, the inner annular cone surface 137, the airflow jet slit 138, and the expansion guide hood 139 sequentially constitute the pressure stabilization section, acceleration section, guide section, converging jet section, and interference isolation guide section of the stretched airflow.

[0054] The large-volume annular airflow buffer chamber 134 allows the compressed air entering from the single air inlet 135 to fully expand and redistribute circumferentially, attenuating the pulsation of intake pressure and local eddies within the buffer chamber. This ensures that the static pressure at the inlet of the acceleration chamber is basically consistent circumferentially, thereby reducing the transmission of intake pulsation to the stretching zone. The tapered guide surface 136 accelerates the airflow smoothly with a small contraction angle, avoiding abrupt changes in the flow channel that could cause airflow separation and eddies. The inner annular conical surface 137 guides the airflow towards the axial direction of the central channel 131 with a large taper, preventing the airflow from making a sharp turn upstream of the slit and generating secondary flow. The airflow jet slit 138 converges inward at an angle of 15° to 30°, causing the annular airflow ejected along the slit to converge and superimpose downstream of the central channel 131 outlet, forming a convergent high-speed traction flow field and fully performing work on the primary jet.

[0055] The expansion hood 139 is independently located downstream of the airflow jet slit 138, so that the airflow that has completed the stretching is slowly decelerated and diffused inside the hood, and the entrained airflow and turbulent vortex of the external environment are isolated outside the stretching zone.

[0056] The synergistic effect of the above five factors results in low turbulence intensity, circumferential uniformity, and axial stability of the drafting flow field within the Venturi coaxial drafting tube 13. The magnitude and direction of the tensile stress experienced by the primary jet during the drafting process remain stable, significantly improving the uniformity of the resulting ultrafine fibers and narrowing the diameter distribution. This avoids problems such as uneven fiber refinement, large diameter dispersion, and fiber oscillation and filament bundling caused by high turbulence intensity and circumferential unevenness of the drafting airflow in the prior art.

[0057] The aforementioned pressure stabilization section, acceleration section, guiding section, converging jet section, and interference isolation and diversion section are integrally formed by the same Venturi coaxial drawing tube 13. The tapered guide surface 136, inner ring cone surface 137, and expansion diversion shroud 139 inside the tube are transitioned by a continuous smooth curved surface. There are no intermediate flanges, no sleeve gaps, and no assembly steps on the tube body. Therefore, no separate alignment is required during assembly, and no pressure equalization chamber, flow rectifier grid, or external guide tube is required outside the tube. Compressed air will not leak at the tube section connection or generate local vortices at the steps. The airflow utilization rate is high and the drawing efficiency is high. The entire drawing tube has a small radial dimension and a compact structure. It can be directly installed below the spinneret 2 and share the same axis with the feed cylinder 1 and the spinneret 2. This shortens the transition distance between the spinneret 2 and the drawing zone, reduces the cooling and oscillation of the primary jet before reaching the drawing zone, and facilitates overall disassembly, cleaning, and array arrangement.

[0058] The compressed air source 15 is connected to the air inlet 135 of the Venturi coaxial drawing tube 13 in sequence through the air pipe connector 16, the flow regulating valve 9, the air preheater unit 8, the high temperature resistant compressed air pipeline 7, and the solenoid valve control unit 5.

[0059] The compressed air pressure is 6–12 bar, and the air temperature after preheating by the air preheater unit 8 is room temperature to 120 °C. The control unit 6 is electrically connected to the piezoelectric driven reciprocating striker 3, the solenoid valve control unit 5, and the air preheater unit 8, respectively, and is used to regulate the operating frequency and amplitude of the piezoelectric driven reciprocating striker 3, regulate the on / off mode of the stretching airflow through the solenoid valve control unit 5, and regulate the preheating temperature of the air preheater unit 8.

[0060] The stretching airflow operates in a continuous or pulsed manner, with the frequency of the pulsed stretching airflow being 10–800 Hz.

[0061] The receiving and forming unit 14 is located downstream of the Venturi coaxial drawing tube 13. In this embodiment, the receiving and forming unit 14 is a receiving screen or receiving roller located below the bottom outlet end ring 140, used to collect the ultrafine PET fibers after secondary drawing and form a nonwoven fiber web.

[0062] Example 2: Preparation method of PET micro / nano-scale fiber nonwoven material The piezoelectric current composite jet device of Example 1 was used for preparation, and the specific method is as follows: (1) Preparation of PET microfiber matrix web: PET short fibers with a linear density of 1.56 dtex and a length of 38 mm were selected as microscale fiber raw materials. The PET short fibers were sequentially opened, mixed, carded, and laid into a web to obtain a surface density of 60 g / m². 2 A PET microfiber matrix web was obtained. The carding machine cylinder speed was 420 r / min, the doffer speed was 28 r / min, and the web was laid in 4 layers, resulting in a fluffy PET microfiber matrix web with a thickness of 1.20 mm. (2) Piezoelectric jet spinning of PET nanofibers: 10.0 g of dried PET chips were weighed and added to 90.0 g of a mixed solvent composed of dichloromethane and trifluoroacetic acid, wherein the mass ratio of dichloromethane to trifluoroacetic acid was 80:20. The mixture was magnetically stirred at 25°C for 12 h to obtain a PET spinning solution with a mass fraction of 10.0 wt%. The obtained spinning solution was filtered through a 0.45 μm PTFE filter membrane and allowed to stand for degassing for 30 min before use. PET nanofibers were prepared using the piezoelectric jet equipment described in Example 1 (oscilloscopes were Shanghai Shengchi Power Supply, models: SC / KPA-1K and SC / KPA-5K, frequency: 20Hz~2kHz / 10kHz / 50kHz adjustable). The feeding device containing the PET spinning solution continuously fed the barrel at a feeding gas pressure of 5 bar. The barrel was heated to 285°C by a heating unit to maintain the spinnability of the PET melt. The ultrafine fiber piezoelectric current composite jet device is equipped with a high-frequency power supply, piezoelectric striking pins, spinnerets, and a jet drawing nozzle. The high-frequency power supply is set to a frequency of 20 kHz, and the air pressure at the jet drawing nozzle is 8 bar. The piezoelectric-driven reciprocating striking pins operate at a frequency of 90 kHz and an amplitude of 0.08 mm, causing PET melt to be ejected through the micro-orifice array of spinneret 2 to form a primary jet. The micro-orifice diameter of the spinneret is 25 μm, the number of micro-orifices is 600, and the center-to-center distance between adjacent micro-orifices is 75 μm. Compressed air is heated to 120 ℃ by an air preheater unit and then introduced into the Venturi coaxial drawing tube at a pressure of 11 bar for continuous secondary drawing of the primary jet. The resulting fibers have an average diameter of 350 nm and a diameter distribution range of 220–500 nm. The piezoelectric jet process parameters are as follows: spinning frequency: 20kHz; drawing pressure: 8bar; receiving distance: 20.0 cm; spinning solution propulsion rate: 0.80 mL / h; spinning environment temperature: 25 ℃; relative humidity: 40% RH; receiving substrate: PET microfiber matrix mesh prepared in step (1); receiving method: flat plate receiving; nozzle transverse reciprocating scanning speed: 80 mm / s; single-sided deposition time: 20 min. During the spinning process, PET nanofibers are directly deposited on the surface and inside the pores of the PET microfiber matrix mesh, forming a cross-scale fiber network structure in which nanofibers and microfibers overlap, entangle, and embed with each other.

[0063] (3) Pre-compression finishing of composite fiber web: The PET nanofiber / PET microfiber composite web obtained in step (2) is placed in a flat hot press for light pre-compression finishing. The hot pressing temperature is 80 ℃, the pressure is 0.20 MPa, and the holding time is 60 s. After pre-compression, the PET nanofibers are further embedded in the microfiber matrix web, and the thickness of the composite web is reduced from 1.20 mm to 0.95 mm, forming a stable physical bonding interface between the nanofiber layer and the microfiber layer.

[0064] (4) Heat setting treatment: The pre-compressed composite fiber web was placed in a hot air setting machine for heat setting treatment. The heat setting temperature was 130 ℃, the treatment time was 5 min, and the hot air velocity was 1.5 m / s. After setting, a PET nanofiber / PET microfiber cross-scale nonwoven material was obtained. The areal density of the obtained material was 68 g / m². 2 The thickness is 0.82 mm, the average pore size is 8.6 μm, the longitudinal breaking strength is 86 N / 5 cm, the transverse breaking strength is 63 N / 5 cm, the filtration efficiency of 0.3 μm particles is 92.5%, and the air permeability is 320 mm / s.

[0065] Comparative Example 1 The difference from Example 2 is that steps (2) and (3) are omitted, piezoelectric jet spraying and secondary stretching are not performed, and only the micron fiber mesh is shaped.

[0066] Comparative Example 2 The difference from Example 2 is that step (2) uses an electrospinning machine to spray out the spinning solution.

[0067] Comparative Example 3 The difference from Example 2 is that step (3) is omitted, that is, the nascent fibers formed by spraying are not subjected to secondary stretching.

[0068] Example 3: Morphological Observation The cross-sectional sample of the multi-scale nonwoven material prepared in Example 2 was cut along the thickness direction, and observed using a scanning electron microscope after being sputter-coated with gold. Figure 9 As shown, PET microfibers form a continuous three-dimensional support framework. PET nanofibers do not merely cover the material surface but penetrate into the microfiber framework. Some nanofibers cross the pores of adjacent microfibers and attach to the surface, forming a micro / nanoscale intercalation structure. The nanofibers in the material of this invention have a more uniform distribution along the thickness direction, and the dense accumulation on the surface is significantly reduced. Scanning electron microscopy observation of the material prepared by the method of this invention shows that the nanofibers are uniformly distributed between the microfiber framework, with no obvious agglomeration or localized surface accumulation, indicating that this method can effectively achieve the synergistic construction of nano / microfibers.

[0069] Experiment 1: Performance Testing To further demonstrate the technical effects of the present invention, the nonwoven materials prepared in Example 2 and Comparative Examples 1-3 were tested for specific surface area, air permeability, filtration efficiency, filtration resistance, nanofiber shedding rate, tensile strength, and surface density uniformity in the width direction. The results are shown in Table 1.

[0070] Each performance indicator was tested using the following methods: (1) Sample pretreatment: Before testing, the samples of Example 2 and Comparative Examples 1 to 3 were placed in a standard atmospheric environment with a temperature of (20±2)℃ and a relative humidity of (65±4)% for at least 24 hours to equilibrate. At least 5 parallel samples were tested for each group of samples, and the average value of the results was taken.

[0071] (2) Specific surface area: The specific surface area was determined according to GB / T 19587-2017 "Determination of specific surface area of ​​solid substances by gas adsorption BET method". Approximately 0.2 g of sample was taken, degassed under low temperature vacuum, and then measured using the nitrogen adsorption BET method. The results are expressed in m... 2 / g represents.

[0072] (3) Air permeability: Tested according to GB / T 5453-1997 "Textiles - Determination of air permeability of fabrics". The test pressure difference is 100 Pa, and the test area is 20 cm². 2 Five positions were selected evenly in the width direction, and the results are expressed in mm / s.

[0073] (4) Filtration efficiency and filtration resistance: The test was conducted in accordance with GB / T 38413-2019 "Test method for filtration performance of fine particulate matter in textiles". Non-oily NaCl aerosol was used as the test medium. Under the same test flow rate and effective filtration area, the concentration of particulate matter upstream and downstream of the sample and the pressure difference across the sample were measured respectively. The filtration efficiency was calculated as η=(1-C2 / C1)×100%, where C1 is the concentration of particulate matter upstream and C2 is the concentration of particulate matter downstream. The filtration resistance was the initial pressure difference after the test stabilized, in Pa.

[0074] (5) Nanofiber shedding rate: The test was conducted in accordance with GB / T 24218.10-2016 "Textiles - Nonwovens - Test Methods - Part 10: Determination of dry lint shedding". A 100 mm × 100 mm sample was placed in a dry lint shedding test device and treated for 10 min under specified vibration and airflow purging conditions. The shed nanofibers and lint were collected and weighed. The nanofiber shedding rate was calculated as: nanofiber shedding rate = mass of shed nanofibers / initial nanofiber load mass in the sample × 100%; where the initial nanofiber load mass was obtained by converting the difference in mass per unit area before and after composite.

[0075] (6) Tensile strength: The test was conducted in accordance with GB / T 24218.3-2010 "Textiles - Test methods - Part 3: Determination of breaking strength and elongation at break (strip method)". The sample size was 50 mm × 200 mm, the clamping distance was 100 mm, the tensile speed was 100 mm / min, and the results were expressed as N / 5 cm.

[0076] (7) Uniformity of surface density in the width direction: The test shall be conducted in accordance with GB / T 24218.1-2009 "Textiles - Test Methods - Part 1: Determination of mass per unit area". At least five 250 mm × 200 mm samples shall be cut from the left, center, right and intervals in the width direction of the sample, and the mass per unit area shall be measured. The coefficient of variation (CV) shall be calculated as (standard deviation / average value) × 100%. The smaller the CV, the more uniform the surface density in the width direction.

[0077] Table 1 Note: Comparative Example 1 did not introduce nanofibers, so the nanofiber shedding rate is not applicable and is indicated by "—"; the data in the table are the average values ​​of 5 parallel samples under the same test conditions.

[0078] As shown in Table 1, compared with Comparative Example 1, Example 2 significantly improves the specific surface area and filtration efficiency due to the introduction of a continuous and uniformly distributed nanofiber layer. Compared with Comparative Example 2, Example 2 achieves a significantly reduced filtration resistance and nanofiber shedding rate by using airflow stretching and synergistic web formation with the microfiber skeleton, transforming the nanofibers from surface covering to an embedded composite structure. This maintains high filtration efficiency while significantly reducing filtration resistance and nanofiber shedding rate. Compared with Comparative Example 3, Example 2 shows further improvements in structural stability, tensile strength, and width-direction surface density uniformity after hot pressing. Therefore, this invention can be used in conjunction with existing nonwoven carding production lines, nanofiber jetting devices, and hot pressing equipment, demonstrating feasibility for continuous preparation and wide-width production. The resulting multi-scale nonwoven material can be used for air filtration, liquid filtration, protective textiles, adsorbent materials, and environmental remediation materials, showing promising industrial application prospects.

[0079] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method for preparing PET micro / nano-scale multi-scale fiber nonwoven material, characterized in that, Includes the following steps: (1) Construction of micron fiber web: PET micron-sized short chopped fibers are opened and combed to form a continuously conveyed micron fiber web; (2) Nanofiber jetting: Piezoelectric jetting is used above the micron fiber web to spray the PET solution through the spinneret to form nano-sized PET fibers, thus forming a PET nascent fiber stream; (3) Secondary stretching and electrostatic embedding of airflow: The nascent PET fibers are stretched twice by high-temperature compressed air to form PET nanofibers with a diameter of 150-220 nm. Under the action of airflow traction and electrostatic adsorption, the PET nanofibers enter the interior of the micron fiber web along the thickness direction to form a cross-scale fiber aggregate with an embedded structure. (4) Uniform deposition control in the width direction: The cross-scale fiber assembly is hot-pressed and shaped to obtain a cross-scale nonwoven material in which nanofibers are distributed on the surface and inside the pores of the PET microfiber skeleton, namely PET micro / nano cross-scale fiber nonwoven material.

2. The method for preparing PET micro / nano-scale multi-scale fiber nonwoven material according to claim 1, characterized in that, In step (1), the diameter of the PET micron-sized short-cut fibers is 10~50 μm and the length is 10~80 mm.

3. The method for preparing PET micro / nano-scale multi-scale fiber nonwoven material according to claim 1, characterized in that, In step (1), the PET solution is prepared by cutting PET slices into micro-slices and then dissolving them in a mixed solvent containing dichloromethane and trifluoroacetic acid to obtain a PET solution; the concentration of the PET solution is 5~15wt%.

4. The method for preparing PET micro / nano-scale multi-scale fiber nonwoven material according to claim 1, characterized in that, In step (1), the combing parameters are: cylinder rotation speed 350-450 r / min, doffer rotation speed 40-60 r / min; the density of the micron fiber web is 20-60 g / m³. 2 .

5. The method for preparing PET micro / nano-scale multi-scale fiber nonwoven material according to claim 1, characterized in that, In step (2), the parameters of the piezoelectric jet injection are: piezoelectric driving frequency of 3 to 10 kHz, driving voltage of 100 to 180V, and reciprocating frequency of 0.5 to 2 Hz.

6. The method for preparing PET micro / nano-scale multi-scale fiber nonwoven material according to claim 1, characterized in that, In step (3), the pressure of the high-temperature compressed air is 0.25–0.40 MPa, and the gas flow rate is 0.25–0.45 m³ / s. 3 / h, at a temperature ranging from room temperature to 120°C.

7. The method for preparing PET micro / nano-scale multi-scale fiber nonwoven material according to claim 1, characterized in that, In step (4), the temperature of the shaping treatment is 50-80℃, the pressure is 0.10-0.20 MPa, and the time is 10-20 s.

8. The PET micro / nano-scale fiber nonwoven material obtained by the method for preparing PET micro / nano-scale fiber nonwoven material according to any one of claims 1 to 8, characterized in that, The PET micro / nano cross-scale fiber nonwoven material includes a PET microfiber skeleton and PET nanofibers embedded inside the PET microfiber skeleton. The PET nanofibers are distributed along the thickness direction of the material on the surface of the PET microfibers and in the pores between adjacent PET microfibers.

9. The PET micro / nano-scale multi-scale fiber nonwoven material according to claim 8, characterized in that, The width of the PET micro / nano cross-scale fiber nonwoven material is 800~1500 mm, and the surface density variation coefficient in the width direction is not greater than 10%.

10. The use of the PET micro / nano-scale multi-scale fiber nonwoven material according to claim 8 or 9 in the preparation of filter products and protective products.