Reductive cleaning process in supercritical fluids

By using a combination of specific chemical agents and process parameters in supercritical fluids, the problem of fiber surface residue caused by dye precipitation was solved, the dye fastness of polyester fibers was improved, and a highly efficient reduction cleaning effect was achieved.

CN123153231APending Publication Date: 2026-11-24YKK CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610686489.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-21
Filing Date
2026-05-19
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In supercritical fluid dyeing, dyes are prone to precipitate, resulting in residues on the fiber surface and affecting fastness. Existing technologies are unable to effectively remove residual dyes.

Method used

The process involves reducing the dye using an alkylene oxide adduct of an alcohol with 8-14 carbon atoms in a supercritical fluid, along with a reducing agent, acid, and water. This is followed by cleaning with an organic solvent. Process parameters such as temperature and pressure are optimized to improve the solubility and removal efficiency of the dye.

Benefits of technology

It significantly improves the dye fastness of polyester fibers, reduces residual dye on the fiber surface, and achieves a highly efficient reduction cleaning effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153231A_ABST
    Figure CN123153231A_ABST
Patent Text Reader

Abstract

Provided is a method for reducing cleaning in a supercritical fluid that can provide polyester fibers with improved fastness. A method for reducing cleaning of polyester fibers, which is performed after a dyeing process in a supercritical fluid, characterized by comprising: a first process in which reducing treatment of polyester fibers is performed in a treatment tank of a supercritical fluid treatment device in the presence of a supercritical fluid, (A) an alkylene oxide adduct of an alcohol having 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, and (D) water; and a second process in which, after the first process, (E) an organic solvent is added to the treatment tank, and cleaning of the polyester fibers is performed in the presence of a supercritical fluid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a method for reducing and cleaning polyester fibers dyed in a supercritical fluid in a supercritical fluid. Background Technology

[0002] Generally, the dyeing process of polyester fibers uses a large amount of water, and after dyeing, a large amount of wastewater containing unadhered dyes and dyeing auxiliaries is discharged, causing water pollution. Therefore, its purification becomes a significant burden for manufacturers. To solve this problem, a method of dyeing polyester fibers in supercritical carbon dioxide has recently been proposed as a method that produces almost no wastewater and efficiently dyes polyester fibers. For example, Japanese Patent Application Publication No. 5-132880 discloses a method for dyeing hydrophobic fibers such as polyester fibers using disperse dyes in supercritical carbon dioxide. Japanese Patent Application Publication No. 2002-371483 discloses a dyeing method characterized by introducing a dye solution into a dyeing tank containing the fabric to be dyed and a supercritical fluid.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 5-132880

[0006] Patent Document 2: Japanese Patent Application Publication No. 2002-371483 Summary of the Invention

[0007] The problem that the invention aims to solve

[0008] In dyeing using supercritical fluids, dyes tend to precipitate out easily due to changes in temperature and pressure. Therefore, sometimes a significant amount of dye remains on the surface of the dyed fiber, leading to a decrease in fastness. One method to improve fastness is to clean the fiber surface after dyeing.

[0009] This disclosure provides a reduction cleaning method in a supercritical fluid that can provide polyester fibers with improved fastness.

[0010] Methods for solving problems

[0011] This disclosure relates to the following matters.

[0012] <Option 1>

[0013] A reduction cleaning method for polyester fibers, comprising performing the reduction cleaning of the polyester fibers after a dyeing process in a supercritical fluid, characterized in that the reduction cleaning method for the polyester fibers includes:

[0014] In the first step, polyester fibers are subjected to reduction treatment in a treatment tank of a supercritical fluid treatment device in the presence of supercritical fluid, (A) an epoxide adduct of an alcohol having 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, and (D) water; and

[0015] In the second step, following the first step, an organic solvent (E) is added to the treatment tank, and the polyester fibers are cleaned in the presence of a supercritical fluid.

[0016] <Option 2>

[0017] A reduction cleaning method for polyester fibers, wherein the reduction cleaning of the polyester fibers is performed after a dyeing process in a supercritical fluid, characterized in that...

[0018] The reduction and cleaning method for the polyester fibers includes the following steps: in the treatment tank of a supercritical fluid treatment device, the polyester fibers are subjected to reduction treatment and cleaning in the presence of supercritical fluid, (A) an epoxide adduct of an alcohol with 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, (D) water and (E) an organic solvent.

[0019] <Option 3>

[0020] The reduction and cleaning method for polyester fibers according to Scheme 1 above is characterized in that, in the second step, water (F) is further added.

[0021] <Option 4>

[0022] The method for reducing and cleaning polyester fibers according to Scheme 1 or 3 above is characterized in that, after the second step, a third step is performed to discharge the supercritical fluid in the treatment tank.

[0023] <Option 5>

[0024] The method for reducing and cleaning polyester fibers according to Scheme 1 or 3 above is characterized in that, after the second step, a fourth step is performed in which supercritical fluid is introduced into the treatment tank and the polyester fibers and the treatment tank are cleaned using the supercritical fluid.

[0025] <Option 6>

[0026] The reduction and cleaning method for polyester fibers according to any one of the above schemes 1 to 5 is characterized in that the reduction treatment is carried out at a temperature of 65°C or higher and 105°C or lower.

[0027] <Option 7>

[0028] The reduction and cleaning method for polyester fibers according to any one of the above schemes 1 to 6 is characterized in that the reduction treatment is carried out at a pressure of 18 MPa or more and 26 MPa or less.

[0029] <Option 8>

[0030] The reduction cleaning method for polyester fibers according to any one of the above schemes 1 to 7 is characterized in that the SP value of the organic solvent (E) is 9 to 15 (cal / cm³). 3 ) 1 / 2 .

[0031] Invention Effects

[0032] According to the present invention, a reduction cleaning method can be provided that can provide polyester fibers with improved fastness. Attached Figure Description

[0033] Figure 1 This is a schematic diagram illustrating the structure of a supercritical fluid processing device. Detailed Implementation

[0034] One embodiment of the reduction cleaning method is a reduction cleaning method in a supercritical fluid, specifically a reduction cleaning method for cleaning dyes or the like adhering to fibers dyed in a supercritical fluid. The reduction cleaning method of one embodiment includes the following steps: in a treatment tank of a supercritical fluid treatment apparatus, a reduction treatment and cleaning of polyester fibers is performed in the presence of supercritical fluid, (A) an alkylene oxide adduct of an alcohol having 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, (D) water, and (E) an organic solvent. The reduction cleaning method of one embodiment includes: a first step, in which the polyester fibers are reduced in a treatment tank of a supercritical fluid treatment apparatus in the presence of supercritical fluid, (A) an alkylene oxide adduct of an alcohol having 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, and (D) water; and a second step, after the first step, in which (E) an organic solvent is added to the treatment tank, and the polyester fibers are cleaned in the presence of supercritical fluid. While not wishing to be bound by theory, it can be considered that polyester fibers can be reduced and cleaned through the following mechanism: By dissolving (B) a reducing agent and (C) an acid in (D) water, and contacting the (B) reducing agent with the dye under acidic conditions, the dye is effectively reduced. Typically, the dyes used in dyeing polyester fibers are not soluble in water but in supercritical fluids. Water, on the other hand, is not soluble in supercritical fluids. Therefore, by using an epoxide adduct of an alcohol with 8-14 carbon atoms (A), it is possible to dissolve (D) water containing (B) a reducing agent and (C) an acid in a supercritical fluid, and then reduce the dye adhering to the surface of the polyester fiber using the (B) reducing agent under acidic conditions. The reduced dye has increased water solubility and is therefore discharged along with (D) water. Furthermore, by using an organic solvent (E), residual dye can be removed, further improving fastness. By using an organic solvent (E) in a second step, which is different from the first step which uses an epoxide adduct of an alcohol with 8 to 14 carbon atoms, a reducing agent, an acid, and water, an improvement in fastness can be expected.

[0035] Supercritical Fluids

[0036] Supercritical fluids are not particularly limited, but supercritical carbon dioxide is preferred.

[0037] <Polyester Fibers>

[0038] Polyester fibers refer to fibers that contain polyester fibers. Polyester fibers can be composed solely of polyester fibers or composed of polyester fibers and other fibers (blended, interwoven, etc.). For example, polyester fibers can contain more than 50%, 60%, 70%, 80%, or 90% by mass of polyester fibers, and can also contain less than 100% or 95% by mass of polyester fibers.

[0039] The form of the fiber is not particularly limited; it can be a raw material or semi-finished product such as cotton, yarn, rope, textiles, woven fabrics, or non-woven fabrics, or a final product such as clothing. Preferably, the fiber product is composed solely of polyester fibers or is composed of polyester fibers and other fibers (blended, twisted, interwoven, cross-knitted, etc.). For example, a fiber product may be a webbing containing polyester fibers.

[0040] <(A) Epoxide adducts of alcohols with 8-14 carbon atoms>

[0041] The alcohol with 8 to 14 carbon atoms used as a starting material for the alkylene oxide adduct of an alcohol with 8 to 14 carbon atoms (also called component (A)) can be a saturated alcohol or an unsaturated alcohol, preferably a saturated alcohol. The alcohol with 8 to 14 carbon atoms can be a monohydric alcohol or a dihydric alcohol. From the viewpoint of reduction and cleaning properties, branched primary alcohols, secondary alcohols, and tertiary alcohols are preferred. Specific examples of alcohols with 8 to 14 carbon atoms include: branched primary alcohols such as 2-ethylhexanol, isononanol, isodecanol, isodecanol, and isodexadecanol; 2-octanol, 2-decanol, 2-undecanol, 2-dodecanol, 2-tridecanol, 2-tetradecanol, 3-octanol, 3-decanol, 3-undecanol, 3-tridecanol, 3-tetradecanol, 4-octanol, 4-decanol, 4-undecanol, 4-dodecanol, 4-tridecanol, 4-tetradecanol, 5-decanol, 5-undecanol, 5-tridecanol, 5-tetradecanol, 6-undecanol, 6- ... Secondary alcohols such as tridecanool, 6-tetradecanool, 7-tetranol, and 7-tetradecanool; saturated tertiary alcohols such as 3,7-dimethyl-3-octanol and 3-methyl-3-decanol; and unsaturated tertiary alcohols such as 5,8-dimethyl-6-dodecyn-5,8-diol, 2,4,7,9-tetramethyl-5-decyn-4,7-diol, 4,7-dimethyl-5-decyn-4,7-diol, 2,3,6,7-tetramethyl-4-ocyn-3,6-diol, 3,6-diethyl-4-ocyn-3,6-diol, and 3,6-dimethyl-4-ocyn-3,6-diol.

[0042] The epoxides added to alcohols having 8 to 14 carbon atoms are not particularly limited, but epoxides having 2 to 4 carbon atoms are preferred. Specifically, examples include ethylene oxide, propylene oxide, butane oxide, and isobutane oxide. From a cleanliness perspective, at least one selected from ethylene oxide, propylene oxide, and butane oxide is preferred, and at least one selected from ethylene oxide and propylene oxide is more preferred. Epoxides can be used alone or in combination. When multiple epoxides are used in combination, the addition of the epoxides can be in any form, such as random addition, block addition, or alternating addition.

[0043] The HLB (Hydrophile Lipophile Balance) of component (A) is preferably 7 to 16. When the HLB is within this range, the solubility in supercritical fluids is particularly good, and it tends to become superior from the viewpoint of improving fastness. As component (A), it is preferable to use an alkylene oxide adduct of an alcohol with 8 to 14 carbon atoms and an HLB of 7 to 16. It is also preferable to use a mixture of alkylene oxide adducts of alcohols with 8 to 14 carbon atoms having different HLBs, resulting in an HLB of 7 to 16, as component (A). That is, it is also preferable to use a mixture containing at least one selected from the group consisting of alkylene oxide adducts of alcohols with 8 to 14 carbon atoms and alkylene oxide adducts of alcohols with 8 to 14 carbon atoms and an HLB greater than 16, and with an HLB in the range of 7 to 16. Furthermore, unless otherwise specified in this disclosure, “HLB” refers to the HLB value calculated by the Griffin method according to the following formula, treating ethylene oxide as a hydrophilic group and all other components as lipophilic groups.

[0044] HLB value = 20 × (molecular weight of the ethylene oxide group of the compound) / (molecular weight of the compound)

[0045] When component (A) contains two or more compounds, the HLB of component (A) is the sum of the products of the mass percentage of each compound and the HLB value of each compound. For example, if component (A) consists of 30% by mass of a compound with an HLB value of 6 and 70% by mass of a compound with an HLB value of 18, its HLB is 14.4 (6 × 30 × 0.01 + 18 × 70 × 0.01).

[0046] As ingredient (A), commercially available products can be used, such as the BLAUNON EH series manufactured by Aoki Oils & Fats Co., Ltd., the SOFTANOL series manufactured by Nippon Catalyst Co., Ltd., the Exxal series manufactured by Exxon Mobil Corporation, and the SURFYNOL 400 series, including SURFYNOL 420 and SURFYNOL 440, manufactured by Nissin Chemical Industries, Ltd. Furthermore, ingredient (A) can be used alone or in combination of two or more.

[0047] <(B) Reducing agent>

[0048] (B) The reducing agent (also called component (B)) is at least one selected from ascorbic acid, sulfinic acid, isoascorbic acid, thioacetic acid, squaric acid, teichoic acid, humic acid, oxalic acid, and formic acid. These are organic acids with reducing properties. As component (B), at least one selected from ascorbic acid and isoascorbic acid is preferred, and ascorbic acid is more preferred. Component (B) can be used alone or in combination of two or more.

[0049] <(C) acid>

[0050] The compound used as (C) acid (also called (C) component) is not particularly limited as long as it is an acid that is not a (B) reducing agent. Specific examples include acetic acid, hydrochloric acid, and trifluoroacetic acid, but acetic acid is preferred. (C) component can be used alone or in combination of two or more.

[0051] <(D) Water>

[0052] As (D) water (also known as (D) component), it is not particularly limited and can include pure water, industrial water, ion-exchange water, etc.

[0053] <(E) Organic Solvents>

[0054] As an organic solvent (also known as an (E) component), it is not particularly limited, but an SP value of 9 to 15 (cal / cm³) is preferred. 3 ) 1 / 2 Organic solvents. While it is not desirable to be bound by theory, by keeping the SP value within the aforementioned range, the solubility of component (E) in both supercritical fluid and water becomes good. Supercritical fluid, water, reduced dye, components (A) to (C), and organic solvent (E) readily dissolve in each other, and the solubility of reduced dye and components (A) to (C) is improved. Therefore, from the viewpoint of improving fastness, it tends to become superior. As a specific example of component (E), tetrahydrofuran (SP value = 9.5 (cal / cm)) can be cited. 3 ) 1 / 2), acetone (SP value = 9.8 (cal / cm³) 3 ) 1 / 2 ), dioxane (SP value = 10.0 (cal / cm³) 3 ) 1 / 2 ), pyridine (SP value = 10.6 (cal / cm) 3 ) 1 / 2 Dimethylformamide (SP value = 12.1 (cal / cm³)) 3 ) 1 / 2 ), Ethanol (SP value = 12.9 (cal / cm³) 3 ) 1 / 2 Methanol (SP value = 14.3 (cal / cm³)) 3 ) 1 / 2 Isopropanol (SP value = 11.5 (cal / cm³)) 3 ) 1 / 2 (E) Components can be used alone or in combination of two or more. Component (E) is preferably selected from at least one of ethanol, methanol, isopropanol, and acetone, and more preferably from at least one of ethanol, methanol, and acetone.

[0055] In this disclosure, the SP value refers to the Hansen solubility parameter, which serves as a benchmark for the solubility of binary solutions. In this disclosure, the SP value (δ) ((cal / cm³)) is defined as follows: 3 ) 1 / 2 ) is the value calculated by the following formula (1).

[0056] δ=(δ d 2 +δ p 2 +δ h 2 ) 1 / 2 ···(1)

[0057] Here, δ d For the London dispersion term, δ p For molecular polarization, δ h This is a hydrogen bond term.

[0058] The SP value (δ) can be calculated using the Hansen Solubility Parameter Software (HSPiPver.4.1.x) or based on the values ​​described in "HANSEN SOLBILITY PARAMETERS" A User's Handbook Second Edition. Furthermore, the SP value when using multiple organic solvents is calculated as a weighted average m of the SP values ​​of each organic solvent. For example, the SP value when using two organic solvents is calculated using the following formula (2).

[0059] m=δ1φ1+δ2φ2 ···(2)

[0060] Here, δ1 and δ2 are the SP values ​​of each organic solvent, and φ1 and φ2 are the volume fractions of each organic solvent.

[0061] <Dosage of each ingredient>

[0062] The amount of component (A) relative to the volume of the treatment tank is preferably 0.001 to 10.0 mL / L, more preferably 0.01 to 5.0 mL / L, and even more preferably 0.05 to 2.0 mL / L. If the amount of component (A) is within the above range, the fastness can be further improved.

[0063] The amount of component (B) relative to the amount of component (D) is preferably 0.1% to 33% by mass, more preferably 3% to 33% by mass. If the amount of component (B) is within the above range, the fastness can be further improved.

[0064] (C) The amount of acid relative to the volume of the treatment tank is preferably 0.001 to 10.0 mL / L, more preferably 0.003 to 5.0 mL / L, and even more preferably 0.01 to 1.0 mL / L. If the amount of acid (C) is within the above range, the reducing power of component (B) can be further improved, and the fastness can be further improved.

[0065] (D) The amount of water relative to the volume of the treatment tank is preferably 0.01 to 20.0 mL / L, more preferably 0.03 to 15.0 mL / L, and even more preferably 0.1 to 10.0 mL / L. If the amount of water in (D) is within the above range, the fastness can be further improved.

[0066] (E) The amount of component relative to the volume of the treatment tank is preferably 0.05 to 12.5 mL / L, more preferably 0.09 to 10.0 mL / L, and even more preferably 0.25 to 7.5 mL / L. When the above amount exceeds 12.5 mL / L, the dye may sometimes be extracted from the fiber, resulting in a decrease in the color concentration of the fiber. If it is 0.05 mL / L or more, thorough cleaning can be performed, and the fastness can be further improved.

[0067] The amount of (F) water (also referred to as (F) component) that can be added in the second step described later is preferably 0.05 to 12.5 mL / L relative to the volume of the treatment tank, more preferably 0.1 to 10.0 mL / L, and even more preferably 0.25 to 7.5 mL / L. If the amount of (F) water is within the above range, thorough cleaning can be achieved, and the fastness can be further improved.

[0068] Supercritical Fluid Processing Unit

[0069] Reference Figure 1 This paper provides a detailed description of an exemplary supercritical fluid processing apparatus that uses supercritical carbon dioxide as the supercritical fluid. Figure 1 The supercritical fluid processing unit includes a carbon dioxide storage tank, a supply pump, a circulation pump, a dissolution tank, a processing tank, and a separation and recovery device. Figure 1 In this context, L refers to the liquid state, G refers to the gas state, and Sc refers to the supercritical state.

[0070] The supply pump is connected to the outlet of the carbon dioxide storage tank and the inlet of the circulation pump via a piping system, supplying carbon dioxide from the storage tank to the circulation pump. The carbon dioxide storage tank stores carbon dioxide in a liquid state, and the supply pump drives the continuous supply of carbon dioxide.

[0071] A heating section (not shown) is provided between the supply pump and the circulation pump. The heating section is capable of making the carbon dioxide after passing through the supply pump into a supercritical state.

[0072] The circulation pump is connected to the outlet of the supply pump and is positioned on the circulation path from the outlet of the treatment tank through the dissolving tank to the inlet of the treatment tank. Specifically, the circulation pump is connected to the first outlet of the treatment tank and the inlet of the dissolving tank. The circulation pump circulates the supercritical carbon dioxide present in the circulation path and within the treatment tank. This enables convection within the treatment tank to be formed during the dyeing and reduction cleaning processes.

[0073] The dissolving tank is connected to the outlet of the circulating pump and the inlet of the treatment tank. Dye is added to the dissolving tank and introduced into the treatment tank, where it dissolves in supercritical carbon dioxide.

[0074] The treatment tank has an inlet connected to the outlet of the dissolving tank, a first outlet connected to the inlet of the circulating pump, and a second outlet connected to the inlet of the separation and recovery device. In the treatment tank, the fiber product to be dyed can be dyed while wound in a bobbin. In this case, the treatment tank is configured to contain and hold the fiber product inside each bobbin. Supercritical carbon dioxide flowing into the treatment tank from the inlet flows radially outward from the central axis of the bobbin and exits from the first outlet. In the dyeing process, the dyed material is dyed and leveled in this state. Components (A) to (E) can be added to the treatment tank either via the dissolving tank or directly to the treatment tank.

[0075] The separation and recovery unit is connected to the second outlet of the processing tank and the inlet of the carbon dioxide storage tank, separating dyes and other impurities from the carbon dioxide. The vaporized carbon dioxide is discharged via a discharge valve (not shown) located in the separation and recovery unit. This allows for the efficient recovery of only carbon dioxide, enabling the reuse of carbon dioxide used in dyeing or reduction cleaning. The recovered carbon dioxide is contained in the carbon dioxide storage tank.

[0076] By installing the supply pump in a pipeline separately from the circulation path, after the dyeing process of the fiber products in the treatment tank is completed, the supercritical carbon dioxide can be circulated in the treatment tank and circulation path using the circulation pump, while the supply pump continuously supplies fresh, pure supercritical carbon dioxide, free of dye, into the treatment tank. This allows the fiber reduction and cleaning process (described later) to be performed continuously after the dyeing process.

[0077] Furthermore, the supercritical fluid processing device is not limited to the above structure and can be modified in various ways.

[0078] The dyes used for dyeing polyester fibers are, for example, at least one selected from the group consisting of direct dyes, reactive dyes, cationic dyes, disperse dyes, oil-soluble dyes, vat dyes, and sulfur dyes. The reduction cleaning method is particularly suitable for reducing and cleaning polyester fibers dyed with disperse dyes. Examples of disperse dyes include azo disperse dyes and quinone disperse dyes. Because the reduction cleaning method of one embodiment has excellent reduction cleaning ability, it can provide products with excellent fastness even in polyester fibers dyed with azo disperse dyes in a dark color. Examples of disperse dyes include compounds classified as CI Disperse Black, CI Disperse Blue, CI Disperse Red, CI Disperse Orange, CI Disperse Yellow, CI Disperse Green, CI Disperse Violet, and CI Disperse Brown.

[0079] [Reduction Cleaning Method]

[0080] The reduction cleaning of polyester fibers in supercritical fluids can be performed either in the same apparatus as the dyeing apparatus or in a different apparatus. The reduction cleaning of polyester fibers in supercritical fluids can be continued continuously immediately after the dyeing process. The steps of an exemplary reduction cleaning method are described below.

[0081] The reduction and cleaning process can be divided into a first reduction treatment step and a second cleaning step, or it can be carried out in a single step. From the viewpoint of improving fastness, it is preferable to divide it into a first step and a second step. When using a single step for reduction treatment and cleaning, the reduction treatment and cleaning of polyester fibers are carried out in the presence of supercritical fluid, (A) an alkylene oxide adduct of an alcohol with 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, (D) water, and (E) an organic solvent. For example, the reduction treatment and cleaning of polyester fibers can be carried out simply by adding components (A) to (E) to the treatment tank of the supercritical fluid treatment device and in the presence of supercritical fluid in which these components are dissolved. The order in which components (A), (B), (C), (D), (E) and the supercritical fluid are added relative to the treatment tank is not particularly limited. Components (A) to (E) can be added separately or pre-mixed, but it is preferable to pre-dissolve the reducing agent (B) in water (D). After reduction treatment and cleaning, the supercritical fluid in the treatment tank is discharged. The discharged supercritical fluid can be transferred to a separation and recovery unit. Alternatively, after discharging the supercritical fluid from the treatment tank, the supercritical fluid can be reintroduced to clean the polyester fibers and the treatment tank. The preferred conditions for this step are the same as those for the fourth step described later.

[0082] When performing reduction treatment and cleaning in a single process, the temperature and pressure of the reduction treatment and cleaning can be appropriately set according to the type of supercritical fluid used. At excessively low temperatures, components (A) to (E) tend to have lower solubility in the supercritical fluid. At excessively low pressures, a supercritical state cannot be achieved, making reduction cleaning impossible.

[0083] For example, when using supercritical carbon dioxide as the supercritical fluid, the temperature for reduction treatment and cleaning is preferably 65°C or higher and 105°C or lower, more preferably 70°C or higher and 100°C or lower, and even more preferably 80°C or higher and 95°C or lower. The pressure for reduction treatment and cleaning is preferably 18 MPa or higher and 26 MPa or lower. If the temperature is within the above pressure range, the carbon dioxide will become supercritical, and components (A) to (E) will dissolve in the supercritical carbon dioxide and fill the entire interior of the treatment tank. By ensuring good solubility of components (A) to (E) in supercritical carbon dioxide, there is a tendency for the adhesion to also improve.

[0084] The holding time after reaching the reduction treatment and cleaning temperature is not particularly limited; for example, it can be between 10 minutes and 300 minutes. Since the degree of reduction treatment and cleaning may vary depending on the holding time, the holding time should be appropriately determined based on the desired degree of reduction treatment and cleaning. If the holding time is too short, sufficient cleaning properties may not be achieved. If the holding time is too long, dye re-adhesion to the polyester fibers may occur, resulting in reduced cleaning properties.

[0085] When the processes are separated, in the first process, the polyester fibers can be reduced in the presence of supercritical fluid, component (A), component (B), component (C), and component (D). In the second process, component (E) is added, and component (F) is added selectively, and the polyester fibers are washed in the presence of supercritical fluid. The supercritical fluid used in the first process can be reused in the second process, or it can be discharged after the first process and reintroduced before the second process; the latter method is preferred. The discharged supercritical fluid can be transferred to a separation and recovery unit. If the supercritical fluid is discharged after the first process, the dye and components (A) to (D) separated from the polyester fibers in the first process are also discharged along with the supercritical fluid.

[0086] (First process)

[0087] In the first step, the reduction treatment of polyester fibers is carried out in the presence of supercritical fluid, (A) an alkylene oxide adduct of an alcohol having 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, and (D) water. For example, the reduction treatment of polyester fibers can be carried out simply by adding (A) an alkylene oxide adduct of an alcohol having 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, and (D) water to the treatment tank of the supercritical fluid treatment apparatus, and in the presence of supercritical fluid in which these components are dissolved. The order in which components (A), (B), (C), (D), and the supercritical fluid are added relative to the treatment tank is not particularly limited. Components (A) to (D) can be added separately or pre-mixed, but it is preferable to pre-dissolve the reducing agent (B) in the water (D).

[0088] The temperature and pressure of the reduction process in the first step can be appropriately set according to the type of supercritical fluid used. At excessively low temperatures, components (A) to (D) tend to have lower solubility in the supercritical fluid. At excessively low pressures, the process will not reach a supercritical state and cleaning will not be possible.

[0089] For example, when using supercritical carbon dioxide as the supercritical fluid, the temperature of the reduction treatment in the first step is preferably 65°C or higher and 105°C or lower, more preferably 70°C or higher and 100°C or lower, and even more preferably 90°C or higher and 100°C or lower. The pressure of the reduction treatment in the first step is preferably 18 MPa or higher and 26 MPa or lower. If the temperature is within the above-mentioned pressure range, the carbon dioxide will become supercritical, and components (A) to (D) will dissolve in the supercritical carbon dioxide and fill the entire interior of the treatment tank. By making the components (A) to (D) readily soluble in supercritical carbon dioxide, there is a tendency for the fastness to also improve.

[0090] The holding time after reaching the reduction treatment temperature is not particularly limited; for example, it can be more than 10 minutes and less than 300 minutes. Since the degree of reduction treatment may vary depending on the holding time, the holding time should be appropriately determined based on the desired degree of reduction. If the holding time is too short, sufficient reducibility may not be achieved.

[0091] The specific temperature and pressure of the reduction process in the first step when using supercritical carbon dioxide as a supercritical fluid are, for example, 85°C and 20 MPa.

[0092] (Second process)

[0093] In the second step, organic solvent (E) is added to the treatment tank, and water (F) is added selectively. The tank is maintained for a specified time in the presence of supercritical fluid and then rinsed. By using component (E) and selectively chosen component (F) in the second step, residual dye and dye reduced in the first step can be removed more effectively. The order in which components (E), (F), and supercritical fluid are added relative to the treatment tank is not particularly limited. Components (E) and (F) can be added separately or pre-mixed.

[0094] The temperature and pressure of the cleaning process in the second step can be appropriately set according to the type of supercritical fluid used. At excessively low temperatures, cleaning performance tends to decrease. Conversely, at excessively high temperatures, cleaning performance also tends to decrease. At excessively low pressures, a supercritical state cannot be achieved, making cleaning impossible. At excessively high pressures, cleaning performance tends to decrease.

[0095] For example, when using supercritical carbon dioxide as the supercritical fluid, the cleaning temperature in the second step is preferably 65°C or higher and 130°C or lower, more preferably 70°C or higher and 130°C or lower, and even more preferably 75°C or higher and 125°C or lower. The cleaning pressure in the second step is preferably 18 MPa or higher and 26 MPa or lower.

[0096] The holding time after reaching the washing temperature is not particularly limited; for example, it can be between 10 minutes and 300 minutes. Since the degree of washing may vary depending on the holding time, the holding time should be appropriately determined based on the desired degree of washing. If the holding time is too short, sufficient washing performance may not be achieved. If the holding time is too long, dye re-adhesion to the polyester fibers may occur, resulting in reduced washing performance.

[0097] In the second step, when supercritical carbon dioxide is used as the supercritical fluid, the specific cleaning temperature and pressure are, for example, 85°C and 20 MPa.

[0098] (Third process)

[0099] Alternatively, a third step can be performed after the second step to discharge the supercritical fluid from the treatment tank. The discharged supercritical fluid can be transferred to a separation and recovery unit. The dyes, components (A) to (E), and any (F) components separated from the polyester fibers in the second step are also discharged along with the supercritical fluid.

[0100] (Fourth process)

[0101] The reduction cleaning method for polyester fibers can also include a fourth step, after the second step, in which supercritical fluid is introduced into a treatment tank and used to clean the polyester fibers and the treatment tank. The fourth step can be performed after the second step or after the third step, which is either a second or third step. In the fourth step, residual dyes and components (A) to (E) are dissolved in the supercritical fluid.

[0102] The temperature and pressure of the cleaning process in the fourth step can be appropriately set according to the type of supercritical fluid used. At excessively low temperatures, the cleaning performance tends to decrease. At excessively low pressures, a supercritical state cannot be achieved, making cleaning impossible.

[0103] For example, when using supercritical carbon dioxide as a supercritical fluid, the cleaning temperature in the fourth step is preferably 50°C or higher and 150°C or lower, more preferably 55°C or higher and 140°C or lower, for example 85°C.

[0104] For example, when using supercritical carbon dioxide as the supercritical fluid, the cleaning pressure in the fourth step is preferably 10 MPa or more and 28 MPa or less, for example, 20 MPa.

[0105] The holding time after reaching the cleaning temperature is not specifically limited; for example, it can be more than 10 minutes and less than 300 minutes.

[0106] Example

[0107] Hereinafter, while showing embodiments, the effects produced by the technology of this disclosure will be described in more detail, but the technology of this disclosure is not limited to the specific examples below.

[0108] (Wet rubbing fastness)

[0109] The wet rubbing fastness test was conducted according to JIS L 0849:2013 and evaluated based on JIS L 0805:2005, with level 3 and above considered as qualified.

[0110] As alkyl oxidase adducts of alcohols with 8 to 14 carbon atoms (A), compounds a to i synthesized in Synthesis Examples 1 to 9 were used.

[0111] <Synthesis example 1>

[0112] 130 g of 2-octanol (manufactured by Tokyo Chemical Industry Co., Ltd.) and 0.37 g of caustic soda were added to a 1 L autoclave and the vessel was sealed. After nitrogen purging, the autoclave was heated to 160 °C, and 158.3 g of ethylene oxide was injected. After aging for 120 minutes, the autoclave was cooled to 120 °C. Degassing was then performed after reaching 120 °C. After degassing, the autoclave was cooled to 80 °C, and 0.19 g of acetic acid (80% by mass) was added. The autoclave was stirred for 30 minutes, thereby synthesizing compound a (ethylene oxide adduct of 2-octanol, ethylene oxide molar addition: 3).

[0113] <Synthesis Examples 2~9>

[0114] Except for the change in the molar number of the starting alcohol and ethylene oxide addition as described in Table 1, compound b~i was obtained in the same manner as in Synthesis Example 1.

[0115] Table 1

[0116]

[0117] The following ingredients were used as other components.

[0118] (B) Reducing agent

[0119] L-Ascorbic acid (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0120] (C) acid

[0121] Acetic acid (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0122] (E) Organic solvents

[0123] Methanol (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0124] Ethanol (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0125] Acetone (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0126] Isopropyl alcohol (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0127] (Making of dyed cloth)

[0128] Using a supercritical fluid treatment apparatus (treatment tank volume = 2700 mL) with dye, 200.0 g of undyed woven tape (made of polyethylene terephthalate (PET)) was wound into a bobbin and exposed to supercritical carbon dioxide along with the dye in the treatment tank. For the dye, a solid dye was prepared in a dissolving tank. Disperse Blue 301 (2.5% owf) was used as the dye. %owf refers to the percentage by weight relative to 1 g of the dyed material. The dye input was 5 g. The dyeing temperature was 125°C, and the dyeing pressure was 25 MPa. The dyeing time was 60 minutes. Afterwards, the temperature and pressure were set below 80°C and atmospheric pressure, and the dyeing process was completed, yielding dyed fabric.

[0129] In Examples 1-11 and 13-24, reduction cleaning was performed through the first, second, third and fourth processes described above.

[0130] [Example 1]

[0131] 0.31 mL of compound a (A), an ascorbic acid aqueous solution obtained by dissolving 0.345 g of ascorbic acid in 1.05 mL of water (D), and an acetic acid aqueous solution obtained by diluting 0.15 mL of acetic acid (C) with 0.04 mL of water (D) were added to the treatment tank (treatment tank volume = 2700 mL) of the supercritical fluid treatment apparatus used to produce the dyed fabric. The mixture was then dissolved in supercritical carbon dioxide at 85°C and 20 MPa for 60 minutes. Next, the supercritical carbon dioxide was transferred to a separation and recovery unit to separate and remove the carbon dioxide from the other components. Then, supercritical carbon dioxide was reintroduced into the treatment tank, and 1.5 mL of methanol (E) and 1.5 mL of water (F) were added. The dyed fabric was washed at 85°C and 20 MPa for 60 minutes, after which the supercritical carbon dioxide was transferred to the separation and recovery unit. Subsequently, supercritical carbon dioxide was reintroduced, and the dyed fabric and treatment tank were cleaned using supercritical carbon dioxide at 80°C and 25 MPa to obtain a reduced-wash fabric. The wet rubbing fastness of the obtained reduced-wash fabric was evaluated. The results are shown in Table 2.

[0132] [Examples 2-11, 13-24, Comparative Examples 1-7]

[0133] Except for the changes to components (A) to (F) as shown in Table 2, the procedure was performed in the same manner as in Example 1, and the reductive cleaning cloth was obtained. Furthermore, in Example 19, an ascorbic acid aqueous solution obtained by dissolving 0.03 g of (B) ascorbic acid in 0.1 mL of (D) water and 0.15 mL of (C) acetic acid were used; in Example 20, an ascorbic acid aqueous solution obtained by dissolving 3.3 g of (B) ascorbic acid in 10 mL of (D) water and 0.15 mL of (C) acetic acid were used. The wet rubbing fastness of the obtained reductive cleaning cloth was evaluated. The results are shown in Table 2.

[0134] [Example 12]

[0135] In Example 12, after a reduction treatment and cleaning process, supercritical fluid was reintroduced and the dyed fabric and treatment tank were cleaned. 0.31 mL of compound a (A), an ascorbic acid aqueous solution obtained by dissolving 0.345 g of ascorbic acid in 1.05 mL of water (D), an acetic acid aqueous solution obtained by diluting 0.15 mL of acetic acid in 0.04 mL of water (D), and 1.5 mL of methanol (E) were added to the treatment tank (treatment tank volume = 2700 mL) of the supercritical fluid treatment apparatus used to produce the dyed fabric. The solution was dissolved in supercritical carbon dioxide at 85°C and 20 MPa for 90 minutes. Next, the supercritical carbon dioxide was conveyed to a separation and recovery unit to separate and remove the carbon dioxide from the other components. Then, supercritical carbon dioxide was reintroduced, and the dyed fabric and treatment tank were cleaned using supercritical carbon dioxide at 85°C and 20 MPa to obtain a reduced-cleaned fabric. The wet rubbing fastness of the obtained reduced-cleaned fabric was evaluated. The results are shown in Table 2.

[0136] Table 2-1

[0137]

[0138] Table 2-2

[0139]

[0140] Table 2-3

[0141]

[0142] Table 2-4

[0143]

[0144] In Comparative Examples 1-7, the wet rubbing fastness was grade 1 or 2. In Examples 1-24, the wet rubbing fastness was significantly improved to grade 3 or higher, resulting in excellent results compared to the comparative examples.

Claims

1. A reduction cleaning method for polyester fibers, wherein the reduction cleaning of the polyester fibers is performed after a dyeing process in a supercritical fluid, characterized in that... The reduction and cleaning method for the polyester fibers includes: In the first step, polyester fibers are reduced in the treatment tank of the supercritical fluid treatment device in the presence of supercritical fluid, (A) alkyl oxidase adduct of alcohol with 8 to 14 carbon atoms, (B) reducing agent, (C) acid and (D) water. as well as In the second step, following the first step, an organic solvent (E) is added to the treatment tank, and the polyester fibers are cleaned in the presence of a supercritical fluid.

2. A reduction cleaning method for polyester fibers, wherein the reduction cleaning of the polyester fibers is performed after a dyeing process in a supercritical fluid, characterized in that... The reduction and cleaning method for the polyester fibers includes the following steps: in the treatment tank of a supercritical fluid treatment device, the polyester fibers are subjected to reduction treatment and cleaning in the presence of supercritical fluid, (A) an epoxide adduct of an alcohol with 8 to 14 carbon atoms, (B) a reducing agent, (C) an acid, (D) water and (E) an organic solvent.

3. The reduction cleaning method for polyester fibers according to claim 1, characterized in that, In the second step, water (F) is added further.

4. The reduction cleaning method for polyester fibers according to claim 1 or 3, characterized in that, Following the second step, a third step is performed to discharge the supercritical fluid from the treatment tank.

5. The reduction cleaning method for polyester fibers according to claim 1 or 3, characterized in that, Following the second step, a fourth step is performed whereby supercritical fluid is introduced into the treatment tank and used to clean the polyester fibers and the treatment tank.

6. The reduction cleaning method for polyester fibers according to any one of claims 1 to 3, characterized in that, The reduction process is carried out at a temperature of 65°C or higher and 105°C or lower.

7. The reduction cleaning method for polyester fibers according to any one of claims 1 to 3, characterized in that, The reduction process is carried out at a pressure of 18 MPa or higher and 26 MPa or lower.

8. The reduction cleaning method for polyester fibers according to any one of claims 1 to 3, characterized in that, (E) The SP value of the organic solvent is 9~15 (cal / cm³). 3 ) 1 / 2 .

Citation Information

Patent Citations

  • Method of dyeing hydrophobic fiber material from supercritical carbon dioxide by disperse dye

    JP1993132880A

  • Method for dyeing and dyed material dyed by using the same method

    JP2002371483A