Preparation method of electromagnetic shielding structural color fabric

By assembling a conductive network of MXene and single-walled carbon nanotubes on cotton fabric and coating it with liquid photonic crystals, the problem of insufficient aesthetics in electromagnetic shielding fabrics was solved, achieving the effect of combining high-efficiency electromagnetic protection with vivid structural color.

CN123153282APending Publication Date: 2026-11-24XINJIANG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610478333.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-13
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing electromagnetic shielding fabrics struggle to combine functionality and aesthetics, and traditional materials are mostly black, failing to meet the demands of multifunctional flexible wearable textiles.

Method used

A conductive network is constructed by synergistically using MXene and single-walled carbon nanotubes, and liquid photonic crystals are assembled on cotton fabric to form an electromagnetic shielding structured fabric. By utilizing the high conductivity of MXene and the structural color effect of photonic crystals, the dual functions of electromagnetic protection and visual aesthetics are achieved.

Benefits of technology

It successfully endows cotton fabrics with excellent electromagnetic shielding properties, while exhibiting a distinct iridescent effect, realizing the dual functions of electromagnetic protection and visual aesthetics of the fabric, and possessing high electromagnetic shielding effectiveness and color saturation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153282A_ABST
    Figure CN123153282A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing an electromagnetically shielded structural colored fabric, belonging to the field of textile processing technology. The method includes: S1, preparing a P-microsphere emulsion, namely a St-MMA-AA microsphere emulsion; S2, preparing a liquid photonic crystal; S3, preparing an Mxene aqueous dispersion; S4, synthesizing the P emulsion, namely an MMA-BA emulsion; and S5, preparing the electromagnetically shielded structural colored fabric. Based on the highly efficient conductive network synergistically constructed by MXene and SWCNTs, excellent electromagnetic shielding performance is successfully endowed to cotton fabric. Simultaneously, utilizing the characteristic that the dark substrate of the MXene-treated fabric can effectively absorb stray light, the liquid photonic crystal is orderly assembled on this substrate to form a structural color with a distinct iridescent effect, achieving a dual integration of electromagnetic protection and visual aesthetics in the fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of textile processing technology, and in particular to a method for preparing an electromagnetically shielded structural colored fabric. Background Technology

[0002] With the widespread adoption of 5G communication and smart electronic devices, electromagnetic radiation has become the third largest environmental hazard after air and water pollution. It not only interferes with the normal operation of precision electronic equipment but also poses a potential threat to human health. Therefore, the demand for highly efficient electromagnetic shielding materials is increasingly urgent in industrial production, national defense, and everyday wearable devices. Fabrics, as flexible and wearable carriers, have become the preferred form of electromagnetic shielding material due to their excellent comfort and fit. The electromagnetic shielding effectiveness of electromagnetic shielding fabrics consists of absorption loss, reflection loss, and multiple reflection loss of electromagnetic waves. To ensure the effectiveness of electromagnetic shielding fabrics and prevent electromagnetic waves from passing through objects, the electromagnetic waves are typically reflected, absorbed, and reflected multiple times by the object, thereby achieving the shielding effect of the electromagnetic shielding fabric.

[0003] MXene, as an emerging two-dimensional material, possesses a unique layered structure, excellent charge transport capabilities, high conductivity, hydrophilicity, and environmental friendliness. In particular, the abundant oxygen-containing functional groups (-OH, -O, -F) on the MXene surface allow it to directly bond with fibers via hydrogen bonds or covalent bonds, mitigating to some extent the problem of the inability to firmly bond conductive metal materials to fabrics. Cotton fabric, naturally hydrophilic, is commonly used as the substrate for MXene shielding fabrics. MXene and cotton fabric can be bonded through capillary forces and hydrogen bonds via methods such as impregnation and spraying. However, most traditional electromagnetic shielding materials are predominantly black and difficult to color due to material properties. For multifunctional flexible wearable textiles, the combination of functionality and aesthetics has become a core requirement.

[0004] Structural colors are generated through light scattering and interference effects in micro- and nanostructures, requiring no harmful chemical reagents and possessing outstanding characteristics such as being environmentally friendly, pollution-free, having high color saturation, and being resistant to fading. Photonic crystals, as the primary source of structural colors, are composite media composed of two media materials with different refractive indices arranged periodically. Due to their unique periodic structure, photonic crystals generate photonic band gaps, preventing light in specific wavelength ranges from propagating within this medium. When light penetrates a photonic crystal, light within a specific wavelength range is reflected in the photonic band gap region, achieving coherent diffraction on the crystal surface, thus displaying vivid structural colors. This process is also known as Bragg diffraction. Notably, electronic shielding textiles prepared using MXene as the main material possess excellent light absorption capabilities, effectively eliminating excess scattered light generated by photonic crystal materials under light, avoiding stray light interference, and resulting in structural color fabrics with purer colors, higher saturation, and more vivid color rendering. Therefore, developing a method combining structural colors with electromagnetic shielding fabrics is of great significance for the development and practical application of functional structural color fabrics. Summary of the Invention

[0005] This invention provides a method for preparing an electromagnetic shielding structured colored fabric, which integrates the dual functions of electromagnetic protection and visual aesthetics.

[0006] According to one aspect of this disclosure, a method for preparing an electromagnetic shielding structural colored fabric is provided, the method comprising: S1, prepare P microsphere emulsion, which is St-MMA-AA microsphere emulsion; S2, preparation of liquid photonic crystals; S3, prepare Mxene aqueous dispersion; S4, P emulsion synthesis, P emulsion is MMA-BA emulsion; S5, Prepare electromagnetic shielding structural colored fabric.

[0007] In one possible implementation, the preparation of the P-microsphere emulsion includes: At room temperature, add 2 g of ammonium bicarbonate and 440 mL of deionized water to a three-necked flask and stir until completely dissolved; Measure 40 mL - 70 mL of 2 g / L SDBS aqueous solution into the three-necked flask above using a graduated cylinder. Weigh 76 g of styrene (St), 4 g of methyl methacrylate (MMA), and 4 g of acrylic acid (AA) and add them into the flask. After the temperature is raised to 80 ℃, 1.432 g of ammonium persulfate (APS) dissolved in 40 mL of deionized water is added at once. After reacting for 6 h, a milky white liquid is obtained. The liquid is then filtered through a 200-mesh nylon filter and stored.

[0008] In one possible implementation, the preparation of a liquid photonic crystal includes: The prepared P microsphere emulsion was centrifuged in a centrifuge tube to remove water from the system and obtain microsphere precipitate. Then, freeze-drying was used to remove all the water from the microsphere precipitate. After grinding the freeze-dried microspheres into powder using a mortar and pestle, add P microsphere powder, deionized water and carbon black in a volume ratio of 1:1:0.5% to the sample vial.

[0009] In one possible implementation, the preparation of the Mxene aqueous dispersion includes: Take 15 mL of concentrated hydrochloric acid into a polytetrafluoroethylene reaction vessel, add 1.6 g of lithium fluoride, stir magnetically, and then add 5 mL of deionized water and stir. Transfer the container to a water bath at 35°C, slowly add 1 g of Ti3AlC2 powder, and react at a constant temperature for 24 h. First, wash the solution three times with 1 mol / L dilute hydrochloric acid solution by centrifugation, then wash with deionized water and centrifuge 15-18 times to obtain an MXene aqueous dispersion.

[0010] In one possible implementation, P emulsion synthesis includes: First, 0.6 g of sodium dodecyl sulfate (SDS) and 80 mL of water were stirred at 350 rpm and heated to 80 °C. Then, methyl methacrylate (MAA) and butyl acrylate (BA) were added for emulsification. After emulsification for 30 min, 0.1 g of potassium persulfate (KPS) dissolved in 10 mL of deionized water was added at once. The mixture was then reacted for 5 h to obtain emulsion P.

[0011] In one possible implementation, the electromagnetic shielding structural colored fabric is prepared by: 0.2 g of single-walled carbon nanotubes and 1 g of SDS surfactant were dispersed in 40 mL of deionized water and then ultrasonically bathed in ice water for 60 min to obtain a uniform dispersion of single-walled carbon nanotubes. MXene and single-walled carbon nanotubes were mixed at a mass ratio of 3:1. The mixture was sonicated in an ice bath and then magnetically stirred for 120 min. The cotton fabric was immersed in the prepared mixed solution 12 times to obtain a conductive fabric with a black base. The black fabric was then immersed in water-based polyurethane (WPU) and dried. After being coated with liquid photonic crystal, it was sintered at 90 °C for 10 min and finally immersed in a P solution with a solid content of 5% and dried.

[0012] Compared with the prior art, the beneficial effects of the present invention are: Here, this study successfully endows cotton fabrics with excellent electromagnetic shielding performance based on the efficient conductive network constructed by MXene and SWCNTs. At the same time, taking advantage of the property that the dark base of the fabric treated with MXene can effectively absorb stray light, liquid photonic crystals are assembled in an orderly manner on the base to form a structural color with a distinct iridescent effect, thus realizing the dual function integration of electromagnetic protection and visual aesthetics of the fabric. Attached Figure Description

[0013] Figure 1 The image shows a scanning electron microscope (SEM) image of P(St-MMA-AA) colloidal microspheres according to an embodiment of the present disclosure.

[0014] Figure 2 The diagram shows the particle size distribution of P(St-MMA-AA) colloidal microspheres according to an embodiment of the present disclosure.

[0015] Figure 3 Digital photographs of LPCs of different particle sizes doped with CB according to an embodiment of this disclosure are shown.

[0016] Figure 4 The reflection spectra of liquid photonic crystals with different particle sizes according to an embodiment of the present disclosure are shown.

[0017] Figure 5 The images shown are SEM images of a MAX phase, an SEM image of MXene, and a TEM image of MXene, according to an embodiment of this disclosure.

[0018] Figure 6 SEM images of different fabrics according to an embodiment of this disclosure are shown.

[0019] Figure 7 SEM images and mapping diagrams of a fabric cross-section according to an embodiment of the present disclosure are shown.

[0020] Figure 8 Digital photographs of different colored electromagnetic shielding structural fabrics according to an embodiment of this disclosure are shown.

[0021] Figure 9 The reflectance spectra of different colored electromagnetic shielding structural fabrics according to an embodiment of this disclosure are shown.

[0022] Figure 10 The graph shows the total electromagnetic shielding performance test results of different immersion times according to an embodiment of the present disclosure.

[0023] Figure 11 A graph showing the total average EMI, SEA, and SER values ​​for different number of immersions according to an embodiment of the present disclosure is presented.

[0024] Figure 12 The diagram shows the test results of the photothermal performance of a structurally colored fabric according to an embodiment of the present disclosure.

[0025] Figure 13 The diagram shows the test results of the electrothermal heating performance of a structurally colored fabric according to an embodiment of the present disclosure.

[0026] Figure 14 A flowchart illustrating a method for preparing an electromagnetic shielding structured colored fabric according to an embodiment of the present disclosure is shown. Detailed Implementation

[0027] Various exemplary embodiments, features, and aspects of this disclosure will now be described in detail with reference to the accompanying drawings. The same reference numerals in the drawings denote elements that have the same or similar functions. Although various aspects of the embodiments are shown in the drawings, they are not necessarily drawn to scale unless specifically indicated otherwise.

[0028] The term “exemplary” as used herein means “serving as an example, embodiment, or illustration.” Any embodiment illustrated herein as “exemplary” is not necessarily to be construed as superior to or better than other embodiments.

[0029] Furthermore, to better illustrate this disclosure, numerous specific details are set forth in the following detailed description. Those skilled in the art will understand that this disclosure can be practiced without certain specific details. In some instances, methods, means, components, and circuits well known to those skilled in the art have not been described in detail in order to highlight the main points of this disclosure.

[0030] According to one aspect of this disclosure, a method for preparing an electromagnetic shielding structural colored fabric is provided, the method comprising: S1, prepare P microsphere emulsion, which is St-MMA-AA microsphere emulsion; S2, preparation of liquid photonic crystals; S3, prepare Mxene aqueous dispersion; S4, P emulsion synthesis, P emulsion is MMA-BA emulsion; S5, Prepare electromagnetic shielding structural colored fabric.

[0031] In one possible implementation, the preparation of the P-microsphere emulsion includes: At room temperature, add 2 g of ammonium bicarbonate and 440 mL of deionized water to a three-necked flask and stir until completely dissolved; Measure 40 mL - 70 mL of 2 g / L SDBS aqueous solution into the three-necked flask above using a graduated cylinder. Weigh 76 g of styrene (St), 4 g of methyl methacrylate (MMA), and 4 g of acrylic acid (AA) and add them into the flask. After the temperature is raised to 80 ℃, 1.432 g of ammonium persulfate (APS) dissolved in 40 mL of deionized water is added at once. After reacting for 6 h, a milky white liquid is obtained. The liquid is then filtered through a 200-mesh nylon filter and stored.

[0032] In one possible implementation, the preparation of a liquid photonic crystal includes: The prepared P microsphere emulsion was centrifuged in a centrifuge tube to remove water from the system and obtain microsphere precipitate. Then, freeze-drying was used to remove all the water from the microsphere precipitate. After grinding the freeze-dried microspheres into powder using a mortar and pestle, add P microsphere powder, deionized water and carbon black in a volume ratio of 1:1:0.5% to the sample vial.

[0033] In one possible implementation, the preparation of the Mxene aqueous dispersion includes: Take 15 mL of concentrated hydrochloric acid into a polytetrafluoroethylene reaction vessel, add 1.6 g of lithium fluoride, stir magnetically, and then add 5 mL of deionized water and stir. Transfer the container to a water bath at 35 °C, slowly add 1 g of Ti3AlC2 powder, and react at a constant temperature for 24 h. First, wash the solution three times with 1 mol / L dilute hydrochloric acid solution by centrifugation, then wash with deionized water and centrifuge 15-18 times to obtain an MXene aqueous dispersion.

[0034] In one possible implementation, P emulsion synthesis includes: First, 0.6 g of sodium dodecyl sulfate (SDS) and 80 mL of water were stirred at 350 rpm and heated to 80 °C. Then, methyl methacrylate (MAA) and butyl acrylate (B) were added for emulsification. After emulsification for 30 min, 0.1 g of potassium persulfate (KPS) dissolved in 10 mL of deionized water was added at once. The mixture was then reacted for 5 h to obtain emulsion P.

[0035] 6. The method for preparing an electromagnetic shielding structural colored fabric according to claim 1, characterized in that the preparation of the electromagnetic shielding structural colored fabric includes: 0.2 g of single-walled carbon nanotubes and 1 g of SDS surfactant were dispersed in 40 mL of deionized water and then ultrasonically bathed in ice water for 60 minutes to obtain a uniform dispersion of single-walled carbon nanotubes. MXene and single-walled carbon nanotubes were mixed at a mass ratio of 3:1. The mixture was sonicated in an ice bath and then magnetically stirred for 120 min. The cotton fabric was immersed in the prepared mixed solution 12 times to obtain a conductive fabric with a black base. The black fabric was then immersed in water-based polyurethane (WPU) and dried. After being coated with liquid photonic crystals, it was sintered at 90 °C for 10 min and finally immersed in a P solution with a solid content of 5% and dried.

[0036] Testing process: Characterization of the microstructure of colloidal microspheres: Colloidal microspheres of different sizes were tested using a scanning electron microscope, and the obtained SEM images were imported into Nano measurer software to measure the particle size of each microsphere.

[0037] Optical property testing of liquid photonic crystals: The prepared LPCs were tested for reflectance spectra using an UltraScan PRO colorimeter, and digital photographs of LPCs of different colors were taken.

[0038] Characterization of the microstructure of MXene: The MAX phase and the successfully prepared MXene were tested using scanning electron microscopy and transmission electron microscopy, and the prepared MXene was analyzed using SEM and TES images.

[0039] Optical property testing of electromagnetic shielding structured colored fabric: The reflectance spectrum of the prepared electromagnetic shielding structural fabric was tested using an UltraScan PRO colorimeter, and digital photographs of electromagnetic shielding structural fabrics of different colors were taken.

[0040] Characterization of the microstructure of electromagnetic shielding structured fabric: Scanning electron microscopy was used to test and analyze the electromagnetic shielding structure fabrics at different stages to determine whether MXene, SWCNTs, and photonic crystal microspheres were successfully loaded onto the cotton fabrics.

[0041] Electromagnetic shielding performance test of fabric: Electromagnetic shielding fabrics were tested using a vector grid analyzer with the waveguide method, and their electromagnetic shielding performance and mechanism were analyzed.

[0042] Test results: Microscopic morphology of colloidal microspheres: P(St-MMA-AA) nanospheres are prepared through soap-free emulsion polymerization. The microscopic morphology of the nanospheres is as follows: Figure 1 As shown, the nanospheres have smooth surfaces, regular morphology, and uniform arrangement. By changing the amount of SDBS, the particle size of the microspheres can be precisely controlled in the range of 203–286 nm, and all samples show good monodispersity (PDI<0.08).

[0043] Based on SEM images, the size and monodispersity of six different P(St-MMA-AA) microspheres were characterized using Nano measurer software. The results are as follows: Figure 2 As shown.

[0044] Preparation of liquid photonic crystals This project prepares photonic crystal powder using freeze-drying and then introduces carbon black (CB) into a liquid photonic crystal system to absorb scattered light, thereby enhancing the saturation of structural colors, such as... Figure 3 As shown, the liquid photonic crystal doped with carbon black exhibits a bright structural color.

[0045] By adjusting the concentration of SDBS (sodium dodecylbenzenesulfonate), the morphology and size of P(St-MMA-AA) microspheres were effectively controlled, and P(St-MMA-AA) microspheres with particle sizes of 203 nm, 215 nm, 230 nm, 236 nm, 262 nm, and 286 nm were prepared. With the increase of SDBS dosage, the particle size of the microspheres showed a decreasing trend, and the structural color exhibited a significant blue shift.

[0046] Figure 4 The reflection spectra of the color-generating fabrics with different photonic crystal structures show that each reflection peak is narrow and high, indicating that the prepared photonic crystal structure color-generating fabrics have high band gap intensity and saturation, and the reflection peaks shift to the short-wavelength direction as the particle size decreases.

[0047] Preparation of MXene: MXene nanosheets were prepared using a chemical etching method. Synthesis was achieved by selectively etching an aluminum layer of the MAX phase, followed by sandwiching and exfoliation processes to obtain dispersions of monolayer or few-layer MXene nanosheets. Figure (a) shows a scanning electron microscope (SEM) image of the MAX phase, revealing a layered structure with tight layer contacts. Figures (b) and (c) show SEM and TEM images of MXene, respectively. Clearly, the MXene sheets are stacked to form wrinkle-like thin layers. Transmission electron microscope images further confirm that the synthesized MXene consists of monolayer or few-layer two-dimensional sheets. These results demonstrate the successful preparation of MXene.

[0048] Preparation of electromagnetic shielding structural colored fabric: Figure 6(a1-a4) are SEM images of the original cotton fabric at different magnifications. The images clearly show the fiber structure of the original cotton fabric, with a relatively smooth surface. (b1-b4) are SEM images of the cotton fabric after being impregnated with a mixed solution of MXene / SWCNTs at different magnifications. It can be seen that the surface pores of the resulting black substrate fabric are filled, the fiber surface is significantly roughened, and uniformly adhered sheet-like material is observed, accompanied by white filamentous structures. This indicates that the sheet-like MXene and filamentous SWCNTs have been successfully loaded onto the fiber surface, jointly constructing a continuous conductive network. (c1-c4) are SEM images of the fabric after being coated with WPU at different magnifications. It can be seen that the fabric pores are filled with WPU, and adhesion occurs between the fibers, forming a dense coating layer that effectively prevents the oxidation of MXene. (d1-d4) are SEM images at different magnifications after the photonic crystal is assembled. It can be seen that a photonic crystal coating with a typical face-centered cubic arrangement structure was successfully constructed on the fabric surface. After PA impregnation, the gaps between the microspheres were filled, and the coating became denser and smoother, thus significantly improving the bonding strength and overall stability of the coating.

[0049] Figure 6 (a1-a4) SEM images of raw cotton fabric at 50, 3000, 5000, and 10000x magnification; (b1-b4) SEM images of fabric after soaking in MXene / SWCNTs at 50, 3000, 5000, and 10000x magnification; (c1-c2) SEM images of fabric after scraping with WPU at 50, 3000, 5000, and 10000x magnification; (d1-d4) SEM images of electromagnetically shielded structured colored fabric at 50, 3000, 5000, and 10000x magnification.

[0050] Figure 7 SEM images and mapping images of the fabric cross-section. Figure 7The last two images show the EDS elemental (O and Ti) mapping images of the fabric cross-section to demonstrate that the fabric has a multi-layered sandwich structure. The SEM images clearly show a sandwich structure in the fabric cross-section, consisting of a WPU layer, an MXene fabric layer, another WPU layer, a photonic crystal, and a PA layer. C is uniformly concentrated in the middle layer, confirming that carbon is the main framework of this layer. Combined with the elemental ratio and high C content, this strongly suggests that the main component of this layer is MXene (Ti3C2Tx), a carbide. Simultaneously, the fabric substrate (cellulose) and possible SWCNTs also contribute C signals. The distribution of Ti and C highly overlaps, concentrated and uniformly distributed in the middle layer. This is the most direct evidence for the existence of MXene, as Ti is the characteristic metallic element of MXene (Ti3C2Tx). The co-distribution of Ti and C indicates the formation of a stable Ti-C bond structure. O is the most widely distributed element, present uniformly in all three layers (top, middle, and bottom). This indicates that the high O content in the intermediate layer of MXene's surface functional groups mainly originates from the abundant -OH and -O end groups on the MXene surface. This is a typical characteristic of MXene and also explains its hydrophilicity and dispersibility. The O elements in the upper and lower planar layers mainly originate from waterborne polyurethane (WPU) and / or polyacrylic acid (PA), which contain a large number of oxygen-containing groups such as C=O, COC, and -OH.

[0051] Figure 8 Digital photographs of structural color fabrics of different colors prepared by coating P(St-MMA-AA) microspheres of different sizes onto a black substrate fabric using the rod coating method show that the fabrics exhibit bright colors. This is attributed to the fact that the black substrate fabric can absorb excess scattered light from the photonic crystal, resulting in higher color saturation of the fabric.

[0052] Figure 9 The reflectance spectra of structurally colored fabrics of different colors were prepared by rod coating on black cotton fabric after LPCs were fabricated from P(St-MMA-AA) microspheres of different particle sizes. The graphs show that as the microsphere particle size decreases, the wavelength of the structurally colored fabric undergoes a blue shift, indicating that the color of the fabric can be achieved by adjusting the microsphere particle size.

[0053] The structured fabric prepared with microspheres of 286 nm in diameter is red; the structured fabric prepared with microspheres of 262 nm in diameter is pink; the structured fabric prepared with microspheres of 236 nm in diameter is yellow; the structured fabric prepared with microspheres of 230 nm in diameter is yellowish-green; the structured fabric prepared with microspheres of 215 nm in diameter is cyan; and the structured fabric prepared with microspheres of 203 nm in diameter is blue. According to the above pattern, the color of the structured fabric becomes bluer as the microsphere particle size decreases.

[0054] Fabric electromagnetic shielding performance test: Figure 10 The electromagnetic shielding effectiveness (EMI SET) of black substrate fabric treated with different immersion cycles was demonstrated in the 8–12 GHz frequency range. The SET value generally increased with increasing immersion cycles, indicating a gradual improvement in the fabric's electromagnetic shielding performance. When the number of immersion cycles reached 20, the highest SET value was approximately 29 dB, demonstrating excellent shielding performance; however, excessive immersion significantly increased the fabric thickness, which is detrimental to the subsequent assembly of photonic crystal structures. Considering the balance between performance and process, 12 immersion cycles were ultimately selected, at which point the average SET was approximately 27 dB, meeting the commercially required standard of above 20 dB across the entire X-band.

[0055] The results confirm that the fabric treated with a mixed solution of MXene and single-walled carbon nanotubes (SWCNTs) possesses excellent conductivity and electromagnetic shielding capabilities. The performance improvement is primarily due to the high conductivity of MXene itself and the continuous conductive network formed by SWCNTs bridging the MXene sheets; these two factors synergistically enhance carrier transport and electromagnetic wave loss capabilities.

[0056] To further analyze the electromagnetic shielding mechanism of the electromagnetic shielding structured fabric, the average values ​​of SER, SEA, and SET were calculated. Figure 11This study demonstrates the changing trends of the electromagnetic shielding effectiveness (ESP) and its components of the structured fabric with increasing immersion counts. Overall, the total shielding effectiveness (SET) shows a significant upward trend, rapidly increasing from approximately 19 dB to approximately 29 dB, clearly indicating the effective improvement in final shielding performance due to the increased number of immersions. Sub-component analysis of reflection loss (SER) and absorption loss (SEA) further reveals the underlying physical mechanisms. Reflection loss (SER) increases relatively slowly throughout the immersion process, gradually increasing from approximately 6 dB to approximately 9 dB, an increase of only 3 dB. This reflects that the impedance matching optimization of the material surface tends to stabilize after multiple immersions. The limited increase in SER in this experiment indicates that after the initial few immersions, the surface properties of the material (such as the formation of the conductive network) have reached a relatively stable state, and the initial reflection capability of electromagnetic waves no longer constitutes a major performance bottleneck. In stark contrast to SER, absorption loss (SEA) exhibits strong growth momentum, jumping from approximately 15 dB initially to approximately 23 dB ultimately, an increase of 8 dB, and is the main contributor to the improvement in total shielding effectiveness (SET). This changing trend profoundly reveals that the shielding structure in this study is undergoing a shift from "reflection-dominated" to "absorption-dominated" mechanisms. The mechanism of absorption loss stems from the effective dissipation of energy through various means after electromagnetic waves enter the material, primarily including conductive loss (eddy current effect), dielectric loss (dipole polarization relaxation), and magnetic loss (hysteresis loss, natural resonance). The dramatic increase in SEA can be attributed to two aspects: First, process iterations (such as layer-by-layer deposition and directional arrangement of fillers) significantly increased the effective thickness of the material or constructed multi-layer structures, thereby lengthening the transmission path of electromagnetic waves within the material and enhancing the opportunity for energy absorption. Second, and more importantly, process optimization (such as uniform dispersion of conductive fillers and directional arrangement of magnetic particles) effectively improved the overall electrical conductivity (σ) and magnetic permeability (μ) of the composite material. Both work together on the absorption term, resulting in a qualitative leap in its ability to "capture" and "digest" electromagnetic waves. Within the experimental frequency band, this enhanced loss effect brought about by internal structural optimization far exceeds the improvement in surface reflection capability.

[0057] Throughout the experiment, the total shielding effectiveness (SET) consistently matched the sum of reflection loss and absorption loss (SET≈SER+SEA), indicating that the loss (SEM) from multiple internal reflections is negligible under the frequency and material thickness conditions studied in this study. This phenomenon also aligns with classical theory: when the absorption loss (SEA) is sufficiently large (typically greater than 10 dB), the small amount of energy entering the material decays rapidly during reflections between internal interfaces, and its contribution to the total shielding effectiveness can be disregarded. Therefore, the total shielding effectiveness in this work is primarily determined by the initial reflection and single-penetration absorption. In summary, the electromagnetic shielding mechanism of this material can be clearly described as follows: in the initial stage of process optimization, reflection and absorption mechanisms work together; as the number of immersion cycles increases, the absorption mechanism gradually becomes dominant. The significant improvement in total shielding effectiveness is mainly attributed to the enhanced electromagnetic wave absorption capacity within the material, stemming from the synergistic enhancement of structural thickness, conductivity, and permeability resulting from process optimization.

[0058] Photothermal properties of fabrics: The surface temperature of the structured colored fabric was tested using an infrared thermal imager to evaluate its photothermal conversion properties. Figure 12 Figure a shows the temperature and time variations of electromagnetically shielded structured colored fabric and raw cotton fabric under xenon lamp illumination at different intensities (250, 500, 700, and 1000 W / cm²). The figure shows that their surface temperatures reach saturation values, which may be attributed to the staggered conductive network of MXene and SWCNTs, providing an efficient transport path by rapidly transferring high-temperature electrons generated by light absorption and localized heat. Furthermore, it can uniformly distribute heat throughout the fabric, thus collectively improving photothermal conversion efficiency. With increasing light intensity, their saturation temperatures show a clear upward trend. When the light intensity is 250, 500, 700, and 1000 W / cm², the saturation temperatures of the electromagnetically shielded structured colored fabric surface are 37.4 ℃, 56.4 ℃, 68.5 ℃, and 86.3 ℃, respectively, and the surface temperature of the structured colored fabric is consistently higher than that of the raw cotton fabric (see Figure a). Figure 12 (b and 12c). Xenon lamps simulated light intensity under different weather conditions, demonstrating that the heating temperature of the structured fabric can meet the needs of outdoor solar heating under various weather conditions. Figure 12 d represents the reflectance spectrum before and after irradiation with different light intensities. The fact that the reflectance spectrum curves before and after irradiation are almost identical reflects the color stability of the structured fabric. To analyze the repeatability and reliability of the photothermal properties of the structured fabric, repeated solar heating and cooling tests (700 W / cm²) were conducted for a total of 5 cycles. Figure 12 The figure shows that the temperature-time profiles of all cycles are nearly consistent during heating and cooling, confirming its photothermal stability. Figure 12The f-value shows an almost consistent reflectance curve during five cycles of heating and cooling at 700 W / cm², confirming its color stability.

[0059] Figure 12 Photothermal properties of structured fabrics: (a) Irradiation time curves and fabric temperature curves of structured fabrics and raw cotton fabrics at light intensities of 250, 500, 700, and 1000 W / m²; (b) Saturation temperatures of structured fabrics and cotton fabrics under different light intensities; (c) Infrared images of the saturation temperatures of structured fabrics and raw cotton fabrics under different light intensities; (d) Reflectance spectra of structured fabrics before and after different light intensities; (e) Temperature change curves of structured fabrics after five cycles at a light intensity of 700 W / m²; (f) Reflectance spectra of structured fabrics before and after five cycles.

[0060] The electrical heating properties of the fabric: To demonstrate that the structural dyed fabric is conductive, conductive copper tape was attached to both ends and a power source was connected. Figure 13 A shows a comparison of the fabric under two states: energized (on) and de-energized (off), briefly illustrating the electrical conductivity of structurally colored fabrics; Joule heating test ( Figure 13 b and Figure 13 c) The experiment was conducted on structured fabrics with different constant DC voltages. Higher voltages resulted in faster electrothermal response and higher saturation temperatures, with the composite fabric benefiting from its efficient three-dimensional highly conductive network. The equilibrium temperatures of the structured fabrics at different voltages (3, 5, 7, 9 V) were 21.8 ℃, 29.8 ℃, 50.9 ℃, and 78.4 ℃, respectively. The equilibrium temperature increased with increasing load voltage, and the temperature reached equilibrium rapidly within 60 seconds. This indicates that the structured fabric can function as a heater, providing rapid heating even in extreme environments (frost, freezing, rain, and snow). Figure 13 Figure d shows the reflectance spectra before and after heating at different voltages. It can be seen that the reflectance remains consistent, indicating that the fabric color does not change after heating at different voltages, demonstrating excellent color stability. To analyze the repeatability and reliability of the Joule heating properties of the structured color fabric, repeated constant voltage heating and cooling tests (7 V) were conducted. Figure 13 The image shows nearly identical temperature-time curves for all cycles during heating and cooling, confirming its Joule thermal stability. To analyze its color stability, reflectance tests were performed on the fabric before and after heating and cooling cycles at constant voltage. Figure 13 The f-value shows a nearly consistent reflectance curve throughout five cycles of heating and cooling, confirming its color stability.

[0061] Figure 13The heating performance of structured fabrics under electric heating: (a) Conductivity of structured fabrics; (b) Infrared images of saturation temperature at different voltages; (c) Time curves and fabric temperature curves of structured fabrics at 3, 5, 7, and 9 V voltages; (d) Reflectance spectra of structured fabrics before and after different voltages; (e) Temperature change curves of structured fabrics after five cycles of heating at 7 V; (f) Reflectance spectra of structured fabrics before and after five cycles.

[0062] Fabric strength To demonstrate the enhancement of fabric fastness by PA, the following fastness tests were conducted. After washing the structured fabric at 500 rpm for 1 hour, the color remained almost unchanged before and after washing. The almost consistent reflectance further illustrates the fabric's excellent wash resistance. After 30 minutes of ultrasonic treatment, the color of the structured fabric remained almost unchanged before and after washing, and the almost consistent reflectance also demonstrates its excellent ultrasonic resistance. A piece of cotton fabric was attached to the bottom of a 200-gram weight to increase friction and slid back and forth 200 times from right to left on the fabric surface. It was observed that the color of the fabric remained almost unchanged before and after washing, and the reflectance spectrum was almost consistent, indicating that the structured fabric has excellent rubbing fastness. After 20 repeated bending cycles, the color of the structured fabric remained almost unchanged before and after washing, with no obvious creases. The almost consistent reflectance also demonstrates the excellent flexibility and bending resistance of the structured fabric. This indicates that the fastness of the structured fabric is improved after impregnation with PA, making it suitable for everyday applications.

[0063] (a) Photographs and reflectance spectra of the object before and after 1 hour of washing; (b) Photographs and reflectance spectra of the object before and after 30 minutes of sonication; (c) Photographs and reflectance spectra of the object before and after 100 rubs with 200 g; (d) Photographs and reflectance spectra of the object before and after 20 bends.

[0064] The various embodiments of this disclosure have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or technical improvements to the embodiments in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing an electromagnetic shielding structural colored fabric, characterized in that, The method includes: S1, prepare P microsphere emulsion, which is St-MMA-AA microsphere emulsion; S2, preparation of liquid photonic crystals; S3, prepare Mxene aqueous dispersion; S4, P emulsion synthesis, P emulsion is MMA-BA emulsion; S5, Prepare electromagnetic shielding structural colored fabric.

2. The method for preparing an electromagnetic shielding structural colored fabric according to claim 1, characterized in that, The preparation of the P microsphere emulsion includes: At room temperature, add 2 g of ammonium bicarbonate and 440 mL of deionized water to a three-necked flask and stir until completely dissolved; Measure 40 mL to 70 mL of 2 g / L SDBS aqueous solution into the three-necked flask above using a graduated cylinder. Weigh 76 g of styrene (St), 4 g of methyl methacrylate (MMA), and 4 g of acrylic acid (AA) and add them into the flask. After the temperature is raised to 80 ℃, 1.432 g of ammonium persulfate (APS) dissolved in 40 mL of deionized water is added at once. After reacting for 6 h, a milky white liquid is obtained. The liquid is then filtered through a 200-mesh nylon filter and stored.

3. The method for preparing an electromagnetic shielding structural colored fabric according to claim 2, characterized in that, The preparation of liquid photonic crystals includes: The prepared P microsphere emulsion was centrifuged in a centrifuge tube to remove water from the system and obtain microsphere precipitate. Then, freeze-drying was used to remove all the water from the microsphere precipitate. After grinding the freeze-dried microspheres into powder using a mortar and pestle, add P microsphere powder, deionized water and carbon black in a volume ratio of 1:1:0.5% to the sample vial.

4. The method for preparing an electromagnetic shielding structural colored fabric according to claim 1, characterized in that, Preparation of Mxene aqueous dispersion includes: Take 15 mL of concentrated hydrochloric acid into a polytetrafluoroethylene reaction vessel, add 1.6 g of lithium fluoride, stir magnetically, and then add 5 mL of deionized water and stir. Transfer the container to a water bath at 35°C, slowly add 1 g of Ti3AlC2 powder, and react at a constant temperature for 24 h. First, wash the solution three times with 1 mol / L dilute hydrochloric acid solution by centrifugation, then wash with deionized water and centrifuge 15-18 times to obtain an MXene aqueous dispersion.

5. The method for preparing an electromagnetic shielding structural colored fabric according to claim 1, characterized in that, P-emulsion synthesis includes: First, 0.6 g of sodium dodecyl sulfate (SDS) and 80 mL of water were stirred at 350 rpm and heated to 80 °C. Then, methyl methacrylate (MAA) and butyl acrylate (BA) were added for emulsification. After emulsification for 30 min, 0.1 g of potassium persulfate (KPS) dissolved in 10 mL of deionized water was added at once. The mixture was then reacted for 5 h to obtain emulsion P.

6. The method for preparing an electromagnetic shielding structural colored fabric according to claim 1, characterized in that, Preparation of electromagnetic shielding structural colored fabric, including: 0.2 g of single-walled carbon nanotubes and 1 g of SDS surfactant were dispersed in 40 mL of deionized water and then ultrasonically bathed in ice water for 60 minutes to obtain a uniform dispersion of single-walled carbon nanotubes. MXene and single-walled carbon nanotubes were mixed at a mass ratio of 3:

1. The mixture was sonicated in an ice bath and then magnetically stirred for 120 min. The cotton fabric was immersed in the prepared mixed solution 12 times to obtain a conductive fabric with a black base. The black fabric was then immersed in water-based polyurethane (WPU) and dried. After being coated with liquid photonic crystal, it was sintered at 90 °C for 10 min and finally immersed in a P solution with a solid content of 5% and dried.