Air-permeable antibacterial nylon fabric and preparation method thereof
By employing steps such as mesoporous ε-polylysine core slow release, skin-contact and back-contact modification, plasma activation, and composite metal growth, the problems of insufficient breathability and short antibacterial effect of nylon fabrics have been solved, resulting in a highly effective antibacterial and breathable nylon fabric suitable for high-end functional antibacterial fabrics.
Patent Information
- Application Number
- CN202611482691.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing nylon fabrics have shortcomings in terms of antibacterial properties, such as insufficient breathability, uneven aggregation of antibacterial components, and short antibacterial duration, making it difficult to meet the high-quality and high-comfort requirements of high-end functional antibacterial nylon fabrics.
The process involves a series of steps, including mesoporous ε-polylysine core slow release, skin-adhesive and back-skin-adhesive side modification, plasma activation, and composite metal growth. ε-polylysine is encapsulated in mesoporous SBA-15 membranes, silane modification addresses thermal failure and compatibility issues, PET masking template is modified to maintain breathability, plasma activation generates ZIF-8/Cu-Zn composite crystals, and N-haloamines regenerate antibacterial properties.
This invention achieves skin-friendly and breathable nylon fabric with high antibacterial efficiency and long-lasting effect. The antibacterial performance remains highly effective even after multiple washes, and the breathability is not affected, reducing the risk of skin irritation.
Smart Images

Figure CN123153284A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nylon fabric technology, specifically to a breathable and antibacterial nylon fabric and its preparation method. Background Technology
[0002] Nylon fiber boasts advantages such as high strength, good abrasion resistance, soft hand feel, and ease of weaving, making it widely used in intimate apparel, functional clothing, and medical protective equipment. To meet the needs of wearable hygiene and antibacterial protection, the industry generally conducts antibacterial modification treatments on nylon fabrics. Currently, the mainstream modification processes are mainly divided into three conventional technical routes: solution blending modification, coating and padding modification, and surface grafting modification. Solution blending modification involves melt-blending antibacterial powder with nylon chips, allowing the antibacterial components to be uniformly fixed inside the fiber matrix. Compared to surface padding, this significantly improves antibacterial wash resistance and durability, preventing the rapid shedding and failure of surface antibacterial components. However, in this technology, the antibacterial components are entirely encapsulated inside the fiber, resulting in insufficient effective antibacterial loading on the fabric surface, leading to weak initial antibacterial efficiency and delayed bacteriostatic effect. Furthermore, conventional inorganic antibacterial powders are prone to agglomeration during melt spinning, resulting in uneven distribution of antibacterial sites on the fabric surface, creating localized antibacterial blind spots, and poor overall antibacterial consistency and stability of the fabric. Padding modification is the most commonly used finishing technology in the industry. It mainly involves attaching functional components such as quaternary ammonium salts and silver-zinc inorganic antibacterial agents to the surface of nylon fabrics through padding or coating. This process is simple to operate, has low modification costs, and a fast initial antibacterial rate. However, the antibacterial components are fixed to the fabric surface only through physical adsorption and resin encapsulation, resulting in weak interfacial adhesion and extremely poor washing stability. After 10-15 conventional washes, a large number of surface antibacterial particles fall off, the number of active sites is greatly reduced, and the antibacterial performance rapidly declines or even completely fails. At the same time, in order to improve the adhesion of antibacterial components, this process is usually combined with resin film formation and curing, which easily blocks the pores of the fabric yarn, inevitably sacrificing the fabric's breathability and moisture permeability, resulting in obvious performance antagonism. Surface grafting modification grafts antibacterial monomers onto the surface of nylon fibers through a chemical reaction. Compared with physical attachment methods, the antibacterial components have a higher bonding strength and better washing stability than ordinary padding processes. However, traditional surface grafting modification can only construct a single antibacterial functional layer on the fabric surface. This results in a limited functional structure without internal antibacterial reservoir replenishment, making it a limited surface modification system. After repeated washing and friction, and long-term wear, the grafted antibacterial functional groups and active sites gradually diminish and cannot be replenished independently, leading to a continuous decline in antibacterial performance and making it difficult to achieve long-lasting and stable antibacterial effects. Furthermore, traditional full-area surface grafting modifies the overall pore structure of the fabric, easily causing pore blockage. This also presents the technical drawback of a trade-off between antibacterial performance and breathability. Moreover, full-area modification can easily lead to direct contact between antibacterial components and the skin, posing a risk of wear-related irritation.
[0003] Patent CN115262213B discloses an antibacterial nylon fabric and its preparation method. The main method involves grafting an antibacterial copper complex onto the nylon fabric using the crosslinking agent epichlorohydrin. After 10 washes, the nylon fabric retains a strong antibacterial effect. Patent CN114318733B discloses a method for preparing an antibacterial nylon fabric. The fabric composition mainly includes 100 parts nylon chips, 7 parts antibacterial nylon masterbatch, 35 parts polyvinylpyrrolidone, 3 parts glyceryl tristearate, 1.5 parts polyvinyl alcohol, and 0.8 parts fatty alcohol polyoxyethylene ether. The fabric is prepared through melt spinning, weaving, and dyeing finishing processes.
[0004] In summary, existing single modification technologies all have inherent limitations and cannot effectively achieve the functions of high breathability, long-lasting antibacterial effect, and low skin irritation of nylon fabrics at present. They are also difficult to meet the high quality and high comfort requirements of high-end functional antibacterial nylon fabrics. Therefore, it is of practical significance to develop a new antibacterial modification technology for nylon fabrics. Summary of the Invention
[0005] The purpose of this invention is to address the shortcomings of existing nylon fabrics, such as insufficient breathability, uneven aggregation of antibacterial components, and short antibacterial duration, by providing a novel method for preparing breathable and antibacterial nylon fabric. Through the synergistic effects of mesoporous ε-polylysine core slow release, skin-contact and back-contact side partitioning modification, plasma activation, and composite metal growth, a nylon fabric with good skin-friendliness and breathability, high antibacterial efficiency, and long duration of antibacterial effect is obtained.
[0006] To achieve the above objectives, this application adopts the following technical solution: A method for preparing a breathable and antibacterial nylon fabric includes the following steps: S1: The mesoporous SBA-15 is immersed in an aqueous solution of ε-polylysine, wherein the pore size D of the SBA-15 and the molecular weight M of ε-polylysine satisfy D ≥ 0.001 × M. 0.5Subsequently, a silane coupling agent is added, and the mixture is modified by heating and reflux with ethanol to obtain a modified powder. In existing technologies, ε-polylysine is mostly used in medical low-temperature antibacterial materials and is conventionally applied in hydrogels and electrospinning low-temperature systems. When it is used in the preparation of nylon fabric in this invention, if added directly, it cannot withstand the high temperature of nylon melt spinning above 270 ℃ and is prone to thermal decomposition and failure. Therefore, in this invention, mesoporous SBA-15 is innovatively used in this step, and the relationship between the pore size D of SBA-15 and the molecular weight M of ε-polylysine is strictly controlled. The pore confinement and encapsulation effect of mesoporous SBA-15 is used to form a molecular-level thermal protective shell. At the same time, the matching relationship between pore size and molecular weight M is clearly defined to ensure that the ε-PL molecules are just confined in the pores but still have enough space to maintain the antibacterial active conformation. By forming a stable antibacterial slow-release channel inside the fiber, it can be used to replenish the loss of surface antibacterial properties over a long period of time. At the same time, the silane modification solves the problems of poor compatibility between inorganic powder and nylon melt, agglomeration and fiber breakage. S2: The modified powder obtained in step S1 is mixed with nylon chips and melt-granulated using a twin-screw extruder to obtain antibacterial masterbatch; the antibacterial masterbatch is blended with nylon chips at a ratio of 2-5:100, and then melt-spun and woven at a gradient temperature to obtain antibacterial nylon fabric; by uniformly dispersing the antibacterial components in a molecular state inside the nylon matrix, stable antibacterial properties are given to the nylon material, while avoiding the phenomenon of particle agglomeration and clogging of the spinneret holes caused by conventional introduction of powder fillers, thus solving the problems of easy agglomeration of powder antibacterial agents in the nylon matrix, uneven distribution of antibacterial sites, and local lack of antibacterial effect; S3: The PET masking template with orthogonal grid cutouts is tightly attached to the skin-contact side of the antibacterial nylon fabric obtained in step S1, and sealed under pressure at room temperature to ensure complete adhesion to the skin-contact side. In the prior art, PET masking templates are often used for one-way moisture wicking and liquid drainage in medical fabrics. This invention is the first to use a single-sided masking structure for antibacterial sites on nylon fabrics, achieving zoned isolation, breathability retention, and reduced irritation. This breaks the traditional concept of "uniform antibacterial modification on both sides" in the textile industry and overcomes the defects of conventional double-sided modification, such as blocked inner pores and significantly reduced breathability. The skin-contact side retains the original structure and fully preserves the breathable pores, while the back side exposes the grid functional area, realizing structured functional zoning.
[0007] S4: The exposed area of the back-side mesh of the fabric shielded in step S3 is subjected to oxygen plasma activation treatment; after treatment, it is immersed in zinc nitrate aqueous solution, and then transferred to 2-methylimidazole solution for in-situ growth to obtain discretely distributed ZIF-8 basic crystal sites; then it is placed in a copper-zinc mixed salt solution to obtain a fabric containing ZIF-8 / Cu-Zn composite crystal material; through plasma activation treatment, sufficient -COOH active anchoring points are generated on the fiber surface to provide a flat and uniform functional substrate for subsequent metal composite crystal loading, avoiding the stacking and agglomeration of multiple functional layers; by obtaining discretely distributed ZIF-8 basic crystal sites through in-situ growth, and then composited with Cu-Zn, while maintaining the stability of the crystal skeleton, temperature and humidity responsive active sites are introduced to achieve controllable antibacterial properties.
[0008] S5: Immerse the fabric containing ZIF-8 / Cu-Zn composite crystal material from step S4 into an aqueous solution of 5,5-dimethylhydantoin precursor and adjust the pH of the solution to 7-8; after immersion, removal, and baking; then place it in a sodium hypochlorite aqueous solution for room temperature soaking, washing, and drying to obtain a breathable and antibacterial nylon fabric.
[0009] Furthermore, in step S1, the SBA-15 has a pore size of 4-6 nm and a specific surface area ≥750 m² / g; the solid-liquid ratio of SBA-15 and ε-polylysine aqueous solution is 1:10-15; the mass fraction of ε-polylysine aqueous solution is 0.8-1.2 wt%; impregnation is carried out at room temperature for 6-8 h; the silane coupling agent is KH-550 with a mass fraction of 1-3 wt%; and the reaction is carried out under reflux at 90-100℃ for 5-7 h.
[0010] Furthermore, in step S2, the mixing mass ratio of modified powder and nylon chips is 1:1.5-2.5; the temperatures of each section of the screw in the twin-screw extruder for melt granulation are 240℃, 250℃, 255℃, 260℃, and 265℃, respectively; the spinning box temperature is 270℃; the spinneret temperature is 275-280℃; and the residence time of the melt in the region above 270℃ is controlled to be ≤3min; the side blowing speed is 0.5-0.6m / s; the total draw ratio is 3.5-4.5; the screw speed is 50-55 r / min; and a weft-knitted nylon fabric with an areal density of 180-220g / m² is obtained.
[0011] Furthermore, in step S3, the grid unit size of the PET masking template is 2 mm × 2 mm, the grid border width is 0.2 mm, and the pressure is 0.3-0.5 MPa.
[0012] Furthermore, a water-soluble polyvinyl alcohol (PVA) protective coating is printed on the PET masking template near the skin-contact side of the fabric, and then dried and cured at 80°C for 2 hours. After plasma activation and ZIF-8 / Cu-Zn composite crystal material are completed, the PVA masking protective layer can be dissolved and removed by washing with 80°C hot water for 30 minutes to 1 hour.
[0013] Furthermore, in step S4, the vacuum degree of oxygen plasma activation treatment is 13-18 Pa, the power is 130-160 W, and the treatment time is 40-50 s; the concentration of zinc nitrate aqueous solution is 0.1-0.3 mol / L, and the immersion time is 40-50 min; the concentration of 2-methylimidazole solution is 0.2-0.4 mol / L, and the reaction time is 2-3 h at room temperature; the copper-zinc mixed salt solution has a copper-zinc molar ratio of 1:3-5 and a total metal ion concentration of 0.1-0.2 mol / L, and the reaction time is 2.5-3.5 h at a temperature of 50-60℃. A discrete point-like in-situ growth process is adopted, and strict temperature and concentration control ensures that the crystals are discretely distributed, unconnected, and without a continuous film. The skin-contact side is a hydrophobic and highly permeable area, while the back side is a hydrophilic and antibacterial functional area. Human sweat is mainly weakly acidic (pH≈4.5~6.0) and contains lactic acid and sodium. + K + Amino acids, etc.; among them, lactic acid can undergo weak coordination with metal sites on the crystal surface, anchoring outward-flipping imidazole ligands, preventing the ligands from rapidly rebounding, and stably maintaining the hydrophilic configuration with the polar groups facing outwards; Na + K + Metal ions can reduce the surface tension of water, promote the spread of sweat on rough crystal interfaces, increase the solid-liquid contact area, and further assist ligand orientation reconstruction; a weakly acidic environment can moderately weaken the metal-imidazolium coordination effect on the crystal surface, making it easier for ligands to flip.
[0014] In a dry state, the crystal surface is enriched with hydrophobic 2-methylimidazolium organic ligands. Mass transfer channels are blocked by the hydrophobic interface, metal ions are locked within the coordination framework, and reactive oxygen species (ROS) cannot be generated, keeping the antibacterial components in a dormant state. When slightly wetted by sweat, water molecules contact the surface of the ZIF-8 / Cu-Zn composite crystal material, driving the imidazolium ligands on the crystal surface to undergo reversible orientation reconstruction. The polar groups turn outward, and the interface changes from hydrophobic to hydrophilic. This excites the Cu-Zn bimetallic sites to generate reactive oxygen species (ROS), which work together with trace metal ions to achieve sterilization. After the sweat evaporates, the orientation of the surface imidazolium ligands spontaneously recovers, the interface changes from hydrophilic to hydrophobic, the mass transfer channels are blocked again, the generation of reactive oxygen species stops, and the crystal returns to a dormant state.
[0015] Furthermore, the ZIF-8 / Cu-Zn composite crystal material has a single crystal point diameter of 8-12μm, a point spacing of 30-50μm, and a functional area coverage of 18-22%, maximizing the preservation of the fabric's breathable pores.
[0016] Further, the 5,5-dimethylhydantoin precursor aqueous solution described in step S5, with a mass fraction of 3-5 wt%, is removed after two dips and two nips, and then baked at 115-125℃ for 3-6 min; subsequently, it is immersed in a 0.1-0.3 wt% sodium hypochlorite aqueous solution at room temperature for 5-15 min. (Traditional N) The common baking temperature for halogenated amine grafting is 140°C. At 160℃, nylon fibers are easily hydrolyzed, yellowed, and their strength decreases; this invention selects 115℃. At 120 ℃, stable grafting of hyaluronic acid monomers and nylon fiber surface groups can be achieved while minimizing heat damage. When the surface antibacterial components are irreversibly lost after multiple washes, the antibacterial properties can be regenerated and repaired through household chlorine-containing washing and care, thus improving the long-lasting antibacterial effect.
[0017] The breathable and antibacterial nylon fabric prepared by the above method.
[0018] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention follows a progressive and synergistic process of mesoporous ε-polylysine core slow release, skin-contact and back-contact modification, plasma activation, and composite metal growth. The core solves the long-term gradient antibacterial replenishment, the partition solves the air permeability antagonism and realizes directional moisture collection and energy enhancement, the dot-shaped composite crystal realizes controllable antibacterial and provides a high specific surface area grafting substrate; N-haloamine realizes the regeneration of antibacterial performance. The front and back depend on each other, layer by layer, and mutually support each other, finally obtaining a nylon fabric with excellent antibacterial performance and good air permeability.
[0019] (2) This invention employs mesoporous confinement modification and silane coupling modification, simultaneously solving the two major problems of thermal failure and compatibility. This also provides a necessary prerequisite for subsequent stable melt spinning, uniform dispersion of antibacterial components, and long-lasting sustained-release antibacterial properties of the fabric. It uses a PET mesh template combined with a single-sided masking process with a PVA water-soluble protective layer, fully preserving the original breathable pores and skin-friendly characteristics of the fabric's skin-contact side, while only opening the mesh functional modification area on the back side. This avoids the defects of poor breathability and poor skin-friendliness inherent in traditional modifications, precisely defining the subsequent functional modification area, and providing a structural basis for plasma activation and crystal point-to-point discrete growth. This lays the groundwork for the preparation of highly breathable, low-irritation, structured intelligent antibacterial fabrics. It utilizes a previously constructed dual-layer system of ε-polylysine slow-release antibacterial within the fiber and ZIF-8 / Cu-Zn responsive antibacterial on the skin-back side. A low-temperature baking process is employed to complete the grafting modification of the hydantoin precursor, avoiding problems such as nylon fiber damage, yellowing, and strength reduction caused by traditional high-temperature baking. Its surface-renewable N-haloamine antibacterial component compensates for the surface antibacterial loss, forming a three-layer composite antibacterial system with the internal slow-release and middle-layer intelligent responsive antibacterial structure. Furthermore, the antibacterial performance can be regenerated and repaired through chlorine-containing washing and conditioning.
[0020] (3) The antibacterial nylon fabric prepared by the present invention has an initial antibacterial rate of over 97% against Escherichia coli. After 30 washes, it still exhibits strong antibacterial properties against Escherichia coli, with an antibacterial rate of over 96%. The antibacterial nylon fabric has an initial antibacterial rate of over 98% against Staphylococcus aureus. After 30 washes, it still exhibits strong antibacterial properties against Staphylococcus aureus, with an antibacterial rate of over 96%. Attached image description: Figure 1 Schematic diagram of the process of bonding antibacterial nylon fabric with PET orthogonal grid template. Detailed Implementation
[0021] The present invention will be further described below with reference to the following embodiments. These embodiments are for illustrative purposes only and are not intended to limit the present invention.
[0022] Example 1 A method for preparing a breathable and antibacterial nylon fabric includes the following steps: S1: Select SBA-15 with a pore size of 4-6 nm and a specific surface area ≥750 m² / g; place the mesoporous SBA-15 in a 0.8 wt% ε-polylysine aqueous solution at a solid-liquid ratio of 1:10 and immerse it at room temperature for 6 hours. The pore size D of the SBA-15 and the molecular weight M of the ε-polylysine satisfy D≥0.001×M 0.5 Subsequently, 1 wt% KH-550 silane coupling agent was added, and the mixture was refluxed with ethanol at 90°C for 5 hours to obtain the modified powder. S2: The modified powder obtained in step S1 and nylon chips are mixed at a mass ratio of 1:1.5 and then melt-granulated using a twin-screw extruder to obtain antibacterial masterbatch. The temperatures of each section of the screw in the twin-screw extruder during melt granulation are 240℃, 250℃, 255℃, 260℃, and 265℃, respectively; the spinning box temperature is 270℃; and the spinneret temperature is 275℃. The residence time of the melt in the region above 270℃ is controlled to be ≤3min. The side blowing speed is 0.5m / s, the total draw ratio is 3.5, and the screw speed is 50 r / min. The antibacterial masterbatch is blended with nylon chips at a ratio of 2:100, and then melt-spun and woven using gradient heating to obtain an antibacterial nylon fabric with an areal density of 180g / m². S3: As Figure 1 As shown, the grid unit size of the PET masking template with orthogonal mesh cutout is 2 mm × 2 mm, and the grid border width is 0.2 mm; the PET template is tightly attached to the skin-contact side of the antibacterial nylon fabric obtained in step S1, and sealed under pressure at room temperature with a pressure of 0.3 MPa to ensure that the skin-contact side is completely tight; S4: The exposed area of the back-side mesh of the fabric shielded in step S3 is subjected to oxygen plasma activation treatment at a vacuum of 13 Pa, a power of 130 W, and a treatment time of 40 s. After treatment, it is immersed in a 0.1 mol / L zinc nitrate aqueous solution for 40 min, and then transferred to a 0.2 mol / L 2-methylimidazole solution for in-situ growth at room temperature for 2 h to obtain discretely distributed ZIF-8 basic crystal sites. Then, it is placed in a copper-zinc mixed salt solution with a copper-zinc molar ratio of 1:3 and a total metal ion concentration of 0.1 mol / L, and composite growth is carried out at 50℃ for 2.5 h to obtain a fabric containing ZIF-8 / Cu-Zn composite crystal material. S5: The fabric containing ZIF-8 / Cu-Zn composite crystal material in step S4 is immersed in a 3 wt% aqueous solution of 5,5-dimethylhydantoin precursor for 1 hour, and the pH of the solution is adjusted to 7-8. After two dips and two nips, it is taken out and baked at 115℃ for 3 minutes. Then it is placed in a 0.1 wt% sodium hypochlorite aqueous solution at room temperature for 5 minutes, washed and dried to obtain a breathable antibacterial nylon fabric.
[0023] Example 2 A method for preparing a breathable and antibacterial nylon fabric includes the following steps: S1: Select SBA-15 with a pore size of 4-6 nm and a specific surface area ≥750 m² / g; place the mesoporous SBA-15 in a 1.2 wt% ε-polylysine aqueous solution at a solid-liquid ratio of 1:15 and immerse it at room temperature for 8 hours. The pore size D of the SBA-15 and the molecular weight M of the ε-polylysine satisfy D≥0.001×M. 0.5Subsequently, 3 wt% KH-550 silane coupling agent was added, and the mixture was refluxed with ethanol at 100°C for 7 h to obtain the modified powder. S2: The modified powder obtained in step S1 and nylon chips are mixed at a mass ratio of 1:2.5 and then melt-granulated using a twin-screw extruder to obtain antibacterial masterbatch. The temperatures of each section of the screw during the twin-screw extruder melt granulation are 240℃, 250℃, 255℃, 260℃, and 265℃, respectively; the spinning box temperature is 270℃; and the spinneret temperature is 280℃. The residence time of the melt in the region above 270℃ is controlled to be ≤3min. The side-blowing air velocity is 0.6m / s, the total draw ratio is 4.5, and the screw speed is 55 r / min. The antibacterial masterbatch is blended with nylon chips at a ratio of 5:100, and then melt-spun and woven using a gradient heating method to obtain an antibacterial nylon fabric with an areal density of 220g / m². S3: The grid unit size of the PET masking template with orthogonal mesh cutout is 2 mm × 2 mm, and the grid border width is 0.2 mm; the PET template is tightly attached to the skin-contact side of the antibacterial nylon fabric obtained in step S1, and sealed under pressure at room temperature with a pressure of 0.5 MPa to ensure that the skin-contact side is completely tight; S4: The exposed area of the back-side mesh of the fabric shielded in step S3 is subjected to oxygen plasma activation treatment at a vacuum of 18 Pa, a power of 160 W, and a treatment time of 50 s. After treatment, it is immersed in a 0.3 mol / L zinc nitrate aqueous solution for 50 min, and then transferred to a 0.4 mol / L 2-methylimidazole solution for in-situ growth at room temperature for 3 h to obtain discretely distributed ZIF-8 basic crystal sites. Then, it is placed in a copper-zinc mixed salt solution with a copper-zinc molar ratio of 1:5 and a total metal ion concentration of 0.2 mol / L, and composite growth is carried out at 60℃ for 3.5 h to obtain a fabric containing ZIF-8 / Cu-Zn composite crystal material. S5: Immerse the fabric containing ZIF-8 / Cu-Zn composite crystal material from step S4 into a 5wt% aqueous solution of 5,5-dimethylhydantoin precursor for 1 hour, and adjust the pH of the solution to 7-8; after two dips and two nips, remove the fabric and bake it at 125℃ for 6 minutes; then soak it in a 0.3wt% sodium hypochlorite aqueous solution at room temperature for 15 minutes, and after washing and drying, obtain a breathable and antibacterial nylon fabric.
[0024] Example 3 A method for preparing a breathable and antibacterial nylon fabric includes the following steps: S1: Select SBA-15 with a pore size of 4-6 nm and a specific surface area ≥750 m² / g; place the mesoporous SBA-15 in a 1 wt% ε-polylysine aqueous solution at a solid-liquid ratio of 1:13 and immerse it at room temperature for 7 h. The pore size D of the SBA-15 and the molecular weight M of the ε-polylysine satisfy D≥0.001×M 0.5 Subsequently, 2 wt% KH-550 silane coupling agent was added, and the mixture was refluxed with ethanol at 95°C for 6.5 h to obtain the modified powder. S2: The modified powder obtained in step S1 and nylon chips are mixed at a mass ratio of 1:2.2 and then melt-granulated using a twin-screw extruder to obtain antibacterial masterbatch. The temperatures of each section of the screw during the twin-screw extruder melt granulation are 240℃, 250℃, 255℃, 260℃, and 265℃, respectively; the spinning box temperature is 270℃; and the spinneret temperature is 275℃. The residence time of the melt in the region above 270℃ is controlled to be ≤3min. The side-blowing air velocity is 0.6m / s, the total draw ratio is 4.2, and the screw speed is 55 r / min. The antibacterial masterbatch is blended with nylon chips at a ratio of 4.5:100, and then melt-spun and woven using a gradient heating method to obtain an antibacterial nylon fabric with an areal density of 200g / m². S3: The grid unit size of the PET masking template with orthogonal mesh cutout is 2 mm × 2 mm, and the grid border width is 0.2 mm; the PET template is tightly attached to the skin-contact side of the antibacterial nylon fabric obtained in step S1, and sealed under pressure at room temperature with a pressure of 0.45 MPa to ensure that the skin-contact side is completely tight; S4: The exposed area of the back-side mesh of the fabric shielded in step S3 is subjected to oxygen plasma activation treatment at a vacuum degree of 15 Pa, a power of 145 W, and a treatment time of 45 s. After treatment, it is immersed in a 0.2 mol / L zinc nitrate aqueous solution for 45 min, and then transferred to a 0.3 mol / L 2-methylimidazole solution for in-situ growth at room temperature for 2.5 h to obtain discretely distributed ZIF-8 basic crystal sites. Then, it is placed in a copper-zinc mixed salt solution with a copper-zinc molar ratio of 1:4 and a total metal ion concentration of 0.2 mol / L, and composite growth is carried out at a temperature of 55℃ for 3 h to obtain a fabric containing ZIF-8 / Cu-Zn composite crystal material. S5: Immerse the fabric containing ZIF-8 / Cu-Zn composite crystal material from step S4 into a 3.5 wt% aqueous solution of 5,5-dimethylhydantoin precursor for 1 hour, and adjust the pH of the solution to 7-8; after two dips and two nips, remove the fabric and bake it at 120℃ for 4.5 minutes; then soak it in a 0.2 wt% sodium hypochlorite aqueous solution at room temperature for 10 minutes, and after washing and drying, obtain a breathable and antibacterial nylon fabric.
[0025] Example 4 A method for preparing a breathable and antibacterial nylon fabric includes the following steps: S1: Select SBA-15 with a pore size of 4-6 nm and a specific surface area ≥750 m² / g; place the mesoporous SBA-15 in a 1 wt% ε-polylysine aqueous solution at a solid-liquid ratio of 1:12 and immerse it at room temperature for 7.5 h. The pore size D of the SBA-15 and the molecular weight M of the ε-polylysine satisfy D≥0.001×M 0.5 Subsequently, 2 wt% KH-550 silane coupling agent was added, and the mixture was refluxed with ethanol at 95°C for 6.5 h to obtain the modified powder. S2: The modified powder obtained in step S1 and nylon chips are mixed at a mass ratio of 1:2.2 and then melt-granulated using a twin-screw extruder to obtain antibacterial masterbatch. The temperatures of each section of the screw in the twin-screw extruder during melt granulation are 240℃, 250℃, 255℃, 260℃, and 265℃, respectively. The spinning box temperature is 270℃, and the spinneret temperature is 275℃. The residence time of the melt in the area above 270℃ is controlled to be ≤3min. The side blowing speed is 0.55m / s, the total draw ratio is 4, and the screw speed is 50 r / min. The antibacterial masterbatch is blended with nylon chips at a ratio of 3:100, and then melt-spun and woven using gradient heating to obtain an antibacterial nylon fabric with an areal density of 190g / m². S3: The grid unit size of the PET masking template with orthogonal mesh cutouts is 2 mm × 2 mm, and the grid border width is 0.2 mm; the PET template is tightly attached to the skin-contact side of the antibacterial nylon fabric obtained in step S1, and sealed under pressure at room temperature at a pressure of 0.45 MPa to ensure that the skin-contact side is completely tight; a layer of water-soluble polyvinyl alcohol (PVA) protective coating is printed on the PET masking template near the skin-contact side of the fabric, and then dried and cured at a temperature of 80°C; S4: The exposed mesh area on the back side of the fabric shielded in step S3 is subjected to oxygen plasma activation treatment at a vacuum degree of 16 Pa, a power of 150 W, and a treatment time of 45 s. After treatment, it is immersed in a 0.2 mol / L zinc nitrate aqueous solution for 50 min, and then transferred to a 0.3 mol / L 2-methylimidazole solution for in-situ growth at room temperature for 2.5 h to obtain discretely distributed ZIF-8 basic crystal sites. Then, it is placed in a copper-zinc mixed salt solution with a copper-zinc molar ratio of 1:4 and a total metal ion concentration of 0.15 mol / L, and composite growth is carried out at 50℃ for 3 h to obtain ZIF-8 / Cu-Zn composite crystal material. It is washed with 80℃ hot water for 30 min to completely dissolve and remove the PVA shielding protective layer, resulting in a fabric containing ZIF-8 / Cu-Zn composite crystal material. S5: The fabric containing ZIF-8 / Cu-Zn composite crystal material obtained in step S4 is immersed in a 4 wt% aqueous solution of 5,5-dimethylhydantoin precursor for 1 hour, and the pH of the solution is adjusted to 7-8; after two dips and two nips, it is taken out and baked at 120℃ for 5 minutes; then it is placed in a 0.2 wt% sodium hypochlorite aqueous solution at room temperature for 12 minutes, washed and dried to obtain a breathable antibacterial nylon fabric.
[0026] Comparative Example 1 The difference from Example 1 is that SBA-15 protection is not used in step S1, but ε-polylysine is added directly, while other processes and parameters remain unchanged.
[0027] Comparative Example 2 The difference from Example 1 is that the temperature setting of the twin-screw extruder in step S2 is not gradient mode, but is carried out at 265°C, while other processes and parameters remain unchanged.
[0028] Comparative Example 3 The difference from Example 1 is that step S3 is missing, while other processes and parameters remain unchanged.
[0029] Comparative Example 4 The difference from Example 1 is that the in-situ growth in zinc nitrate aqueous solution and 2-methylimidazole solution was not obtained, and discrete ZIF-8 basic crystal sites were not obtained; only Cu-Zn crystal material was available, and other processes and parameters remained unchanged.
[0030] Comparative Example 5 The difference from Example 1 is that Cu-Zn crystal material is missing, and only ZIF-8 basic crystal is available, while other processes and parameters remain unchanged.
[0031] Comparative Example 6 The difference from Example 1 is that it was not soaked in sodium hypochlorite aqueous solution at room temperature, washed and dried, while other processes and parameters remained unchanged.
[0032] The performance indicators of the breathable and antibacterial nylon fabrics prepared in each embodiment and comparative example were tested. Air permeability was tested according to GB / T 5453-2025, and antibacterial performance was tested according to GB / T 20944.3. Simultaneously, antibacterial performance after 50 washes was tested according to GB / T 12490. Specific test results are as follows: Table 1 Results of each test test Breathability (mm / s) Escherichia coli inhibition rate % Staphylococcus aureus inhibition rate % 50 washes to inhibit E. coli % Staphylococcus aureus inhibition rate after 50 water washes % Example 1 97.2 98.3 98.1 96.2 95.7 Example 2 88.4 99.1 98.9 97.6 96.1 Example 3 92.5 98.6 98.4 96.7 96.2 Example 4 99.3 98.4 98.2 96.2 96.8 Comparative Example 1 96.7 87.1 86.4 72 71.4 Comparative Example 2 90 93.5 93.1 81.2 80.7 Comparative Example 3 75.2 97.4 97.1 88.1 87.5 Comparative Example 4 94.1 92.7 92.2 80.4 79.7 Comparative Example 5 95 94.4 94 83.1 82.5 Comparative Example 6 96.8 89.5 89.1 75.2 74.7 Data from Comparative Example 1 and Example 1 show that, due to the lack of protection and dispersion of ε-polylysine by the SBA-15 mesoporous carrier in the process steps, ε-polylysine is easily migrated and lost during subsequent processing and washing. After 50 washes, the antibacterial rates against Escherichia coli and Staphylococcus aureus are only around 70%, indicating poor antibacterial durability. The air permeability is similar to that of Example 1, indicating that the SBA-15 carrier loading did not affect the pore structure of the fabric.
[0033] Data from Comparative Example 2 and Example 1 show that, due to the absence of a gradient heating step, the modified powder is unevenly dispersed in the nylon matrix, and local agglomeration easily blocks the internal micropores, resulting in a significant decrease in air permeability. Due to the uneven dispersion of antibacterial components, the initial antibacterial rate of Escherichia coli and the antibacterial rate of Staphylococcus aureus both decrease significantly after 50 washes.
[0034] Data from Comparative Example 3 and Example 1 show that, due to the absence of PET mesh shielding module technology, a large number of ZIF-8 / Cu-Zn composite crystals were grown on both sides of the fabric. The pores between fibers were filled and blocked by the crystals over a large area, resulting in a significant reduction in air permeability.
[0035] As can be seen from the data of Comparative Example 4 and Example 1, due to the lack of ZIF-8 as an anchoring point, Cu-Zn metal crystals are difficult to firmly adhere to the surface of nylon fibers. The crystals are prone to agglomeration and detachment, resulting in a significant decrease in both the initial antibacterial rate and the antibacterial rate after 50 washes.
[0036] Data from Comparative Example 5 and Example 1 show that, due to the presence of only ZIF-8 and the lack of the synergistic antibacterial effect of Cu-Zn metal ions, the antibacterial activity is limited; this leads to a significant decrease in both the initial antibacterial rate and the antibacterial rate after 50 washes; however, the air permeability remains basically unchanged, and it does not have a significant impact on the pore structure of the fabric.
[0037] Data from Comparative Example 6 and Example 1 show that no N-haloamine active antibacterial sites were formed on the outermost side, resulting in reduced antibacterial performance compared to Example 1. After washing with water, no antibacterial components were replenished, leading to severe loss of antibacterial activity and a significant decrease in antibacterial performance.
[0038] The foregoing description of specific exemplary embodiments of the invention is for illustrative and explanatory purposes. These descriptions are not intended to limit the invention to the precise forms disclosed, and it will be apparent that many changes and variations can be made in accordance with the foregoing teachings. The exemplary embodiments were chosen and described in order to explain the specific principles of the invention and its practical application, thereby enabling those skilled in the art to implement and utilize various different exemplary embodiments of the invention, as well as various different choices and variations. The scope of the invention is intended to be defined by the claims and their equivalents.
Claims
1. A process for the preparation of a breathable antibacterial nylon fabric, characterized in that, Includes the following steps: S1: mesoporous SBA-15 is immersed in an aqueous solution of epsilon-polylysine, the pore size D of the SBA-15 and the molecular weight M of the epsilon-polylysine satisfy D≥0.001×M 0.5 ; then a silane coupling agent is added, and the modified powder is obtained by heating and refluxing in ethanol; S2: Mix the modified powder obtained in step S1 with nylon chips, and melt granulate the mixture using a twin-screw extruder to obtain antibacterial masterbatch; blend the antibacterial masterbatch with nylon chips at a ratio of 2-5:100, and melt spin and weave the mixture to obtain antibacterial nylon fabric. S3: The PET masking template with orthogonal grid cutouts is tightly attached to the skin-contact side of the antibacterial nylon fabric obtained in step S2, and sealed under pressure at room temperature to ensure a tight fit; S4: The exposed area of the back side mesh of the fabric shielded in step S3 is subjected to oxygen plasma activation treatment; after treatment, it is immersed in zinc nitrate aqueous solution, and then transferred to 2-methylimidazole solution for in-situ growth to obtain discrete ZIF-8 basic crystal sites; then it is placed in copper-zinc mixed salt solution to obtain fabric containing ZIF-8 / Cu-Zn composite crystal material. S5: Immerse the fabric containing ZIF-8 / Cu-Zn composite crystal material obtained in step S4 into an aqueous solution of 5,5-dimethylhydantoin precursor and adjust the pH of the solution to 7-8; after immersion, removal and baking; then place it in a sodium hypochlorite aqueous solution for room temperature soaking, washing and drying to obtain a breathable antibacterial nylon fabric.
2. A process for the preparation of an anti-bacterial and breathable polyamide fabric as claimed in claim 1, wherein, In step S1, the SBA-15 has a pore size of 4-6 nm and a specific surface area ≥750 m² / g; the solid-liquid ratio of SBA-15 and ε-polylysine aqueous solution is 1:10-15; the mass fraction of ε-polylysine aqueous solution is 0.8-1.2 wt%; impregnation is carried out at room temperature for 6-8 h; the silane coupling agent is KH-550 with a mass fraction of 1-3 wt%; and the reaction is carried out under reflux at 90-100℃ for 5-7 h.
3. A process for the preparation of an anti-bacterial and breathable polyamide fabric as claimed in claim 1, wherein, In step S2, the mixing mass ratio of modified powder and nylon chips is 1:1.5-2.5; the temperatures of each section of the screw in the twin-screw extruder for melt granulation are 240℃, 250℃, 255℃, 260℃, and 265℃, respectively; the spinning box temperature is 270℃; and the spinneret temperature is 275-280℃. The residence time of the melt in the region above 270℃ is controlled to be ≤3min; the side blowing speed is 0.5-0.6m / s; the total draw ratio is 3.5-4.5; and the screw speed is 50-55 r / min. Weaving yields a weft-knitted nylon fabric with an areal density of 180-220g / m².
4. The process for preparing an anti-bacterial and breathable nylon fabric as claimed in claim 1, wherein, In step S3, the grid unit size of the PET masking template is 2 mm × 2 mm, the grid border width is 0.2 mm, and the pressure is 0.3-0.5 MPa.
5. A process for the preparation of an anti-bacterial and breathable nylon fabric as claimed in claim 4, wherein, A water-soluble polyvinyl alcohol (PVA) protective coating is printed on the PET masking template near the skin-contact side of the fabric, and then dried and cured at 80°C for 2 hours.
6. A process for the preparation of an anti-bacterial and breathable nylon fabric as claimed in claim 1, wherein, In step S4, the vacuum degree of oxygen plasma activation treatment is 13-18 Pa, the power is 130-160 W, and the treatment time is 40-50 s; the concentration of zinc nitrate aqueous solution is 0.1-0.3 mol / L, and the immersion time is 40-50 min; the concentration of 2-methylimidazole solution is 0.2-0.4 mol / L, and the reaction time is 2-3 h at room temperature; the copper-zinc mixed salt solution has a copper-zinc molar ratio of 1:3-5 and a total metal ion concentration of 0.1-0.2 mol / L, and the reaction time is 2.5-3.5 h at a temperature of 50-60℃.
7. The method for preparing a breathable and antibacterial nylon fabric according to claim 1, characterized in that, The ZIF-8 / Cu-Zn composite crystal material has a single crystal point diameter of 8-12 μm, a point spacing of 30-50 μm, and a functional area coverage of 18-22%.
8. The method for preparing a breathable and antibacterial nylon fabric according to claim 1, characterized in that, The 5,5-dimethylhydantoin precursor aqueous solution in step S5 has a mass fraction of 3-5 wt%. After two dips and two nips, it is taken out and baked at 115-125℃ for 3-6 min. Then it is soaked in 0.1-0.3 wt% sodium hypochlorite aqueous solution at room temperature for 5-15 min.
9. The breathable and antibacterial nylon fabric prepared by the preparation method according to any one of claims 1-8.
Citation Information
Patent Citations
A method for preparing antibacterial nylon fabric
CN114318733B