Crystal alumina fiber high temperature insulation sealing gasket infiltrant, preparation method and crystal alumina fiber high temperature insulation sealing gasket
By using a wetting agent composed of coupling agents and film-forming agents, the compression ratio and structural strength of crystalline alumina fiber high-temperature insulating gaskets are improved, solving the problems of brittle fracture, powder shedding, and edge chipping, and achieving higher dimensional stability and service life.
Patent Information
- Application Number
- CN202611561086.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-24
AI Technical Summary
Crystalline alumina fiber high-temperature insulating gaskets are prone to brittle fracture, powdering, and edge chipping under high-temperature conditions. They also have a high compressibility, making it difficult to adapt to local defects at the joint surface, resulting in short service life and poor sealing performance.
An impregnating agent containing coupling agent, film-forming agent, antistatic agent and pH adjuster is used to improve the interfacial bonding strength between fiber and film-forming agent through chemical bonding. A composite film-forming system is formed by combining polyurethane and polyvinyl alcohol polymers to improve the flexibility and structural strength of the fiber.
It significantly reduces the compression rate of the gasket, improves dimensional stability and compressive strength, avoids powder shedding and edge chipping, and enhances the rigidity and service life of the gasket.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature sealing materials technology, and particularly relates to the impregnating agent for crystalline alumina fiber high-temperature insulating sealing gaskets, its preparation method, and crystalline alumina fiber high-temperature insulating sealing gaskets. Background Technology
[0002] In high-temperature industrial kilns, electric heating equipment, power electrical systems, new energy, and metallurgical and chemical industries, flange mating surfaces, cavity seals, and electrical isolation components are subjected to multiple coupled conditions such as high-temperature alternating current, continuous pressure, hot air erosion, and electrical insulation. Therefore, the sealing gaskets used must simultaneously possess comprehensive properties such as high-temperature insulation, sealing compensation, electrical insulation, creep resistance, and long-term stability.
[0003] Currently, conventional high-temperature sealing products mostly use materials such as aluminosilicate fiber, glass fiber, graphite, and ordinary ceramic fiber. However, all of these materials have significant limitations: silicate fiber gaskets have a high compressibility and poor resilience, making them prone to compaction deformation and thickness reduction under long-term high-temperature and high-pressure conditions, leading to air and heat leakage; at the same time, due to their high impurity content, their insulation performance decreases significantly at high temperatures, posing a risk of electrical leakage. Glass fiber has a limited upper temperature resistance and is prone to aging and pulverization, resulting in a short service life; although graphite materials have good temperature resistance, they are conductive and lack insulation capabilities. While rigid ceramic fibers have high rigidity, they lack compression buffering properties and cannot effectively compensate for assembly errors and thermal deformation.
[0004] In contrast, crystalline alumina fibers possess advantages such as stable crystal phase, excellent temperature resistance, high volume resistivity, good chemical inertness, and outstanding high-temperature creep resistance. Insulating gaskets made from these fibers, through their three-dimensional interwoven fiber structure, can achieve moderate compression bonding while maintaining stable high-temperature insulation performance and structural strength. This effectively overcomes the shortcomings of traditional materials, such as insufficient temperature resistance, insulation failure, and large permanent deformation, making them suitable for harsh high-temperature insulation and sealing applications.
[0005] However, crystalline alumina fiber high-temperature insulating gaskets still have significant shortcomings: they are inherently rigid and brittle, with poor compression resilience and flexibility, making them difficult to adapt to local defects at the joint surface. Furthermore, they are prone to brittle fracture, powdering, and edge chipping during processing or use. In practical applications, these gaskets often need to possess a denser structure, sufficient rigidity, compressive strength, and long-term dimensional stability. Therefore, there is an urgent need to develop a wetting agent spray coating that can effectively improve the gasket's compressibility, thereby further enhancing its overall applicability. Summary of the Invention
[0006] In view of this, the purpose of this invention is to provide an impregnating agent for high-temperature insulating gaskets made of crystalline alumina fibers, a method for preparing the same, and the resulting high-temperature insulating gaskets made of crystalline alumina fibers. In this invention, the high-temperature insulating gaskets made of crystalline alumina fibers coated with this impregnating agent can effectively improve problems such as compression ratio, powder shedding, and edge chipping in high-temperature insulating gaskets made of crystalline alumina fibers, resulting in a denser gasket structure, sufficient rigidity, resistance to flattening, and dimensional stability.
[0007] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides a sizing agent for high-temperature insulating gaskets made of crystalline alumina fibers, wherein the solid mass of the sizing agent accounts for 3.7 to 8.7% of the total mass of the sizing agent; the sizing agent comprises the following components, and the percentage of the mass of each component relative to the solid mass of the sizing agent is expressed as follows: Coupling agent: 0.3~0.6%; Film-forming agent: 15~32%; The film-forming agent comprises a first polymer component and a second polymer component, wherein the first polymer component is a polyurethane polymer and the second polymer component is a polyvinyl alcohol polymer, and the mass ratio of the first polymer component to the second polymer component is (11~14):1.
[0008] Preferably, the first polymer component is an aqueous polyurethane emulsion with a molecular weight of 1800-2400 and an average particle size of the dispersed phase greater than 0.1 μm.
[0009] Preferably, the second polymer component is a polyvinyl alcohol solution with a molecular weight of 25,000 to 35,000.
[0010] Preferably, the coupling agent is a silane coupling agent; the silane coupling agent is a silane coupling agent containing propylamino or acryloyloxy groups.
[0011] Preferably, the silane coupling agent comprises γ-methacryloxypropyltrimethoxysilane and / or γ-aminopropyltriethoxysilane.
[0012] Preferably, the wetting agent further includes an antistatic agent, wherein the mass of the antistatic agent accounts for 0.1 to 0.3% of the solid mass of the wetting agent.
[0013] Preferably, the antistatic agent is a cationic antistatic agent and / or a nonionic antistatic agent.
[0014] Preferably, the wetting agent further includes a pH adjuster, wherein the mass of the pH adjuster accounts for 0.2 to 0.3% of the solid mass of the wetting agent.
[0015] Preferably, the pH adjuster is an organic acid, which is selected from any one or more of citric acid, acetic acid, or formic acid.
[0016] Preferably, the wetting agent comprises the following components, and the percentage of the mass of each component relative to the solid mass of the wetting agent is expressed as follows (if less than 100%, make up with water): Coupling agent 0.3~0.6%; Film-forming agent 15~32%; Antistatic agent 0.1~0.3%; pH adjuster 0.2~0.3%; Ethanol 10-15%.
[0017] Secondly, the present invention provides a method for preparing the above-mentioned crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent, comprising the following steps: Hydrolysis is performed by adding a coupling agent to a solvent adjusted by an optional pH adjuster; then an aqueous solution of an optional antistatic agent and an aqueous solution of a film-forming agent are added and mixed evenly to obtain the wetting agent.
[0018] Thirdly, the present invention provides a high-temperature insulating gasket made of crystalline alumina fiber, which is prepared by the crystalline alumina fiber high-temperature insulating gasket impregnating agent involved in the above technical solution.
[0019] Preferably, the compression rate of the crystalline alumina fiber high-temperature insulating gasket is 30-50%.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: First, a composite film-forming system was formed by mixing polyurethane polymers and polyvinyl alcohol polymers at a mass ratio of (11~14):1, achieving a balance between gasket compressibility and structural strength. The polyurethane polymers form a moderately flexible adhesive film between the fibers, providing bundled properties; the polyvinyl alcohol polymers enhance the tensile strength of the fibers. The synergistic effect of these two components reduces the compressibility of the crystalline alumina fiber gasket from 40%~60% to 30%~50%, making the gasket less prone to excessive flattening and significantly improving dimensional stability.
[0021] Secondly, the interfacial chemical bonding of the coupling agent improves the interfacial adhesion strength between the fiber and the film-forming agent, effectively eliminating powder shedding and edge chipping of the gasket. After hydrolysis, the silane coupling agent reacts with the hydroxyl groups on the surface of the alumina fiber to form chemical bonds, and the organic groups react with the polymer of the film-forming agent, thereby improving the overall structural strength of the gasket at the molecular level.
[0022] Third, through the synergistic combination of the above-mentioned technical features, the high-temperature insulating gasket structure of crystalline alumina fiber is made denser, with moderate rigidity and less prone to flattening, resulting in a significant improvement in product appearance and service life. Detailed Implementation
[0023] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0024] The technical problem to be solved by the present invention is to provide a sizing agent for high-temperature insulating gaskets made of crystalline alumina fibers. High-temperature insulating gaskets made of crystalline alumina produced by coating with this sizing agent can effectively improve the problems of compression rate, powder shedding, and edge chipping of high-temperature insulating gaskets made of crystalline alumina, making the gasket structure denser, more rigid, less prone to flattening, and dimensionally stable.
[0025] Based on this, the present invention provides a sizing agent for high-temperature insulating gaskets made of crystalline alumina fibers. This sizing agent is used to coat high-temperature insulating gaskets made of crystalline alumina fibers, improving the bonding properties between fibers, reducing the gasket's compression ratio, minimizing powder shedding and edge chipping, and enhancing dimensional stability.
[0026] It should be noted that continuous fiber impregnation agents completely coat the monofilaments, primarily focusing on bundling, lubrication, and antistatic properties, reducing fiber breakage during high-speed processing, and are suitable for filament weaving and resin composites. Fiber blanket gasket adhesives, on the other hand, only bond at fiber intersections in a dotted manner, while also allowing for short fiber dispersion and preserving porosity. They are used for shaping heat-insulating and sealing gaskets. The film-forming methods, processes, and intended uses of these two types of adhesives are completely different.
[0027] Specifically, the technical solution of this application is described from the following aspects.
[0028] In a first aspect, the present invention provides a sizing agent for high-temperature insulating gaskets made of crystalline alumina fibers, wherein the solid mass of the sizing agent accounts for 3.7% to 8.7% of the total mass of the sizing agent, such as 3.7%, 4%, 5%, 5.7%, 6%, 6.7%, 7%, 7.7%, 8%, or 8.7%, etc.; the sizing agent comprises the following components, and the percentage of the mass of each component relative to the solid mass of the sizing agent is expressed as follows: Coupling agent: 0.3~0.6%; Film-forming agent: 15~32%.
[0029] In this invention, the wetting agent includes 0.3-0.6% (percentage of the solid mass of the wetting agent) of coupling agent, specifically 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, or 0.6%, etc.
[0030] The coupling agent is a silane coupling agent; specifically, a silane coupling agent containing propylamino or acryloyloxy groups. Silane coupling agents are organosilicon compounds containing two groups with different chemical properties in their molecules. They generally contain both inorganic and organic groups. The inorganic groups hydrolyze into silanol groups, which react with the hydroxyl groups on the surface of alumina-based ceramics, while the organic groups react with the resin groups being reinforced. Through chemical bonding, they improve the adhesion between the polymer and the inorganic material, thereby significantly improving the performance of the fiber material. Therefore, the coupling agent plays a coupling role between the ceramic fiber and the matrix resin. The selection of the coupling agent is crucial to the strength of the ceramic fiber; thus, the selection of the coupling agent is one of the key focuses of this invention.
[0031] In some embodiments of the present invention, the coupling agent may be selected from γ-methacryloxypropyltrimethoxysilane coupling agent and / or γ-aminopropyltriethoxysilane coupling agent.
[0032] In some preferred embodiments of the present invention, the coupling agent is preferably a combination of γ-methacryloxypropyltrimethoxysilane coupling agent and γ-aminopropyltriethoxysilane coupling agent, wherein the mass ratio of γ-methacryloxypropyltrimethoxysilane coupling agent to γ-aminopropyltriethoxysilane coupling agent in this combination is 1~5:1, preferably 1.5~4:1, and more preferably 2:1. The reason for preferring this combination is that the two silanes, through co-hydrolysis and co-condensation, form a uniform and dense hybrid silane protective layer on the surface of the insulating blanket, effectively improving surface wettability and suppressing fiber agglomeration defects. This compound system can adapt to a dual curing mechanism, achieving simultaneous cross-linking of the interface and matrix, significantly improving the interface stability, mechanical properties, and damp heat resistance of the high-temperature resistant insulating blanket, while optimizing the surface insulation protection effect, thus overcoming the shortcomings of single silane modification with limited functional groups, uneven surface coating, and limited heat resistance and insulation strengthening effect.
[0033] In this invention, the use of coupling agents can improve the mechanical properties of fiber materials. The coupling agents are hydrolyzed and dispersed in aqueous solutions, and have high amino activity, which can improve the compatibility between inorganic materials and epoxy resins, and improve the bundle properties, protection and processing technology of alumina fibers.
[0034] In this invention, the wetting agent comprises 15-32% (percentage of the solid mass of the wetting agent) of film-forming agent, specifically 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, or 32%, preferably 18-32%, and more preferably 20-24%.
[0035] Film-forming agents, as the main component of sizing agents, play a role in protecting fibers, ensuring continuous fiber production, and have a decisive influence on the mechanical strength of the final fiber product. Therefore, the selection of film-forming agents is another key aspect of this invention.
[0036] In this invention, the film-forming agent comprises a first polymer component (i.e., the first film-forming agent) and a second polymer component (i.e., the second film-forming agent). The first polymer component is a polyurethane polymer, and the second polymer component is a polyvinyl alcohol polymer. The total content of these components is 15-32%, preferably 20-32%, and more preferably 24-30%.
[0037] In this invention, the film-forming agents can be prepared by the user based on existing literature or commercially available products can be used. Studies have found that excessive use of the first film-forming agent can lead to excessively stiff fibers; conversely, excessive use of the second film-forming agent can result in easily dispersed fibers with poor bundle adhesion, affecting the application process. Therefore, in this invention, the mass ratio of the first film-forming agent to the second film-forming agent is (11~14):1, such as 11:1, 11.5:1, 12:1, 12.5:1, 13:1, 13.5:1, or 14:1, etc.
[0038] Furthermore, the first film-forming agent is an aqueous polyurethane emulsion with a molecular weight of 1800-2400, preferably 2000-2200, and an average dispersed phase particle size >0.1 μm; the second film-forming agent is polyvinyl alcohol with a molecular weight of 25000-35000, preferably 28000-30000. Using an aqueous polyurethane emulsion with a relatively large molecular weight results in better fiber aggregation, less fuzz, but stiffer yarn; using a polyvinyl alcohol solution can enhance the tensile strength and abrasion resistance of the fibers. This invention combines an aqueous polyurethane emulsion and a polyvinyl alcohol solution, which not only balances the aggregation and yarn quality of the crystalline alumina fiber high-temperature insulating gasket, but also avoids the formation of fuzz and fibrous strands in the crystalline alumina fiber high-temperature insulating gasket, resulting in a denser gasket structure, sufficient rigidity, resistance to flattening, and dimensional stability.
[0039] Through the above technical solution, polyurethane polymers, with their relatively low molecular weight, form a moderately flexible adhesive film between fibers, providing flexibility; polyvinyl alcohol polymers, with their higher molecular weight, enhance the tensile strength and abrasion resistance of the fibers. The two are formulated in a specific mass ratio, avoiding both excessive polyurethane leading to overly stiff fibers and excessive polyvinyl alcohol causing fiber disarray, thus achieving a balance between compressibility and structural strength. After hydrolysis, the coupling agent forms chemical bonds with the hydroxyl groups on the alumina fiber surface. The organic groups react with the film-forming agent polymer, improving the interfacial adhesion between the fiber and the film-forming agent through chemical bonding, thereby enhancing the overall structural strength at the molecular level.
[0040] Furthermore, in some embodiments of the present invention, the wetting agent further includes an antistatic agent, wherein the mass of the antistatic agent accounts for 0.1 to 0.3% of the solid mass of the wetting agent, such as 0.1%, 0.15%, 0.2%, 0.25%, or 0.3%, etc.
[0041] In this invention, the antistatic agent is a cationic antistatic agent and / or a nonionic antistatic agent.
[0042] As a preferred embodiment, the antistatic agent used in this invention is cationic; specifically, the antistatic agent is cationic. During the molding process of polymer materials, when the mixture is in a molten state, if it contains a sufficient concentration of antistatic agent, the antistatic agent molecules will form the densest orientation arrangement at the interface between the film-forming agent and air; wherein, the lipophilic groups extend into the resin interior, and the hydrophilic groups extend into the resin exterior. After the film-forming agent cures, the hydrophilic groups on the antistatic agent molecules are all aligned towards the air side, forming a monomolecular conductive layer. During processing and use, stretching, friction, etc., can cause defects in the antistatic agent molecular layer on the material surface, and the antistatic performance will decrease accordingly. However, after a period of time, the antistatic agent molecules inside the material will continuously migrate to the surface, allowing the damaged areas to recover and regain their antistatic effect.
[0043] Furthermore, in some embodiments of the present invention, the wetting agent further includes a pH adjuster, wherein the mass of the pH adjuster accounts for 0.2 to 0.3% of the solid mass of the wetting agent, such as 0.2%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, or 0.3%, etc.
[0044] In this invention, the pH adjuster mainly serves to assist the coupling agent in dispersing and to adjust the pH value of the prepared wetting agent. The pH adjuster of this invention uses organic acids, such as any one or more of citric acid, acetic acid, or formic acid.
[0045] In summary, in some embodiments of the present invention, the wetting agent comprises the following components, and the percentage of the mass of each component relative to the solid mass of the wetting agent is expressed as follows: Coupling agent 0.3~0.6%; Film-forming agent 15~32%; Antistatic agent 0.1~0.3%; pH adjuster 0.2~0.3%; Ethanol 10-15%.
[0046] The ethanol is an analytical grade ethanol solution. The ethanol content is 10-15% (percentage of the solid mass of the wetting agent), specifically 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, or 15%, etc.
[0047] Secondly, the present invention provides a method for preparing the above-mentioned crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent, comprising the following steps: Hydrolysis is performed by adding a coupling agent to a solvent adjusted by an optional pH adjuster; then an aqueous solution of an optional antistatic agent and an aqueous solution of a film-forming agent are added and mixed evenly to obtain the wetting agent.
[0048] Preferably, the above preparation method includes the following steps: Polyvinyl alcohol is heated and hydrolyzed to obtain a polyvinyl alcohol colloidal solution; a coupling agent is added to a solvent adjusted by a pH adjuster for hydrolysis; an antistatic agent is pre-dissolved and added; polyurethane polymers and polyvinyl alcohol polymers are diluted separately and added; the mixture is stirred evenly to obtain the impregnating agent.
[0049] In some embodiments of the present invention, the preparation method of the crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent includes the following steps: 1S: If polyvinyl alcohol is used as a film-forming agent, preheat the polyvinyl alcohol to hydrolyze it to obtain a uniform colloidal solution; 2S: Add pH adjuster, water, alcohol solution, etc. to the container, and add coupling agent for hydrolysis during stirring; 3S: Add the antistatic agent to the container after pre-dissolving it; 4S: Dilute each film-forming agent separately and add them to the container; 5S: Add ethanol, make up the remaining water, and stir until homogeneous.
[0050] Furthermore, the preparation method includes the following steps: 1S: Weigh the amount of PVA and water according to the required concentration ratio of PVA, mix them, and heat to 80~90℃, preferably 85℃, and stir to dissolve for later use. 2S: Prepare a solvent solution according to the ratio of water to alcohol solution, adjust the pH of the solvent to 4 using a pH adjuster, and add a silane coupling agent that meets the requirements of solute and solvent under stirring to carry out hydrolysis; 3S: Dissolve the antistatic agent in 10-20 times its volume of water, stir to dilute, and then add to the container; 4S: Dissolve the first film-forming agent and the second film-forming agent in 10 to 15 times their volume of water, stir to dilute, and then add to the container.
[0051] 5S: Add ethanol, make up the remaining water, and stir until homogeneous.
[0052] In step 2S, a pH adjuster is added during the pre-dispersion operation of the coupling agent.
[0053] The present invention also provides the application of the impregnating agent of the crystalline alumina fiber high-temperature insulating gasket in the preparation of the crystalline alumina fiber high-temperature insulating gasket.
[0054] Thirdly, the present invention provides a high-temperature insulating gasket made of crystalline alumina fiber, which is prepared by the crystalline alumina fiber high-temperature insulating gasket impregnating agent involved in the above technical solution.
[0055] In this invention, the compression rate of the crystalline alumina fiber high-temperature insulating sealing gasket is 30-50%.
[0056] To further illustrate the present invention, the following embodiments provide a detailed description. The components of the wetting agent used in the following embodiments of the present invention are as follows: Coupling agent: γ-Methacryloxypropyltrimethoxysilane coupling agent, product brand name KH-570; γ-aminopropyltriethoxysilane coupling agent, product brand name KH-550; Film-forming agent: Waterborne polyurethane emulsion, Anda Huatai; PVA, product designation 2099; Antistatic agent: Octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, Shandong Yousuo; pH adjuster: acetic acid.
[0057] It should be noted that the specific types and contents of the components selected above do not limit the scope of protection of this application.
[0058] Examples 1-2
[0059] This embodiment provides a sizing agent for high-temperature insulating gaskets made of crystalline alumina fibers, the preparation method of which includes the following steps: 1S: Weigh the amount of PVA and water according to the required concentration ratio of the second film-forming agent PVA, mix them, and heat at 85°C while stirring to dissolve them for later use. 2S: Prepare a solvent solution according to the ratio of water to alcohol solution, adjust the pH of the solvent to 4 using a pH adjuster, and add the silane coupling agent required for the solute and solvent under stirring to hydrolyze it; 3S: Dissolve the antistatic agent in 10 times its volume of water, stir to dilute, and then add to the container; 4S: Dissolve the first film-forming agent in 10 times its volume of water, stir to dilute, and then add it to the container.
[0060] 5S: Add ethanol, make up the remaining water, and stir until homogeneous.
[0061] The formulation is shown in Table 1 (the proportions of each group are expressed as a percentage of the solid mass of the wetting agent).
[0062] Table 1
[0063] To further illustrate the beneficial effects of the present invention, wetting agent formulations with different content ratios were used as comparative examples. The formulations of the comparative examples are designed as follows: Comparative Example 1 Coupling agent: γ-aminopropyltriethoxysilane coupling agent, product brand KH-550, 0.4%; Lubricant: OED, 0.5%; Film-forming agent: Waterborne polyurethane emulsion, Anda Huatai, 8%; PVA, product brand 2099, 2%; Antistatic agent: 0.2%; pH adjuster: Acetic acid, 0.2%; Ethanol, 15%.
[0064] Comparative Example 2
[0065] Coupling agent: γ-Methacryloxypropyltrimethoxysilane coupling agent, product brand KH-570, 0.5%; Lubricant: OED, 0.5%; Film-forming agent: Waterborne polyurethane emulsion, Anda Huatai, 16%; PVA, product brand 2099, 2%; Antistatic agent: 0.2%; pH adjuster: Acetic acid, 0.2%; Ethanol, 10%.
[0066] Comparative Example 3
[0067] Coupling agent: γ-Methacryloxypropyltrimethoxysilane coupling agent, product brand KH-570, 0.4%; γ-aminopropyltriethoxysilane coupling agent, product brand KH-550, 0.2%; Film-forming agent: Waterborne polyurethane emulsion, Anda Huatai, 5%; PVA, product brand 2099, 2%; Antistatic agent: 0.2%; pH adjuster: Acetic acid, 0.2%; Ethanol, 15%.
[0068] Comparative Example 4
[0069] Coupling agent: γ-Methacryloxypropyltrimethoxysilane coupling agent, product brand KH-570, 0.4%; γ-aminopropyltriethoxysilane coupling agent, product brand KH-550, 0.2%; Film-forming agent: Waterborne polyurethane emulsion, Anda Huatai, 9%; PVA, product brand 2099, 2%; Antistatic agent: 0.2%, pH adjuster: Acetic acid, 0.2%; Ethanol, 15%.
[0070] Performance testing
[0071] The testing method is as follows: (1) Room temperature environment 21~30℃; the indenter deflection of the testing machine should be corrected in advance; (2) Place a 100×100 mm alumina fiber blanket sample in the center; (3) Apply an initial load of 14 kPa, maintain for 15 s, and read the thickness P; (4) Load to the total load (100 kPa / 200 kPa, as specified in the contract) within 10 s, stabilize the pressure for 60 s, and read the thickness M; (5) Test three samples under the same conditions and take the arithmetic mean.
[0072] The core calculation formula is: Compression ratio C = (PM) / P × 100%.
[0073] The test must strictly follow the established timing parameters. It is strictly forbidden to use ordinary gaskets for high-pressure loads or use pre-treated samples under pressure to avoid irreversible plastic deformation of the fiber blanket and distortion of the reference thickness, which would lead to invalid test data. The final result is the average of three groups of samples.
[0074] The test results are shown in Table 2: Table 2
[0075] In the above examples and comparative examples, the amount used was 42 mL for each side of the sprayed material, with two sides sprayed simultaneously.
[0076] As can be seen from the above formulation test examples, through the design of components and component content, the overall performance of the crystalline alumina fiber high-temperature insulating gasket impregnator of this application is better than that of the comparative data, and its fiber products have high quality and stability.
[0077] Specifically, the test results above show that the crystalline alumina fiber gasket produced using the sizing agent formulation of this invention has a significantly lower compression ratio than the comparative example, decreasing from 40%~60% to 30%~50%, and the gasket is less prone to excessive flattening. Furthermore, the gasket in the embodiment exhibits no flaking, while the comparative example shows varying degrees of flaking. This fully demonstrates that the technical solution of combining polyurethane polymers and polyvinyl alcohol polymers in a specific ratio in this invention can effectively improve the compression ratio and reduce flaking and edge breakage problems of crystalline alumina fiber gaskets.
[0078] In summary, the fibers produced using the crystalline alumina fiber high-temperature insulating gasket impregnating agent of the present invention can significantly improve the compression ratio of gasket products, improve the appearance of gaskets, and solve the problem of slagging.
[0079] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A sizing agent for high-temperature insulating and sealing gaskets made of crystalline alumina fibers, characterized in that, The solid mass of the wetting agent accounts for 3.7% to 8.7% of the total mass of the wetting agent; the wetting agent comprises the following components, and the percentage of the mass of each component in the solid mass of the wetting agent is expressed as follows: Coupling agent: 0.3~0.6%; Film-forming agent: 15~32%; The film-forming agent comprises a first polymer component and a second polymer component, wherein the first polymer component is a polyurethane polymer and the second polymer component is a polyvinyl alcohol polymer, and the mass ratio of the first polymer component to the second polymer component is (11~14):
1.
2. The crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent according to claim 1, characterized in that, The first polymer component is an aqueous polyurethane emulsion, wherein the molecular weight of the aqueous polyurethane emulsion is 1800~2400 and the average particle size of the dispersed phase is greater than 0.1 μm; The second polymer component is a polyvinyl alcohol solution with a molecular weight of 25,000 to 35,000.
3. The crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent according to claim 1 or 2, characterized in that, The coupling agent is a silane coupling agent; the silane coupling agent is a silane coupling agent with propylamino or acryloyloxy groups.
4. The crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent according to claim 3, characterized in that, The silane coupling agent includes γ-methacryloxypropyltrimethoxysilane and / or γ-aminopropyltriethoxysilane.
5. The crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent according to claim 1, characterized in that, The wetting agent further includes an antistatic agent, wherein the mass of the antistatic agent accounts for 0.1-0.3% of the solid mass of the wetting agent; The antistatic agent is a cationic antistatic agent and / or a nonionic antistatic agent.
6. The crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent according to claim 1, characterized in that, The wetting agent further includes a pH adjuster, wherein the mass of the pH adjuster accounts for 0.2-0.3% of the solid mass of the wetting agent; The pH adjuster is an organic acid, which is selected from any one or more of citric acid, acetic acid, or formic acid.
7. The crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent according to claim 6, characterized in that, The wetting agent comprises the following components, and the percentage of each component by mass relative to the solid mass of the wetting agent is expressed as follows: Coupling agent 0.3~0.6%; Film-forming agent 15~32%; Antistatic agent 0.1~0.3%; pH adjuster 0.2~0.3%; Ethanol 10-15%.
8. A method for preparing a sizing agent for high-temperature insulating gaskets made of crystalline alumina fibers as described in any one of claims 1 to 7, characterized in that, Includes the following steps: Hydrolysis is performed by adding a coupling agent to a solvent adjusted by an optional pH adjuster; then an aqueous solution of an optional antistatic agent and an aqueous solution of a film-forming agent are added and mixed evenly to obtain the wetting agent.
9. A high-temperature insulating sealing gasket made of crystalline alumina fiber, characterized in that, The crystalline alumina fiber high-temperature insulating gasket impregnating agent is prepared from any one of the crystalline alumina fiber high-temperature insulating sealing gaskets according to claims 1 to 7 or from the crystalline alumina fiber high-temperature insulating sealing gasket impregnating agent prepared by the preparation method according to claim 8.
10. The crystalline alumina fiber high-temperature insulating sealing gasket according to claim 9, characterized in that, Its compression rate is 30-50%.