Waterproof and breathable composite fabric and preparation method thereof

By combining a modified TPU waterproof and breathable membrane with nylon elastic knitted fabric, the problems of low moisture permeability, insufficient hydrostatic pressure resistance, poor hydrolysis resistance, and poor low-temperature performance of thermoplastic polyurethane membranes in waterproof and breathable composite fabrics are solved, achieving high-efficiency waterproof and breathable performance and durability.

CN123153288APending Publication Date: 2026-11-24SHANGHAI YOULAN TEXTILE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611579012.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing thermoplastic polyurethane membranes used in waterproof and breathable composite fabrics suffer from problems such as low moisture permeability, insufficient hydrostatic pressure resistance, poor hydrolysis resistance, poor low-temperature performance, and failure of waterproof performance after repeated stretching.

Method used

By constructing triazole glycidylamine, sulfobetaine triazole, oxazoline long-chain triazole and triazole betaine silicon modifier, a modified TPU waterproof and breathable membrane is composited with nylon elastic knitted fabric to form a microphase separation structure and chemical bond connection, thereby improving the membrane's waterproofness, moisture permeability, hydrolysis resistance and low-temperature toughness.

Benefits of technology

It achieves improved moisture permeability, enhanced hydrostatic pressure resistance, improved low-temperature flexibility and creep resistance in high-humidity environments, while maintaining long-lasting modification effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to a kind of waterproof and breathable composite fabric and its preparation method, belong to textile material technical field;The present application will be 1-allyl-1H-1,2,4-triazole-3-amine and epoxy chloropropane ring-opening ring triazole glycidyl amine;With (3-(methylethylene amide) propyl) dimethyl-(3-sulfonic acid) ammonium azo-michael addition is obtained sulfobetaine triazole;With 2-heptadecyl-4-methyl-2-oxazoline-4-methanol etherification is obtained oxazoline long-chain triazole;With monohydrogen end-capped polydimethylsiloxane silicon hydrogen addition is obtained triazole betaine silicon modifier;With polyethylene glycol, 4,4'-diphenylmethane diisocyanate prepolymer, with polytetrahydrofuran diol and chain extender film-forming, obtain modified TPU waterproof and breathable film;With chinlon elastic knitted fabric composite, obtain waterproof and breathable composite fabric;Triazole ring, sulfobetaine, oxazoline ring, polysiloxane and heptadecyl synergy, improve waterproof and moisture permeable, hydrolysis resistance and low-temperature toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of textile materials technology, specifically relating to a waterproof and breathable composite fabric and its preparation method. Background Technology

[0002] With the development of outdoor sportswear, protective clothing, and functional textiles, waterproof and breathable fabrics need to block liquid water penetration while allowing water vapor to pass through in order to maintain wearing comfort. Existing waterproof and breathable materials mainly include polytetrafluoroethylene (PTFE) microporous membranes, polyurethane coatings, and thermoplastic polyurethane membranes. Among them, thermoplastic polyurethane membranes, due to their advantages such as good elasticity, abrasion resistance, and soft hand feel, are often combined with nylon elastic knitted fabrics for the production of sportswear, outdoor clothing, and other products requiring elasticity and comfort.

[0003] However, existing thermoplastic polyurethane membranes have the following main problems when used in waterproof and breathable composite fabrics: First, the thermoplastic polyurethane molecular chain contains hydrophilic groups such as ether bonds and urethane bonds. Water vapor conduction depends on the molecular diffusion of hydrophilic segments, resulting in insufficient driving force for moisture transfer and a low moisture permeability rate in high humidity environments. Simultaneously, the hydrophilic groups are easily wetted and penetrated by liquid water, leading to insufficient hydrostatic pressure resistance, making it difficult to simultaneously achieve both waterproof and breathable performance. Second, polyester-type thermoplastic polyurethane molecular chains contain a large number of ester groups, which are prone to hydrolytic chain breakage under humid and hot environments and repeated washing conditions, leading to a gradual decline in the membrane's mechanical properties, hardening, reduced toughness, and decreased waterproof durability. Third, thermoplastic polyurethane membranes have poor low-temperature performance. At low temperatures, the molecular chain mobility decreases, increasing membrane rigidity and decreasing toughness. Furthermore, thin membranes are prone to creep and pore deformation under high-pressure water impact. When laminated with nylon elastic knitted fabric, the membrane is prone to micro-cracks during repeated stretching and bending, damaging the waterproof barrier performance and causing waterproofing failure.

[0004] Therefore, there is an urgent need to provide a waterproof and breathable composite fabric that can comprehensively solve the above problems. Summary of the Invention

[0005] The purpose of this invention is to provide a waterproof and breathable composite fabric and its preparation method, so as to solve the problems mentioned in the background art.

[0006] The objective of this invention can be achieved through the following technical solutions: A method for preparing a waterproof and breathable composite fabric includes the following steps: S1: 1-Allyl-1H-1,2,4-triazol-3-amine is reacted with epichlorohydrin in the presence of a catalyst to open the ring, and then the ring is closed under alkaline conditions to obtain triazolyl glycidylamine. The chemical reaction equation is: S2: Triazole glycidylamine is reacted with (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium via an aza-Michael addition reaction to give sulfobetaine triazole; The chemical reaction equation is: S3: The sulfobetaine triazole is subjected to a ring-opening etherification reaction with 2-heptadecyl-4-methyl-2-oxazoline-4-methanol in the presence of a catalyst to obtain oxazoline long-chain triazole; The chemical reaction equation is: S4: Oxazoline long-chain triazole is reacted with monohydrogen-terminated polydimethylsiloxane in the presence of a platinum catalyst to obtain triazole betaine silicon modifier. The chemical reaction equation is: S5: Triazole betaine silica modifier, polyethylene glycol, and 4,4'-diphenylmethane diisocyanate are prepolymerized in the presence of a catalyst to obtain a modified isocyanate prepolymer component; polytetrahydrofuran glycol and a chain extender are mixed to obtain a polyol component; the polyol component is mixed and reacted with the modified isocyanate prepolymer component to form a film, resulting in a modified TPU waterproof and breathable membrane; the modified TPU waterproof and breathable membrane is laminated with nylon elastic knitted fabric using dotted hot melt adhesive to obtain a waterproof and breathable composite fabric.

[0007] Furthermore, the molar ratio of 1-allyl-1H-1,2,4-triazol-3-amine to epichlorohydrin is 1:1.05–1.3, the catalyst for the ring-opening reaction in S1 is tetrabutylammonium bromide, the alkaline condition is an aqueous sodium hydroxide solution, the amount of tetrabutylammonium bromide is 2%–5% of the mass of 1-allyl-1H-1,2,4-triazol-3-amine, and the molar ratio of sodium hydroxide to 1-allyl-1H-1,2,4-triazol-3-amine is 1.0–1.2:1.

[0008] Furthermore, the molar ratio of triazole glycidylamine to (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 1:1.0 to 1.2.

[0009] Furthermore, the molar ratio of sulfobetaine triazole to 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 1:1.1 to 1.5, and the catalyst for the ring-opening etherification reaction in S3 is potassium carbonate, with the amount of potassium carbonate accounting for 5% to 10% of the mass of 2-heptadecyl-4-methyl-2-oxazoline-4-methanol.

[0010] Furthermore, the molar ratio of oxazoline long-chain triazole to monohydrogen-terminated polydimethylsiloxane is 1:1.0 to 1.2, and the platinum catalyst in S4 is the Karstedt platinum catalyst, with the amount of Karstedt platinum catalyst accounting for 0.01% to 0.03% of the mass of monohydrogen-terminated polydimethylsiloxane.

[0011] Further, by weight, the content of triazole betaine silicon modifier is 8-12 parts, polyethylene glycol is 40-60 parts, polytetrahydrofuran glycol is 20-40 parts, 4,4'-diphenylmethane diisocyanate is 13.7-29.1 parts, chain extender is 2-5 parts, and the chain extender is 1,4-butanediol.

[0012] Furthermore, in S1, the ring-opening reaction temperature is 40–60 °C and the time is 2–4 h; the ring-closing reaction temperature is 0–10 °C and the time is 0.5–1 h; in S2, the aza-Michael addition reaction temperature is 10–25 °C and the time is 4–8 h.

[0013] Furthermore, the ring-opening etherification reaction in S3 is carried out at a temperature of 60–80 °C for 6–10 h; the hydrosilylation reaction in S4 is carried out at a temperature of 80–100 °C for 6–10 h.

[0014] Furthermore, in S5, the prepolymerization reaction temperature is 80–90℃ and the time is 1–2 h; the mixing reaction temperature is 80–100℃, the stirring speed is 700–900 rpm, and the time is 3–5 min.

[0015] A waterproof and breathable composite fabric is prepared by any of the above preparation steps.

[0016] The beneficial effects of this invention are: 1) This invention constructs a triazole glycidylamine structure by nucleophilic ring-opening and ring-closing reactions of 1-allyl-1H-1,2,4-triazole-3-amine and epichlorohydrin. A sulfobetaine group is introduced via aza-Michael addition, followed by base-catalyzed selective ring-opening of an epoxy group with hydroxymethyl groups to introduce an oxazoline ring and a heptadecanyl long chain. A long-chain polysiloxane is then introduced via hydrosilylation, yielding a triazole betaine silicone modifier containing a triazole ring, a sulfobetaine group, an oxazoline ring, a heptadecanyl long chain, and a long-chain polysiloxane. This modifier is grafted onto the thermoplastic polyurethane backbone via hydroxyl groups to form a modified TPU waterproof and breathable membrane, which is then composited with nylon elastic knitted fabric. In this modifier, long-chain polysiloxane and heptadecanyl long chains are enriched on the membrane surface, forming a low surface energy hydrophobic barrier that makes it difficult for liquid water to wet and penetrate, thus improving hydrostatic pressure resistance. The sulfobetaine group has superhydrophilicity, providing high-density water vapor transport channels, which improves the dissolution and diffusion efficiency of water vapor in the membrane. As hydrophobic segments, the long-chain polysiloxane and heptadecanyl long chains form a microphase separation structure with the hydrophilic sulfobetaine. Water vapor is preferentially transported along the hydrophilic channels, while liquid water is blocked by the hydrophobic regions, thereby improving waterproofness while maintaining moisture permeability. The polysiloxane chain has an extremely low silicon-oxygen bond rotation barrier, maintaining high flexibility even at low temperatures, thus providing low-temperature flexibility for the polyurethane film. The rigid structure of the oxazoline ring provides molecular chain support, and its synergistic effect with sulfobetaine's ionic aggregation restricts chain slippage under high temperatures and continuous external forces, contributing to improved creep resistance. Simultaneously, the oxazoline ring can undergo ring-opening addition reactions with the carboxyl groups generated by hydrolysis, consuming the carboxyl groups and blocking their autocatalytic hydrolysis, thereby improving hydrolysis resistance. Therefore, this invention, through the synergistic combination of long-chain polysiloxane, heptadecanyl long chain, sulfobetaine, and oxazoline ring, can simultaneously improve waterproof performance, moisture permeability, hydrolysis resistance, and low-temperature toughness.

[0017] 2) In this invention, the sulfobetaine groups have antistatic properties, which help reduce static charge accumulation and dust adsorption; at the same time, the ion aggregation between sulfobetaines serves as a reversible physical cross-linking point, which can absorb energy and reform during repeated stretching and bending, thus helping to improve the elasticity and fatigue resistance of the membrane; the long-chain polysiloxanes are enriched on the membrane surface, which can reduce the surface friction coefficient, help reduce wear marks and local weak areas, and help improve the hydrostatic pressure retention rate after repeated friction; in addition, the triazole ring has the ability to absorb ultraviolet light, which helps to improve the weather resistance of the membrane; the polysiloxane segments are connected to the polyurethane matrix by chemical bonds, which makes them less prone to migration and precipitation, thus helping to maintain the long-term effect of modification. Detailed Implementation

[0018] The technical solutions of the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of this application. Based on the embodiments in this application specification, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection claimed in this application.

[0019] The raw materials used in this invention are not particularly restricted in terms of their source; they can be purchased from the market or prepared using conventional methods known to those skilled in the art.

[0020] Monohydrogen-terminated polydimethylsiloxane: molecular weight 2000; Polyethylene glycol: molecular weight 2000; Polytetrahydrofurandiol: Molecular weight 2000; Nylon stretch knitted fabric: Item No. WK-0006, weight 170g / m² 2 Composition: 85% nylon, 15% spandex; width: 64 / 65 inches; double-sided plain weave. Dotted hot melt adhesive: Lubrizol PEARLBOND® 125 / H, melting point 130~140℃, weight 12g / m³ 2 .

[0021] Example 1 A method for preparing a waterproof and breathable composite fabric includes the following steps: S1: Under nitrogen protection and anhydrous conditions, 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin were dissolved in anhydrous ethanol. After stirring and dissolving, tetrabutylammonium bromide catalyst was added, and the reaction was stirred at 40°C for 2 h. After the reaction was completed, the temperature was lowered to 0°C, and sodium hydroxide aqueous solution (mass fraction 25%) was slowly added dropwise. After the addition was complete, stirring was continued for 0.5 h. The mixture was filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was extracted with ethyl acetate and water (volume ratio of ethyl acetate to water 1:1). The organic phase was dried with anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was purified by silica gel column chromatography (eluent was a mixture of ethyl acetate and petroleum ether in a volume ratio of 1:3) to obtain triazolyl glycidylamine.

[0022] The molar ratio of 1-allyl-1H-1,2,4-triazol-3-amine to epichlorohydrin is 1:1.05; the amount of tetrabutylammonium bromide is 2% of the mass of 1-allyl-1H-1,2,4-triazol-3-amine; the ratio of anhydrous ethanol to the total mass of 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin is 6 mL:1 g; and the molar ratio of sodium hydroxide to 1-allyl-1H-1,2,4-triazol-3-amine is 1.0:1.

[0023] S2: Under nitrogen protection, triazole glycidylamine was dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium was added, and the mixture was stirred and reacted at 10°C for 4 hours. After the reaction was completed, most of the solvent was removed by vacuum distillation. The residue was precipitated with acetone, filtered, and the filter cake was washed three times with acetone and dried under vacuum to obtain sulfobetaine triazole.

[0024] The molar ratio of triazole glycidylamine to (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 1:1.0, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of triazole glycidylamine and (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 8 mL:1 g.

[0025] S3: Under nitrogen protection, sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol were dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, potassium carbonate catalyst was added, and the mixture was stirred at 60°C for 6 hours. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the solvent was removed by vacuum distillation. The residue was extracted with ethyl acetate and water (ethyl acetate to water volume ratio of 1:1). The organic phase was dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation. The residue was purified by silica gel column chromatography (eluent was a 1:1 volume mixture of ethyl acetate and petroleum ether) to obtain oxazoline long-chain triazole.

[0026] The molar ratio of sulfobetaine triazole to 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 1:1.1, the amount of potassium carbonate used accounts for 5% of the mass of 2-heptadecyl-4-methyl-2-oxazoline-4-methanol, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 8 mL:1 g.

[0027] S4: Under nitrogen protection, oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane were dissolved in anhydrous toluene. After stirring and dissolving, Karstedt platinum catalyst was added, and the reaction was carried out at 80°C for 6 hours. After the reaction was completed, the mixture was cooled to room temperature, and the solvent was removed by vacuum distillation. The residue was precipitated with methanol, filtered, and the filter cake was washed three times with methanol and dried under vacuum to obtain triazole betaine silicon modifier.

[0028] The molar ratio of oxazoline long-chain triazole to monohydrogen-terminated polydimethylsiloxane is 1:1.0, the amount of Karstedt platinum catalyst is 0.01% of the mass of monohydrogen-terminated polydimethylsiloxane, and the mass ratio of anhydrous toluene to the total mass of oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane is 8 mL:1 g.

[0029] S5: Under nitrogen protection, triazole betaine silica modifier, polyethylene glycol, and 4,4'-diphenylmethane diisocyanate were added to a reactor in a specific ratio and stirred at 80°C for 1 hour to obtain a modified isocyanate prepolymer component. Polytetrahydrofuran glycol and chain extender 1,4-butanediol were mixed in a specific ratio to obtain a polyol component. The polyol component was mixed with the catalyst dibutyltin dilaurate, and then the modified isocyanate prepolymer component was added. The mixture was stirred at 700 rpm for 3 minutes, with the temperature controlled at 80°C, until uniformly mixed. The mixture was then coated onto a release film with a coating thickness of 0.22 mm and cured at 110°C for 3 minutes. The release film was then peeled off to obtain a modified TPU waterproof and breathable membrane. The modified TPU waterproof and breathable membrane was then hot-pressed with nylon elastic knitted fabric at 140°C and 0.3 MPa using a dot-matrix hot-melt composite method. After cooling, a waterproof and breathable composite fabric was obtained.

[0030] The composition, by weight, includes 8 parts of triazole betaine silicon modifier, 40 parts of polyethylene glycol, 20 parts of polytetrahydrofuran glycol, 13.7 parts of 4,4'-diphenylmethane diisocyanate, 2 parts of 1,4-butanediol, and 0.05 parts of dibutyltin dilaurate.

[0031] Example 2 A method for preparing a waterproof and breathable composite fabric includes the following steps: S1: Under nitrogen protection and anhydrous conditions, 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin were dissolved in anhydrous ethanol. After stirring and dissolving, tetrabutylammonium bromide catalyst was added, and the reaction was stirred at 45°C for 2.5 h. After the reaction was completed, the temperature was lowered to 2.5°C, and sodium hydroxide aqueous solution (mass fraction 25%) was slowly added dropwise. After the addition was complete, stirring was continued for 0.6 h. The mixture was filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was extracted with ethyl acetate and water (volume ratio of ethyl acetate to water 1:1). The organic phase was dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was purified by silica gel column chromatography (eluent was a mixture of ethyl acetate and petroleum ether in a volume ratio of 1:3) to obtain triazolyl glycidylamine.

[0032] The molar ratio of 1-allyl-1H-1,2,4-triazol-3-amine to epichlorohydrin is 1:1.11; the amount of tetrabutylammonium bromide is 2.8% of the mass of 1-allyl-1H-1,2,4-triazol-3-amine; the ratio of anhydrous ethanol to the total mass of 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin is 7 mL:1 g; and the molar ratio of sodium hydroxide to 1-allyl-1H-1,2,4-triazol-3-amine is 1.05:1.

[0033] S2: Under nitrogen protection, triazole glycidylamine was dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium was added, and the mixture was stirred and reacted at 14°C for 5 h. After the reaction was completed, most of the solvent was removed by vacuum distillation. The residue was precipitated with acetone, filtered, and the filter cake was washed three times with acetone and dried under vacuum to obtain sulfobetaine triazole.

[0034] The molar ratio of triazole glycidylamine to (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 1:1.05, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of triazole glycidylamine and (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 9 mL:1 g.

[0035] S3: Under nitrogen protection, sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol were dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, potassium carbonate catalyst was added, and the mixture was stirred at 65°C for 7 hours. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the solvent was removed by vacuum distillation. The residue was extracted with ethyl acetate and water (ethyl acetate to water volume ratio of 1:1). The organic phase was dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation. The residue was purified by silica gel column chromatography (eluent was a 1:1 volume mixture of ethyl acetate and petroleum ether) to obtain oxazoline long-chain triazole.

[0036] The molar ratio of sulfobetaine triazole to 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 1:1.2, the amount of potassium carbonate used accounts for 6.3% of the mass of 2-heptadecyl-4-methyl-2-oxazoline-4-methanol, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 9 mL:1 g.

[0037] S4: Under nitrogen protection, oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane were dissolved in anhydrous toluene. After stirring and dissolving, Karstedt platinum catalyst was added, and the reaction was carried out at 85°C with stirring for 7 hours. After the reaction was completed, the mixture was cooled to room temperature, and the solvent was removed by vacuum distillation. The residue was precipitated with methanol, filtered, and the filter cake was washed three times with methanol and dried under vacuum to obtain the triazole betaine silicon modifier.

[0038] The molar ratio of oxazoline long-chain triazole to monohydrogen-terminated polydimethylsiloxane is 1:1.05, the amount of Karstedt platinum catalyst is 0.015% of the mass of monohydrogen-terminated polydimethylsiloxane, and the ratio of anhydrous toluene to the total mass of oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane is 9 mL:1 g.

[0039] S5: Under nitrogen protection, triazole betaine silica modifier, polyethylene glycol, and 4,4'-diphenylmethane diisocyanate were added to a reactor in a specific ratio and stirred at 83°C for 1.3 h to obtain a modified isocyanate prepolymer component. Polytetrahydrofuran glycol and chain extender 1,4-butanediol were mixed in a specific ratio to obtain a polyol component. The polyol component was mixed with the catalyst dibutyltin dilaurate, and then the modified isocyanate prepolymer component was added. The mixture was stirred at 750 rpm for 3.5 min, with the temperature controlled at 85°C, and mixed evenly. The mixture was then coated onto a release film with a coating thickness of 0.22 mm and cured at 110°C for 3 min. The release film was then peeled off to obtain a modified TPU waterproof and breathable membrane. The modified TPU waterproof and breathable membrane was then hot-pressed with nylon elastic knitted fabric at 140°C and 0.3 MPa through dot-matrix hot-melt bonding. After cooling, a waterproof and breathable composite fabric was obtained.

[0040] The composition, by weight, includes 9 parts of triazole betaine silicon modifier, 45 parts of polyethylene glycol, 25 parts of polytetrahydrofuran glycol, 17.6 parts of 4,4'-diphenylmethane diisocyanate, 2.8 parts of 1,4-butanediol, and 0.09 parts of dibutyltin dilaurate.

[0041] Example 3 A method for preparing a waterproof and breathable composite fabric includes the following steps: S1: Under nitrogen protection and anhydrous conditions, 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin were dissolved in anhydrous ethanol. After stirring and dissolving, tetrabutylammonium bromide catalyst was added, and the reaction was stirred at 50°C for 3 h. After the reaction was completed, the temperature was lowered to 5°C, and sodium hydroxide aqueous solution (mass fraction 25%) was slowly added dropwise. After the addition was complete, stirring was continued for 0.75 h. The mixture was filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was extracted with ethyl acetate and water (volume ratio of ethyl acetate to water 1:1). The organic phase was dried with anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was purified by silica gel column chromatography (eluent was a mixture of ethyl acetate and petroleum ether in a volume ratio of 1:3) to obtain triazolyl glycidylamine.

[0042] The molar ratio of 1-allyl-1H-1,2,4-triazol-3-amine to epichlorohydrin is 1:1.18; the amount of tetrabutylammonium bromide used accounts for 3.5% of the mass of 1-allyl-1H-1,2,4-triazol-3-amine; the ratio of anhydrous ethanol to the total mass of 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin is 8 mL:1 g; and the molar ratio of sodium hydroxide to 1-allyl-1H-1,2,4-triazol-3-amine is 1.1:1.

[0043] S2: Under nitrogen protection, triazole glycidylamine was dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium was added, and the mixture was stirred and reacted at 18°C ​​for 6 hours. After the reaction was completed, most of the solvent was removed by vacuum distillation. The residue was precipitated with acetone, filtered, and the filter cake was washed three times with acetone and dried under vacuum to obtain sulfobetaine triazole.

[0044] The molar ratio of triazole glycidylamine to (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 1:1.1, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of triazole glycidylamine and (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 10mL:1g.

[0045] S3: Under nitrogen protection, sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol were dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, potassium carbonate catalyst was added, and the mixture was stirred at 70°C for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the solvent was removed by vacuum distillation. The residue was extracted with ethyl acetate and water (ethyl acetate to water volume ratio of 1:1). The organic phase was dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation. The residue was purified by silica gel column chromatography (eluent was a 1:1 volume mixture of ethyl acetate and petroleum ether) to obtain oxazoline long-chain triazole.

[0046] The molar ratio of sulfobetaine triazole to 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 1:1.3, the amount of potassium carbonate used accounts for 7.5% of the mass of 2-heptadecyl-4-methyl-2-oxazoline-4-methanol, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 10 mL:1 g.

[0047] S4: Under nitrogen protection, oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane were dissolved in anhydrous toluene. After stirring and dissolving, Karstedt platinum catalyst was added, and the reaction was stirred at 90°C for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, and the solvent was removed by vacuum distillation. The residue was precipitated with methanol, filtered, and the filter cake was washed three times with methanol and dried under vacuum to obtain triazole betaine silicon modifier.

[0048] The molar ratio of oxazoline long-chain triazole to monohydrogen-terminated polydimethylsiloxane is 1:1.1, the amount of Karstedt platinum catalyst is 0.02% of the mass of monohydrogen-terminated polydimethylsiloxane, and the ratio of anhydrous toluene to the total mass of oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane is 10 mL: 1 g.

[0049] S5: Under nitrogen protection, triazole betaine silica modifier, polyethylene glycol, and 4,4'-diphenylmethane diisocyanate were added to a reactor in a specific ratio and stirred at 85°C for 1.5 h to obtain a modified isocyanate prepolymer component. Polytetrahydrofuran glycol and chain extender 1,4-butanediol were mixed in a specific ratio to obtain a polyol component. The polyol component was mixed with the catalyst dibutyltin dilaurate, and then the modified isocyanate prepolymer component was added. The mixture was stirred at 800 rpm for 4 min, with the temperature controlled at 90°C, until uniformly mixed. The mixture was then coated onto a release film with a coating thickness of 0.22 mm and cured at 110°C for 3 min. The release film was then peeled off to obtain a modified TPU waterproof and breathable membrane. The modified TPU waterproof and breathable membrane was then hot-pressed with nylon elastic knitted fabric at 140°C and 0.3 MPa using a dot-matrix hot-melt composite method. After cooling, a waterproof and breathable composite fabric was obtained.

[0050] The composition, by weight, is as follows: 10 parts of triazole betaine silicon modifier, 50 parts of polyethylene glycol, 30 parts of polytetrahydrofuran glycol, 21.4 parts of 4,4'-diphenylmethane diisocyanate, 3.5 parts of 1,4-butanediol, and 0.13 parts of dibutyltin dilaurate.

[0051] Example 4 A method for preparing a waterproof and breathable composite fabric includes the following steps: S1: Under nitrogen protection and anhydrous conditions, 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin were dissolved in anhydrous ethanol. After stirring and dissolving, tetrabutylammonium bromide catalyst was added, and the reaction was stirred at 55°C for 3.5 h. After the reaction was completed, the temperature was lowered to 7.5°C, and sodium hydroxide aqueous solution (mass fraction 25%) was slowly added dropwise. After the addition was complete, stirring was continued for 0.9 h. The mixture was filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was extracted with ethyl acetate and water (volume ratio of ethyl acetate to water 1:1). The organic phase was dried with anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was purified by silica gel column chromatography (eluent was a mixture of ethyl acetate and petroleum ether in a volume ratio of 1:3) to obtain triazolyl glycidylamine.

[0052] The molar ratio of 1-allyl-1H-1,2,4-triazol-3-amine to epichlorohydrin is 1:1.24; the amount of tetrabutylammonium bromide used accounts for 4.3% of the mass of 1-allyl-1H-1,2,4-triazol-3-amine; the ratio of anhydrous ethanol to the total mass of 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin is 9 mL:1 g; and the molar ratio of sodium hydroxide to 1-allyl-1H-1,2,4-triazol-3-amine is 1.15:1.

[0053] S2: Under nitrogen protection, triazole glycidylamine was dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium was added, and the mixture was stirred at 21°C for 7 hours. After the reaction was completed, most of the solvent was removed by vacuum distillation. The residue was precipitated with acetone, filtered, and the filter cake was washed three times with acetone and dried under vacuum to obtain sulfobetaine triazole.

[0054] The molar ratio of triazole glycidylamine to (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 1:1.15, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of triazole glycidylamine and (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 11 mL:1 g.

[0055] S3: Under nitrogen protection, sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol were dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, potassium carbonate catalyst was added, and the mixture was stirred at 75°C for 9 hours. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the solvent was removed by vacuum distillation. The residue was extracted with ethyl acetate and water (ethyl acetate to water volume ratio of 1:1). The organic phase was dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation. The residue was purified by silica gel column chromatography (eluent was a 1:1 volume mixture of ethyl acetate and petroleum ether) to obtain oxazoline long-chain triazole.

[0056] The molar ratio of sulfobetaine triazole to 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 1:1.4, the amount of potassium carbonate used accounts for 8.8% of the mass of 2-heptadecyl-4-methyl-2-oxazoline-4-methanol, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 11 mL:1 g.

[0057] S4: Under nitrogen protection, oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane were dissolved in anhydrous toluene. After stirring and dissolving, Karstedt platinum catalyst was added, and the reaction was stirred at 95°C for 9 hours. After the reaction was completed, the mixture was cooled to room temperature, and the solvent was removed by vacuum distillation. The residue was precipitated with methanol, filtered, and the filter cake was washed three times with methanol and dried under vacuum to obtain triazole betaine silicon modifier.

[0058] The molar ratio of oxazoline long-chain triazole to monohydrogen-terminated polydimethylsiloxane is 1:1.15, the amount of Karstedt platinum catalyst is 0.025% of the mass of monohydrogen-terminated polydimethylsiloxane, and the ratio of anhydrous toluene to the total mass of oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane is 11 mL:1 g.

[0059] S5: Under nitrogen protection, triazole betaine silica modifier, polyethylene glycol, and 4,4'-diphenylmethane diisocyanate were added to a reactor in a specific ratio and stirred at 88°C for 1.8 h to obtain a modified isocyanate prepolymer component. Polytetrahydrofuran glycol and chain extender 1,4-butanediol were mixed in a specific ratio to obtain a polyol component. The polyol component was mixed with the catalyst dibutyltin dilaurate, and then the modified isocyanate prepolymer component was added. The mixture was stirred at 850 rpm for 4.5 min, with the temperature controlled at 95°C, and mixed evenly. The mixture was then coated onto a release film with a coating thickness of 0.22 mm and cured at 110°C for 3 min. The release film was then peeled off to obtain a modified TPU waterproof and breathable membrane. The modified TPU waterproof and breathable membrane was then hot-pressed with nylon elastic knitted fabric at 140°C and 0.3 MPa through dot-matrix hot-melt bonding. After cooling, a waterproof and breathable composite fabric was obtained.

[0060] The composition, by weight, is as follows: 11 parts of triazole betaine silicon modifier, 55 parts of polyethylene glycol, 35 parts of polytetrahydrofuran glycol, 25.3 parts of 4,4'-diphenylmethane diisocyanate, 4.3 parts of 1,4-butanediol, and 0.16 parts of dibutyltin dilaurate.

[0061] Example 5 A method for preparing a waterproof and breathable composite fabric includes the following steps: S1: Under nitrogen protection and anhydrous conditions, 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin were dissolved in anhydrous ethanol. After stirring and dissolving, tetrabutylammonium bromide catalyst was added, and the reaction was stirred at 60°C for 4 hours. After the reaction was completed, the temperature was lowered to 10°C, and sodium hydroxide aqueous solution (mass fraction 25%) was slowly added dropwise. After the addition was complete, stirring was continued for 1 hour. The mixture was filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was extracted with ethyl acetate and water (volume ratio of ethyl acetate to water 1:1). The organic phase was dried with anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation of the filtrate. The residue was purified by silica gel column chromatography (eluent was a mixture of ethyl acetate and petroleum ether in a volume ratio of 1:3) to obtain triazolyl glycidylamine.

[0062] The molar ratio of 1-allyl-1H-1,2,4-triazol-3-amine to epichlorohydrin is 1:1.3; the amount of tetrabutylammonium bromide used accounts for 5% of the mass of 1-allyl-1H-1,2,4-triazol-3-amine; the ratio of anhydrous ethanol to the total mass of 1-allyl-1H-1,2,4-triazol-3-amine and epichlorohydrin is 10 mL:1 g; and the molar ratio of sodium hydroxide to 1-allyl-1H-1,2,4-triazol-3-amine is 1.2:1.

[0063] S2: Under nitrogen protection, triazole glycidylamine was dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium was added, and the reaction was stirred at 25°C for 8 hours. After the reaction was completed, most of the solvent was removed by vacuum distillation. The residue was precipitated with acetone, filtered, and the filter cake was washed three times with acetone and dried under vacuum to obtain sulfobetaine triazole.

[0064] The molar ratio of triazole glycidylamine to (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 1:1.2, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of triazole glycidylamine and (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 12mL:1g.

[0065] S3: Under nitrogen protection, sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol were dissolved in anhydrous N,N-dimethylformamide. After stirring and dissolving, potassium carbonate catalyst was added, and the mixture was stirred at 80°C for 10 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the solvent was removed by vacuum distillation. The residue was extracted with ethyl acetate and water (ethyl acetate to water volume ratio of 1:1). The organic phase was dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation. The residue was purified by silica gel column chromatography (eluent was a 1:1 volume mixture of ethyl acetate and petroleum ether) to obtain oxazoline long-chain triazole.

[0066] The molar ratio of sulfobetaine triazole to 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 1:1.5, the amount of potassium carbonate used accounts for 10% of the mass of 2-heptadecyl-4-methyl-2-oxazoline-4-methanol, and the mass ratio of anhydrous N,N-dimethylformamide to the total mass of sulfobetaine triazole and 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 12 mL:1 g.

[0067] S4: Under nitrogen protection, oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane were dissolved in anhydrous toluene. After stirring and dissolving, Karstedt platinum catalyst was added, and the reaction was carried out at 100℃ for 10 h. After the reaction was completed, the mixture was cooled to room temperature, the solvent was removed by vacuum distillation, the residue was precipitated with methanol, filtered, the filter cake was washed three times with methanol, and dried under vacuum to obtain triazole betaine silicon modifier.

[0068] The molar ratio of oxazoline long-chain triazole to monohydrogen-terminated polydimethylsiloxane is 1:1.2, the amount of Karstedt platinum catalyst is 0.03% of the mass of monohydrogen-terminated polydimethylsiloxane, and the mass ratio of anhydrous toluene to the total mass of oxazoline long-chain triazole and monohydrogen-terminated polydimethylsiloxane is 12 mL:1 g.

[0069] S5: Under nitrogen protection, triazole betaine silica modifier, polyethylene glycol, and 4,4'-diphenylmethane diisocyanate were added to a reactor in a specific ratio and stirred at 90°C for 2 hours to obtain a modified isocyanate prepolymer component. Polytetrahydrofuran glycol and chain extender 1,4-butanediol were mixed in a specific ratio to obtain a polyol component. The polyol component was mixed with the catalyst dibutyltin dilaurate, and then the modified isocyanate prepolymer component was added. The mixture was stirred at 900 rpm for 5 minutes, with the temperature controlled at 100°C, until uniformly mixed. The mixture was then coated onto a release film with a coating thickness of 0.22 mm and cured at 110°C for 3 minutes. The release film was then peeled off to obtain a modified TPU waterproof and breathable membrane. The modified TPU waterproof and breathable membrane was then hot-pressed with nylon elastic knitted fabric at 140°C and 0.3 MPa using a dot-matrix hot-melt composite method. After cooling, a waterproof and breathable composite fabric was obtained.

[0070] The composition, by weight, includes 12 parts of triazole betaine silicon modifier, 60 parts of polyethylene glycol, 40 parts of polytetrahydrofuran glycol, 29.1 parts of 4,4'-diphenylmethane diisocyanate, 5 parts of 1,4-butanediol, and 0.2 parts of dibutyltin dilaurate.

[0071] Comparative Example 1 The difference between this comparative example and Example 1 is that no triazole betaine silicon modifier is added in S5, while the remaining steps are the same as in Example 1.

[0072] Experimental Example 1 The waterproof and breathable composite fabrics obtained in Examples 1-5 and Comparative Example 1 were subjected to the following performance tests, and the test results are shown in Table 1.

[0073] (1) Static pressure resistance: Refer to GB / T 4744-2013 standard to test the static pressure resistance value.

[0074] (2) Moisture permeability: The moisture permeability was tested at 38℃ and 90%RH in accordance with GB / T 12704.1-2009 standard.

[0075] (3) Tensile strength: The tensile strength was tested in accordance with GB / T 3923.1-2013 standard.

[0076] (4) Hydrolysis resistance: According to GB / T 7141-2008 standard, the sample was aged at 80℃ and 95% relative humidity for 500h, and the tensile strength retention rate was tested.

[0077] (5) Low temperature toughness: According to GB / T 4744-2013 standard, the hydrostatic pressure retention rate was tested after the sample was bent 100 times at -40℃.

[0078] (6) Creep resistance: The creep deformation rate was tested for 100h at 80℃ and 10MPa stress, in accordance with GB / T 11546.1-2008 standard.

[0079] (7) Antistatic properties: Surface resistivity was tested in accordance with GB / T 31838.2-2019 standard.

[0080] (8) Weather resistance: The tensile strength retention rate was tested after UV aging for 500 hours in accordance with GB / T 16422.3-2022 standard.

[0081] (9) Wear resistance: Refer to GB / T 21196.2-2007 standard to test the hydrostatic pressure retention rate after 1000 friction cycles.

[0082] (10) Fatigue resistance: According to GB / T 3923.1-2013 standard, the hydrostatic pressure retention rate was tested after the sample was repeatedly stretched 1000 times (stretch rate 10%).

[0083] (11) Long-term performance: According to GB / T 8629-2017 standard, the hydrostatic pressure retention rate and moisture permeability retention rate were tested after 20 water washes.

[0084] Table 1 As shown in Table 1, the performance of Examples 1-5 is superior to that of Comparative Example 1. Regarding waterproofing and breathability, Examples 1-5 exhibit higher hydrostatic pressure resistance and breathability than Comparative Example 1, indicating that the modifier of this invention can simultaneously improve the waterproofing and breathability of the material. Regarding mechanical properties and durability, Examples 1-5 show higher tensile strength, tensile strength retention rate after damp heat aging, tensile strength retention rate after UV aging, hydrostatic pressure retention rate after friction, hydrostatic pressure retention rate after repeated stretching, and hydrostatic pressure and breathability retention rates after washing than Comparative Example 1, indicating that the modifier of this invention can effectively improve the mechanical properties, hydrolysis resistance, weather resistance, wear resistance, fatigue resistance, and long-lasting performance of the material. Regarding low temperature and creep resistance, Examples 1-5 show higher hydrostatic pressure retention rate after bending at -40℃ and lower creep deformation rate at 80℃ than Comparative Example 1, indicating that the modifier of this invention can effectively improve the low-temperature toughness and creep resistance of the material. Regarding antistatic properties, the surface resistivity of Examples 1-5 was lower than that of Comparative Example 1, indicating that the modifier of the present invention can effectively improve the antistatic properties of the material. The above results demonstrate that the waterproof and breathable composite fabric prepared by the present invention exhibits improvements in waterproofness, moisture permeability, hydrolysis resistance, low-temperature toughness, creep resistance, antistatic properties, weather resistance, abrasion resistance, fatigue resistance, and longevity.

[0085] The descriptions of the above embodiments are merely illustrative of the methods and core ideas of the present invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a waterproof and breathable composite fabric, characterized in that, Includes the following steps: S1: 1-Allyl-1H-1,2,4-triazol-3-amine is reacted with epichlorohydrin in the presence of a catalyst to open the ring, and then the ring is closed under alkaline conditions to obtain triazolyl glycidylamine. S2: Triazole glycidylamine is reacted with (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium via an aza-Michael addition reaction to give sulfobetaine triazole; S3: The sulfobetaine triazole is subjected to a ring-opening etherification reaction with 2-heptadecyl-4-methyl-2-oxazoline-4-methanol in the presence of a catalyst to obtain oxazoline long-chain triazole; S4: Oxazoline long-chain triazole is reacted with monohydrogen-terminated polydimethylsiloxane in the presence of a platinum catalyst to obtain triazole betaine silicon modifier. S5: Triazole betaine silica modifier, polyethylene glycol and 4,4'-diphenylmethane diisocyanate are prepolymerized in the presence of a catalyst to obtain a modified isocyanate prepolymer component; polytetrahydrofuran glycol and chain extender are mixed to obtain a polyol component; the polyol component is mixed and reacted with the modified isocyanate prepolymer component to form a film to obtain a modified TPU waterproof and breathable membrane; A waterproof and breathable composite fabric is obtained by bonding a modified TPU waterproof and breathable membrane with a nylon elastic knitted fabric using dot-matrix hot melt adhesive.

2. The method for preparing a waterproof and breathable composite fabric according to claim 1, characterized in that, The molar ratio of 1-allyl-1H-1,2,4-triazol-3-amine to epichlorohydrin is 1:1.05–1.

3. The catalyst for the ring-opening reaction in S1 is tetrabutylammonium bromide, the alkaline condition is an aqueous sodium hydroxide solution, the amount of tetrabutylammonium bromide is 2%–5% of the mass of 1-allyl-1H-1,2,4-triazol-3-amine, and the molar ratio of sodium hydroxide to 1-allyl-1H-1,2,4-triazol-3-amine is 1.0–1.2:

1.

3. The method for preparing a waterproof and breathable composite fabric according to claim 1, characterized in that, The molar ratio of triazole glycidylamine to (3-(methylvinylamide)propyl)dimethyl-(3-sulfonic acid)ammonium is 1:1.0 to 1.

2.

4. The method for preparing a waterproof and breathable composite fabric according to claim 1, characterized in that, The molar ratio of sulfobetaine triazole to 2-heptadecyl-4-methyl-2-oxazoline-4-methanol is 1:1.1 to 1.

5. The catalyst for the ring-opening etherification reaction in S3 is potassium carbonate, and the amount of potassium carbonate used accounts for 5% to 10% of the mass of 2-heptadecyl-4-methyl-2-oxazoline-4-methanol.

5. The method for preparing a waterproof and breathable composite fabric according to claim 1, characterized in that, The molar ratio of oxazoline long-chain triazole to monohydrogen-terminated polydimethylsiloxane is 1:1.0 to 1.

2. The platinum catalyst in S4 is the Karstedt platinum catalyst, and the amount of Karstedt platinum catalyst accounts for 0.01% to 0.03% of the mass of monohydrogen-terminated polydimethylsiloxane.

6. The method for preparing a waterproof and breathable composite fabric according to claim 1, characterized in that, By weight, the components are: 8-12 parts of triazole betaine silicon modifier, 40-60 parts of polyethylene glycol, 20-40 parts of polytetrahydrofuran glycol, 13.7-29.1 parts of 4,4'-diphenylmethane diisocyanate, 2-5 parts of chain extender, and 1,4-butanediol.

7. The method for preparing a waterproof and breathable composite fabric according to claim 1, characterized in that, In S1, the ring-opening reaction temperature is 40–60℃ and the time is 2–4 h; the ring-closing reaction temperature is 0–10℃ and the time is 0.5–1 h; in S2, the aza-Michael addition reaction temperature is 10–25℃ and the time is 4–8 h.

8. The method for preparing a waterproof and breathable composite fabric according to claim 1, characterized in that, The ring-opening etherification reaction in S3 is carried out at a temperature of 60–80 °C for 6–10 h; the hydrosilylation reaction in S4 is carried out at a temperature of 80–100 °C for 6–10 h.

9. The method for preparing a waterproof and breathable composite fabric according to claim 1, characterized in that, The prepolymerization reaction temperature in S5 is 80–90℃, and the time is 1–2 h; the mixing reaction temperature is 80–100℃, the stirring speed is 700–900 rpm, and the time is 3–5 min.

10. A waterproof and breathable composite fabric, characterized in that, Waterproof and breathable composite fabric is prepared by the preparation method described in any one of claims 1 to 9.