A functional leather preparation method based on laser micro-hole structure

By using ultraviolet laser layer etching technology to prepare a four-layer structure in leather, the problems of controlling light transmittance, breathability and hand feel of existing leather have been solved. This has enabled the preparation of leather with high light transmittance, high breathability and soft light effect, which is suitable for products such as car interior ambient lighting and seats.

CN123153290APending Publication Date: 2026-11-24SUZHOU GREENTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611266580.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing leathers are difficult to precisely control in terms of light transmittance, breathability, and feel. Chemical foaming causes VOC release and pore wall hardening, while mechanical punching causes edge chipping and reduced strength, making it impossible to achieve light-transmitting zones and gradient soft light effects.

Method used

A four-layer structure leather is prepared on a modified blended fabric base layer using ultraviolet laser layer etching technology. The leather includes a base coating of buffer silicone rubber, a middle coating of light-shielding and light-softening composite layer, and a top coating of wear-resistant matte silicone resin. Through the partitioned arrangement of micropores and co-vulcanization, a three-dimensional labyrinth design is formed, with blind holes in the base coating, semi-through holes in the middle coating, and fully through holes in the top coating, avoiding chemical foaming and thermal processing.

Benefits of technology

It achieves precise zoned control of light transmittance, breathability, and feel, reduces VOC emissions, improves the abrasion resistance and tear resistance of leather, meets automotive standards, and is suitable for mass production of multiple product categories.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153290A_ABST
    Figure CN123153290A_ABST
Patent Text Reader

Abstract

This invention relates to the field of functional leather technology and discloses a method for preparing functional leather based on laser microporous structure. This method comprises, from bottom to top, a modified blended base fabric layer, a base coating of buffer silicone rubber, a middle coating of light-shielding and light-softening composite layer, and a top coating of wear-resistant matte silicone resin layer. The four layers are co-vulcanized and bonded together to form a bubble-free preform. All light-transmitting and breathable micropores in the leather body are formed by layer-by-layer etching with ultraviolet laser, eliminating chemically foamed pores. This allows for simultaneous application of solid high-gloss logos, gradient soft light effects, and light-shielding coverage on a single fabric. Combined with a three-dimensional labyrinth design of through-holes in the top layer, semi-transparent in the middle layer, and blind holes in the bottom layer, it ensures high breathability and moisture permeability while solving the problems of dust accumulation and glare associated with straight pores. Simultaneously, 355nm ultraviolet chemical etching avoids carbonization and hardening of the pore walls caused by heat burns, preserving the skin-friendly feel and tear resistance of silicone leather.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional leather technology, specifically to a method for preparing functional leather based on laser microporous structures. Background Technology

[0002] Artificial leather is made by foaming or coating various formulations of PVC and PU onto a woven or non-woven fabric base. It can be processed according to different requirements for strength, color, gloss, and patterns. It has the characteristics of a wide variety of colors and patterns, good waterproof performance, neat edges, high utilization rate, and relatively low price compared to genuine leather. However, most artificial leathers cannot achieve the same feel and elasticity as genuine leather. Its cross-section shows tiny air bubbles, a thin film on the fabric base or surface, and dry artificial fibers.

[0003] Existing leather is produced through chemical internal foaming, resulting in disordered cell structure, difficulty in precise parameter control, large fluctuations in light transmittance, and the easy release of VOCs from residual auxiliaries. It is also impossible to achieve light transmission zone separation, and moisture can easily penetrate, causing the base fabric to mold. Furthermore, when using mechanical steel molds for punching, it can cause edge chipping, fiber breakage, and a sharp drop in the strength of the punched area. After bending, it is easy to tear and enlarge the holes. The fixed hole arrangement makes it impossible to achieve gradual soft light, and it is prone to dust accumulation and glare.

[0004] Furthermore, existing laser drilling methods result in hardened hole walls due to melting, leading to a poorer feel; they can only penetrate a single layer and cannot achieve differentiated micropores in the top, middle, and bottom layers, making it impossible to control air permeability and light transmission in different zones. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing functional leather based on laser microporous structure, so as to solve the problems mentioned in the background art.

[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for preparing functional leather based on laser microporous structure, comprising, from bottom to top, a modified blended base fabric layer, a base coating buffer silicone rubber layer, a middle coating light-shielding and light-softening composite layer, and a top coating wear-resistant matte silicone resin layer; The four layers are co-vulcanized and sealed together to form a bubble-free blank. All the light-transmitting and breathable micropores of the leather body are formed by ultraviolet laser layer etching, and there are no chemically foamed pores. The micropores are divided into three types of staggered arrangement: blind pores in the base coating, semi-through pores in the intermediate coating, and fully through pores in the top coating; the base fabric has a basis weight of 110 to 135 g / m².

[0007] Preferably, the thickness of the primer buffer silicone rubber layer is 0.22 to 0.32 mm, the depth of the blind hole is approximately 0.17 mm thick and the pore diameter is 12 to 25 μm; the thickness of the intermediate coating soft light composite layer is 0.18 to 0.27 mm, the semi-through hole penetrates the intermediate coating and ends at the upper surface of the primer, and the pore diameter is 8 to 18 μm; the thickness of the topcoat layer is 0.08 to 0.14 mm, the fully through hole connects the topcoat and intermediate coating, and the pore diameter is 5 to 12 μm; and the base fabric is a 65% polyester and 35% nylon blended needle-punched nonwoven fabric.

[0008] Preferably, the weight proportions of each layer of slurry are as follows: Primer slurry: 55 parts vinyl silicone resin, 16 parts methyl phenyl silicone oil, 9 parts modified aluminum hydroxide, 4.2 parts hydrogen-containing crosslinking agent, 0.25 parts platinum catalyst, 7 parts nano-silica, and 1.8 parts leveling agent; Intermediate coating slurry: 62 parts methyl silicone resin, 12 parts low-viscosity vinyl silicone oil, 6 parts silica powder, nano... 3.5 parts, crosslinking agent 3.8 parts, platinum catalyst 0.2 parts, wetting agent 1.5 parts; Topcoat slurry: 68 parts high-hardness silicone resin, 9 parts short-chain silicone oil, 5 parts montmorillonite, 6 parts wear-resistant silica powder, 3.2 parts crosslinking agent, 0.18 parts platinum catalyst, and 2.2 parts matting additive; the entire formula contains no chemical foaming agents.

[0009] Preferably, it includes the following steps: S1: Plasma activation pretreatment of the base fabric; S2: Three layers of silicone resin slurry are applied by a three-stage scraper and pre-baked at low temperature in stages; S3: Gradient heating and overall co-vulcanization to produce bubble-free, dense, integrated raw leather; S4: The blank is fixed by vacuum adsorption using an ultraviolet cold laser, and three-level micropores are etched by laser etching in layers and sections. S5: Low-temperature setting and embossing are followed by post-processing to obtain the finished product.

[0010] Preferably, the S3 vulcanization process consists of a first stage of holding at 135°C for 7 minutes and a second stage of holding at 172°C for 14 minutes, with no foaming process throughout; the S4 laser is a 355nm nanosecond ultraviolet cold laser with a single pulse energy of 0.2 to 0.4mJ, which is a non-contact cold processing and non-thermal carbonization.

[0011] Preferably, in step S4, the micropores are arranged in zones: the micropore density in the area corresponding to the ambient light is 450 to 700 pores / cm², and the micropore density in the non-transparent covering area is 80 to 220 pores / cm², so as to achieve gradual soft light by relying on the pore density.

[0012] Compared with the prior art, the beneficial effects achieved by the present invention are: First, this invention replaces traditional chemical foaming and physical punching with ultraviolet laser cold processing, enabling precise zoned control of light, air, and touch. The aperture and arrangement can be freely defined through CAD programming. The density of through holes on the upper layer of a single fabric decreases radially, achieving a brightness transition from high brightness in the center to soft light at the edges. Combined with a three-dimensional labyrinth design of through holes in the top layer, semi-transparent in the middle layer, and blind holes in the bottom layer, it not only ensures high air permeability and moisture permeability but also solves the problems of dust easily entering and glare caused by straight holes. At the same time, 355nm ultraviolet chemical etching avoids carbonization and hardening of the pore walls caused by heat burns, preserving the skin-friendly feel and bending and tear resistance of silicone leather.

[0013] Secondly, this invention eliminates the risk of additive precipitation through post-laser perforation, reducing VOC to below 8μg / g and stably achieving V0 flame retardancy, meeting automotive standards. The post-laser perforation process eliminates interface defects between foam layers, preventing cracking and delamination in extremely cold or hot environments. The yield of mass-produced products is improved compared to chemical foaming, and multiple types of products suitable for ambient lighting, seats, or dashboards can be produced from the same raw leather by simply adjusting the laser program, reducing usage costs. Attached Figure Description

[0014] Figure 1 This is a schematic diagram of the layered structure of the present invention.

[0015] The coating consists of: 1. Modified blended base fabric layer; 2. Base coating buffer silicone rubber layer; 3. Intermediate coating light-shielding and light-softening composite layer; 4. Top coating wear-resistant matte silicone resin layer. Detailed Implementation

[0016] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0017] Please see Figure 1 A method for preparing functional leather based on laser microporous structure includes, from bottom to top, a modified blended base fabric layer, a base coating buffer silicone rubber layer, a middle coating light-shielding and light-softening composite layer, and a top coating wear-resistant matte silicone resin layer; the four layers are co-vulcanized and sealed to form a bubble-free preform; all light-transmitting and breathable micropores in the leather body are formed by ultraviolet laser layer etching, and there are no chemically foamed pores; the micropores are divided into three types of staggered arrangement: base coating blind pores, middle coating semi-through pores, and top coating fully through pores; the base fabric is a 65% polyester and 35% nylon blended needle-punched nonwoven fabric with a basis weight of 110 to 135 g / m².

[0018] The cooled and shaped dense raw leather is laid flat on a vacuum adsorption laser platform under a negative pressure of -0.07MPa to prevent deformation during drilling. A 355nm ultraviolet nanosecond cold laser with a wavelength of 355nm and a single pulse energy of 0.2 to 0.4mJ is used. Drilling is performed layer by layer and section by section according to the preset CAD dot matrix drawing. The laser is used for non-contact cold processing without thermal melting or carbonization, resulting in smooth hole walls without burrs. The drilling is carried out in three steps. Full-through-hole processing of top coating: The laser focuses on the top coating, penetrates the top coating and intermediate coating, and stops at the upper surface of the base coating to generate a fully through-hole; Semi-through hole processing in intermediate coating: Adjust the laser focal length to move it down, only etch the intermediate coating layer, and the depth stops at the surface of the primer coating to form a semi-through micropore, which is arranged 30 to 80 μm off from the micropores in the top coating. Blind hole processing in the base coating: Fine-tune the laser focus again, and etch the inside of the base coating at a fixed point. The depth of the blind hole is 60% to 75% of the thickness of the base coating, preferably 0.15 to 0.19 mm, without penetrating the base coating, to form a moisture-retaining blind hole in the bottom layer. Zoned control: The ambient light corresponding area is densely perforated, the central control logo position is hollowed out with micro-perforations according to the pattern, and the side covering area is sparsely perforated. A single roll of leather can achieve differentiated light transmission and breathability in multiple areas. Base fabric pretreatment: After dust removal, the base fabric is subjected to argon plasma corona treatment, a thin adhesive layer is rolled and pre-baked at 85℃ for 1.5 min; Layered coating: Apply three layers of slurry in sequence with a scraper: primer, intermediate coat and top coat. The coating speed is 7-9 m / min. Each layer is pre-baked in sections: primer 95℃×2.2min, intermediate coat 105℃×2min, top coat 110℃×1.8min. Overall co-vulcanization: Gradual vulcanization of raw leather, holding at 135℃ for 7 min and at 172℃ for 14 min, to obtain dense, bubble-free, integrated raw leather; Ultraviolet laser layered drilling: The raw leather is fixed by vacuum adsorption, and the 355nm nanosecond ultraviolet laser is used to etch holes in different areas; the hole density in the ambient light area is 450~700 holes / cm², and the hole density in the covering area is 80~220 holes / cm². The top coating through holes, the intermediate coating semi-through holes, and the bottom coating blind holes are processed in sequence. Post-processing: Set at 115℃ for 3 minutes, then emboss and slit to obtain the finished product; Dust penetration rate test method: Take a 10cm×10cm sample and clamp it in a differential pressure fixture (ISO12103-1A2 dust source, 0–80μm, median diameter). (≈10μm), 2.0g of ash was added upstream, and suction was maintained at ΔP=500Pa for 10min. The mass of ash on the back of the sample, m_back, was weighed, and the ash penetration rate was defined as m_back / 2.0g×100%. The ash penetration rate of the example was ≤1.2%; the ash penetration rate of the single-layer straight hole control on the market was 7.5-9.0%, that is, the ash penetration rate increased by about 7 times, and the ash penetration rate increased from 1.2% to 8.7%, which is a relative increase of about 7.3 times.

[0019] Example 1 In this embodiment: the base fabric is a 120g / ㎡ polyester-nylon blended needle-punched fabric; plasma corona treatment is performed at 120W; the three-layer slurry is prepared according to the above ratio; the coating speed is 8m / min; the segmented pre-drying parameters are executed according to S2; vulcanization: 135℃ for 7min → 172℃ for 14min, resulting in a bubble-free, dense raw leather; laser parameters: 355nm ultraviolet laser; lamp area pore density 620 pores / cm², pore diameter 9~14μm; side coating area 130 pores / cm², pore diameter 6~9μm; bottom coating blind hole pore diameter 18μm, pore spacing 1.2mm; Actual measured data of finished product: light transmittance 39%, V0 flame retardant rating, breathable 3250g / kg VOC 7.2mg / kg, yellowing resistance grade 4.5, abrasion resistance 6800 times, soft and uniform light without glare, and no holes or tears when bent and wrapped.

[0020] Comparative Example 1 Silicone leather of the same thickness, chemically foamed, with the same light transmittance of 38% and breathability of 3500g / m². However, the light transmittance of the same rolled leather fluctuates by 11%, and it cannot adjust the light in local areas. After long-term aging at 60℃, the VOC increases to 12.5μg / g.

[0021] Comparative Example 2 The commercially available single-layer 355nm laser-drilled silicone leather of the same material has the same overall thickness as this invention. However, it only has full-through holes on one side, which means that light transmission cannot be divided into zones, there is obvious glare, and the gray transmittance rate increases from 1.2% to 8.7%, which is about 7.3 times higher. After bending, the tear strength at the drilled area decreases by 28%, which is used to highlight the advantages of the three-dimensional labyrinth hole of this invention.

[0022] Example 2 In this embodiment: the base fabric is a 130g / ㎡ polyester-nylon blended nonwoven fabric, treated with 120W argon plasma corona treatment, and each coating slurry is prepared according to the proportions in claim 3; the coating speed is 7m / min, and the pre-baking is done in stages: base coat 95℃×2.2min, intermediate coat 105℃×2min, top coat 110℃×1.8min; the vulcanization process is 135℃×7min and 172℃×14min.

[0023] Laser processing: The main seat area has a pore density of 380 pores / cm², with a pore diameter of 7–13 μm; the seat edging has sparse perforations of 110 pores / cm², with a pore diameter of 5–8 μm; the base coating has blind perforations with a pore diameter of 15 μm and a pore spacing of 1.5 mm. Finished product performance: Light transmittance 31%, flame retardancy V0, moisture permeability 3320 g / cm². VOC 7.5μg / g, yellowing resistance grade 4.5, abrasion resistance 6600 cycles, excellent breathability, no stuffiness or sweating even after sitting for a long time.

[0024] Example 3 In this embodiment: the base fabric is a blended needle-punched fabric of 110g / ㎡, and a thin adhesive layer is applied after plasma pretreatment; the ratio of the three-layer slurry remains unchanged, the coating speed is 9m / min, and the pre-drying and vulcanization parameters are the same as in Example 2.

[0025] Laser processing: The main body of the instrument panel has a hole density of 95 holes / cm², with a hole diameter of 5-7μm. Only the ambient light strip has a localized density of 520 holes / cm², with a hole diameter of 8-12μm. The base coating has a blind hole diameter of 13μm and a hole spacing of 1.8mm. Finished product performance: Overall light transmittance 24%, flame retardancy V0, moisture permeability 2050g / cm². VOC 6.9μg / g, weather resistant and sun resistant, not easy to yellow, excellent coating and shaping effect; All the above properties were measured according to industry standards: VOC according to VDA278, detection limit 0.1μg / g, TVOC summation report; flame retardancy according to FMVSS302 / UL94V-0 vertical burning, sample 100×50mm; abrasion resistance according to Taber5135, CS-10 wheel, 1000g load; moisture permeability according to ASTME96-16MethodB; yellowing resistance according to ISO105-B06, xenon lamp 72.

[0026] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0027] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A functional leather based on laser microporous structure, characterized in that: From bottom to top, it consists of a modified blended fabric base layer, a base coating buffer silicone rubber layer, a middle coating light-shielding and light-softening composite layer, and a top coating wear-resistant matte silicone resin layer. The four layers are co-vulcanized and sealed together to form a bubble-free blank. All the light-transmitting and breathable micropores of the leather body are formed by ultraviolet laser layer etching, and there are no chemically foamed pores. The micropores are divided into three types of staggered arrangement: blind pores in the base coating, semi-through pores in the intermediate coating, and fully through pores in the top coating; the base fabric has a basis weight of 110 to 135 g / m².

2. The functional leather based on laser microporous structure according to claim 1, characterized in that: The thickness of the primer buffer silicone rubber layer is 0.22 to 0.32 mm, and the depth of the blind holes is approximately 0.17 mm for the primer layer and 12 to 25 μm for the hole diameter. The thickness of the intermediate coating soft light composite layer is 0.18 to 0.27 mm, and the semi-through holes penetrate the intermediate coating and stop at the upper surface of the primer layer, with a hole diameter of 8 to 18 μm. The thickness of the topcoat layer is 0.08 to 0.14 mm, and the fully through holes connect the topcoat and intermediate coating, with a hole diameter of 5 to 12 μm. The base fabric is a needle-punched nonwoven fabric blended with 65% polyester and 35% nylon.

3. The functional leather based on laser microporous structure according to claim 1, characterized in that: The formulations of each layer of slurry, by weight, are as follows: Primer slurry: 55 parts vinyl silicone resin, 16 parts methyl phenyl silicone oil, 9 parts modified aluminum hydroxide, 4.2 parts hydrogen-containing crosslinking agent, 0.25 parts platinum catalyst, 7 parts nano-silica, and 1.8 parts leveling agent; Intermediate coating slurry: 62 parts methyl silicone resin, 12 parts low-viscosity vinyl silicone oil, 6 parts silica powder, nano... 3.5 parts, crosslinking agent 3.8 parts, platinum catalyst 0.2 parts, wetting agent 1.5 parts; Topcoat slurry: 68 parts high-hardness silicone resin, 9 parts short-chain silicone oil, 5 parts montmorillonite, 6 parts wear-resistant silica powder, 3.2 parts crosslinking agent, 0.18 parts platinum catalyst, and 2.2 parts matting additive; The entire formula contains no chemical foaming agents.

4. A method for preparing functional leather with a laser-embedded microporous structure as described in any one of claims 1 to 3, characterized in that, Includes the following steps: S1: Plasma activation pretreatment of the base fabric; S2: Three layers of silicone resin slurry are applied by a three-stage scraper and pre-baked at low temperature in stages; S3: Gradient heating and overall co-vulcanization to produce bubble-free, dense, integrated raw leather; S4: The blank is fixed by vacuum adsorption using an ultraviolet cold laser, and three-level micropores are etched by laser etching in layers and sections. S5: Low-temperature setting and embossing are followed by post-processing to obtain the finished product.

5. The method for preparing functional leather with laser-embedded microporous structure according to claim 4, characterized in that: The S3 vulcanization process consists of a first stage of holding at 135°C for 7 minutes and a second stage of holding at 172°C for 14 minutes, with no foaming process throughout. The S4 laser is a 355nm nanosecond ultraviolet cold laser with a single pulse energy of 0.2 to 0.4mJ, which is a non-contact cold processing process with no thermal carbonization.

6. The method for preparing functional leather with laser-embedded microporous structure according to claim 4, characterized in that: In step S4, the micropores are arranged in zones: the micropore density in the area corresponding to the ambient light is 450 to 700 pores / cm², and the density in the non-transparent area is 80 to 220 pores / cm², so as to achieve gradual soft light by relying on the pore density.