An inkjet printing ink, a preparation method and application thereof

By using thiourea dioxide (TDO) to replace traditional reducing agents and optimizing the formulation and potential control, the stability and printing effect problems of inkjet printing inks have been solved, achieving long-term stability and excellent printing performance of inks at high concentrations.

CN123153291APending Publication Date: 2026-11-24WEIXINGLAN (JIANGSU) NEW MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202611361651.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing inkjet printing inks have poor stability at high concentrations and are prone to oxidation, leading to printhead clogging. Furthermore, traditional reducing agents such as sodium hydrosulfite have insufficient stability, affecting printing results.

Method used

Using thiourea dioxide (TDO) as an environmentally friendly and stable reducing agent, and optimizing the ratio of dyes and auxiliaries and the oxidation-reduction potential (ORP), a high-concentration and high-stability inkjet printing ink system is formed, avoiding premature oxidation and aggregation of dyes.

Benefits of technology

It achieves long-term stability of inkjet printing inks during formulation, storage and printing processes, ensuring smooth printing and deep color of patterns, and obtaining good fastness performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This application relates to an inkjet printing ink, its preparation method, and its application. The ink comprises, by weight percentage: 1-15% vat dye, 1-10% thiourea dioxide, 0.5-5% alkali, 1-8% dispersant, 10-45% viscosity modifier, 0.1-3% surfactant, 0.01-1% pH adjuster, and the balance being water. This invention, by optimizing the reduction system and using thiourea dioxide as the reducing agent, combined with specific auxiliary agent ratios and pH control, solves the problems of traditional vat inkjet printing inks, such as easy oxidation at high concentrations, particle agglomeration, printhead clogging, poor stability, and insufficient color fastness. It also exhibits good inkjet stability, storage stability, and printability. After printing, the ink develops color through oxidation, resulting in good pattern depth and excellent dry and wet rubbing fastness. It is suitable for digital inkjet printing on fabrics such as cotton and polyester.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of digital printing technology, specifically relating to an inkjet printing ink, its preparation method, and its application. Background Technology

[0002] Vat dyes, with their excellent colorfastness, vibrant colors, and good lightfastness, play an important role in the dyeing of cellulosic fibers. Traditional vat dyeing processes require reducing the dye to a soluble leuco form under strong alkaline conditions and reducing agents, followed by oxidation to develop the color after dyeing the fiber. However, high-concentration vat dye solutions are highly susceptible to oxidation upon contact with air, forming insoluble particles that lead to instability in the ink system and easily clog the precision printheads of inkjet printers. Furthermore, sodium hydrosulfite reduction systems exhibit poor stability, with rapid performance degradation during storage and printing.

[0003] Several ink patents for inkjet printing already exist in the prior art. For example, CN115538198A discloses an antibacterial digital printing direct-to-garment ink, which imparts antibacterial properties by adding graphene quantum dots. However, it mainly targets disperse dye systems and does not solve the fundamental stability problem of vat dyes in inkjet applications. CN114892422A relates to a smokeless, high-penetration ink that reduces smoke by mixing pigments with different sublimation temperatures, but it belongs to a thermal sublimation transfer system, which differs from the redox color development mechanism of vat dyes. CN118048071A provides a waterproof thermal sublimation ink for uncoated paper, focusing on resin modification and waterproofing. CN103450740A discloses a thermal sublimation ink formulation for industrial printheads, but its core is still the thermal transfer application of disperse dyes.

[0004] Therefore, developing a reduction inkjet printing ink that can adapt to the inkjet printing environment, maintain excellent dispersion stability at high concentrations, and achieve normal oxidation and color development and good fastness after printing has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] To address the aforementioned technical problems, this application provides an inkjet printing ink, its preparation method, and its application. The inkjet printing ink provided in this application utilizes thiourea dioxide (TDO) as an environmentally friendly and stable reducing agent, and optimizes the dye, auxiliary agent ratio, and oxidation-reduction potential (ORP), achieving high concentration and high stability of vat dyes in the inkjet ink system. This results in a smooth printing process, good color depth, and high fastness.

[0006] To achieve this objective, the following technical solution is adopted in this application: In a first aspect, this application provides an inkjet printing ink, which comprises the following components in weight percentage: 1-15% vat dye, 1-10% thiourea dioxide, 0.5-5% alkali agent, 1-8% dispersant, 10-45% viscosity modifier, 0.1-3% surfactant, 0.01-1% pH adjuster, and the balance being water.

[0007] The inkjet printing ink provided in this application uses TDO instead of traditional sodium hydrosulfite as a reducing agent. TDO has a mild and stable reduction potential, with a standard potential of -1100 mV vs SCE. Its decomposition products are urea and sulfate, which are non-polluting. This allows the ink to maintain a stable reduced state for a long time during the preparation, storage and printing process, effectively avoiding the problem of printhead clogging caused by premature oxidation and aggregation of dyes.

[0008] In some embodiments, with the total mass of the inkjet printing ink being 100%, the mass percentage of the vat dye is 1-15%, for example, it can be 1%, 3%, 5%, 6%, 8%, 10%, 12% or 15%, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0009] In some embodiments, the TDO mass percentage is 1-10% based on the total mass of the inkjet printing ink as 100%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, and specific point values ​​between the above point values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0010] In some embodiments, based on the total mass of the inkjet printing ink as 100%, the mass percentage of the alkali agent is 0.5-5%, for example, it can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0011] In some embodiments, the mass percentage of the dispersant is 1-8%, based on the total mass of the inkjet printing ink as 100%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7% or 8%, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0012] In some embodiments, the viscosity modifier has a mass percentage content of 10-45% based on the total mass of the inkjet printing ink as 100%, for example, it can be 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0013] In some embodiments, the surfactant content is 0.1-3% by mass, based on the total mass of the inkjet printing ink as 100%. For example, it can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0014] In some embodiments, based on the total mass of the inkjet printing ink as 100%, the mass percentage of the pH adjuster is 0.01-1%, for example, it can be 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0015] In some embodiments, the mass ratio of the vat dye to thiourea dioxide is 1:(0.5-2), where "0.5-2" can be, for example, 0.5, 0.8, 1, 1.2, 1.5, 1.8 or 2, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0016] In this application, insufficient TDO will lead to incomplete reduction, while excessive TDO will lead to over-reduction or increased side reactions.

[0017] In some embodiments, the vat dye includes any one or a combination of at least two of indole, pyridine, or anthraquinone vat dyes.

[0018] In some embodiments, the indole-based vat dyes include indigo and / or 6,6'-dibromoindigo.

[0019] In some embodiments, the pyridine-based vat dyes include sapphire blue and / or N-acetylglucosamine blue.

[0020] In some embodiments, the anthraquinone vat dyes include any one or a combination of at least two of Vat Blue 4, Vat Yellow GCN, or Vat Red FBB.

[0021] In some embodiments, the alkaline agent includes any one or a combination of at least two of sodium hydroxide, sodium carbonate, or potassium carbonate.

[0022] In some embodiments, the alkaline agent is a mixture of sodium hydroxide and sodium carbonate in a mass ratio of (1-3):1, where "1-3" can be, for example, 1, 1.5, 2, 2.5, or 3, and specific values ​​between these ranges. For space limitations and for the sake of brevity, this application will not exhaustively list all the specific values ​​included in the range. Sodium hydroxide provides a strongly alkaline environment to promote reduction, while sodium carbonate acts as a buffer to stabilize the pH.

[0023] In some embodiments, the mass ratio of the dispersant to the vat dye is (0.5-1.5):1, where "0.5-1.5" can be, for example, 0.5, 0.8, 1, 1.2 or 1.5, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0024] In some embodiments, the dispersant comprises any one or a combination of at least two of sodium lignosulfonate or acrylic polymer dispersants.

[0025] In some embodiments, the acrylic polymer dispersant comprises sodium polyacrylate and / or sodium salt of acrylic-maleic anhydride copolymer.

[0026] In some embodiments, the preferred total mass percentage of the viscosity modifier is 20-35%, for example, it can be 20%, 25%, 30% or 35%, and specific values ​​between the above points. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0027] In some embodiments, the viscosity modifier includes any one or a combination of at least two of ethylene glycol, glycerol, diethylene glycol, sorbitol, or polyethylene glycol.

[0028] In some embodiments, the surfactant comprises any one or a combination of at least two of acetylenic diol nonionic surfactants or fatty acid polyoxyethylene esters, preferably 2,4,7,9-tetramethyl-5-decyn-4,7-diol and / or polyoxyethylene sorbitan fatty acid esters.

[0029] In some embodiments, the oxidation-reduction potential of the inkjet printing ink is -600 mV to -850 mV, for example, it can be -600 mV, -650 mV, -700 mV, -800 mV or -850 mV, as well as specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0030] In this application, a mild redox potential effectively maintains the dissolved state of the leuco dye and prevents premature oxidation.

[0031] In some embodiments, the pH adjuster includes any one or a combination of at least two of the following: a sodium dihydrogen phosphate-disodium hydrogen phosphate buffer system, a borax-sodium hydroxide buffer system, monoethanolamine, or diethanolamine.

[0032] In some embodiments, the concentrations of sodium dihydrogen phosphate and disodium hydrogen phosphate in the aqueous solution of the sodium dihydrogen phosphate-disodium hydrogen phosphate buffer system are 0.1-0.5 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0033] In some embodiments, the concentrations of borax and sodium hydroxide in the aqueous solution of the borax-sodium hydroxide buffer system are 0.05-0.2 mol / L, for example, 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, or 0.2 mol / L, as well as specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list all the specific values ​​included in the range.

[0034] In some embodiments, the monoethanolamine or diethanolamine is added in the form of pure product or aqueous solution, wherein the mass fraction of the aqueous solution is 10%-30%, for example, it can be 10%, 15%, 20%, 25% or 30%, and specific values ​​between the above points. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0035] In this application, the pH adjuster is mainly used to fine-tune the pH of the system, and the alkali agent provides the main alkaline environment.

[0036] Secondly, this application provides a method for preparing the inkjet printing ink described in the first aspect, comprising the following steps: (1) Preparation of reducing solution: Mix vat dye, thiourea dioxide, dispersant and water, add alkali and mix to obtain reducing solution; (2) Preparation of inkjet printing ink: Add humectant, viscosity modifier, surfactant, pH modifier and the remaining water to the reducing solution, mix and obtain the inkjet printing ink.

[0037] In some embodiments, the reduction temperature for mixing the vat dye, thiourea dioxide, dispersant, and water in step (1) is 60-75°C, for example, 60°C, 65°C, 70°C, or 75°C, and specific values ​​between these values. For space limitations and for the sake of brevity, this application will not exhaustively list all the specific values ​​included in the range. The mixing time is 20-40 minutes, for example, 20, 25, 30, 35, or 40 minutes, and specific values ​​between these values. For space limitations and for the sake of brevity, this application will not exhaustively list all the specific values ​​included in the range.

[0038] In some embodiments, the mixing time for adding the alkali agent in step (1) is 30-60 minutes, for example, it can be 30, 35, 40, 45, 50, 55 or 60 minutes, and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific values ​​included in the range.

[0039] Thirdly, this application provides a textile inkjet printing method, which uses the inkjet printing ink provided in the first aspect to print textile patterns.

[0040] The textile inkjet printing method provided in this application involves loading ink into an inkjet printer and printing directly onto fabrics such as cotton. The printed leuco pattern undergoes natural oxidation in the air for 2-12 hours or is treated with an oxidizing agent such as a 0.5-3% hydrogen peroxide solution for 10-30 minutes, rapidly developing the original dye color. Finally, the excess dye is removed by washing with water and soaping, resulting in a printed fabric with a bright pattern and excellent fastness. Here, "2-12" can be, for example, 2, 4, 6, 8, 10, or 12; "0.5-3" can be, for example, 0.5, 1, 1.5, 2, 2.5, or 3; and "10-30" can be, for example, 10, 15, 20, 25, or 30. The numerical ranges mentioned include not only the values ​​listed above but also any values ​​within the ranges not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list all the specific values ​​included in the ranges.

[0041] Compared with the prior art, this application has at least the following beneficial effects: 1. Excellent stability: TDO is used instead of traditional sodium hydrosulfite as a reducing agent. TDO has a mild and stable reduction potential, with a standard potential of -1100 mV vs SCE. Its decomposition products are urea and sulfate, which are non-polluting. This allows the ink to maintain a stable reduced state for a long time during the preparation, storage and printing process. It can also be prepared and used immediately, and the method is simple.

[0042] 2. Optimized formulation system: By precisely controlling the ratio of TDO to dye, and combining it with a composite alkali agent of NaOH and Na2CO3, the rheological properties of inkjet printing ink are not only adjusted to achieve a viscosity of 5-12 mPa•s and a surface tension of 28-35 mN / m, but also meet the jetting requirements of industrial inkjet printheads.

[0043] 3. Wide applicability to dyes: The formulation system provided in this application is applicable to a variety of vat dyes such as indigo and anthraquinone. By adjusting the amount of TDO and the ratio of alkali, stable leuco inks can be obtained, and the color depth and fastness meet the requirements of industrial applications.

[0044] 4. Excellent performance for use: After oxidation and water washing to fix the color, the printed pattern exhibits good dry and wet rubbing fastness, meeting the requirements for textile use. Detailed Implementation

[0045] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0046] Unless otherwise specified, the raw materials involved in the following specific embodiments of this application are all conventional materials in the art, and can be purchased from commercially available products. Some raw material information is as follows: The indigo (CI Vat Blue 1, CAS 482-89-3) used in Examples 1-14 and Comparative Examples 1-6 was purchased from Zhejiang Longsheng Group Co., Ltd.; the reduced yellow GCN (CI Vat Yellow 2, CAS 129-09-9) was purchased from Zhejiang Runtu Co., Ltd.; and the indigoidine (CAS 2435-59-8, molecular formula C) was purchased from Zhejiang Runtu Co., Ltd. 10 H8N4O4) is a biosynthesized natural blue pigment, purchased from Nanjing Hegu Life Biotechnology Co., Ltd.; the reduced blue 4 (CI Vat Blue 4, CAS81-77-6) was purchased from Jiangsu Changzhou Yabang Group Co., Ltd. The N-acetyl indigoidine (molecular formula C8N4O4) is also present. 12 H 10 N4O5 was provided by Nanjing Hegu Life Biotechnology Co., Ltd., and can be prepared using the method described in patent CN120905108A. The structure of N-acetylglucosamine is shown in formula (I): Formula (I).

[0047] Example 1 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: Blue violet extract: 12.0 g (6%) TDO: 10.0 g (5%) Sodium hydroxide: 3.0 g (1.5%) Sodium carbonate: 1.0 g (0.5%) Sodium lignosulfonate: 10 g (5%) Ethylene glycol: 8.0 g (4%) Glycerol: 20.0 g (10%) Polyethylene glycol 400: 12.0 g (6%) 2,4,7,9-Tetramethyl-5-decyn-4,7-diol: 0.4 g (0.2%) Sodium dihydrogen phosphate-disodium hydrogen phosphate buffer (0.3 mol / L): 1.0 g (0.5%) Deionized water: Add to a total weight of 200 g The preparation method includes the following steps: (1) Preparation of reducing solution: Add vat dyes Blue, TDO, sodium lignosulfonate and 60 mL of water to a 1 L high-pressure reactor. Stir at 65 °C and 500 rpm for 30 minutes. Add sodium hydroxide and sodium carbonate (pre-dissolved in 5 times their mass of water), and continue stirring for 45 minutes. The solution becomes a clear blue-gray reduced state, and the reducing solution is obtained.

[0048] (2) Preparation of inkjet printing ink: Add ethylene glycol, glycerol, polyethylene glycol 400, 2,4,7,9-tetramethyl-5-decyn-4,7-diol and the remaining water to the reducing solution, stir and mix evenly at room temperature, add sodium dihydrogen phosphate-disodium hydrogen phosphate buffer (0.3 mol / L) and stir evenly to obtain the inkjet printing ink.

[0049] Example 2 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: N-acetylglucosamine: 10.0 g (5%) TDO: 8.0 g (4%) Sodium hydroxide: 3.0 g (1.5%) Sodium salt of acrylic acid-maleic anhydride copolymer: 5.0 g (2.5%) Diethylene glycol: 20.0 g (10%) Polyethylene glycol 600: 20.0 g (10%) Polyoxyethylene sorbitan fatty acid ester (Tween 80): 0.6 g (0.3%) Borax-sodium hydroxide buffer (0.1 mol / L): 1.0 g (0.5%) Deionized water: Add to a total weight of 200 g The preparation method differs from Example 1 only in that the reduction temperature is 75°C and the mixing time for adding the alkali is 20 minutes; the remaining steps are the same as in Example 1.

[0050] Example 3 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: Reduced Yellow GCN: 16.0 g (8%) TDO: 8.0 g (4%) Sodium hydroxide: 4.0 g (2%) Sodium carbonate: 2.0 g (1%) Sodium lignosulfonate: 8.0 g (4%) Diethylene glycol: 15.0 g (7.5%) Sorbitol: 15.0 g (7.5%) 2,4,7,9-Tetramethyl-5-decyn-4,7-diol: 0.8 g (0.4%) Monoethanolamine 30% aqueous solution: 1.0 g (0.5%) Deionized water: Add to a total weight of 200 g The preparation method differs from that of Example 1 only in that the reduction temperature is 60°C and the mixing time with the alkali is 40 minutes. The remaining steps are the same as those in Example 1.

[0051] Example 4 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: Indigo: 20.0 g (10%) TDO: 16.0 g (8%) Sodium hydroxide: 3.0 g (1.5%) Sodium carbonate: 3.0 g (1.5%) Sodium polyacrylate: 10.0 g (5%) Ethylene glycol: 12.0 g (6%) Glycerol: 18.0 g (9%) Polyethylene glycol 400: 10.0 g (5%) Polyoxyethylene sorbitan fatty acid ester: 1.0 g (0.5%) Sodium dihydrogen phosphate-disodium hydrogen phosphate buffer (0.5 mol / L): 0.02 g (0.01%) Deionized water: Add to a total weight of 200 g The preparation method differs from Example 1 only in that the reduction temperature is 72°C, and the mixing time with alkali is extended to 50 minutes due to the difficulty of reducing indigo. The remaining steps are the same as in Example 1.

[0052] Example 5 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: 6,6'-Dibromoindigo: 30.0 g (15%) TDO: 20.0 g (10%) Sodium hydroxide: 10.0 g (5%) A mixture of sodium lignosulfonate and sodium salt of acrylic acid-maleic anhydride copolymer (mass ratio 1:1): 16.0 g (8%) Glycerol: 50.0 g (25%) Polyethylene glycol 600: 40.0 g (20%) 2,4,7,9-Tetramethyl-5-decyn-4,7-diol and polyoxyethylene sorbitan fatty acid ester mixture (mass ratio 1:1): 6.0 g (3%) Diethanolamine 20% aqueous solution: 2.0 g (1%) Deionized water: Add to a total weight of 200 g.

[0053] The preparation method differs from Example 1 only in that the reduction temperature is 75°C and the mixing time with the alkali is 60 minutes; the remaining steps are the same as in Example 1.

[0054] Example 6 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: Reduced Blue 4: 2.0 g (1%) TDO: 2.0 g (1%) Sodium hydroxide: 1.0 g (0.5%) Sodium lignosulfonate: 2.0 g (1%) Ethylene glycol: 10.0 g (5%) Glycerol: 10.0 g (5%) 2,4,7,9-Tetramethyl-5-decyn-4,7-diol: 0.2 g (0.1%) Sodium dihydrogen phosphate-disodium hydrogen phosphate buffer (0.1 mol / L): 2.0 g (1%) Deionized water: Add to a total weight of 200 g The preparation method is the same as in Example 1.

[0055] Example 7 This embodiment provides an inkjet printing ink, which differs from Example 1 only in that: 12.0 g of vat dye indigo is replaced with a mixture of 6.0 g of indigo and 6.0 g of vat dye indigo, and the TDO dosage is adjusted to 12.0 g (6%) to fully reduce the two dyes. The remaining components and preparation method are the same as in Example 1.

[0056] Example 8 This embodiment provides an inkjet printing ink, which differs from Example 1 only in that: 4.0 g of sodium hydroxide and 2.0 g of sodium carbonate are replaced with 6.0 g of sodium carbonate, the total alkali content remains unchanged, a weak alkali system is provided, the amount of TDO is increased to 12.0 g, and the remaining components and preparation method are the same as in Example 1.

[0057] Example 9 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: Blue-eyed blue: 10 g (5%) TDO: 20 g (10%) Sodium hydroxide: 4.0 g (2%) Sodium lignosulfonate: 5.0 g (2.5%) Ethylene glycol: 40.0 g (20%) Polyethylene glycol 400: 30.0 g (15%) 2,4,7,9-Tetramethyl-5-decyn-4,7-diol: 1.0 g (0.5%) Diethanolamine 10% aqueous solution: 2.0 g (1%) Deionized water: Add to a total weight of 200 g The preparation method is the same as in Example 1.

[0058] Example 10 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: Blue Spectrum: 10.0 g (5%) TDO: 10.0 g (5%) Sodium hydroxide: 5.0 g (2.5%) Sodium lignosulfonate: 15.0 g (7.5%) Ethylene glycol: 40.0 g (20%) Sorbitol: 10.0 g (5%) 2,4,7,9-Tetramethyl-5-decyn-4,7-diol: 1.0 g (0.5%) Borax-sodium hydroxide buffer (0.2 mol / L): 0.06 g (0.03%) Deionized water: Add to a total weight of 200 g The preparation method is the same as in Example 1.

[0059] Example 11 This embodiment provides an inkjet printing ink, which comprises the following components by weight percentage: Blue violet extract: 12.0 g (6%) TDO: 10.0 g (5%) Sodium hydroxide: 4.0 g (2%) Sodium carbonate: 2.0 g (1%) Sodium lignosulfonate: 4.0 g (2%) Ethylene glycol: 22.0 g (11%) Glycerol: 28.0 g (14%) Polyethylene glycol 400: 20.0 g (10%) 2,4,7,9-Tetramethyl-5-decyn-4,7-diol: 3.0 g (1.5%) Borax-sodium hydroxide buffer (0.05 mol / L): 2.0 g (1%) Deionized water: Add to a total weight of 200 g The preparation method is the same as in Example 1.

[0060] Example 12 This embodiment provides an inkjet printing ink, which differs from Example 6 only in the use of 5.0 g of Vapor Blue 4. The remaining components and preparation method are the same as in Example 6.

[0061] Example 13 This embodiment provides an inkjet printing ink, which differs from Example 6 only in that it uses 5.0 g TDO, while the remaining components and preparation method are the same as in Example 6.

[0062] Example 14 This embodiment provides an inkjet printing ink, which differs from Example 6 only in that it uses 4.0 g of sodium lignosulfonate; the remaining components and preparation method are the same as in Example 6.

[0063] Comparative Example 1 This comparative example provides an inkjet printing ink, which differs from Example 1 only in that: 10.0 g of TDO is replaced with 12.0 g (6%) of sodium dithionite (sodium hydrosulfite), and the alkali is adjusted to 4.0 g (2%) of sodium hydroxide and 2.0 g (1%) of sodium carbonate. The remaining components and preparation method are the same as in Example 1.

[0064] Preparation method: Due to the poor stability of sodium hydrosulfite, it needs to be prepared under nitrogen protection.

[0065] Comparative Example 2 This comparative example provides an inkjet printing ink, which differs from Example 1 only in that the amount of TDO is reduced to 1.0 g (0.5%), while the other components and preparation method are the same as in Example 1.

[0066] Comparative Example 3 This comparative example provides an inkjet printing ink, which differs from Example 1 only in that the amount of TDO is increased to 30.0 g (15%), while the other components and preparation method are the same as in Example 1.

[0067] Comparative Example 4 This comparative example provides an inkjet printing ink, which differs from Example 1 only in that sodium lignosulfonate (0% dispersant) is not added, while the other components and preparation method are the same as in Example 1.

[0068] Comparative Example 5 This comparative example provides an inkjet printing ink, which differs from Example 1 only in that it does not contain 2,4,7,9-tetramethyl-5-decyn-4,7-diol (0% surfactant), while the other components and preparation method are the same as in Example 1.

[0069] Comparative Example 6 This comparative example provides an inkjet printing ink, which differs from Example 1 only in that: the alkali is 8.0 g (4%) sodium hydroxide and 4.0 g (2%) sodium carbonate, the total alkali content is 6%, the pH is adjusted to 11.5, and the remaining components and preparation method are the same as in Example 1.

[0070] Test case The inks prepared in Examples 1-14 and Comparative Examples 1-6 were subjected to performance tests, and the test methods are as follows: 1. Initial state: refers to the appearance of the ink obtained after step (2). Visually observe whether it is clear and whether there is any sediment.

[0071] 2. Viscosity: Measured using a rotational viscometer (Brookfield DV2T, 25℃, 100 rpm), unit mPa•s.

[0072] 3. Surface tension: Measured using a surface tension meter (Krüss K100, hanging plate method, 25℃), unit mN / m.

[0073] 4. Oxidation-reduction potential (ORP): Directly measured using an ORP meter (Mettler Toledo Seven Excellence, 25℃), unit mV.

[0074] 5. Stability test: Store in a sealed container at room temperature away from light.

[0075] 6. Print Test: Load ink into the inkjet printer and print at approximately 30 m... 2 The inkjet print is performed at a printing speed of / h, directly onto the cotton fabric. The printed leuco pattern is left to stand in the air for 10 minutes to allow natural oxidation and color development. It is then fixed at 95℃ for 10 minutes, followed by two washes with water to remove unfixed dyes and residual auxiliaries. Finally, it is soaped with a soaping solution of 2 g / L soap flakes and 1 g / L soda ash at 60℃ for 10 minutes to thoroughly remove any loose dye. It can then be air-dried.

[0076] The dried fabric was tested for performance using the following methods: Color depth (K / S value) and L value: Measured using a spectrophotometer (Datacolor 650) under a D65 light source and a 10° viewing angle. The K / S value is calculated according to the Kubelka-Munk formula; a higher K / S value indicates a deeper color depth. The L value is the lightness index of the CIE Lab color space, where L=0 represents pure black and L=100 represents pure white. A lower L value indicates a deeper color and better color depth. K / S and L values ​​are negatively correlated, and they characterize color depth from different perspectives.

[0077] Dry and wet rubbing fastness: According to GB / T 3920-2008 "Textiles - Tests for color fastness - Color fastness to rubbing", a dry rubbing fastness of grade 4 is excellent, and grade 3-4 is good; a wet rubbing fastness of grade 3 is excellent, and grade 2-3 is good.

[0078] Table 1 The ink prepared in Example 1 exhibits excellent printing smoothness, a color depth L value of 26.8, a dry rubbing fastness of grade 4, and a wet rubbing fastness of grade 3. After being stored at room temperature away from light for 3 months, the ORP remains above -750 mV, with no precipitation and no degradation in printing performance.

[0079] The ink prepared in Example 2 printed smoothly, with an L value of 28.5 after oxidation. Its color depth was superior to the L value of 32.1 in Example 1. It exhibited a dry rubbing fastness of grade 4 and a wet rubbing fastness of grade 3. No precipitation occurred, and the ORP decrease was <50 mV.

[0080] The ink prepared in Example 3, after printing on cotton fabric, showed a bright yellow color upon oxidation, with a K / S value of 12.5, a dry rubbing fastness of 3-4, and a wet rubbing fastness of 2-3.

[0081] Example 4: The ink turns dark blue after oxidation, with an L value of 25.3, indicating excellent color depth. It has a dry rubbing fastness of grade 4 and a wet rubbing fastness of grade 3.

[0082] Example 5: After oxidation, the ink has an L value of 22.6, excellent color depth, dry rubbing fastness grade 4, and wet rubbing fastness grade 3.

[0083] Example 6: The ink prints smoothly, producing a light bluish-gray pattern. After being exposed to air for 8 hours or sprayed with a 1% hydrogen peroxide solution for 15 minutes, the pattern oxidizes to a dark blue. After soaping, the ink sample tested showed a dry rubbing fastness of grade 3 and a wet rubbing fastness of grade 2. After standing for one day, it could still print normally, with the ORP remaining above -680 mV.

[0084] The inkjet printing ink provided in Example 7 is a clear green color that is a mixture of yellow-green and blue-gray. After oxidation, it turns into a deep blue color, combining the vividness of indigo with the fastness of blue. It has a dry rubbing fastness of grade 4 and a wet rubbing fastness of grade 3.

[0085] The inkjet printing ink provided in Example 8 has an ORP-760 mV viscosity of 9.2 mPa•s. Printing tests show that it takes 12 hours to fully oxidize in air, which is a slow oxidation rate but has better stability.

[0086] Within two hours of preparing the ink provided in Comparative Example 1, the ink became cloudy and developed particulate sediment, with the ORP rapidly dropping from -800mV to -400mV. When tested in a printer, printouts stopped after 5 minutes of continuous printing, and inspection of the printhead revealed blue particles clogging it.

[0087] After adding alkali and stirring for 60 minutes, the ink prepared in Comparative Example 2 was still turbid and contained unreduced dye particles.

[0088] The finished ink of Comparative Example 3 had an ORP as low as -950 mV. Excessive reduction caused damage to the dye structure, and the color depth decreased after oxidation, with an L value of 38.5. It also produced an off-odor from urea decomposition products.

[0089] In Comparative Example 4, dye aggregation was obvious during the reduction process, the solution was semi-transparent, and contained a large number of fine particles. Although the supernatant could be filtered after centrifugation, frequent line breaks occurred during printing, and dye deposits were found at the printhead.

[0090] The surface tension of the ink obtained in Comparative Example 5 was too high at 48 mN / m, and after 30 minutes of standby in the printer, printhead drying caused breakage holes, resulting in poor printing smoothness.

[0091] Comparative Example 6: The inkjet printing ink had an initial ORP of -850 mV and a pH of 11.5. The strong alkalinity caused partial hydrolysis of the viscosity modifier PEG400. After 7 days, the viscosity increased from 8.8 to 15.2 mPa•s. The viscosity was unstable and there was a risk of corrosion to the inkjet printhead.

[0092] The test results above show that the ink system based on TDO reduction in this application exhibits high stability, reliable printing and cleaning, and high dry / wet rubbing fastness. Furthermore, the proportions of each component and process parameters must be strictly controlled within the scope of the claims. The absence of any key component or deviation from the parameters will lead to a significant decrease in performance. Specifically: Examples 1-7 show that the ink is applicable to a variety of vat dyes such as indigo and anthraquinone. By adjusting the amount of TDO and the ratio of alkali, stable leuco inks can be obtained, and the color depth and fastness meet the requirements for industrial applications.

[0093] Examples 6 and 12-14 show that when the proportion of vat dye is high, insufficient TDO leads to insufficient reduction, while when the proportion of TDO is high, the dye is over-reduced. Furthermore, when the ratio of dispersant to vat dye is less than 0.5:1, the vat dye is not sufficiently dispersed, ink particles easily agglomerate, and ink lines break during printing. When the ratio of dispersant to vat dye is greater than 1.5:1, viscosity increases and surface tension decreases, easily causing ink splattering and ink leakage.

[0094] Comparative Example 1 shows that the ink system based on TDO reduction is significantly superior to the traditional sodium hydrosulfite system in terms of stability, printing reliability, color depth and fastness.

[0095] Comparative Examples 2-3 show that if the TDO content in the ink is too low, the reduction is insufficient; if the TDO content is too high, the reduction is excessive and side reactions occur.

[0096] Comparative Example 4 shows that without a dispersant, ink particles tend to agglomerate, making line breaks more likely.

[0097] Comparative Example 5 shows that printing smoothness is worse without surfactants.

[0098] Comparative Example 6 shows that strong alkalinity causes partial hydrolysis of the viscosity modifier PEG400, resulting in viscosity instability.

[0099] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. An inkjet printing ink, characterized in that, The inkjet printing ink comprises the following components by weight percentage: 1-15% vat dye, 1-10% thiourea dioxide, 0.5-5% alkali agent, 1-8% dispersant, 10-45% viscosity modifier, 0.1-3% surfactant, 0.01-1% pH adjuster, and the balance being water.

2. The inkjet printing ink as described in claim 1, characterized in that, The mass ratio of the vat dye to thiourea dioxide is 1:(0.5-2); And / or, the vat dye includes any one or a combination of at least two of indole, pyridine, or anthraquinone vat dyes; And / or, the indole-based vat dyes include indigo and / or 6,6'-dibromoindigo; And / or, the pyridine-based vat dyes include Vibranium and / or N-acetylenol; And / or, the anthraquinone vat dyes include any one or a combination of at least two of Vat Blue 4, Vat Yellow GCN, or Vat Red FBB.

3. The inkjet printing ink as described in claim 1 or 2, characterized in that, The alkaline agent includes any one or a combination of at least two of sodium hydroxide, sodium carbonate, or potassium carbonate. And / or, the alkaline agent is a mixture of sodium hydroxide and sodium carbonate in a mass ratio of (1-3):

1.

4. The inkjet printing ink as described in any one of claims 1-3, characterized in that, The mass ratio of the dispersant to the vat dye is (0.5-1.5):1; And / or, the dispersant comprises any one or a combination of at least two of sodium lignosulfonate or acrylic polymer dispersants; And / or, the acrylic polymer dispersant includes sodium polyacrylate and / or sodium salt of acrylic-maleic anhydride copolymer.

5. The inkjet printing ink according to any one of claims 1-4, characterized in that, The viscosity modifier includes any one or a combination of at least two of ethylene glycol, glycerol, diethylene glycol, sorbitol, or polyethylene glycol; And / or, the surfactant comprises any one or a combination of at least two of acetylenic diol nonionic surfactants or fatty acid polyoxyethylene esters, preferably 2,4,7,9-tetramethyl-5-decyn-4,7-diol and / or polyoxyethylene sorbitan fatty acid esters. And / or, the oxidation-reduction potential of the inkjet printing ink is -600 mV to -850 mV.

6. The inkjet printing ink according to any one of claims 1-5, characterized in that, The pH adjuster includes any one or a combination of at least two of the following: sodium dihydrogen phosphate-disodium hydrogen phosphate buffer system, borax-sodium hydroxide buffer system, monoethanolamine or diethanolamine.

7. The inkjet printing ink according to any one of claims 1-6, characterized in that, In the sodium dihydrogen phosphate-disodium hydrogen phosphate buffer system, the concentrations of sodium dihydrogen phosphate and disodium hydrogen phosphate in the aqueous solution are 0.1-0.5 mol / L; And / or, in the borax-sodium hydroxide buffer system, the concentration of borax and sodium hydroxide in the aqueous solution is 0.05-0.2 mol / L; And / or, the monoethanolamine or diethanolamine is added in the form of pure product or aqueous solution, wherein the aqueous solution has a mass fraction of 10%-30%.

8. A method for preparing inkjet printing ink as described in any one of claims 1-7, characterized in that, The preparation method includes the following steps: (1) Preparation of reducing solution: Mix vat dye, thiourea dioxide, dispersant and water, add alkali and mix to obtain reducing solution; (2) Preparation of inkjet printing ink: Add humectant, viscosity modifier, surfactant, pH modifier and the remaining water to the reducing solution, mix and obtain the inkjet printing ink.

9. The preparation method according to claim 8, characterized in that, In step (1), the reduction temperature for mixing the vat dye, thiourea dioxide, dispersant and water is 60-75℃, and the mixing time is 20-40 minutes. And / or, the mixing time for adding the alkali agent in step (1) is 30-60 minutes.

10. A method for inkjet printing textiles, characterized in that, Textile patterns are printed using inkjet printing ink as described in any one of claims 1-7.

Citation Information

Patent Citations

  • Sublimation ink-jetting ink used for industrial nozzle and manufacturing method thereof

    CN103450740A

  • Smoke-free or less-smoke high-strength permeable ink and preparation method thereof

    CN114892422A

  • Antibacterial digital printing direct-injection ink and preparation method thereof

    CN115538198A

  • Preparation method of water-based waterproof thermal sublimation ink for uncoated paper

    CN118048071A

  • Genetic engineering strain for improving settleability of N-acetyl blue product as well as construction method and application of genetic engineering strain

    CN120905108A