A three-dimensional printed fabric, a forming process and a slurry

By employing a progressively smaller printing layer and sizing layer structure in 3D printed fabrics, the problem of poor smoothness in the side transition of 3D printing is solved, resulting in a 3D print with a gradually narrowing shape, which improves the stability and smoothness of the print.

CN123153293APending Publication Date: 2026-11-24FUJIAN HUAFENG NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611538301.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies have poor side transition smoothness in 3D printing, making it difficult to form a 3D print with a gradually narrowing shape, and the sides of the print are prone to retaining interlayer marks.

Method used

A three-dimensional skeleton structure with at least three progressively smaller printing layers is adopted. The three-dimensional skeleton is formed by sequential drying and stretch printing, and then a stretch layer is covered. Water-based polyurethane stretch paste is used to trim the transition area between adjacent printing layers.

Benefits of technology

It achieves a smooth transition effect on the surface of the 3D printed material, reduces step marks on the sides of the print, and improves the stability and smoothness of the print.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153293A_ABST
    Figure CN123153293A_ABST
Patent Text Reader

Abstract

This invention discloses a three-dimensional printed fabric, molding process, and a paste, relating to the field of shoe upper printing technology. The three-dimensional printed fabric includes a base layer, a three-dimensional skeleton formed by stacking at least three progressively smaller printed layers, and a paste layer covering the transition area between adjacent printed layers. During molding, at least three screens with progressively smaller printed pattern sizes are used. The three-dimensional paste is printed layer by layer on the same printing position on the base fabric in descending order of size. After each printing, the paste is dried, and then the three-dimensional skeleton is paste-printed and dried again. The paste contains an aqueous polyurethane dispersion, fumed silica, a drying inhibitor, and thickening components with different shear responses. This invention combines layered molding with paste covering, which can improve the drying collapse and interlayer step problems of the print, and is suitable for conical three-dimensional printing on fabrics such as shoe uppers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of shoe upper printing technology, specifically to a three-dimensional printing fabric, molding process, and sizing paste. Background Technology

[0002] Currently, in the industry, when creating 3D printing on fabric surfaces such as shoe uppers, the printed pattern can exhibit a raised texture effect. Water-based polyurethane paste can be applied to the base fabric through screen printing and forms a printed layer of a certain thickness after drying. For 3D printing, in addition to creating a certain raised height, it is also necessary to prevent the top from collapsing and to ensure that the sides taper smoothly from the bottom to the top. Therefore, high requirements are placed on the printing and shaping of the paste and the maintenance of its shape after drying.

[0003] Existing processes can increase the thickness of the printed layer by layering paste through multiple screen printing processes. However, simply using the same or similar printed patterns to repeatedly overprint mainly achieves thickness accumulation, making it difficult to form a three-dimensional print with a gradually narrowing shape, and the sides of the print are also prone to retaining interlayer marks. Summary of the Invention

[0004] The technical problem to be solved by this application is to provide a three-dimensional printing fabric, molding process and sizing paste to solve the defect of poor smoothness of side transition in the existing three-dimensional printing.

[0005] To achieve the above objectives, the inventors have provided a technical solution:

[0006] A three-dimensional printed fabric, comprising:

[0007] grassroots level;

[0008] A three-dimensional skeleton is disposed on the base layer and includes at least three printed layers stacked sequentially along the thickness direction of the base layer; in the thickness direction of the base layer, the size of all printed layers decreases layer by layer in the direction away from the base layer;

[0009] A sizing layer that at least covers the transition area formed between adjacent printing layers.

[0010] To achieve the above objectives, the inventors provided a second technical solution:

[0011] A molding process for use in the above-mentioned three-dimensional printed fabric includes the following steps:

[0012] S1: Provide at least three printing screens with the same printing pattern and successively smaller sizes;

[0013] S2: In order of decreasing size of the printed pattern, the printing screens are used sequentially to apply the three-dimensional paste to the same printed pattern on the base fabric, and the paste is dried after each printing to form a three-dimensional skeleton.

[0014] S3: After the printing and drying of the three-dimensional paste are completed, the three-dimensional skeleton is subjected to paste printing and then dried to obtain conical printed fabric.

[0015] To achieve the above objectives, the inventors have provided a third technical solution:

[0016] A sizing agent for use in the above-mentioned three-dimensional printing process, comprising a water-based polyurethane sizing agent for the sizing printing;

[0017] By weight, the waterborne polyurethane slurry comprises: 85-90 parts of waterborne polyurethane dispersion, 1-2 parts of fumed silica, 1-5 parts of drying inhibitor, 1-2 parts of high-shear polyurethane associative thickener, 0.5-1.0 parts of medium-shear polyurethane associative thickener, 0.2-0.6 parts of low-shear thickener, 0.4-0.6 parts of defoamer, 0.5-1.0 parts of dispersant, and 2-4 parts of crosslinking agent.

[0018] Unlike existing technologies, the advantages of the above technical solution are as follows: the three-dimensional skeleton is formed by at least three printing layers with progressively smaller dimensions. The bottom printing layer provides a larger adhesion range for the upper printing layer, and each layer supports the sizing layer. The sizing layer covers the transition area between adjacent printing layers, which helps to reduce exposed steps and forms an outer surface that gradually tapers from the base layer to the top of the printing layer, making the resulting three-dimensional printing surface smooth.

[0019] The above description of the invention is merely an overview of the technical solution of this application. In order to enable those skilled in the art to better understand the technical solution of this application and to implement it based on the description and drawings, and to make the above-mentioned objectives and other objectives, features and advantages of this application easier to understand, the following description is provided in conjunction with the specific embodiments and drawings of this application. Attached Figure Description

[0020] The accompanying drawings are only used to illustrate the principles, implementation methods, applications, features, and effects of specific embodiments of the present invention and other related contents, and should not be considered as limitations on this application.

[0021] In the accompanying drawings of the instruction manual:

[0022] Figure 1 This is a cross-sectional view of the three-dimensional printed fabric in this invention;

[0023] Figure 2 This is a product image of the three-dimensional printed fabric in this invention.

[0024] The reference numerals used in the above figures are explained as follows:

[0025] 1. Base layer; 2. Three-dimensional skeleton; 21. Printing layer; 3. Stamping layer. Detailed Implementation

[0026] To illustrate the possible application scenarios, technical principles, implementable specific solutions, and achievable objectives and effects of this application in detail, the following description, in conjunction with the listed specific embodiments and accompanying drawings, provides a detailed explanation. The embodiments described herein are merely illustrative of the technical solutions of this application and are therefore intended to limit the scope of protection of this application.

[0027] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.

[0028] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.

[0029] In the description of this application, the term "and / or" is used to describe the logical relationship between objects, indicating that three relationships can exist. For example, A and / or B means: A exists, B exists, and A and B exist simultaneously. Additionally, the character " / " in this document generally indicates that the preceding and following objects have an "or" logical relationship.

[0030] In this application, terms such as “first” and “second” are used only to distinguish one entity or operation from another, and do not necessarily require or imply any actual quantity, hierarchy or order relationship between these entities or operations.

[0031] Without further limitations, the use of terms such as “comprising,” “including,” “having,” or other similar open-ended expressions in this application is intended to cover non-exclusive inclusion, which does not exclude the presence of additional elements in a process, method, or product that includes the stated elements, such that a process, method, or product that includes a list of elements may include not only those defined elements but also other elements not expressly listed, or elements inherent to such a process, method, or product.

[0032] In this application, expressions such as "greater than", "less than", and "exceeding" are understood to exclude the stated number; expressions such as "above", "below", and "within" are understood to include the stated number. Furthermore, in the description of the embodiments of this application, "multiple" means two or more (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups" and "multiple times", unless otherwise explicitly specified.

[0033] In the description of the embodiments of this application, the space-related expressions used, such as "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "vertical," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential," indicate the orientation or positional relationship based on the orientation or positional relationship shown in the specific embodiments or drawings. They are only for the purpose of describing the specific embodiments of this application or for the reader's understanding, and do not indicate or imply that the device or component referred to must have a specific position, a specific orientation, or be constructed or operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0034] Unless otherwise expressly specified or limited, the terms "installation," "connection," "linking," "fixing," and "setting," as used in the description of the embodiments of this application, should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral arrangement; it can be a direct connection or an indirect connection through an intermediate medium; it can be a relationship of two components combined together, an interaction relationship between two components, or a connection within two structures. Those skilled in the art to which this application pertains can understand the specific meaning of the above terms in the embodiments of this application according to the specific circumstances.

[0035] Existing processes can increase the thickness of the printed layer by layering paste through multiple screen printing processes. However, simply using the same or similar printed patterns to repeatedly overprint mainly achieves thickness accumulation, making it difficult to form a three-dimensional print with a gradually narrowing shape, and the sides of the print are also prone to retaining interlayer marks.

[0036] Traditional thick plate overprinting can increase the amount of paste buildup through repeated screen printing and successive drying, but the number of printing and drying passes increases with the required thickness. If the coating is continuously thickened along the same contour, the outer edge of the coating is often quite steep, making it difficult to obtain a gradually tapering side. When the coating is too thick, it may also affect the flexibility required for the shoe upper to bend and increase the risk of cracking or peeling.

[0037] When using a slurry-drawing method to directly form high protrusions, the water-based polyurethane slurry will shrink as the moisture evaporates during the drying process after printing. The protrusions that have not yet set are prone to sinking at the top or deformation in shape, affecting the stability of the three-dimensional printing form.

[0038] Specifically, when water and other volatile components escape from waterborne polyurethane wet slurry, capillary action and volume shrinkage may occur inside the wet film. Without the formation of internal support, relying solely on a single slurry application to achieve a high protrusion can easily cause the undried top and sides to change shape under shrinkage and their own weight, resulting in a sunken top, concave sides, or a near-frustum shape; the degree of this change depends on the slurry formulation, application rate, and drying conditions.

[0039] In fabrics such as shoe uppers that require repeated bending, the aforementioned problems also involve support and shape retention during the protrusion molding process: single-layered water-based polyurethane wet paste is prone to drying shrinkage, while simply increasing the thickness layer by layer makes it difficult to adjust the outer contour between layers. This application uses overprinting and subsequent sizing to enable the three-dimensional skeleton to provide support and the sizing layer to provide interlayer transition.

[0040] Reference Figure 1 and Figure 2 A three-dimensional printed fabric, comprising:

[0041] Grassroots level 1;

[0042] The three-dimensional skeleton 2 is disposed on the base layer 1 and includes at least three printed layers 21 stacked sequentially along the thickness direction of the base layer 1; in the thickness direction of the base layer 1, the size of all printed layers 21 decreases layer by layer in the direction away from the base layer 1.

[0043] The sizing layer 3 covers at least the transition area formed between adjacent printing layers 21.

[0044] It is understandable that the printed layers 21 of the three-dimensional skeleton 2 are stacked sequentially. The printed layer 21 closer to the base layer 1 has a larger printing area, which makes the three-dimensional skeleton 2 and the base layer 1 form a larger contact area. The upper printed layer 21 is supported by the already formed lower printed layer 21, which helps to maintain the raised height. The size difference between adjacent printed layers 21 forms an interlayer transition on the outside of the skeleton. After the sizing layer 3 covers this area, the originally visible steps gradually turn into a more continuous surface.

[0045] When each printed layer 21 uses a circular printed pattern with its center overlapping, the outer edges of the printed layers 21 gradually converge towards the center from the direction closest to the base layer 1 to the direction furthest from the base layer 1. In the longitudinal section, a stepped transition is formed between adjacent outer edges, and multiple printed layers 21 together constitute an internal skeleton that approximates a stepped cone. The sizing layer 3 at least covers this stepped transition area and connects adjacent outer edges, thereby changing the outer surface from a gradually receding contour to a more continuous sloping transition.

[0046] When printing water-based polyurethane 3D paste, each printing layer 21 is dried separately before the next printing pass, so that the subsequent wet paste is supported by the already formed printing layer 21, avoiding the concentrated accumulation of paste required to form the entire raised area. The larger size of the bottom printing layer 21 also allows for a larger contact area between the skeleton and the base layer 1, which is beneficial to improving adhesion stability; the bonding and layer-by-layer support between each printing layer helps to reduce the overall collapse caused by drying shrinkage, but the degree of its effect still depends on the materials and process conditions.

[0047] A molding process for use in the above-mentioned three-dimensional printed fabric includes the following steps:

[0048] S1: Provide at least three printing screens with the same printing pattern and successively smaller sizes;

[0049] S2: Following the order of printing pattern size from largest to smallest, each printing screen is used sequentially to apply the three-dimensional printing paste to the same printing pattern on the base fabric, and drying is performed after each printing to form a three-dimensional skeleton;

[0050] S3: After completing the printing and drying of the three-dimensional paste, the three-dimensional skeleton is stretched and printed, and then dried to obtain the conical printed fabric.

[0051] In practice, the shoe material base fabric (base layer 1) is first laid flat on the printing table. Then, each screen is aligned with the same printed pattern on the base fabric according to the printing sequence. Water-based polyurethane 3D printing paste can be used. The first layer is printed with the largest printed pattern. After this layer dries, the next layer is printed with a smaller printed pattern, and so on, until at least three printing screens have completed printing in sequence. Each layer of paste dries before the next printing is performed, allowing subsequent wet paste to be applied to the already formed printed layer.

[0052] When laying the base fabric, the area to be printed should be kept flat, avoiding obvious wrinkles or uneven local tension, so as to reduce the offset of the printed pattern during each printing plate. The printing pattern of each screen should correspond to the same printing pattern of the previous screen, and the subsequent printing layer 21 should fall within the printing area of ​​the previous printing layer 21; in this way, the first larger printing layer 21 can provide support for the subsequent smaller printing layers 21.

[0053] After forming the three-dimensional skeleton 2, a stretch printing process is performed on its outer surface; the stretch printing paste covers the transition area between adjacent printing layers 21 and is dried to form the stretch layer 3.

[0054] Understandably, printing larger printing layers 21 first, followed by smaller printing layers 21, can form a gradually converging three-dimensional skeleton 2 on the base layer 1. Drying each printing pass separately disperses the drying shrinkage of the paste throughout the forming process, reducing the possibility of top collapse due to applying a thick layer of wet paste at once. Applying paste after the three-dimensional skeleton 2 is formed allows for the preservation of layered support while covering the steps between adjacent layers, resulting in a smoother transition on the printed sides.

[0055] In some embodiments, when printing the 3D paste in S2, the printing centers of the printed patterns on the base fabric of each printing screen coincide; in two adjacent printing screens, the printed pattern of the later printing screen is proportionally smaller than the printed pattern of the previous printing screen. In this way, the outer edges of each printed layer can gradually converge around a common center, reducing unevenness on the sides caused by local misalignment, while leaving space for the transition area between subsequent paste layers.

[0056] For example, when the printed pattern is circular, the diameter of the printed pattern on the later screen in an adjacent screen is (1-α) times that of the previous screen, where 0 < α < 10%. For three screens, the largest, middle and smallest printed patterns are used in sequence, and the centers of each layer are kept in registration; this printed pattern relationship is conducive to forming a relatively uniform transition area between adjacent printing layers 21.

[0057] In some embodiments, in step S3, the printing screen with the largest printing pattern size among all printing screens is used to perform 2 to 3 strokes of printing on the three-dimensional skeleton, and drying is performed after each stroke. The strokes are applied in stages so that the paste gradually covers the steps of the three-dimensional skeleton 2. Each stroke is dried before the next stroke is performed, which can reduce the flow when too much wet paste is applied at once, so that the formed strokes can provide support for the next printing, and gradually refine the printed sides.

[0058] In some embodiments, in step S3, the sizing process specifically involves applying sizing paste to the largest printing screen of the printed pattern, and then applying the sizing paste to the outer surface of the three-dimensional skeleton through the printing screen, so that the sizing paste covers the transition area between adjacent printing layers of the three-dimensional skeleton. The largest printing screen can cover the entire printing range of the three-dimensional skeleton 2, which is beneficial for the sizing paste to reach the transition area between each adjacent printing layer 21, avoiding the paste from only thickening at the top of the skeleton; after being transferred by the screen, the paste spreads and stays in the transition area, so that the layered stepped shape gradually becomes a continuously converging shape.

[0059] In the sizing stage, water-based polyurethane sizing paste is first applied to the printing screen with the largest print pattern size, and then squeegeed into the printing area corresponding to the three-dimensional skeleton 2. When the printing screen leaves, the sizing paste, which has a certain degree of viscoelasticity, can be drawn and cover the edges of the printing layers 21 at different heights; subsequently, it spreads between adjacent steps, forming a sloping transition connecting each printing layer 21. Applying the sizing paste in stages and drying it each time gradually covers the interlayer traces still visible from the previous application.

[0060] A stretching paste for use in the above-mentioned 3D printing molding process, wherein the stretching paste is a water-based polyurethane stretching paste;

[0061] By weight, the waterborne polyurethane slurry comprises: 85-90 parts of waterborne polyurethane dispersion, 1-2 parts of fumed silica, 1-5 parts of drying inhibitor, 1-2 parts of high-shear polyurethane associative thickener, 0.5-1.0 parts of medium-shear polyurethane associative thickener, 0.2-0.6 parts of low-shear thickener, 0.4-0.6 parts of defoamer, 0.5-1.0 parts of dispersant, and 2-4 parts of crosslinking agent.

[0062] Understandably, the waterborne polyurethane dispersion provides the film-forming matrix for the sizing layer 3; fumed silica facilitates the formation of a recoverable interparticle network, while alkali-swellable acrylic thickeners provide structural retention during sizing in static or low-shear conditions. Together, these components restrict the flow of the sizing in the interlayer transition region. High-shear and medium-shear polyurethane associative thickeners regulate the viscoelasticity during sizing, screen separation, and sizing spread on the stepped surface, enabling the sizing to transfer, pull, and cover adjacent printing layers 21. Drying inhibitors slow down excessively rapid surface drying during printing, allowing time for localized sizing; dispersants help ensure uniform powder distribution, defoamers reduce bubble defects, and crosslinking agents contribute to the overall integrity of the coating after drying. The combination of these components gives the sizing sizing a combination of printability, coverage of transition areas, and retention of the three-dimensional printing morphology before drying.

[0063] For high-shear polyurethane associative thickeners, their hydrophobic groups can form reversible associative structures with particles in the aqueous polyurethane dispersion, affecting the viscoelasticity of the paste during the squeegee and screen separation stages, allowing the paste to be transferred from the screen while also possessing a certain degree of traction. For medium-shear polyurethane associative thickeners with a high content of polyoxyethylene segments, they supplement and regulate the flow state of the paste during squeegee pressure application and spread along the interlayer region. The synergistic effect of these two types of associative thickeners helps the paste to cross steps rather than remaining only on the highest printing layer 21.

[0064] After the printing process stops, the shear force on the slurry decreases. Alkali-swellable acrylic thickeners, under suitable swelling conditions, can provide a low-shear structure and a certain degree of structural recovery. If fumed silica with hydroxyl groups on its surface is used, the particles can form a rebuildable dispersion network through hydrogen bonding and mutual contact. The combined effect of these two mechanisms provides shape retention for the wet slurry in the interlayer transition region, reducing the possibility of the slurry flowing as a whole due to its own weight before drying. This medium shear rate corresponds to approximately 1–100 seconds. -1 The rheological response, with low shear, can correspond to less than 1s. -1 Or the rheological state at rest.

[0065] During the static drying stage, the polyurethane associative network may still slowly loosen, and the slurry retains limited localized spreading, which helps to smooth out the scratches left by the screen and interlayer abrupt changes to some extent. Simultaneously, the alkali-swellable acrylic thickener and fumed silica work together to restrict large-scale flow, allowing for a balance between surface finishing and maintaining the overall morphology. The slow-drying agent acts as a drying inhibitor, reducing the hindering effect of premature surface drying on localized spreading; after the slurry dries and forms a film, the crosslinking agent helps maintain the integrity of the coating.

[0066] In some embodiments, the high-shear polyurethane associative thickener is a hydrophobic group-modified ethoxylated polyurethane polymer with a molecular weight of 30,000 to 50,000. The hydrophobic groups can reversibly associate with polymer particles in the aqueous polyurethane dispersion, giving the paste suitable viscoelasticity during printing and screen separation, which is beneficial for the paste to cover the step transition region as it moves with the screen; the molecular weight range provides a specific material selection for forming the above-mentioned associative structure.

[0067] Preferably, the amount of high-shear polyurethane associative thickener is 1.2 to 1.8 parts. When this amount is used, the high-shear thickening component can be combined with the medium-shear thickening component to maintain the required slurry carrying capacity during slurry transfer and pulling, and to retain a certain degree of fluidity for subsequent spreading along the stepped transition zone.

[0068] In some embodiments, the medium-shear polyurethane associative thickener is a nonionic polyurethane thickener with a higher polyoxyethylene segment content than the high-shear polyurethane associative thickener. Preferably, the amount of the medium-shear polyurethane associative thickener is 0.6 to 0.8 parts. This medium-shear thickening component can adjust the flow response of the paste during doctor blade action and interlayer spreading, making the paste easier to transfer through the screen and cover the transition area between adjacent printing layers 21; when combined with the high-shear thickening component, it can balance the traction during paste application and the local spreading after printing.

[0069] In some embodiments, the low-shear thickener is an alkali-swellable acrylic thickener. Preferably, the amount of alkali-swellable acrylic thickener used is 0.3 to 0.4 parts. The alkali-swellable acrylic thickener provides a low-shear structure under system conditions suitable for its swelling, and, in conjunction with fumed silica, inhibits extensive downward flow of the slurry before drying; simultaneously, the slurry retains limited localized flow to reduce screen marks and interlayer step marks.

[0070] The above-mentioned waterborne polyurethane printing paste can be prepared according to the listed weight parts and its components can be fully dispersed. The drying inhibitor can be a slow-drying agent that slows down the drying speed of the printing paste. When this printing paste is used on a dried three-dimensional skeleton 2, the paste transfer is regulated by a polyurethane associative thickener during the squeegee and screen separation stages. During the post-printing settling stage, the shape is maintained by an alkali-swellable acrylic thickener and fumed silica. Limited local spreading before drying helps reduce surface marks, while the low-shear structure restricts overall paste flow.

[0071] Example 1

[0072] Reference Figure 1 and Figure 2 A three-dimensional printed fabric includes a base layer 1, a three-dimensional skeleton 2, and a sizing layer 3; the three-dimensional skeleton 2 is disposed on the base layer 1 and includes at least three printed layers 21 stacked sequentially along the thickness direction of the base layer 1; in the thickness direction of the base layer 1, the size of all printed layers 21 decreases layer by layer in the direction away from the base layer 1; the sizing layer 3 completely covers the outside of the three-dimensional skeleton 2 and includes the outer surface of the printed layers 21 and the transition area.

[0073] Example 2

[0074] In this embodiment, a shoe material base fabric is used as the base layer 1. Three printing screens with the same circular printed pattern are selected, and the size of the printed pattern on the three printing screens decreases sequentially. The printed pattern is circular. The diameter of the largest printed pattern is 10mm. The diameter of the printed pattern on the second screen is 95% of that of the first screen, and the diameter of the printed pattern on the third screen is 95% of that of the second screen. During printing, the centers of the corresponding printed patterns on the three screens are made to coincide on the base fabric.

[0075] A molding process for use in the three-dimensional printed fabric of Example 1 includes the following steps:

[0076] S1: Lay the base fabric flat on the printing table, and use three screens with printing patterns of decreasing size in sequence;

[0077] S2: Following the order of printing pattern size from largest to smallest, water-based polyurethane 3D paste is printed onto the same printing pattern on the base fabric using each printing screen in sequence, and dried after each printing to form a 3D skeleton; specifically, when printing the 3D paste, the center of the printing pattern of all printing screens coincides in the thickness direction of the printing screen; in two adjacent printing screens, the printing pattern of the lower printing screen is proportionally smaller than the printing pattern of the upper printing screen;

[0078] S3: After the printing and drying of the 3D paste, the 3D skeleton is subjected to stretch printing. The stretch paste is applied to the printing screen with the largest printing pattern, and then applied to the outer surface of the 3D skeleton through this printing screen, so that the stretch paste covers the transition area between adjacent printing layers of the 3D skeleton, and then dried to obtain the conical printed fabric. The printing screen with the largest printing pattern size among all printing screens is used, and the 3D skeleton is subjected to 2-3 stretch printing passes.

[0079] Example 3

[0080] A slurry for use in Example 1 and Example 2, comprising a water-based polyurethane slurry for slurry printing;

[0081] By weight, the waterborne polyurethane thickener comprises 88.7 parts waterborne polyurethane dispersion, 1.5 parts fumed silica, 3.0 parts drying inhibitor, 1.5 parts high-shear polyurethane associative thickener, 0.7 parts medium-shear polyurethane associative thickener, 0.35 parts low-shear thickener, 0.5 parts defoamer, 0.75 parts dispersant, and 3 parts crosslinking agent, which are fully dispersed before being used as the thickener. The high-shear polyurethane associative thickener is a hydrophobic modified ethoxylated polyurethane polymer with a molecular weight of approximately 40,000; the medium-shear polyurethane associative thickener is a nonionic polyurethane thickener with a higher polyoxyethylene segment content than the high-shear polyurethane associative thickener. As a preferred option, the aqueous polyurethane dispersion is available from Wanhua Chemical's Tekspro-7351 (anionic aliphatic polyester polyurethane dispersion); the fumed silica is hydrophilic fumed silica, available from Evonik's AEROSIL-200; the drying inhibitor is propylene glycol; the high-shear polyurethane thickener is a nonionic polyurethane associative thickener, commercially available from Wanhua Chemical's Vesmody-U300; and the medium-shear polyurethane thickener is a hydrophobic modified... The following thickeners are available: a polyurethane associative thickener (Vesmody-U604 from Wanhua Chemical); a low-shear thickener (alkali-swellable acrylic emulsion, ASE) from Dow Chemical (ACRYSOL-ASE-60, a cross-linked polymer emulsion containing acidic groups); a defoamer (a polyether siloxane copolymer defoamer, Foamex-810 from Evonik); a water-based dispersant (a copolymer containing high pigment affinity groups, Dispers-755 W from Evonik); and a water-dispersible isocyanate cross-linker (HDI-based, Aquolin-270 from Wanhua Chemical).

[0082] Finally, it should be noted that although the above embodiments have been described in the text and drawings of this application, this should not limit the scope of patent protection of this application. Any technical solutions that are based on the essential concept of this application and utilize the content described in the text and drawings of this application, resulting in equivalent structural or procedural substitutions or modifications, as well as the direct or indirect application of the technical solutions of the above embodiments to other related technical fields, are all included within the scope of patent protection of this application.

Claims

1. A three-dimensional printed fabric, characterized in that, include: grassroots level; A three-dimensional skeleton is disposed on the base layer and includes at least three printed layers stacked sequentially along the thickness direction of the base layer; in the thickness direction of the base layer, the size of all printed layers decreases layer by layer in the direction away from the base layer; A sizing layer that at least covers the transition area formed between adjacent printing layers.

2. A forming process for use in the volumetrically printed fabric of claim 1, characterized by, Includes the following steps: S1: Provide at least three printing screens with the same printing pattern and successively smaller sizes; S2: In order of decreasing size of the printed pattern, the printing screens are used sequentially to apply the three-dimensional paste to the same printed pattern on the base fabric, and the paste is dried after each printing to form a three-dimensional skeleton. S3: After the printing and drying of the three-dimensional paste are completed, the three-dimensional skeleton is subjected to paste printing and then dried to obtain conical printed fabric.

3. The three-dimensional printing molding process according to claim 2, characterized in that, In S2, when printing the three-dimensional paste, the centers of the printed patterns of all the printing screens coincide in the thickness direction of the printing screens; In two adjacent printing screens, the printed pattern on the lower printing screen is proportionally smaller than the printed pattern on the upper printing screen.

4. The three-dimensional printing molding process according to claim 2, characterized in that, In step S3, the printing screen with the largest printing pattern size among all printing screens is used to perform 2 to 3 printing passes on the three-dimensional skeleton, and drying is performed after each printing pass.

5. The three-dimensional printing molding process according to claim 4, characterized in that, In step S3, the stretch printing specifically involves applying stretch paste to the largest printing screen of the printed pattern, and then applying the stretch paste to the outer surface of the three-dimensional skeleton through the printing screen, so that the stretch paste covers the transition area between adjacent printing layers of the three-dimensional skeleton.

6. A sizing paste for use in the stereolithography process according to any one of claims 2 to 5, comprising using a water-based polyurethane sizing paste for the sizing process; The waterborne polyurethane slurry comprises, by weight: The mixture contains 85-90 parts of waterborne polyurethane dispersion, 1-2 parts of fumed silica, 1-5 parts of drying inhibitor, 1-2 parts of high-shear polyurethane associative thickener, 0.5-1.0 parts of medium-shear polyurethane associative thickener, 0.2-0.6 parts of low-shear thickener, 0.4-0.6 parts of defoamer, 0.5-1.0 parts of dispersant, and 2-4 parts of crosslinking agent.

7. The waterborne polyurethane grouting material according to claim 6, characterized in that, The high-shear polyurethane associative thickener is a hydrophobic group-modified ethoxylated polyurethane polymer with a molecular weight of 30,000 to 50,000.

8. The waterborne polyurethane grouting material according to claim 7, characterized in that, The amount of the high-shear polyurethane associative thickener is 1.2 to 1.8 parts.

9. The waterborne polyurethane grouting material according to claim 6 or 7, characterized in that, The medium-shear polyurethane associative thickener is a nonionic polyurethane thickener, and its polyoxyethylene segment content is higher than that of the high-shear polyurethane associative thickener.

10. The waterborne polyurethane slurry according to claim 9, characterized in that, The low-shear thickener is an alkali-swellable acrylic thickener.