A wet toilet paper substrate and a preparation method and application thereof

By using two-stage gradient screening and differentiated beating of softwood pulp, combined with lyocell short fibers, a wet toilet paper substrate was prepared. This solved the problems of wet lint shedding and pipe blockage in the wet toilet paper substrate, achieving a balance between wet strength and flushing properties, and improving the user experience.

CN123153302APending Publication Date: 2026-11-24河南逸祥领研科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611430505.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing flushable wet toilet paper substrates exhibit significant lint and fiber shedding during wet wiping, leaving a lot of lint-like residue on the skin. Furthermore, the addition of PAE-type wet-strength resins can easily clog the pipe network, making it difficult to balance wet strength and flushability.

Method used

By performing two-stage gradient sieving on softwood pulp to remove fine short fibers, and by subjecting long and medium-length fibers to differentiated low-temperature pulping treatment, the pulp is then mixed with lyocell short fibers under low shear to form physical entanglement points and reversible hydrogen bonds, thus preparing a wet toilet paper substrate.

Benefits of technology

Without adding permanent wet-strength resin, it improves lint shedding and wet strength properties, maintains the washability of the substrate, and enhances the user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153302A_ABST
    Figure CN123153302A_ABST
Patent Text Reader

Abstract

This invention provides a wet toilet paper substrate, its preparation method, and its application. The preparation method includes: performing a two-stage gradient sieving of softwood pulp to separately retain long-fiber and medium-long-fiber components, while removing fine short fibers; differentially beating the long-fiber and medium-long-fiber components at 20-30°C, followed by blending to obtain graded, broom-modified softwood pulp; wherein the freeness of the long-fiber component is lower than that of the medium-long-fiber component; mixing the graded, broom-modified softwood pulp with lyocell short fibers at low shear to obtain a mixed pulp; and sequentially subjecting the mixed pulp to wet web forming, hydroentangling consolidation, and drying to obtain the wet toilet paper substrate. This invention solves the problem of existing flushable wet toilet paper substrates struggling to balance wet strength and flushability, thereby improving the user experience.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of disposable hygiene products technology, and in particular to wet toilet paper substrates, their preparation methods, and applications. Background Technology

[0002] Current flushable toilet paper substrates are generally made from wood pulp and lyocell fibers through wet web forming and hydroentanglement reinforcement. This type of substrate has low wet strength, resulting in significant lint and fiber shedding during wet wiping, leaving a lot of lint-like residue on the skin. However, adding PAE-type wet strength resins to improve wet strength can easily clog the web. Therefore, existing toilet paper substrates struggle to balance wet strength and flushability, thus reducing the user experience. Summary of the Invention

[0003] In view of the above problems, the present invention is proposed to provide a wet toilet paper substrate, its preparation method, and its application that overcome or at least partially solve the above problems. It can solve the problem that existing flushable wet toilet paper substrates are difficult to balance wet strength and flushability, thereby improving the user experience.

[0004] Specifically, the present invention provides a method for preparing a wet toilet paper substrate, comprising: S1. The softwood pulp is subjected to two-stage gradient sieving to separate the long fiber component and the medium-long fiber component, and to remove the fine short fibers. S2. The long fiber component and the medium-long fiber component are subjected to differential beating at 20~30℃, and then compounded to obtain graded broom-modified softwood pulp; wherein the beating degree of the long fiber component is lower than that of the medium-long fiber component. S3. The graded broom-modified softwood pulp is mixed with low-shear Lyocell short fibers to obtain a mixed pulp. S4. The mixed slurry is sequentially subjected to wet web forming, hydroentanglement and drying to obtain wet toilet paper substrate.

[0005] Optionally, the first-stage sieve gap of the two-stage gradient screening is 1.2 mm, and the second-stage sieve gap is 0.6 mm; The softwood pulp is bleached sulfate softwood pulp; The two-stage gradient sieving of softwood pulp includes: The bleached sulfate softwood pulp was prepared into a low-concentration pulp with a mass fraction of 0.5% to 0.8%; The low-concentration slurry is subjected to a first-stage sieve to retain the long fiber component. The material that passes through the first-stage screening is then subjected to a second-stage screening to retain the medium-length fiber component and remove the fine and short fibers.

[0006] Optionally, the two-stage gradient screening adopts a two-stage hydraulic classifier screen in series, with a classifier inlet pressure of 0.15~0.25MPa, a screen drum rotation speed of 800~1000r / min, a classifier water flow velocity of 1.2~1.8m / s, and a classifier screen rotor linear velocity of 12~15m / s.

[0007] Optionally, step S2 includes: The long fiber component is pulped at a beating degree of 28~30°SR to obtain a first modified pulp with a fibrillation rate of 15%~20%. The medium-length fiber component is pulped at a beating degree of 35~37°SR to obtain a second modified pulp with a fibrillation rate of 35%~40%. The first modified pulp and the second modified pulp are mixed to obtain graded broom-modified softwood pulp.

[0008] Optionally, before mixing the first modified slurry and the second modified slurry, the method further includes: Both the first modified slurry and the second modified slurry were adjusted to a target concentration of 2.9% to 3.1%; In the graded broom-modified softwood pulp, the mass ratio of the first modified pulp to the second modified pulp is 7:3 to 8:2.

[0009] Optionally, in step S2, the differentiated pulping adopts a dual-disc mill with a disc mill working gap of 0.2~0.5mm, a linear velocity of 8~12m / s, and a single-path pulp circulation of 2~3 times; each disc mill is equipped with a circulating cooling water circuit and an online temperature sensor, and the pulp temperature is stably controlled at 20~30℃ through closed-loop heat exchange.

[0010] Optionally, in step S3: the mass ratio of the graded broom-modified softwood pulp to the lyocell short fiber is 65:35 to 80:20; the length of the lyocell short fiber is 5~8mm and the fineness is 1.5~2.0D; the stirring linear velocity of the low-shear mixing is ≤1.5m / s and the stirring time is 5~8min; Step S4 includes: diluting the mixed slurry to a web-forming concentration of 0.15% to 0.25%, then sequentially performing wet web forming and hydroentangling to obtain a fiber web; and drying the fiber web to a moisture content of 8% to 10% using hot air at 105 to 110°C to obtain the wet toilet paper substrate.

[0011] On the other hand, the present invention also provides a wet toilet paper substrate, which is prepared by any of the methods described above.

[0012] In another aspect, the present invention also provides a wet toilet paper, comprising a wet toilet paper substrate as described above and a wetting liquid.

[0013] On another front, a method for preparing wet toilet paper includes: Wet toilet paper substrate is prepared using any of the methods described above; The wet toilet paper substrate is impregnated with a wetting liquid, with the liquid content controlled at 200%~250%, and then cut to obtain wet toilet paper.

[0014] In the preparation method of the wet toilet paper substrate of the present invention, the softwood pulp is precisely graded at the pulping stage to remove easily detached fine short fibers; then, the graded long fiber component and medium-long fiber component are subjected to differentiated low-temperature beating treatment, so that the long fibers retain their length and skeleton strength, and the medium-long fibers are fully split and bristled to increase entanglement points; finally, the two pulps are blended and mixed with lyocell short fibers under low shear. This method can simultaneously improve lint shedding performance and wet strength performance without adding permanent wet strength resin, and does not affect flushability.

[0015] Furthermore, the mass percentage of fine fibers in the wet toilet paper substrate is ≤6%, and the wet shedding rate is ≤2.2mg / 100cm². 2 Wet tensile strength ≥2.8N / 5cm, water disintegration time ≤43s.

[0016] The above and other objects, advantages and features of the present invention will become more apparent to those skilled in the art from the following detailed description of specific embodiments of the invention in conjunction with the accompanying drawings. Attached Figure Description

[0017] The following sections will describe some specific embodiments of the invention in detail by way of example and not limitation, with reference to the accompanying drawings. The same reference numerals in the drawings denote the same or similar parts or portions. Those skilled in the art should understand that these drawings are not necessarily drawn to scale. In the drawings: Figure 1 This is a schematic microstructure diagram of softwood pulp according to an embodiment of the present invention; Figure 2 This is a schematic microstructure diagram of a first modified slurry according to an embodiment of the present invention; Figure 3 This is a schematic microstructure diagram of a second modified slurry according to an embodiment of the present invention; Figure 4 This is a schematic structural diagram of graded broom-modified softwood pulp according to an embodiment of the present invention.

[0018] Figure label: 1. Softwood pulp; 11. Long fiber; 12. Medium-length fiber; 13. Fine short fiber; 2. First modified slurry; 3. Second modified slurry; 4. Graded broom-modified softwood pulp. Detailed Implementation

[0019] In the description of this embodiment, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature, that is, include one or more of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified. When a feature "includes or contains" one or more of the features it encompasses, unless otherwise specifically described, this indicates that other features are not excluded and may be further included.

[0020] This invention provides a method for preparing a wet toilet paper substrate, which may include the following steps: S1. The softwood pulp 1 is subjected to two-stage gradient sieving to retain long fiber component 11 and medium-long fiber component 12 respectively, and the fine short fiber 13 is removed. S2. After differentially beating the long fiber component 11 and the medium-long fiber component 12 at 20~30℃, they are compounded to obtain graded broom-modified softwood pulp 4; wherein, the beating degree of the long fiber component is lower than that of the medium-long fiber component. S3. Mix graded broom-modified softwood pulp 4 with low-shear Lyocell short fibers to obtain a mixed pulp. S4. The mixed slurry is sequentially subjected to wet web forming, hydroentanglement and drying to obtain wet toilet paper substrate.

[0021] Specifically, the applicant has found in long-term production practice that existing flushable toilet paper substrates exhibit significant lint and fiber shedding during wet wiping, leaving a large amount of lint-like residue on the skin. After analyzing the existing manufacturing process, the applicant found that: Figure 1 As shown, the softwood pulp 1 includes long fibers 11, medium-length fibers 12, and fine short fibers 13. In existing flushable wet toilet paper substrate production processes, the pulping stage uses direct beating of whole wood pulp, resulting in a large number of fine short fibers with a length <0.6mm mixed in the pulp, which makes the substrate prone to shedding. However, to compensate for insufficient wet strength, existing technologies add PAE-type permanent wet strength resins to the pulp, which reduces the flushability of the wet toilet paper substrate. Based on the above findings, this embodiment is proposed to solve the problem of difficulty in simultaneously achieving low wet shedding rate and high flushability.

[0022] In this embodiment, the softwood pulp is precisely graded at the pulping stage to remove easily detached fine short fibers. Then, the graded long fiber and medium-length fiber components undergo differentiated low-temperature beating treatments to ensure that the long fibers retain their length and skeletal strength, while the medium-length fibers are fully fluffed to increase entanglement points. Finally, the two pulps are blended and mixed with lyocell short fibers using low-shear mixing. This method can simultaneously improve lint shearing and wet strength properties without adding permanent wet-strength resin, and without affecting washability.

[0023] In other words, the pulping process has already eliminated easily detachable short fibers through grading, reducing the source of lint at its origin. At the same time, the long fiber component forms the backbone of the three-dimensional network, while the medium and long fiber components, after being fully split and bristled, fill the gaps in the backbone, forming more physical entanglement points and reversible hydrogen bond points with the lyocell short fibers. This makes the substrate structurally stable and less prone to lint when wiped wet. The fibers are bonded by physical entanglement and reversible hydrogen bonds, without permanent cross-linking structures. After being rinsed with flowing water, the hydrogen bonds are quickly dissociated, and the fibers are evenly dispersed, simultaneously meeting the requirements for strength and washability.

[0024] Furthermore, pulping at 20~30℃ can keep the fiber surface layer moderately soft. During the pulping process, the fiber mainly undergoes surface fibrillation, avoiding excessive fiber cutting and thermal degradation caused by frictional heat.

[0025] In some embodiments of the present invention, the first-stage sieve gap of the two-stage gradient screening is 1.2 mm, and the second-stage sieve gap is 0.6 mm.

[0026] The softwood pulp is bleached sulfate softwood pulp.

[0027] Step S1 may specifically include the following steps: S11. The bleached sulfate softwood pulp is prepared into a low-concentration pulp with a mass fraction of 0.5% to 0.8%.

[0028] S12. The low-concentration slurry is subjected to a first-stage sieve to retain the long-fiber component. Specifically, the oversize material from the first-stage sieve is mainly composed of long-fiber components.

[0029] S13. The undersize material from the first-stage screening is subjected to a second-stage screening to retain the medium- and long fiber components and remove fine and short fibers. Specifically, the oversize material from the second-stage screening is mainly composed of medium- and long fiber components.

[0030] Specifically, the raw material is bleached sulfate softwood pulp board with an average fiber length of 2.5~3.0mm. After the pulp board is soaked at room temperature for 30 minutes, it is sent to the pre-deconstruction unit to break up the flocs and prepare a low-concentration pulp with a mass fraction of 0.5%~0.8%, which is then pumped into a two-stage series rotary pressure classifier.

[0031] In this embodiment, the wood pulp is prepared into a low-concentration pulp of 0.5% to 0.8%, which allows the fibers to be fully dispersed in water. This avoids pulp flocculation and clogging of the screen due to excessively high concentration, and also avoids insufficient equipment processing capacity and reduced grading efficiency due to excessively low concentration.

[0032] After the first stage of screening, long fibers with a length of ≥1.2mm in the low-concentration slurry are retained on the screen and collected separately, with a retention rate of ≥85%.

[0033] After the second-stage screening, medium-length fibers with a length between 0.6 and 1.2 mm in the first-stage undersize material are retained on the screen and collected separately; fine short fibers with a length < 0.6 mm pass through the screen and are discharged, collected from the bottom recovery outlet.

[0034] After two-stage gradient screening, the mass percentage of fine fibers in the pulp entering the pulping process is ≤6%. The long fiber component and the medium-long fiber component are of uniform length, providing a stable raw material basis for the subsequent two-stage differentiated pulping.

[0035] In some embodiments of the present invention, the two-stage gradient screening adopts a two-stage hydraulic classifying screen in series, with a classifying inlet pressure of 0.15~0.25MPa (e.g., 0.16MPa, 0.18MPa, 0.2MPa, 0.22MPa or 0.24MPa), a screen drum rotation speed of 800~1000r / min (e.g., 810r / min, 850r / min, 900r / min, 950r / min or 990r / min), a classifying water flow velocity of 1.2~1.8m / s (e.g., 1.3m / s, 1.4m / s, 1.5m / s, 1.6m / s or 1.7m / s), and a classifying screen rotor linear velocity of 12~15m / s (e.g., 12.5m / s, 13m / s, 13.5m / s, 14m / s or 14.5m / s).

[0036] The inlet pressure for classification is set to 0.15~0.25MPa to ensure a stable classification flow field within the screen drum. Too low a pressure results in insufficient flow velocity and reduced classification efficiency, while too high a pressure can force fibers through the screen, reducing classification accuracy. The screen drum rotation speed is set to 800~1000 r / min, coupled with a rotor linear velocity of 12~15 m / s, to create a uniform swirling flow field within the drum, promoting precise separation of fibers of different lengths under centrifugal force and fluid resistance. The classification water flow velocity is set to 1.2~1.8 m / s to moderately scour the fibers at the screen openings, ensuring smooth passage of medium and long fibers to the next stage while preventing short, fine fibers from clogging the screen. These parameters work together to enable the two-stage hydraulic classifier to achieve stable, continuous, and precise fiber length classification under low-concentration feed conditions, with a long fiber retention rate ≥85% and a fine fiber mass percentage ≤6% in the classified pulp.

[0037] In some embodiments of the present invention, the grading screen device has two or more screen drums and is equipped with a dual-screen switching and automatic backwashing structure. When the screen gaps of the first-stage screen drum or the second-stage screen drum show signs of clogging, it can be switched to the standby screen drum to continue operation, while the clogged screen drum is backwashed online, achieving continuous mass production without stopping the machine.

[0038] In some embodiments of the present invention, step S2 may specifically include: S21. The long fiber component is pulped at a beating degree of 28~30°SR to obtain a first modified pulp 2 with a fibrillation rate of 15%~20%; S22. The medium-length fiber component is pulped at a beating degree of 35~37°SR to obtain a second modified pulp 3 with a fibrillation rate of 35%~40%; S23. The first modified pulp 2 and the second modified pulp 3 are mixed to obtain graded broom-modified softwood pulp 4.

[0039] like Figure 2 As shown, the surface of the long fibers exhibits slight fibrillation; as Figure 3 As shown, the surface of the medium-length fibers is fully bristled.

[0040] Specifically, the long fiber component is lightly beaten with a low beating degree of 28~30°SR, only moderately fracturing the fiber surface while keeping the fiber body intact. The fracturing rate is controlled at 15%~20%. At this beating degree, the long fibers still have high mechanical strength. After being mixed with lyocell short fibers to form a web, the long fibers can build the backbone of a three-dimensional network, providing wet mechanical strength support for the substrate.

[0041] The medium-length fiber component is lightly beaten with a relatively high beating degree of 35-37°SR to promote full fibrillation at the fiber ends, with the fibrillation rate controlled at 35%-40%. At this beating degree, the specific surface area of ​​the medium-length fibers is significantly increased, and the surface fibrillation ends can fill the gaps in the long fiber skeleton during the subsequent web formation process, forming more physical entanglement sites and reversible hydrogen bond points with the lyocell short fibers, thereby improving the overall bonding density of the fiber network.

[0042] In some embodiments, before the step of "mixing the first modified slurry and the second modified slurry", the method further includes adjusting both the first modified slurry and the second modified slurry to a target concentration of 2.9% to 3.1%. This setting ensures that the two slurries have consistent concentrations during compounding, guaranteeing a stable and controllable compounding ratio and preventing fluctuations in the freeness of the compounded slurry due to concentration differences, thus avoiding impacts on the consistency of the final substrate performance.

[0043] In some embodiments, in graded broom-modified softwood pulp, the mass ratio of the first modified pulp to the second modified pulp is 7:3 to 8:2. Within this ratio range, a better balance is achieved between the strength of the long fiber skeleton and the entanglement bonding force of the medium and long fibers, and the resulting substrate exhibits good overall performance in terms of wet shedding rate, wet tensile strength, and washability.

[0044] In some embodiments, in step S2, the differentiated pulping adopts a dual-disc mill with a disc mill working gap of 0.2~0.5mm, a linear velocity of 8~12m / s, and a single-path pulp circulation of 2~3 times; each disc mill is equipped with a circulating cooling water circuit and an online temperature sensor, and the pulp temperature is stably controlled at 20~30℃ through closed-loop heat exchange.

[0045] Specifically, the graded long-fiber and medium-length-fiber components are fed into two disc mills via independent pipelines, forming two parallel pulping branches that do not interfere with each other. In each disc mill, an online temperature sensor monitors the pulp temperature in real time, and a closed-loop heat exchange system adjusts the cooling water flow rate based on the temperature feedback to stably control the pulp temperature at 20~30℃.

[0046] The grinding disc adopts a dispersive oblique tooth grinding disc. Under the above-mentioned gap and linear speed combination, the grinding disc mainly acts on the surface of the fiber to separate and bristle, without cutting the fiber body. The single pulp circulation is 2 to 3 times to gradually separate and bristle the fiber, avoiding fiber damage caused by excessive pulping in a single cycle.

[0047] In some embodiments, in step S3: the mass ratio of the graded broom-modified softwood pulp to the lyocell short fiber is 65:35 to 80:20; the length of the lyocell short fiber is 5~8 mm, and the fineness is 1.5~2.0D; the stirring linear velocity of the low-shear mixing is ≤1.5 m / s, and the stirring time is 5~8 min.

[0048] Specifically, lyocell staple fibers are first dispersed in a pre-dispersing machine, then slowly added to a mixing tank in proportion, and mixed with graded and beneficiated modified softwood pulp under low shear conditions. The stirring linear velocity is controlled at ≤1.5m / s, and the stirring time is 5~8min. This ensures uniform fiber dispersion without clumping, while avoiding secondary breakage of lyocell staple fibers and modified wood pulp fibers caused by high shear, preventing the formation of new fine staple fibers, and ensuring that the modification effect of grading and beneficiation is not compromised.

[0049] In some embodiments, step S4 includes: diluting the mixed slurry to a web-forming concentration of 0.15% to 0.25%, then sequentially performing wet web forming and hydroentangling to obtain a fiber web; and drying the fiber web to a moisture content of 8% to 10% using hot air at 105 to 110°C to obtain a wet toilet paper substrate.

[0050] Specifically, diluting the mixed slurry to a web concentration of 0.15%~0.25% ensures smooth web formation while maintaining uniform fiber dispersion. Excessive concentration can lead to decreased web uniformity, while insufficient concentration affects web formation efficiency. Hydroentangling consolidation can employ segmented high-pressure hydroentangling with pressures of 70 bar, 110 bar, and 90 bar respectively. This gradient pressure hydroentangling helps form a stable three-dimensional entangled network, improving the overall wet strength and abrasion resistance of the substrate without the addition of adhesives. A slurry-to-web speed ratio of 0.9 facilitates the directional alignment of fibers on the formed web. The formed web is then hot-air dried at 105~110℃ to a moisture content of 8%~10%, which helps to fix the fiber entanglement structure and ensures stable liquid retention in subsequent impregnation processes.

[0051] In some embodiments of the present invention, the fine short fibers are separately loosened and then blended into the low-grade wiping cloth slurry at a ratio of 10% to 20% for resource utilization. Specifically, the fine short fibers are collected from the recovery outlet at the bottom of the grading screen.

[0052] In some embodiments, wet web forming employs a three-layer gradient forming process, resulting in a surface layer enriched with long fiber components. Because the long fiber components are longer and more firmly entangled with the web, this surface enrichment of long fibers reduces the probability of hair loss in areas of skin friction contact, further enhancing the user experience.

[0053] In some embodiments, step S4 further includes a step of testing the dry basis properties of the wet toilet paper substrate after drying; unqualified dry basis substrate is recycled to the mixing process in step S3 after pulping and descaling to reduce raw material loss.

[0054] This invention also provides a wet toilet paper substrate prepared by any of the above-described method embodiments. The wet toilet paper substrate has a fine fiber mass percentage of ≤6% and a wet shedding rate of ≤2.2 mg / 100 cm³. 2Wet tensile strength ≥2.8N / 5cm, water disintegration time ≤43s.

[0055] This invention also provides a wet toilet paper, which includes a wet toilet paper substrate and a wetting liquid.

[0056] This invention also provides a method for preparing wet toilet paper, which may include the following steps: preparing a wet toilet paper substrate using any of the methods described above; impregnating the wet toilet paper substrate with a wetting liquid, controlling the liquid content to be 200%~250%, and then cutting it to obtain wet toilet paper.

[0057] Specifically, the wetting solution is used to prepare the wet toilet paper and can use cosmetic-grade, mild ingredients without any irritating chemical residues. Because no permanent wet-strength resins such as PAE are added during the preparation of the wet toilet paper substrate, the fibers are bonded together by physical entanglement and reversible hydrogen bonds. Therefore, the wet toilet paper has a stable structure and does not shed easily when wiped wet. After being flushed with running water, the hydrogen bonds are quickly dissociated and the fibers are evenly dispersed, thus meeting both the requirements for strength and flushability.

[0058] To further illustrate the present invention, the present invention will be described in detail below with reference to specific embodiments and comparative examples.

[0059] Example 1 This embodiment provides a method for preparing a wet toilet paper substrate, specifically including the following steps: Two-stage gradient screening: Commercial bleached sulfate softwood pulp (NBKP) with an average fiber length of 2.5–3.0 mm was used. After soaking at room temperature for 30 minutes, the pulp was pre-decomposed to prepare a low-consistency pulp with a mass fraction of 0.6%. This pulp was then pumped into a two-stage tandem rotary pressure classifier. The first-stage screen had a 1.2 mm sieve opening, retaining the long fiber component. The material passing through the first stage screen entered the second-stage screen, with a 0.6 mm sieve opening, retaining the medium- and long fiber component. Fine short fibers (<0.6 mm in length) were passed through the screen and discharged for recycling. The inlet pressure for classification was 0.2 MPa, the screen drum speed was 900 r / min, and the classification water flow velocity was 1.5 m / s. After two-stage classification, the mass percentage of fine fibers was 5.8%.

[0060] Differential low-temperature pulping: Long-fiber and medium-long-fiber components are fed into two separate double-disc mills, with closed-loop heat exchange to stably control the pulp temperature at 25℃. The mill discs are of the dispersive type with helical teeth, a disc-to-disc working gap of 0.3mm, a linear velocity of 10m / s, and a single-path cycle of 2-3 times. The long-fiber branch has a freeness of 29°SR and a fibrillation rate of 17%, yielding the first modified pulp; the medium-long-fiber branch has a freeness of 36°SR and a fibrillation rate of 37%, yielding the second modified pulp. Both paths are uniformly concentrated to 3.0%. The first and second modified pulps are fed into a mixing tank at a mass ratio of 7.5:2.5 and mixed uniformly at low speed for 5 minutes to obtain graded fibrillated modified softwood pulp.

[0061] The fiber splitting rate was observed using a 100x bright-field optical microscope. Five fields of view were randomly selected for each sample, and 20 fibers were counted in each field of view. Fibers with a splitting length on the fiber surface ≥ 1 / 2 of the fiber diameter were considered to be effective splitting. The proportion of effective splitting fibers to the total number of counted fibers was calculated, and the average value was taken from three parallel tests.

[0062] Low-damage, gentle pulping: Take 70 parts by weight of graded broom-modified softwood pulp and 30 parts by weight of lyocell staple fiber. The lyocell staple fiber specifications are 5~8mm in length and 1.5~2.0D in fineness. It is first broken up by a pre-de-fibering machine and then slowly added to the mixing tank in proportion. The stirring speed is 180rpm, the stirring time is 6min, and the stirring linear velocity is ≤1.5m / s.

[0063] Web forming, hydroentangling, and drying: The mixed pulp is diluted to a web-forming concentration of 0.2%, and then wet-formed and hydroentangled to form a web. The pulp-to-web speed ratio is 0.9, and the hydroentangling pressure is set in stages at 70 bar, 110 bar, and 90 bar. The web is then hot-air dried at 105-110℃ to a moisture content of 8%-10%, yielding the wet toilet paper substrate. The basis weight of the wet toilet paper substrate is 80 g / m². 2 .

[0064] Testing revealed that the fine fiber content of the wet toilet paper substrate obtained in this embodiment was 5.8%, and the wet shedding rate was 1.7~2.1 mg / 100cm². 2 The wet tensile strength is 2.9~3.3 N / 5cm, and the water disintegration time is 34~38s, which meets the disintegration performance requirements.

[0065] Example 2 This embodiment provides a method for preparing a wet toilet paper substrate, which differs from Embodiment 1 in that: the amount of lyocell short fiber is increased to 35 parts, and the amount of softwood pulp is reduced to 65 parts; the grading water flow rate is adjusted to 1.2 m / s; the beating temperature is adjusted to 20℃, the freeness of the long fiber branch is 28°SR, and the freeness of the medium and long fiber branch is 35°SR; the blending mass ratio of the first modified pulp to the second modified pulp is adjusted to 7:3. The remaining steps and parameters are the same as in Embodiment 1.

[0066] Testing revealed that the fine fiber content of the wet toilet paper substrate obtained in this embodiment was 5.9%, and the wet shedding rate was 1.8~2.2 mg / 100cm². 2 The wet tensile strength is 2.8~3.0 N / 5cm, and the water disintegration time is 39~43s, which meets the disintegration performance requirements.

[0067] Example 3 This embodiment provides a method for preparing a wet toilet paper substrate, which differs from Embodiment 1 in that: the amount of lyocell short fiber is reduced to 20 parts, and the amount of softwood pulp is increased to 80 parts; the grading water flow rate is adjusted to 1.8 m / s; the beating temperature is adjusted to 30℃, the beating degree of the long fiber branch is 30°SR, and the beating degree of the medium and long fiber branch is 37°SR; the blending ratio of the first modified pulp to the second modified pulp is adjusted to 8:2. The remaining steps and parameters are the same as in Embodiment 1.

[0068] Testing revealed that the fine fiber content of the wet toilet paper substrate obtained in this embodiment was 5.7%, and the wet shedding rate was 1.8~2.2 mg / 100cm². 2 The wet tensile strength is 3.0~3.4 N / 5cm, and the water disintegration time is 31~35s, which meets the disintegration performance requirements.

[0069] Comparative Example 1 The traditional, standardized pulping process is employed, without any grading steps. The raw material is bleached sulfate softwood pulp, which is soaked, loosened, and then formulated into a pulp. The entire pulp is uniformly pulped to 28°SR without grading or separate pulping. Subsequently, it is blended with lyocell staple fibers, wet-laid, hydroentangled, and dried to obtain the wet toilet paper substrate.

[0070] Testing revealed that the fine fiber content of the obtained substrate was 9.8-10.4%, and the wet shedding rate was 5.4-6.2 mg / 100cm². 2 The wet tensile strength is 2.0~2.4 N / 5cm, and the water disintegration time is 30~34s.

[0071] Comparative Example 2 The traditional, standardized pulping process was adopted, without any grading step. All pulp was uniformly pulped to 35°SR. The remaining steps were the same as in Comparative Example 1.

[0072] Testing revealed that the fine fiber content of the obtained substrate was 10.9-11.7%, and the wet shedding rate was 5.8-7.2 mg / 100cm². 2 The wet tensile strength is 1.9~2.1 N / 5cm, and the water disintegration time is 28~32s.

[0073] Comparative Example 3 The two-stage gradient grading process is retained, while the differentiated pulping for each fiber group is eliminated. The long fiber and medium-length fiber components are combined and pulped uniformly to 28°SR. The remaining steps are the same as in Comparative Example 1.

[0074] Testing revealed that the fine fiber content of the obtained substrate was 6.4-6.8%, and the wet shedding rate was 4.8-5.4 mg / 100cm². 2 The wet tensile strength is 2.1~2.5 N / 5cm, and the water disintegration time is 32~36s.

[0075] Comparative Example 4 The grading process was eliminated, but differentiated pulping by branch was retained. The raw materials were directly divided into two branches without grading, and then pulped to 28°SR and 35°SR respectively before being blended. The remaining steps were the same as in Comparative Example 1.

[0076] Testing revealed that the fine fiber content of the obtained substrate was 9.5-10.1%, and the wet shedding rate was 4.4-5.4 mg / 100cm². 2 The wet tensile strength is 2.2~2.6 N / 5cm, and the water disintegration time is 29~33s.

[0077] Comparative Example 5 The two-stage grading was retained, but the differentiation between different fiber groups was eliminated. The graded long-fiber and medium-length-fiber components were combined and uniformly pulped to 37°SR. The remaining steps were the same as in Comparative Example 1.

[0078] Testing revealed that the fine fiber content of the obtained substrate was 7.6-8.2%, and the wet shedding rate was 3.9-4.5 mg / 100cm². 2 The wet tensile strength is 2.0~2.4 N / 5cm, and the water disintegration time is 31~35s.

[0079] Comparative Example 6 This comparative example provides a method for preparing a wet toilet paper substrate. The difference from Example 1 is that the pulping temperature is adjusted to 40°C, while the other parameters are the same as in Example 1.

[0080] Testing revealed that the fine fiber content of the wet toilet paper substrate obtained in this comparative example was 5.8%, and the wet shedding rate was 2.5~3.1 mg / 100cm². 2 The wet tensile strength was 2.3~2.7 N / 5cm, and the water disintegration time was 28~32s. Compared with Example 1, the shedding rate increased significantly and the wet tensile strength decreased after the pulping temperature was raised to 40℃.

[0081] The test data from the above examples and comparative examples show that the lint rate was reduced by about 12% when only the grading process was used (Comparative Example 3), and by about 15.5% when only the separate pulping process was used (Comparative Example 4). However, when the grading and separate pulping processes were coupled (Example 1), the lint rate was reduced by about 67%, which is much higher than the sum of the effects of a single process. The wet tensile strength was also increased by about 40.9%, indicating that the coupling of the two processes produced a synergistic effect.

[0082] Therefore, those skilled in the art should recognize that although numerous exemplary embodiments of the present invention have been shown and described in detail herein, many other variations or modifications conforming to the principles of the present invention can be directly determined or derived from the disclosure of the present invention without departing from the spirit and scope of the invention. Thus, the scope of the present invention should be understood and construed as covering all such other variations or modifications.

Claims

1. A method for preparing a wet toilet paper substrate, characterized in that, include: S1. The softwood pulp is subjected to two-stage gradient sieving to separate the long fiber component and the medium-long fiber component, and to remove the fine short fibers. S2. The long fiber component and the medium-long fiber component are subjected to differential beating at 20~30℃, and then compounded to obtain graded broom-modified softwood pulp; wherein the beating degree of the long fiber component is lower than that of the medium-long fiber component. S3. The graded broom-modified softwood pulp is mixed with low-shear Lyocell short fibers to obtain a mixed pulp. S4. The mixed slurry is sequentially subjected to wet web forming, hydroentanglement and drying to obtain wet toilet paper substrate.

2. The method according to claim 1, characterized in that, The first-stage sieve gap of the two-stage gradient screening is 1.2 mm, and the second-stage sieve gap is 0.6 mm. The softwood pulp is bleached sulfate softwood pulp; The two-stage gradient sieving of softwood pulp includes: The bleached sulfate softwood pulp was prepared into a low-concentration pulp with a mass fraction of 0.5% to 0.8%; The low-concentration slurry is subjected to a first-stage sieve to retain the long fiber component. The material that passes through the first-stage screening is then subjected to a second-stage screening to retain the medium-length fiber component and remove the fine and short fibers.

3. The method according to claim 1, characterized in that, The two-stage gradient screening adopts a two-stage hydraulic classifier screen in series, with a classifier inlet pressure of 0.15~0.25MPa, a screen drum rotation speed of 800~1000r / min, a classifier water flow velocity of 1.2~1.8m / s, and a classifier screen rotor linear velocity of 12~15m / s.

4. The method according to claim 1, characterized in that, Step S2 includes: The long fiber component is pulped at a beating degree of 28~30°SR to obtain a first modified pulp with a fibrillation rate of 15%~20%. The medium-length fiber component is pulped at a beating degree of 35~37°SR to obtain a second modified pulp with a fibrillation rate of 35%~40%. The first modified pulp and the second modified pulp are mixed to obtain graded broom-modified softwood pulp.

5. The method according to claim 4, characterized in that, Before mixing the first modified slurry and the second modified slurry, the method further includes: Both the first modified slurry and the second modified slurry were adjusted to a target concentration of 2.9% to 3.1%; In the graded broom-modified softwood pulp, the mass ratio of the first modified pulp to the second modified pulp is 7:3 to 8:

2.

6. The method according to claim 1, characterized in that, In step S2, the differentiated pulping adopts a dual-disc mill with a working gap of 0.2~0.5mm and a linear velocity of 8~12m / s. The single-path pulp is circulated 2~3 times. Each disc mill is equipped with a circulating cooling water circuit and an online temperature sensor. The pulp temperature is stably controlled at 20~30℃ through closed-loop heat exchange.

7. The method according to claim 1, characterized in that, In step S3: the mass ratio of the graded broom-modified softwood pulp to the lyocell short fiber is 65:35 to 80:20; the length of the lyocell short fiber is 5~8mm and the fineness is 1.5~2.0D; the stirring linear velocity of the low-shear mixing is ≤1.5m / s and the stirring time is 5~8min; Step S4 includes: diluting the mixed slurry to a web-forming concentration of 0.15%~0.25%, and then sequentially performing wet web forming and hydroentangling to obtain a fiber web; The fiber web is dried to a moisture content of 8% to 10% using hot air at 105 to 110°C to obtain the wet toilet paper substrate.

8. A wet toilet paper substrate, characterized in that, The wet toilet paper substrate is prepared by the method described in any one of claims 1 to 7.

9. A type of wet toilet paper, characterized in that, Includes the wet toilet paper substrate and wetting liquid as described in claim 8.

10. A method for preparing wet toilet paper, characterized in that, include: Wet toilet paper substrate is prepared by the method described in any one of claims 1 to 7; The wet toilet paper substrate is impregnated with a wetting liquid, with the liquid content controlled at 200%~250%, and then cut to obtain wet toilet paper.