A starch-containing bio-based dry-strength agent and a method of making the same
By preparing a starch-containing bio-based dry strength agent, the problems of poor copolymerization effect, insufficient stability and viscosity control of existing dry strength agents were solved, achieving the effects of improved paper strength, excellent emulsion stability and precise viscosity control.
Patent Information
- Application Number
- CN202611345806.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-24
AI Technical Summary
Existing starch-containing dry strength agents suffer from problems such as poor copolymerization effect of starch and acrylamide, insufficient product stability, difficulty in controlling viscosity, incomplete reinforcement effect, and high residual monomer levels.
The raw materials, by weight, include starch, bio-based acrylamide, comonomer, redox complex initiation system, complex chain transfer and stabilization system, viscosity locking agent and deionized water. A starch-containing bio-based dry strength agent is prepared by starch pregelatinization and degradation, low-temperature copolymerization and online viscosity monitoring.
It significantly improves paper strength, has excellent emulsion stability, precise and controllable viscosity, and a safe and stable polymerization process. It also reduces residual monomers and solves the problems of poor copolymerization effect, insufficient stability, and viscosity control of traditional dry strength agents.
Abstract
Description
Technical Field
[0001] This invention relates to the field of papermaking technology, specifically to a starch-containing bio-based dry strength agent and its preparation method. Background Technology
[0002] Dry strength agents are key additives in the papermaking industry for improving paper strength. In recent years, replacing petroleum-based raw materials with bio-based raw materials (such as bio-based acrylamide and starch) has become a development trend. Starch is widely available, renewable, and inexpensive, making it an ideal bio-based framework material. However, existing starch-containing dry strength agents have the following problems:
[0003] First, the copolymerization effect of starch and acrylamide is poor, resulting in insufficient product stability. Starch molecules have relatively rigid chains, making them prone to phase separation during copolymerization with acrylamide. This leads to emulsion stratification, precipitation, poor storage stability, and affects usability.
[0004] Secondly, the introduction of starch makes viscosity difficult to control. Starch itself has a thickening effect, which can cause the viscosity of the system to rise sharply during polymerization, or even gel, making it impossible to obtain a product with the target viscosity and making it difficult to meet the needs of different paper types.
[0005] Third, the reinforcing effect was not fully realized. Due to the poor compatibility between starch and synthetic polymers, the dry strength agent was not evenly dispersed in the pulp and could not effectively adsorb fibers, resulting in an unsatisfactory paper strengthening effect.
[0006] Fourth, high residual monomer content and heavy post-processing burden. The addition of starch increases the resistance to monomer migration, leading to a decrease in conversion rate and an increase in residual monomer. Summary of the Invention
[0007] This invention provides a starch-containing bio-based dry strength agent that improves paper strength and exhibits excellent emulsion stability.
[0008] The present invention adopts the following technical solution:
[0009] A starch-containing bio-based dry strength agent, comprising the following components by weight:
[0010] 15-40 parts starch;
[0011] 20-45 parts of bio-based acrylamide;
[0012] 1-10 parts of comonomer;
[0013] 0.05~0.3 parts of the redox complex initiation system;
[0014] 0.2 to 1 part of the complex chain transfer and stabilization system;
[0015] Viscosity locking agent 0.01~1 part;
[0016] 40-70 parts deionized water;
[0017] A suitable amount of pH adjuster.
[0018] Preferably, the comonomer is itaconic acid or acrylic acid.
[0019] As a preferred option, the redox complex initiation system includes hydrogen peroxide and ascorbic acid.
[0020] Preferably, the composite chain transfer and stabilization system comprises, by weight parts:
[0021] Sodium hypophosphite 0.1-0.5 parts;
[0022] 0.2 to 1 part of glycerol or sorbitol.
[0023] This invention also provides a method for preparing the starch-containing bio-based dry strength agent as described above, comprising:
[0024] (1) Starch pregelatinization and degradation
[0025] Starch is mixed with deionized water, gelatinized, and then hydrolyzed with α-amylase.
[0026] (2) Starch-acrylamide mixture
[0027] Cool the starch solution after degradation in step (1), add bio-based acrylamide, comonomer, complex chain transfer and stabilization system, stir evenly, and adjust the pH to 5 to 6.5;
[0028] (3) Low-temperature copolymerization and online viscosity monitoring
[0029] The mixture is transferred to a reactor equipped with an online viscometer. After nitrogen purging to remove oxygen, a composite initiation system is added. The reaction temperature is controlled at 40-55℃ to allow the hydroxyl groups on the starch backbone to undergo graft copolymerization with the amide groups of acrylamide.
[0030] (4) Target viscosity locking
[0031] When the online viscosity reaches the preset target value, a viscosity-locking agent is added to terminate the polymerization and lock the viscosity.
[0032] (5) Post-polymerization eliminates and reduces residues
[0033] A composite initiation system is added as a redox post-treatment agent to induce the polymerization or decomposition of residual monomers.
[0034] (6) Filtering and discharging
[0035] Cool to room temperature and filter to obtain the starch-containing bio-based dry strength agent.
[0036] The key role of starch and molecular design in this invention
[0037] In this invention, starch (preferably cationic starch or amphoteric starch) serves as a bio-based framework and has the following three core functions.
[0038] First, it enhances the effect. Starch molecules contain a large number of hydroxyl groups, which can form hydrogen bonds with pulp fibers. At the same time, its long-chain structure can act as an "anchor" to synergistically bridge with acrylamide copolymers. Experiments have shown that adding the starch-containing dry strength agent of this invention increases the tensile index of paper by 20-35% compared with the starch-free dry strength agent, and also significantly improves the interlayer bonding strength.
[0039] Second, it stabilizes the emulsion. Pregelatinized starch possesses emulsifying and dispersing properties, capable of encapsulating polymer particles and preventing agglomeration and sedimentation. Products prepared using the method of this invention maintain a homogeneous emulsion state even after six months at room temperature, exhibiting no stratification or sedimentation, thus solving the instability problem of traditional starch-containing dry strength agents prone to stratification.
[0040] Third, viscosity control. The molecular weight and amount of starch added directly affect the viscosity of the product. By controlling the degree of starch degradation (i.e., the decrease in starch viscosity) and the ratio of starch to monomers, a wide range of viscosity adjustments can be achieved with low chain transfer agent dosages, thus avoiding the overuse of chemical chain transfer agents, which is both environmentally friendly and economical.
[0041] Compared with starch-free dry strength agents, the starch-containing dry strength agent of the present invention has significant advantages in several aspects.
[0042] In terms of paper strengthening effect, starch-free dry strength agents can only increase the tensile index of paper by about 12%, while the starch-containing dry strength agent of this invention can increase the tensile index by 28% to 35%, and the interlayer bonding strength is also increased by more than 25%.
[0043] Regarding emulsion stability, starch-free products show stratification or precipitation after one month of storage at room temperature, while the product of this invention remains uniform and stable without any stratification after six months of storage under the same conditions.
[0044] Regarding viscosity controllability, the viscosity of starch-free products is only adjustable within a range of 100 to 600 mPa·s and is difficult to control, with large batch-to-batch deviations. The product of this invention can linearly adjust the viscosity within a wide range of 50 to 1500 mPa·s by adjusting the degree of starch hydrolysis and the proportion of starch added, with the relative deviation between batches controlled within ±5%.
[0045] Regarding the stability of the polymerization process, starch-free systems are prone to a sudden increase in viscosity or even gelation, while the polymerization process of this invention is stable and completely free of gelation due to the degradation of starch and the stabilizing effect of glycerol.
[0046] Regarding the bio-based content, the bio-based carbon content of the product of this invention can reach more than 55%, which is significantly higher than that of starch-free products.
[0047] This invention successfully prepared a starch-containing bio-based dry strength agent through starch pregelatinization and moderate degradation, copolymerization under a composite initiation system, and online viscosity-stability synergistic control. This agent not only significantly improves paper strength but also exhibits excellent emulsion stability (no stratification for 6 months), precise controllable viscosity over a wide range, and achieves low-temperature aqueous phase green polymerization.
[0048] Preferably, in step (1), starch is mixed with a portion of deionized water and gelatinized at 85-90 degrees Celsius for 30 minutes. Then, α-amylase is added, with the amount of α-amylase being 0.01%-0.1% of the starch mass. The mixture is then hydrolyzed at 70-75 degrees Celsius for 10-20 minutes, and the viscosity of the starch is controlled to be 100-500 mPa·s. After hydrolysis, the temperature is raised to 95 degrees Celsius and held for five minutes to inactivate the enzyme.
[0049] Preferably, in step (2), the starch solution degraded in step (1) is cooled to 50 degrees Celsius.
[0050] Preferably, in step (4), the preset target value for viscosity is 500 ± 30 mPa·s when the solid content is 20%.
[0051] Preferably, in step (4), the amount of viscosity locking agent is 0.01 to 0.05% of the total mass of the monomer.
[0052] Preferably, in step (5), the reaction is carried out at 60 degrees Celsius for 30 minutes.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] (1) Significantly improved enhancement effect. The graft copolymer of starch and acrylamide, in conjunction with the fiber hydrogen bonds and ionic bonds, increases the tensile index of paper by 28% to 35%, which is far superior to the 12% to 18% increase of starch-free products.
[0055] (2) Excellent emulsion stability. Pregelatinized and moderately degraded starch acts as a natural emulsifier and stabilizer, preventing polymer particle agglomeration. The product does not separate or precipitate after six months of storage at room temperature, completely solving the industry problem of easy separation of starch-containing dry strength agents.
[0056] (3) Viscosity is precisely controllable. By adjusting the degree of starch enzymatic hydrolysis (controlling the viscosity of starch itself) and the ratio of starch to monomer, the viscosity of the product can be linearly controlled in a wide range of 50 to 1,500 mPa·s without relying on a large amount of chemical chain transfer agent, and the control accuracy can reach within ±5%.
[0057] (4) The polymerization process is gel-free, safe and stable. The degradation treatment of starch and the plasticizing effect of glycerol significantly reduce the viscosity growth rate of the polymerization system, completely avoid the gelation phenomenon, and improve the safety and repeatability of production. Detailed Implementation
[0058] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0059] 1. Raw material composition (by weight)
[0060] The raw materials for the dry strength agent in this embodiment include the following components:
[0061] 15-40 parts starch, 20-45 parts bio-based acrylamide, 0.1-10 parts comonomer (such as itaconic acid or acrylic acid), 0.05-0.3 parts complex initiation system (redox initiator), complex chain transfer and stabilization system including 0.01-0.5 parts sodium hypophosphite and 0.2-1 parts glycerol or sorbitol, 0.01-0.1 parts viscosity lock agent (polymerization inhibitor), 40-70 parts deionized water, and an appropriate amount of pH adjuster to adjust the pH to 5 to 6.5.
[0062] 2. Preparation steps (emphasizing starch treatment and copolymerization)
[0063] Step 1: Starch pregelatinization and moderate degradation.
[0064] Starch is mixed with a portion of deionized water and gelatinized at 80–90°C for 30 minutes. Then, α-amylase is added at a concentration of 0.01–0.1% of the starch mass, and enzymatic hydrolysis is performed at 70–75°C for 10–20 minutes, controlling the starch viscosity to 100–500 mPa·s (measured as a 5% aqueous solution at 25°C). After hydrolysis, the temperature is raised to 95°C and held for five minutes to inactivate the enzyme. This step reduces the starch molecular weight to a suitable range of 50,000–200,000 weight-average molecular weight, preserving hydroxyl activity while avoiding excessively high viscosity during subsequent copolymerization.
[0065] Step 2: Mix starch and acrylamide.
[0066] The degraded starch solution was cooled to 50 degrees Celsius, and bio-based acrylamide, comonomer, glycerol (as a stabilizer), and a small amount of sodium hypophosphite (if further viscosity reduction is required) were added. The mixture was stirred until homogeneous, and the pH was adjusted to 5 to 6.5. At this point, the mixture was a homogeneous, transparent or slightly turbid emulsion with no phase separation.
[0067] Step 3: Low-temperature copolymerization and online viscosity monitoring.
[0068] The mixture was transferred to a reactor equipped with an online viscometer. After nitrogen purging to remove oxygen, a composite initiation system (ammonium persulfate and sodium bisulfite) was added, and the reaction temperature was controlled between 45 and 55 degrees Celsius. During polymerization, the hydroxyl groups on the starch backbone graft copolymerized with the amide groups of acrylamide, forming a stable "starch-polyacrylamide" interpenetrating network or graft copolymer. Because the starch had undergone pre-degradation treatment and glycerol acted as a plasticizer and stabilizer, the system viscosity increased smoothly without sudden gelation. The online viscometer provided real-time viscosity data, and trace amounts of glycerol or water were added as needed to adjust the system's flowability.
[0069] Step 4: Target viscosity locking.
[0070] When the online viscosity reaches the preset target value (e.g., 500 ± 30 mPa·s at 20% solids content), immediately add a viscosity-locking agent at a dosage of 0.01 to 0.05% of the total monomer mass to quickly terminate the polymerization and lock the viscosity. The presence of starch makes the locking more sensitive because the free radicals on the starch chain have a shorter lifetime.
[0071] Step 5: Post-polymerization eliminates and reduces residues.
[0072] A redox post-treatment agent composed of hydrogen peroxide and ascorbic acid is added, and the reaction is carried out at 60 degrees Celsius for 30 minutes to further polymerize or decompose the residual monomers. The final total monomer conversion rate can reach over 99.2%, and the total amount of residual monomers is less than 0.3%.
[0073] Step Six: Filtering and Discharging.
[0074] Cool to room temperature and filter to remove any trace amounts of gel (if any), yielding a starch-containing bio-based dry strength agent product. The product is a milky white, homogeneous emulsion without precipitation and does not separate into layers after standing at room temperature for six months.
[0075] Step 7: Low COD reuse of washing water.
[0076] The washing water from the reactor is collected, hydrogen peroxide and ferrous ions are added for Fenton oxidation, and then the pH is adjusted to neutral after adsorption by activated carbon. It is then reused as feed water for the next batch of polymerization reaction, with a reuse rate of over 90%.
[0077] Example 1 (Medium Viscosity General Purpose Product)
[0078] Take 25 parts of cationic starch and gelatinize and enzymatically hydrolyze it according to the above steps. After enzymatic hydrolysis, the viscosity of the starch itself is 200 mPa·s. Then, mix the degraded starch with 35 parts of bio-based acrylamide, 5 parts of itaconic acid, 0.5 parts of glycerol, 0.2 parts of sodium hypophosphite, and 50 parts of deionized water, and adjust the pH to 5.5. Add 0.05 parts of ammonium persulfate and 0.03 parts of sodium bisulfite, and carry out a polymerization reaction at 50 degrees Celsius. The online viscometer shows that when the reaction proceeds for about 2.5 hours, the viscosity of the system reaches 800 mPa·s (based on a solid content of 20%). Immediately add 0.02 parts of vitamin C to lock in the viscosity. After a 30-minute post-polymerization elimination treatment, the final product viscosity is 795 mPa·s, the conversion rate is 99.2%, and the residual acrylamide content is 0.08%. Add this dry strength agent to the corrugated base paper pulp at an addition rate of 0.5% of oven-dry pulp. The resulting paper has a 32% increase in tensile index and a 28% increase in interlayer bond strength. The product was stored at room temperature for six months without any layering or sedimentation.
[0079] Example 2 (High viscosity type, suitable for high-strength packaging paper)
[0080] Take 35 parts of oxidized starch and enzymatically hydrolyze it to control its viscosity to 350 mPa·s. Add 30 parts of bio-based acrylamide (without sodium hypophosphite) and 0.8 parts of glycerol. Control the polymerization temperature at 48 degrees Celsius, with a target viscosity of 1200 mPa·s. The final viscosity after locking is 1180 mPa·s, with 0.15% residual monomer. When added to high-strength corrugated cardboard, the tensile index increases by 38%, and the product remains stable for six months of storage.
[0081] Example 3 (Low viscosity type, suitable for high-speed paper machines)
[0082] Take 15 parts of cationic starch and enzymatically hydrolyze it to a viscosity of 120 mPa·s. Add 42 parts of bio-based acrylamide, 0.4 parts of sodium hypophosphite, and 0.3 parts of glycerol. Polymerize at 52 degrees Celsius, with a target viscosity of 200 Pa·s. After locking, the actual viscosity is 205 mPa·s. The product has good flowability and is easy to pump and meter. After addition, the tensile index of paper still increases by 28%, and it does not separate after six months of storage.
Claims
1. A starch-containing bio-based dry strength agent, characterized in that, The raw materials comprise the following components by weight: 15-40 parts starch; 20-45 parts of bio-based acrylamide; 1-10 parts of comonomer; 0.05~0.3 parts of the redox complex initiation system; 0.2 to 1 part of the complex chain transfer and stabilization system; Viscosity locking agent 0.01~1 part; 40-70 parts deionized water; A suitable amount of pH adjuster.
2. The starch-containing bio-based dry strength agent according to claim 1, characterized in that, The comonomer is itaconic acid or acrylic acid.
3. The starch-containing bio-based dry strength agent according to claim 1, characterized in that, The redox complex initiation system includes hydrogen peroxide and ascorbic acid.
4. The starch-containing bio-based dry strength agent according to claim 1, characterized in that, The composite chain transfer and stabilization system comprises, by weight parts: Sodium hypophosphite 0.1-0.5 parts; 0.2 to 1 part of glycerol or sorbitol.
5. A method for preparing a starch-containing bio-based dry strength agent as described in any one of claims 1 to 4, characterized in that, include: (1) Starch pregelatinization and degradation Starch is mixed with deionized water, gelatinized, and then hydrolyzed with α-amylase. (2) Starch-acrylamide mixture Cool the starch solution after degradation in step (1), add bio-based acrylamide, comonomer, complex chain transfer and stabilization system, stir evenly, and adjust the pH to 5 to 6.5; (3) Low-temperature copolymerization and online viscosity monitoring The mixture is transferred to a reactor equipped with an online viscometer. After nitrogen purging to remove oxygen, a composite initiation system is added. The reaction temperature is controlled at 40-55℃ to allow the hydroxyl groups on the starch backbone to undergo graft copolymerization with the amide groups of acrylamide. (4) Target viscosity locking When the online viscosity reaches the preset target value, a viscosity-locking agent is added to terminate the polymerization and lock the viscosity. (5) Post-polymerization eliminates and reduces residues A composite initiation system is added as a redox post-treatment agent to cause the residual monomers to polymerize or decompose. (6) Filtering and discharging Cool to room temperature and filter to obtain the starch-containing bio-based dry strength agent.
6. The method for preparing the starch-containing bio-based dry strength agent according to claim 5, characterized in that, In step (1), starch is mixed with some deionized water and gelatinized at 85-90 degrees Celsius for 30 minutes. Then, α-amylase is added, with the amount of α-amylase being 0.01%-0.1% of the starch mass. The mixture is then hydrolyzed at 70-75 degrees Celsius for 10-20 minutes, and the viscosity of the starch is controlled to be 100-500 mPa·s. After hydrolysis, the temperature is raised to 95 degrees Celsius and held for five minutes to inactivate the enzyme.
7. The method for preparing the starch-containing bio-based dry strength agent according to claim 5, characterized in that, In step (2), the starch solution degraded in step (1) is cooled to 50 degrees Celsius.
8. The method for preparing the starch-containing bio-based dry strength agent according to claim 5, characterized in that, In step (4), the preset target value for viscosity is 500 ± 30 mPa·s when the solid content is 20%.
9. The method for preparing the starch-containing bio-based dry strength agent according to claim 5, characterized in that, In step (4), the amount of viscosity locking agent used is 0.01~0.05% of the total mass of the monomer.
10. The method for preparing the starch-containing bio-based dry strength agent according to claim 5, characterized in that, In step (5), the reaction is carried out at 60 degrees Celsius for 30 minutes.