Multi-environment responsive intelligent heat-sensitive paper, preparation method and application

By integrating humidity and pH response indicator layers onto thermal paper, the problem of single response in traditional thermal paper is solved, enabling the integration and logical recording of multi-parameter environmental information, which is suitable for food and drug packaging and cold chain logistics monitoring.

CN123153307APending Publication Date: 2026-11-24HUNAN DINGYIYUAN TECH DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611269084.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing thermal paper can only respond to temperature stimuli and cannot integrate environmental information such as humidity and pH value. Furthermore, existing additional function solutions increase costs and separate information, making it impossible to achieve logical recording.

Method used

Humidity and pH response indicator layers are integrated into thermal paper. Interference is avoided through physical spatial separation and material selection. A semi-permeable protective layer is used for protection, enabling multiple environmental responses.

Benefits of technology

It achieves independent responses to temperature, humidity, and pH, provides comprehensive environmental information, supports logic decoding for environmental failure analysis, and is suitable for food and drug packaging and cold chain logistics monitoring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153307A_ABST
    Figure CN123153307A_ABST
Patent Text Reader

Abstract

This invention relates to the field of thermal recording materials technology, specifically to a multi-environmentally responsive smart thermal paper, its preparation method, and its applications. The thermal paper includes a humidity response indicator layer and a pH response indicator layer; the humidity response indicator layer is located on either side of the main thermal color-developing layer, and the pH response indicator layer is located on the side of the main thermal color-developing layer away from the substrate; on the plane of the main thermal color-developing layer, the projections of the humidity response indicator layer and the pH response indicator layer are independent of each other. This thermal paper simultaneously possesses the ability to respond to multiple key environmental parameters such as temperature, humidity, and pH value, providing users with logical decoding basis to distinguish possible causes of product degradation. Through scientific spatial layering design and material selection, chemical interference and color overlap between response layers are avoided, ensuring the independence and clarity of each response signal without affecting the basic functions of thermal printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermal recording materials technology, and more specifically, to a multi-environmentally responsive smart thermal paper, its preparation method, and its applications. Background Technology

[0002] With the rapid development of the Internet of Things (IoT) and smart packaging technologies, the demand for smart label materials that can record and indicate the environmental history of products is increasing. In particular, in the logistics and storage of pharmaceuticals, vaccines, fresh food and precision electronic products, the compliance of environmental parameters such as temperature, humidity and chemical pollution is directly related to product quality and end-use safety. Thermal paper, as one of the most widely used information recording media, is an ideal substrate for carrying such smart functions.

[0003] However, traditional thermal paper technology is based on the thermal melting reaction of colorless dyes and color developers. Its function is completely limited to the response to the single physical stimulus of temperature. It can only be used to record graphic information or thermal history and cannot provide any information about humidity or chemical contamination.

[0004] Currently, the industry has made many attempts to expand the functions of thermal paper. For example, antibacterial agents are added to the thermal coating to achieve passive protection, or photochromic materials are added for ultraviolet anti-counterfeiting verification. In recent years, some independent indicator labels for environmental humidity or specific gases have also emerged, such as humidity indicator cards made of salts such as cobalt chloride, and oxygen or carbon dioxide indicator labels made of specific chemicals. However, these solutions are all additional items independent of thermal recording paper. They not only increase costs and labeling processes, but more importantly, their recorded information is separate from the graphic information of thermal paper, making it impossible to achieve synchronous association and traceability of the two on the same sheet of paper.

[0005] Furthermore, the anti-counterfeiting and antibacterial functions in existing thermal paper technologies with additional features are passive or triggered applications, rather than being used to actively record and differentiate environmental failure modes. Therefore, they cannot solve the technical problem of integrated and logical recording of multiple parameters such as temperature, humidity, and pH. How to integrate the response functions of three key environmental parameters affecting the lifespan of goods—temperature, humidity, and chemical pollution—on a single thermal paper and perform logical decoding through a combination of color development states remains a gap that has not been addressed by existing technologies. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a multi-environmentally responsive smart thermal paper, its preparation method and application.

[0007] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: This invention provides a multi-environmentally responsive smart thermal paper, comprising a substrate on which a main thermal color-developing layer is provided; and further comprising a humidity response indicator layer and a pH response indicator layer; The humidity response indicator layer is located on either side of the main thermal color-developing layer, and the pH response indicator layer is located on the side of the main thermal color-developing layer away from the substrate; on the plane where the main thermal color-developing layer is located, the projections of the humidity response indicator layer and the pH response indicator layer are independent of each other.

[0008] Based on the above technical solution, the present invention can be further improved as follows.

[0009] Furthermore, the humidity response indicator layer is an irreversible wet-induced color-changing material, and the pH response indicator layer is an irreversible pH-induced color-changing material.

[0010] Furthermore, it also includes a semi-permeable protective layer; the semi-permeable protective layer is located on the pH response indicator layer and completely covers the main thermosensitive color development layer.

[0011] Furthermore, the material of the semi-permeable protective layer is a cellulose acetate semi-permeable membrane, a polyvinyl alcohol film, a microporous polypropylene film, or a silicone coating.

[0012] Furthermore, the material of the humidity response indicator layer includes a deliquescent hygroscopic salt, a latent acid generator, and a colorless dye; or, the material of the humidity response indicator layer includes a cobalt salt complex.

[0013] Furthermore, the material of the pH response indicator layer includes microcapsules encapsulating a pH indicator and a locked reactant; The capsule wall material of the microcapsules includes polymeric MDI, urea-formaldehyde, melamine-formaldehyde, gelatin, or gum arabic. The pH indicator includes natural pigment pH indicators or chemical pH indicators; The locking reactant is a metal ion or a borate; the metal ion is at least one selected from zinc ions, copper ions, iron ions, calcium ions, aluminum ions, manganese ions, or lead ions; and the borate is at least one selected from sodium borate, metaborate, or perborate. Furthermore, the D of the microcapsules 50 The microcapsules have a diameter of 1.0–5.0 μm and a density of D. 90 The microcapsules are less than or equal to 10.0 μm and have an encapsulation efficiency of 80%–95%.

[0014] The present invention also provides a method for preparing a multi-environmentally responsive smart thermal paper as described above, including the steps of preparing the humidity response indicator layer and the pH response indicator layer on the main thermal color development layer.

[0015] This invention also provides the application of the aforementioned multi-environmentally responsive smart thermal paper as a medium for environmental history recording and failure mode analysis.

[0016] This invention also provides a method for detecting the environmental history of a product using the aforementioned multi-environmentally responsive smart thermal paper, characterized by comprising the following steps: Thermal printing is performed on the main thermal color-developing layer of the smart thermal paper to record graphic and textual information, and the initial optical state of the main thermal color-developing layer, the humidity response indicator layer, and the pH response indicator layer is obtained. After the product has undergone storage or transportation, the change in optical density ΔOD or color difference ΔE* of the main thermal colorimetric layer, the humidity response indicator layer and the pH response indicator layer relative to their respective initial optical states is measured. Compare each ΔOD or ΔE* with its corresponding preset judgment threshold; The environmental history and failure mode of the product are determined based on the comparison results of the main thermal color-developing layer, the humidity response indicator layer, and the pH response indicator layer. The determination method is as follows: When only the main thermal color-developing layer is in a color-developing state, it is considered normal; When the main thermal color-developing layer and the humidity response indicator layer are both in a color-developing state, while the pH response indicator layer is in a non-color-developing state, it is determined to be high humidity or damp exposure. When the main thermosensitive color-developing layer and the pH response indicator layer are both in a color-developing state, while the humidity response indicator layer is in a non-color-developing state, it is determined that the liquid is in contact with corrosive or polluting liquid. When the main thermal color-developing layer, the humidity response indicator layer, and the pH response indicator layer are all in a color-developing state, it is determined to be a severe environmental degradation.

[0017] The beneficial effects of this invention are as follows: (1) The multi-environmental responsive smart thermal paper of the present invention breaks through the limitation of traditional thermal paper only responding to a single stimulus of temperature. By integrating independent response functions to three key environmental parameters—temperature, humidity, and pH value—on the same sheet of paper, it can provide comprehensive and multi-dimensional environmental safety information and achieve a complete record of complex environmental history. (2) The multi-environment response type smart thermal paper of the present invention avoids chemical interference and color overlap between different response layers through the multi-layer structure design of physical space separation and the compatibility screening of each layer material, ensuring the clarity, stability and independence of each response signal of temperature, humidity and pH, while not sacrificing the original graphic printing performance of thermal paper. (3) The multi-environment response type intelligent thermal paper of the present invention utilizes the independent color development states of the three-layer response system and their combination to construct an environmental failure analysis mechanism that can be logically decoded, so that users can not only identify the environmental anomalies of the product, but also distinguish different failure modes such as high temperature and high humidity exposure and chemical pollution, providing key data support for quality traceability and problem location. (4) The multi-environmentally responsive smart thermal paper of the present invention uses a semi-permeable composite protective layer as the outermost layer. While effectively protecting each functional layer from mechanical damage and liquid water pollution, it allows water vapor and acidic or alkaline gas molecules to pass through to trigger the internal response layer, thus taking into account both structural protection and the sensitivity of environmental response. (5) The multi-environmental responsive smart thermal paper of the present invention upgrades traditional thermal paper from a low-value-added graphic record consumable to a high-value-added smart environmental history record and logic analysis platform, which is particularly suitable for food and drug packaging, medical sterilization indication and cold chain logistics monitoring fields with extremely high requirements for safety and quality traceability. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of the layer structure of a multi-environmentally responsive smart thermal paper according to the present invention; Figure 2 This is a schematic diagram of another layer structure of the multi-environmentally responsive smart thermal paper of the present invention.

[0019] The attached diagram lists the components represented by each number as follows: 1. Substrate; 2. Main thermosensitive color development layer; 3. Humidity response indicator layer; 4. pH response indicator layer; 5. Semi-permeable protective layer. Detailed Implementation

[0020] The principles and features of the present invention are described below. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.

[0021] like Figure 1-2 As shown, the multi-environment-responsive smart thermal paper of the present invention includes a substrate 1, on which a main thermal color-developing layer 2 is provided; it also includes a humidity response indicator layer 3 and a pH response indicator layer 4; the humidity response indicator layer 3 is located on any side of the main thermal color-developing layer 2, and the pH response indicator layer 4 is located on the side of the main thermal color-developing layer 2 away from the substrate 1; on the plane where the main thermal color-developing layer 2 is located, the projections of the humidity response indicator layer 3 and the pH response indicator layer 4 are independent of each other.

[0022] This invention relates to a multi-environmental responsive smart thermal paper. Temperature, humidity, and pH responses are designed within physically independent and spatially separated coatings, forming a "multi-layered spatially separated" integrated architecture. This achieves multiple responses without mutual interference. In this thermal paper, the main thermal color-developing layer 2 records conventional images and text; the humidity response indicator layer 3 generates an irreversible color change when the relative humidity exceeds a preset threshold; and the pH response indicator layer 4 generates an irreversible color change when the environmental acidity or alkalinity changes. This "spatial encoding" ensures that the three types of color signals do not overlap, facilitating independent observation and interpretation by the user.

[0023] In this invention, the projections of the humidity response indicator layer 3 and the pH response indicator layer 4 are independent of each other, meaning that the two do not overlap, to prevent their color changes from affecting each other and causing detection and judgment failure.

[0024] Preferably, the multi-environmentally responsive smart thermal paper of the present invention further includes a semi-permeable protective layer 5; it is located on the pH response indicator layer 4 and completely covers the main thermal color development layer 2.

[0025] Preferably, the semi-permeable protective layer 5 is made of a semi-permeable material, which allows water vapor and gas molecules to pass through to trigger the humidity response indicator layer 3 and the pH response indicator layer 4, while blocking liquid water and oil. This layer protects each functional layer from mechanical damage and liquid water contamination, while allowing water vapor and acid / alkaline gas molecules to pass through and trigger the reaction of the internal response layer.

[0026] Preferably, the water vapor permeability of the semi-permeable protective layer 5 is 150–500 g / (m²). 2 •24h), liquid water hydrostatic pressure withstands ≥50 cm H2O.

[0027] Preferably, the semi-permeable material is a cellulose acetate semi-permeable membrane, a polyvinyl alcohol (PVA) film, a microporous polypropylene film, or a silicone coating.

[0028] Preferably, the semi-permeable material is a cellulose acetate semi-permeable membrane.

[0029] Preferably, the thickness of the semi-permeable protective layer 5 is 2 μm.

[0030] The humidity response indicator layer 3 of the present invention is a wet-induced color-changing material, and existing materials can be used directly. The selection criteria are that the response humidity threshold is adjustable and the color change is irreversible.

[0031] Preferably, the response trigger threshold of the humidity response indicator layer 3 is 70% RH±5% (25℃), specifically referring to the lowest RH that is visible to the naked eye (ΔE*≥5) after 24 hours of constant temperature and humidity chamber RH gradient placement; the complete color change humidity is ≥90% RH (25℃), specifically referring to color saturation (ΔE*≥20) after 24 hours of placement.

[0032] The wet-sensitive color-changing material of the humidity response indicator layer 3 can also be non-existent materials, including cobalt-free chemical locking systems, cobalt-containing systems, and other systems.

[0033] The cobalt-free chemical locking system comprises deliquescent hygroscopic salts, latent acid generators, and colorless dyes. Its humidity response principle is as follows: when the relative humidity exceeds a preset threshold, the deliquescent hygroscopic salts in the humidity response zone accumulate moisture, triggering the latent acid generator to release acid (or activating the latent chromogenic component). The released acid undergoes an irreversible colorimetric reaction with the colorless dye—the dye lactone ring irreversibly opens and is subsequently locked by addition / coupling / chelation, generating a stable chromophore. This chromophore does not revert after environmental dehumidification, thus faithfully recording any previous high-humidity exposure.

[0034] Preferably, the mass ratio of the deliquescent hygroscopic salt, the latent acid generating agent, and the colorless dye is (2-5):(3-8):(5-10); the deliquescent hygroscopic salt can be LiCl, MgCl2, NaCl, etc., the latent acid generating agent can be a sulfonate ester (methyl p-toluenesulfonate) or an anhydride (phthalic anhydride), and the colorless dye can be ODB-2, CVL, or GN-2.

[0035] The cobalt-containing system primarily consists of cobalt salt complexes, along with organic solvents and binders. Its humidity-responsive principle is as follows: In low-humidity environments, the cobalt salt complexes exist in a specific coordination form, exhibiting a color (e.g., blue). When the ambient humidity rises above a threshold, water molecules, acting as ligands, enter the coordination layer of cobalt ions, altering the coordination field and causing an irreversible color change (e.g., turning pink). This change is irreversible due to the rearrangement of the coordination structure.

[0036] Preferably, the cobalt salt complex is a cobalt chloride-hexamethylenetetramine complex, the organic solvent is anhydrous ethanol, and the binder is an aqueous polyurethane binder, with a mass ratio of 5:20:10.

[0037] Other moisture-sensitive materials, such as certain crystal violet lactone derivatives, certain metal oxide films, or conjugated polymers containing hydrophilic groups, can also achieve humidity-responsive color change.

[0038] The pH response indicator layer 4 of the present invention is a color-changing material containing a pH indicator and a locking reactant, which is used to produce an irreversible color change when the surface of the smart thermal paper comes into contact with acidic or alkaline liquids, or when a local pH change is formed due to the dissolution of acidic / alkaline gases in the surrounding environment on the surface and the adsorption of moisture.

[0039] pH indicators can be existing natural pigment pH indicators (such as anthocyanins, curcumin, etc.) or chemical pH indicators (such as phenolphthalein, bromocresol green, etc.); indicators with different color change ranges can be selected to suit different application scenarios. For example, methyl red (color change range pH 4.4-6.2, red to yellow) can be used to detect acidic leaks, and phenolphthalein (pH 8.2-10.0, colorless to red) or thymolphthalein can be used to detect alkaline leaks.

[0040] The locking reactants are metal ions or borates. The metal ions are at least one of zinc ions, copper ions, iron ions, calcium ions, aluminum ions, manganese ions, or lead ions, and the borates are at least one of sodium borate, metaborate, or perborate.

[0041] The principle behind metal ions acting as locking reactants is that when a pH indicator changes color upon contact with acidic or alkaline liquids, the metal ions form stable coordination complexes (chelates) with the indicator molecules, "locking" the color change and preventing it from reverting to its original state due to liquid evaporation or neutralization. Borates, on the other hand, can achieve irreversible color locking by forming borate ester bonds with pH indicators containing ortho-biphenol structures.

[0042] Preferably, the lock reactant and pH indicator are mixed in a mass ratio of (1-3):(0.5-2).

[0043] Specifically, for different pH indicators, the preferred types of locking reactants, the dosage per unit of pH indicator, and the mechanism of action are shown in the table below: Table 1 pH indicators and locking reactants can be directly coated to form a pH response indicator layer 4, or they can be chemically bonded to the surface of fibers or microspheres to form reactive fillers, which are then added to the coating. Alternatively, they can be pre-encapsulated in a microcapsule structure to isolate them from the outside world under normal conditions.

[0044] After the microcapsule structure is formed, when corrosive or contaminating acidic / alkaline liquids penetrate the thermal paper and come into contact with the microcapsules, the capsule wall ruptures, and the released pH indicator comes into contact with the liquid and undergoes an irreversible color reaction with the locked reactants in the capsule core, generating a stable colored state that does not recover with the evaporation / neutralization of the liquid, thereby recording chemical contamination / leakage events.

[0045] Preferably, the capsule wall material includes polymeric MDI, urea-formaldehyde, melamine-formaldehyde, gelatin, or gum arabic. Preferred, D of microcapsules 50 The diameter is 1.0–5.0 μm, D 90 Less than or equal to 10.0 μm, with an encapsulation efficiency of 80%–95%.

[0046] The main thermosensitive color-developing layer 2 of the present invention can be made of existing thermosensitive color-developing materials.

[0047] Preferably, the initial color development temperature T0 of the main thermal color development layer 2 is 70–80℃, the optimal color development temperature T is 100–120℃, and the color development sensitivity is OD≥1.40 when the printing energy is ≤0.45 mJ / dot.

[0048] The thermal color-developing material of the main thermal color-developing layer 2 includes colorless dyes and color developers, which are used to form graphic information under the action of the thermal printhead.

[0049] Preferably, the colorless dye includes BK-15, and the color developer includes bisphenol A.

[0050] Preferably, the material of the main thermal color-developing layer 2 also includes a sensitizer (such as phenyl benzoate, 1,2-diphenoxyethane) and a binder (such as polyvinyl alcohol).

[0051] Preferably, the mass parts of each component of the main heat-sensitive color-developing layer 2 are as follows, based on mass parts: 5-10 parts of colorless dye, 10-40 parts of color developer, 10-40 parts of sensitizer, and 4-20 parts of binder; wherein, based on 1 part of colorless dye, the amount of sensitizer is 0.8-1.5 parts.

[0052] The substrate 1 of this invention is paper or dense PET.

[0053] The preparation method of the multi-environmentally responsive smart thermal paper of the present invention includes the steps of preparing a humidity response indicator layer 3 and a pH response indicator layer 4 on the main thermal color development layer 2, and also includes the step of preparing a semi-permeable protective layer 5.

[0054] Specifically, the preparation method includes the following steps: S1. Preparation of the main heat-sensitive color-developing coating layer Colorless dyes, color developers, sensitizers, and binders are mixed, ground, and dispersed in a certain proportion to obtain the main heat-sensitive coating.

[0055] Preferably, the particle size of the milled material is less than or equal to 1 μm.

[0056] S2. Preparation of humidity-responsive indicator coating The wet-sensitive material is mixed with binder and solvent, and stirred evenly in the dark to obtain a humidity-responsive coating.

[0057] S3. Preparation of pH-responsive indicator coating A coating is prepared by dissolving a pH indicator and a locking reactant in a suitable solvent and mixing them with a binder. This coating can be applied directly.

[0058] When microencapsulation is used, pH indicators and locking reactants are dissolved in a suitable solvent, mixed with binders and wall materials (for microencapsulation), and pH-responsive microcapsule emulsions are prepared by an emulsification-curing method.

[0059] Preferably, the pH indicator and locking reactant are dissolved in ethyl acetate, and the wall material monomer is added to obtain an oil phase. This oil phase is then dispersed in an aqueous phase containing 2 wt% PVA under high-speed shear, and the mixture is heated to 60°C and reacted for 2 hours to obtain a microcapsule emulsion containing the pH indicator.

[0060] S4, multi-layer coating.

[0061] On substrate 1, following the designed layer structure sequence, the main heat-sensitive color development layer coating is applied and cured sequentially using methods such as bar coating, scraping coating, or gravure coating; the humidity response indicator layer coating is applied and cured; and the pH response indicator layer coating is applied and cured.

[0062] Preferably, the coating amount of the main heat-sensitive color-developing layer is 5 g / m² (dry weight), the coating amount of the humidity response indicator layer is 2 g / m² (dry weight), and the coating amount of the pH response indicator layer is 3 g / m² (dry weight).

[0063] Preferably, the curing method is light-protected drying, and the drying temperature is 50℃.

[0064] S5. Prepare a semi-permeable protective layer.

[0065] A semi-permeable protective layer 5 is applied over the coating obtained in step S4, and then dried and cured to obtain the finished smart thermal paper.

[0066] The multi-environmentally responsive smart thermal paper of this invention can be used as a medium for environmental history recording and failure mode analysis; its application scenarios include food and drug packaging, medical sterilization indication, cold chain logistics monitoring, etc.

[0067] The present invention provides a method for detecting the environmental history of a product using multi-environmentally responsive smart thermal paper, comprising the following steps: Thermal printing is performed on the main thermal color development layer 2 of the smart thermal paper to record graphic and text information, and to obtain the initial optical state of the main thermal color development layer 2, humidity response indicator layer 3 and pH response indicator layer 4. After the product has undergone storage or transportation, the optical density change ΔOD or color difference ΔE* of the main thermal color development layer 2, humidity response indicator layer 3 and pH response indicator layer 4 relative to their respective initial optical states are measured respectively; wherein, the optical density change ΔOD is measured by a spectrophotometer and the color difference ΔE* is measured by a colorimeter.

[0068] Compare each ΔOD or ΔE* with its corresponding preset judgment threshold; Preferably, the preset threshold for the humidity response zone and the pH response zone is a color difference ΔE*≥5.

[0069] The environmental history and failure mode of the product are determined based on the comparison results of the main thermal color development layer 2, humidity response indicator layer 3 and pH response indicator layer 4. The determination method is as follows: When only the main thermal color-developing layer 2 is in a color-developing state, it is considered normal; When the main thermal color-developing layer 2 and the humidity response indicator layer 3 are both in a color-developing state, while the pH response indicator layer 4 is in a non-color-developing state, it is determined to be high humidity or exposed to moisture. When the main thermosensitive color-developing layer 2 and the pH response indicator layer 4 are both in a color-developing state, while the humidity response indicator layer 3 is in a non-color-developing state, it is determined that the liquid is in contact with corrosive or polluting liquid. When the main thermal color-developing layer 2, humidity response indicator layer 3, and pH response indicator layer 4 are all in a color-developing state, it is determined to be a serious environmental degradation.

[0070] The effects of the present invention will be specifically illustrated below through specific embodiments: Example 1 The specific layer structure of the thermal paper in this embodiment is as follows: Figure 1 As shown.

[0071] In this embodiment, the substrate 1 is a 70g / m² base paper.

[0072] The preparation process of the main heat-sensitive color-developing layer coating is as follows: take 10 parts of fluorane black dye (BK-15), 15 parts of bisphenol A, 10 parts of sensitizer (phenyl benzoate), and 50 parts of polyvinyl alcohol (PVA-224) aqueous solution (10wt%), grind them in a sand mill until the average particle size is less than 1μm, and set aside for later use.

[0073] The preparation process of the humidity response indicator coating is as follows: Dissolve 5 parts of cobalt chloride-hexamethylenetetramine complex in 20 parts of anhydrous ethanol, add 10 parts of water-based polyurethane binder, stir for 30 minutes in the dark, and set aside.

[0074] The preparation process of pH-responsive indicator microcapsules is as follows: 1 part bromocresol green and 1 part zinc chloride are dissolved in 10 parts ethyl acetate, and 2 parts polymethylene polyphenyl isocyanate are added as wall material monomers. This oil phase is dispersed in an aqueous phase containing 2 wt% PVA under high-speed shear, and the reaction is carried out at 60℃ for 2 hours to obtain a microcapsule emulsion containing a pH indicator. The microcapsules are yellow at pH < 3.8 and blue at pH > 5.4, and the color change is due to Zn... 2+ It forms a stable chelate with bromocresol green, resulting in irreversible locking.

[0075] Multilayer Coating: On the base paper, firstly, a main thermosensitive color-developing layer coating is applied using a rod coater at a coating weight of 5 g / m² (dry weight), and dried at 60°C to obtain the main thermosensitive color-developing layer 2. Then, on one edge area above the main thermosensitive color-developing layer 2, a humidity-responsive indicator layer coating is applied using a slit coater at a coating weight of 2 g / m² (dry weight), and dried at 50°C in the dark to obtain the humidity-responsive indicator layer 3. Next, a pH-responsive microcapsule emulsion is mixed with a PVA solution and applied to the other edge area of ​​the main thermosensitive color-developing layer 2 at a coating weight of 3 g / m² (dry weight), and dried at 50°C to obtain the pH-responsive indicator layer 4.

[0076] Apply a protective layer: Coat the outermost layer with a 2μm thick cellulose acetate semipermeable membrane as a semipermeable protective layer 5.

[0077] The above steps produce a smart thermal paper that can display black text and images, humidity status (blue to pink), and pH pollution status (yellow to blue) in three independent areas.

[0078] Example 2 This embodiment is basically the same as Embodiment 1, except for the implementation method of pH response indicator layer 4.

[0079] Specifically, this embodiment does not prepare microcapsules, but instead directly dissolves a pH indicator (such as phenolphthalein) in an alkaline resin to form a red coating when the pH is greater than 8.2. This method is simpler, but it is necessary to ensure that the coating is completely spatially separated from other layers and does not pre-react with the color-developing agent of the main thermosensitive layer.

[0080] Example 3 This embodiment is basically the same as Embodiment 1, except for the order of the layer structure.

[0081] Specifically, such as Figure 2 As shown, in this embodiment, the humidity response indicator layer 3 is disposed between the substrate 1 and the main thermal colorimetric layer 2. This design utilizes the buffering properties of the substrate 1 to slow down the humidity response speed, enabling the recording of longer-term cumulative high-humidity exposure.

[0082] Comparative Example 1 This comparative example is a commercially available traditional single-temperature-responsive thermal paper, which only contains a substrate layer and a main thermal color developing layer, and has no humidity or pH response function.

[0083] Comparative Example 2 In this comparative example, humidity-responsive material and pH indicator were directly added when preparing the main heat-sensitive color-developing coating, without stratification.

[0084] Result: The coating color was chaotic, the sensitivity of the thermochromic color was greatly reduced, and all response signals could not be identified at all.

[0085] The thermal paper of the above embodiments and comparative examples was subjected to performance tests. The test methods are shown in Table 2, and the test results are shown in Table 3.

[0086] Table 2 Test Methods Table 3 Test Results Results Analysis: Examples 1-3 successfully achieved independent and clear responses to the triple stimuli of temperature, humidity, and pH. Users can accurately infer the environmental state of the product by observing the color combinations in different areas. Comparative Example 1 could only record temperature information. Comparative Example 2 demonstrates that without spatial separation, multiple response materials will interfere with each other, leading to overall functional failure. Example 1 exhibits the best overall performance.

[0087] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A multi-environmentally responsive smart thermal paper, comprising a substrate (1), wherein a main thermal color-developing layer (2) is disposed on the substrate (1); characterized in that, It also includes a humidity response indicator layer (3) and a pH response indicator layer (4); The humidity response indicator layer (3) is located on any side of the main thermal color-developing layer (2), and the pH response indicator layer (4) is located on the side of the main thermal color-developing layer (2) away from the substrate (1); on the plane where the main thermal color-developing layer (2) is located, the projections of the humidity response indicator layer (3) and the pH response indicator layer (4) are independent of each other.

2. The multi-environment responsive smart thermal paper according to claim 1, characterized in that, The humidity response indicator layer (3) is an irreversible wet-induced color-changing material, and the pH response indicator layer (4) is an irreversible pH-induced color-changing material.

3. The multi-environment responsive smart thermal paper according to claim 1, characterized in that, It also includes a semi-permeable protective layer (5); the semi-permeable protective layer (5) is located on the pH response indicator layer (4) and completely covers the main thermosensitive color development layer (2).

4. The multi-environment responsive smart thermal paper according to claim 3, characterized in that, The semi-permeable protective layer (5) is made of cellulose acetate semi-permeable membrane, polyvinyl alcohol film, microporous polypropylene film or silicone coating.

5. A multi-environmentally responsive smart thermal paper according to any one of claims 1-4, characterized in that, The material of the humidity response indicator layer (3) includes a deliquescent hygroscopic salt, a latent acid generator and a colorless dye; or, the material of the humidity response indicator layer (3) includes a cobalt salt complex.

6. A multi-environmentally responsive smart thermal paper according to any one of claims 1-4, characterized in that, The material of the pH response indicator layer (4) includes microcapsules encapsulating a pH indicator and a locked reactant; The capsule wall material of the microcapsules includes polymeric MDI, urea-formaldehyde, melamine-formaldehyde, gelatin, or gum arabic. The pH indicator includes natural pigment pH indicators or chemical pH indicators; The locking reactant is a metal ion or a borate; the metal ion is at least one of zinc ion, copper ion, iron ion, calcium ion, aluminum ion, manganese ion or lead ion, and the borate is at least one of sodium borate, metaborate or perborate.

7. The multi-environment responsive smart thermal paper according to claim 6, characterized in that, The microcapsule's D 50 The microcapsules have a diameter of 1.0–5.0 μm and a density of D. 90 The microcapsules are less than or equal to 10.0 μm and have an encapsulation efficiency of 80%–95%.

8. A method for preparing a multi-environmentally responsive smart thermal paper as described in any one of claims 1-7, characterized in that, The steps include preparing the humidity response indicator layer (3) and the pH response indicator layer (4) on the main thermosensitive color development layer (2).

9. The application of the multi-environmentally responsive smart thermal paper as described in any one of claims 1-7 as a medium for environmental history recording and failure mode analysis.

10. A method for detecting the environmental history of a product using multi-environmentally responsive smart thermal paper as described in any one of claims 1-7, characterized in that, Includes the following steps: Thermal printing is performed on the main thermal color development layer (2) of the smart thermal paper to record graphic information and obtain the initial optical state of the main thermal color development layer (2), the humidity response indicator layer (3) and the pH response indicator layer (4); After the product has been stored or transported, the optical density change ΔOD or color difference ΔE* of the main thermal color rendering layer (2), the humidity response indicator layer (3) and the pH response indicator layer (4) relative to their respective initial optical states are measured. Compare each ΔOD or ΔE* with its corresponding preset judgment threshold; The environmental history and failure mode of the product are determined based on the comparison results of the main thermal color development layer (2), the humidity response indicator layer (3) and the pH response indicator layer (4); The determination method is as follows: When only the main thermal color-developing layer (2) is in a color-developing state, it is judged to be normal; When the main thermal color-developing layer (2) and the humidity response indicator layer (3) are both in a color-developing state, while the pH response indicator layer (4) is in a non-color-developing state, it is determined to be high humidity or exposed to moisture. When the main thermosensitive color-developing layer (2) and the pH response indicator layer (4) are both in a color-developing state, while the humidity response indicator layer (3) is in a non-color-developing state, it is determined that the liquid is in contact with corrosive or polluting liquid. When the main thermal color-developing layer (2), the humidity response indicator layer (3) and the pH response indicator layer (4) are all in a color-developing state, it is determined to be a serious environmental degradation.