A high cohesive stability low-z-direction strength liquid packaging paper and a method for manufacturing the same
By constructing a high-proportion BCTMP core layer, a low beating degree design, and interlayer composite reinforcement, a directional venting channel is built, which solves the contradiction between the Z-direction strength and interlayer adhesion of liquid packaging paper, achieves decoupling of low Z-direction strength and interlayer bonding force, and directional gas release, thus improving the foaming problem of lamination composite.
Patent Information
- Application Number
- CN202611366225.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-24
AI Technical Summary
When improving interlayer adhesion, existing liquid packaging paper results in increased Z-axis strength and decreased air permeability. Stress cannot be released during die-cutting and creasing, and internal gas cannot be released in a directional manner during lamination, causing blistering problems at the creasing lines.
By designing a paper base layer and constructing a coating layer with a specific ratio, a high proportion of BCTMP core layer and a low beating degree design are adopted. Combined with a differential composite reinforcement system between layers, directional exhaust channels are constructed. Highly active aldehyde-based microparticle polymers are used to form chemical covalent bonds, which enhances the interlayer bonding force and releases gas in a directional manner.
This achieves decoupling between low Z-axis strength and interlayer bonding force, reduces paper cohesion, avoids blistering at indentation lines, ensures directional gas release during lamination, and improves paper bonding stability and air permeability.
Smart Images

Figure CN123153309A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of papermaking technology, and more specifically, to a liquid packaging paper with high adhesion stability and low Z-axis strength, a method for preparing the liquid packaging paper with high adhesion stability and low Z-axis strength, and an application of the liquid packaging paper with high adhesion stability and low Z-axis strength. Background Technology
[0002] Liquid packaging paper is a biodegradable and recyclable multi-layered food-grade packaging material. It is widely used in the packaging of beverage cartons such as milk and juice after printing, laminating, and filling the base paper roll.
[0003] In recent years, as liquid packaging paper has developed towards lightweight and high functionality, the industry has faced two prominent performance conflict issues: Firstly, there is a contradiction between interlayer adhesion and Z-axis strength. To prevent fiber layer separation during downstream processing such as printing, lamination, and filling, existing technologies typically increase the beating degree of the pulp to expose more hydrogen bonds, thereby improving interlayer adhesion. However, increasing the beating degree increases the internal fiber weaving density of the paper, strengthens the paper's cohesion, reduces air permeability, and increases Z-axis strength. Excessively high Z-axis strength prevents the effective release of internal stress during downstream die-cutting and creasing, making the crease location prone to problems such as paper surface cracking, crease opening, and blistering at the creasing line. In other words, interlayer adhesion stability and Z-axis strength are positively correlated, constituting an "irreconcilable performance conflict."
[0004] Secondly, there is a conflict between gas release and blistering during the lamination process. Liquid packaging paper undergoes a lamination (extrusion coating) process before being made into packaging boxes. This process is carried out under high temperature and high pressure. If the gas inside the paper cannot be effectively released, it will overflow from the front of the paper, forming blistering or hollow defects at the crease lines, severely affecting the product's appearance and filling seal.
[0005] Therefore, there is an urgent need to develop a liquid packaging paper and its preparation method that can simultaneously achieve interlayer bonding stability and low Z-axis strength, and can control the directional release of gas to eliminate the foaming problem of lamination composite. Summary of the Invention
[0006] To address the technical problems of existing liquid packaging papers that increase beating degree to improve interlayer adhesion, leading to increased Z-axis strength, increased paper cohesion, and reduced air permeability, resulting in stress unreleased during die-cutting and creasing, and preventing directional gas release during lamination, causing bubbling and blurring of the creasing lines, this invention provides a liquid packaging paper with high adhesion stability and low Z-axis strength, a method for preparing such a paper, and its application. Through specific layer ratios and beating degree gradient design, a high proportion of BCTMP in the core layer imparts bulk and compressibility to the paper. Combined with a differentiated interlayer composite reinforcement system, this achieves decoupling between low Z-axis strength and interlayer adhesion. Simultaneously, by strengthening the core layer for air permeability and sealing the front surface with a coating, directional venting channels are constructed, improving filling delamination and lamination bubbling issues.
[0007] In a first aspect, the present invention provides a liquid packaging paper with high adhesion stability and low Z-direction strength, comprising a paper base layer and a coating layer. The paper base layer comprises, from the front to the back, a surface layer, a liner layer, a core layer and a bottom layer, wherein the surface layer, liner layer, core layer and bottom layer are respectively prepared from surface layer slurry, liner layer slurry, core layer slurry and bottom layer slurry. The surface slurry is composed of the following components by mass percentage: 50-60% bleached softwood sulfate pulp and 40-50% bleached hardwood sulfate pulp; in the surface slurry, the freeness of the bleached softwood sulfate pulp is 24-27°SR and the freeness of the bleached hardwood sulfate pulp is 28-31°SR. The lining slurry is composed of the following components by mass percentage: 50-60% bleached softwood sulfate pulp and 40-50% bleached hardwood sulfate pulp; in the lining slurry, the freeness of the bleached softwood sulfate pulp is 23-26°SR, and the freeness of the bleached hardwood sulfate pulp is 28-31°SR. The core pulp is composed of the following components by mass percentage: 40-50% bleached chemithermomechanical pulp, 25-35% bleached softwood sulfate pulp, and 15-35% waste paper; in the core pulp, the freeness of the bleached chemithermomechanical pulp is 15-25°SR, the freeness of the bleached softwood sulfate pulp is 18-24°SR, and the freeness of the waste paper is 30-40°SR. The underlying slurry consists of the following components by mass percentage: 100% unbleached softwood sulfate pulp with a freeness of 19~21°SR; The beating degree of the bleached softwood sulfate pulp in the surface layer slurry, the beating degree of the bleached softwood sulfate pulp in the lining slurry, and the beating degree of the bleached softwood sulfate pulp in the core layer slurry decreases sequentially. A starch-reinforcing layer is provided between the surface layer and the liner, and a composite reinforcing layer is provided between the liner and the core layer and between the core layer and the bottom layer. The composite reinforcing layer contains starch and a microparticle polymer containing highly active aldehyde groups.
[0008] Furthermore, the liquid packaging paper has a front air permeability ≤1.0mL / min, a cross-sectional air permeability ≥1.8mL / min, a Z-direction strength ≤400kPa, and an interlayer bonding force ≥220J / m².
[0009] Furthermore, the total basis weight of the liquid packaging paper is 295~305g / m²; the basis weight of the surface layer of the paper base layer is 45~55g / m², the basis weight of the lining layer is 30~40g / m², and the basis weight of the bottom layer is 45~55g / m².
[0010] Further, the coating layer includes a back coating layer applied to the bottom layer of the paper substrate and a base coating layer, a substrate coating layer, and a top coating layer applied sequentially to the top layer of the paper substrate; the coatings of the base coating layer and the substrate coating layer each independently contain the following components in parts by weight: 10-20 parts latex, 93-100 parts calcium carbonate, and 0-7 parts calcined clay; the coating of the top coating layer contains the following components in parts by weight: 15-20 parts latex, 70-90 parts calcium carbonate, and 10-30 parts kaolin.
[0011] Furthermore, the particulate polymer containing highly active aldehyde groups is glyoxalized polyacrylamide particulates.
[0012] Furthermore, rosin sizing agent is added to the core layer slurry at an amount of 18-25 kg / t slurry.
[0013] In a second aspect, the present invention provides a method for preparing a liquid packaging paper with high adhesion stability and low Z-axis strength as described in any one of the first aspects, comprising the following steps: S1. The components of the surface slurry, lining slurry, core slurry and bottom slurry are crushed, deslag removed, impurity removed, milled and mixed to obtain the surface slurry, lining slurry, core slurry and bottom slurry respectively. S2. After removing sand from each layer of slurry obtained in step S1, spray them onto the wire section for filtration and shaping, and then vacuum dewater them to obtain a wet paper web consisting of a top layer, a liner layer, a core layer, and a bottom layer. Spray starch between the top layer and the liner layer, and spray a mixture of starch and a microparticle polymer containing highly active aldehyde groups between the liner layer and the core layer and between the core layer and the bottom layer. Composite the obtained wet paper webs consisting of the top layer, the liner layer, the core layer, and the bottom layer to obtain a composite wet paper web. S3. The composite wet paper web obtained in step S2 is dehydrated, pressed, pre-dried, sized, post-dried, and hard-calendered to obtain the paper base layer; S4. Prepare a coating on the surface and bottom layers of the paper base obtained in step S3, and then calender it to obtain liquid packaging paper.
[0014] Further, in step S2, the vacuum conditions for vacuum dehydration are -50~0 kPa; in the sprayed starch, the amount of starch sprayed between the surface layer and the liner layer is 1.0~3.0 kg / t slurry, the amount of starch sprayed between the liner layer and the core layer is 3.0~6.0 kg / t slurry, the amount of starch sprayed between the core layer and the bottom layer is 5.0~8.0 kg / t slurry, and the amount of the microparticle polymer containing highly active aldehyde groups used per ton of paper at oven dryness is 0.2~0.5 kg / t slurry, which is added with starch at a concentration of 2%.
[0015] Further, in step S2, the slurry spraying speed ratio to the mesh section is 0.950~0.960, the slurry spraying speed ratio to the mesh section is 0.950~0.960, the core layer slurry spraying speed ratio to the mesh section is 0.980~0.990, and the bottom layer slurry spraying speed ratio to the mesh section is 0.980~0.990.
[0016] Furthermore, in step S3, The pressing includes ordinary pressing, shoe pressing and smooth pressing; the pressure of ordinary pressing is 120~180kN / m, the pressure of shoe pressing is 660~760kN / m, and the pressure of smooth pressing is 10~50kN / m. The pre-drying process utilizes a two-stage stepped heating drying method, with the temperature of the low-temperature stage being 60~100℃ and the temperature of the high-temperature stage being 90~160℃. The post-drying process utilizes a first-stage temperature and a second-stage temperature, with the first-stage temperature being 90~160℃ and the second-stage temperature being 60~100℃. The pressure of the hard calendering is 10~50kN / m.
[0017] Further, the preparation of coatings on the surface layer and the bottom layer of the paper substrate obtained in step S3 includes: applying a primer coating of 8~12 g / m² to the surface layer and drying it to prepare a primer coating; then applying a substrate coating of 6~8 g / m² to the primer coating and drying it to prepare a substrate coating; then applying a top coating of 5~9 g / m² to the substrate coating and drying it to prepare a top coating; and applying a back coating of 0.8~2.2 g / m² to the bottom layer and drying it to prepare a back coating.
[0018] Further, in step S1, rosin sizing agent is added to the core layer slurry at a dosage of 18-25 kg / t slurry. Thirdly, the present invention provides an application of a high-adhesion-stability, low-Z-direction-strength liquid packaging paper according to any one of the first aspects in the preparation of liquid packaging materials or prefabricated liquid packaging boxes.
[0019] Beneficial effects
[0020] This invention achieves the following beneficial effects through systematic structural design and multi-dimensional process synergy: This invention achieves decoupling between low Z-axis strength and interlayer bonding stability. The core layer utilizes a high proportion of bleached chemithermomechanical pulp combined with a low beating design, imparting high bulk and moderate compressibility to the paper. This effectively reduces paper cohesion and Z-axis strength, allowing internal stress to be released through the micro-compression of the fiber network during indentation. Simultaneously, the invention incorporates a starch-and-highly-active aldehyde-containing microparticle polymer composite reinforcement layer between the core and liner layers and between the core and bottom layers. The highly active aldehyde groups of the microparticle polymer form covalent bonds with the fiber hydroxyl groups, compensating for the loss of fiber hydrogen bonding due to the reduced beating. This composite reinforcement layer, in contrast to the interlayer starch reinforcement layer, creates a differentiated design, resulting in a significant reduction in Z-axis strength while simultaneously improving interlayer bonding.
[0021] A directional ventilation channel with low air permeability on the front and high air permeability on the cut surface was constructed. The surface layer and liner layer use a low proportion of bleached softwood sulfate pulp combined with a high proportion of bleached hardwood sulfate pulp, along with a low-calcined clay formulation in the surface coating, forming a dense front sealing layer that effectively reduces front air permeability. The high proportion of bleached chemithermomechanical pulp coarse fibers in the core layer creates large capillary channels running through the thickness direction of the cardboard, significantly improving cut surface air permeability. These two components work synergistically to allow internal gases to be released directionally from the cardboard cut surface during lamination, preventing bubbling on the front at the indentation lines. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0023] Figure 1 A schematic flowchart illustrating a method for preparing a liquid packaging paper with high adhesion stability and low Z-axis strength according to an embodiment of the present invention; Figure 2 A diagram illustrating the mechanism of action of increasing the amount of rosin sizing agent in the core layer slurry provided in this embodiment of the invention; Figure 3 A schematic diagram of the internal structure of the core layer provided for an embodiment of the present invention; Figure 4 A schematic diagram of the structure of a packaging paper provided for an embodiment of the present invention; Figure 5A complete production process flow diagram of liquid packaging paper is provided for embodiments of the present invention; Figure 6 A physical comparison of conventional liquid packaging paper and the liquid packaging paper prepared according to the present invention. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] In this invention, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0026] It should be noted that if the embodiments of the present invention involve directional indicators (such as up, down, left, right, front, back, etc.), the directional indicators are only used to explain the relative positional relationship and movement of the components in a specific posture. If the specific posture changes, the directional indicators will also change accordingly.
[0027] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are feasible for those skilled in the art. If the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.
[0028] To better understand the above technical solutions, the present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0029] This invention provides a liquid packaging paper with high adhesion stability and low Z-direction strength, comprising a paper base layer and a coating layer. The paper base layer comprises, from front to back, a surface layer, a liner layer, a core layer and a bottom layer. The surface layer, liner layer, core layer and bottom layer are respectively prepared from surface layer slurry, liner layer slurry, core layer slurry and bottom layer slurry. The surface slurry is composed of the following components by mass percentage: 50-60% bleached softwood sulfate pulp and 40-50% bleached hardwood sulfate pulp; in the surface slurry, the freeness of the bleached softwood sulfate pulp is 24-27°SR and the freeness of the bleached hardwood sulfate pulp is 28-31°SR. The lining slurry is composed of the following components by mass percentage: 50-60% bleached softwood sulfate pulp and 40-50% bleached hardwood sulfate pulp; in the lining slurry, the freeness of the bleached softwood sulfate pulp is 23-26°SR, and the freeness of the bleached hardwood sulfate pulp is 28-31°SR. The core pulp is composed of the following components by mass percentage: 40-50% bleached chemithermomechanical pulp, 25-35% bleached softwood sulfate pulp, and 15-35% waste paper; in the core pulp, the freeness of the bleached chemithermomechanical pulp is 15-25°SR, the freeness of the bleached softwood sulfate pulp is 18-24°SR, and the freeness of the waste paper is 30-40°SR. The underlying slurry consists of the following components by mass percentage: 100% unbleached softwood sulfate pulp with a freeness of 19~21°SR; The beating degree of the bleached softwood sulfate pulp in the surface layer slurry, the beating degree of the bleached softwood sulfate pulp in the lining slurry, and the beating degree of the bleached softwood sulfate pulp in the core layer slurry decreases sequentially. A starch-reinforcing layer is provided between the surface layer and the liner, and a composite reinforcing layer is provided between the liner and the core layer and between the core layer and the bottom layer. The composite reinforcing layer contains starch and a microparticle polymer containing highly active aldehyde groups.
[0030] This invention also provides a method for preparing liquid packaging paper with high adhesion stability and low Z-axis strength, such as... Figure 1 As shown, it includes the following steps: S1. The components of the surface slurry, lining slurry, core slurry and bottom slurry are crushed, deslag removed, impurity removed, milled and mixed to obtain the surface slurry, lining slurry, core slurry and bottom slurry respectively. S2. After removing sand from each layer of slurry obtained in step S1, spray them onto the wire section for filtration and shaping, and then vacuum dewater them to obtain a wet paper web consisting of a top layer, a liner layer, a core layer, and a bottom layer. Spray starch between the top layer and the liner layer, and spray a mixture of starch and a microparticle polymer containing highly active aldehyde groups between the liner layer and the core layer and between the core layer and the bottom layer. Composite the obtained wet paper webs consisting of the top layer, the liner layer, the core layer, and the bottom layer to obtain a composite wet paper web. S3. The composite wet paper web obtained in step S2 is dehydrated, pressed, pre-dried, sized, post-dried, and hard-calendered to obtain the paper base layer; S4. Prepare a coating on the surface and bottom layers of the paper base obtained in step S3, and then calender it to obtain liquid packaging paper.
[0031] Unless otherwise specified, all percentages in this invention refer to mass percentages, and all parts refer to parts by weight. The liquid packaging paper provided by this invention includes a paper base layer and a coating layer. The paper base layer, from front to back, includes a surface layer, a liner layer, a core layer, and a bottom layer. The four-layer structure of the paper base layer is prepared by surface layer pulp, liner layer pulp, core layer pulp, and bottom layer pulp through multi-layer paper machine wire forming, lamination, drying, and other processes.
[0032] The top layer is the front printing layer of the liquid packaging paper, requiring good surface smoothness and printability, while also serving as a front seal. The liner layer, located between the top and core layers, acts as a transition and provides reinforcement. The core layer is the main contributor to the paperboard's thickness, giving the paper bulk and compressibility, while also providing venting at the cut surfaces. The bottom layer is the back of the paperboard, requiring high strength and tear resistance to ensure the structural stability of the packaging box.
[0033] The coating layer is applied to the surface of the paper base layer and includes a back coating layer applied to the base layer and a primer coating layer, a substrate coating layer, and a top coating layer applied sequentially to the top layer. Through multi-layer coating, the surface properties and printability of the paper can be further improved, while the air permeability of the front side can be controlled by optimizing the coating formulation.
[0034] This invention employs a separate pulping process, in which different types of fiber raw materials in each layer of pulp are separately broken down, deslag-removed, impurity-removed, and refined to achieve their respective freeness requirements before being mixed in proportion for pulping. Separate pulping allows for individual control of the freeness based on the characteristics of different fiber raw materials, resulting in an optimal combination of fiber morphology and strength properties in each layer of pulp.
[0035] The surface layer slurry consists of the following components by weight percentage: 50-60% bleached softwood sulfate pulp (NBKP) and 40-50% bleached hardwood sulfate pulp (LBKP). The surface layer slurry is prepared by separately pulping and then mixing. The freeness of the bleached softwood sulfate pulp is controlled at 24-27°SR, and the freeness of the bleached hardwood sulfate pulp is controlled at 28-31°SR. Using a higher proportion of bleached hardwood sulfate pulp (40-50%) in the surface layer, combined with an appropriate freeness, allows for a denser interweaving of the surface layer fibers, which helps reduce air permeability on the front side. The relatively high freeness of the bleached softwood sulfate pulp in the surface layer (24-27°SR) ensures sufficient surface strength and lint resistance, meeting the requirements of high-speed printing.
[0036] The lining slurry consists of the following components by mass percentage: 50-60% bleached softwood sulfate pulp (NBKP) and 40-50% bleached hardwood sulfate pulp (LBKP). The lining slurry is prepared by separately pulping and then mixing the components. The freeness of the bleached softwood sulfate pulp is controlled at 23-26°SR, and the freeness of the bleached hardwood sulfate pulp is controlled at 28-31°SR. The lining slurry ratio is similar to that of the surface layer, but the freeness of the bleached softwood sulfate pulp is slightly lower than that of the surface layer (23-26°SR vs. 24-27°SR). This results in a slightly lower fiber weave density in the lining compared to the surface layer, which is beneficial for forming a performance gradient transition from the surface layer to the core layer.
[0037] The core pulp consists of the following components by weight percentage: 40-50% bleached chemithermomechanical pulp (BCTMP), 25-35% bleached softwood sulfate pulp (NBKP), and 15-35% waste paper. The core pulp is prepared by beating the pulp separately and then mixing them. The freeness of the bleached chemithermomechanical pulp is controlled at 15-25°SR, the freeness of the bleached softwood sulfate pulp is controlled at 18-24°SR, and the freeness of the waste paper is controlled at 30-40°SR.
[0038] The core layer is the core functional layer. Bleached chemithermomechanical pulp (BCTMP) is made from wood chips through chemical pretreatment and thermomechanical refining. It has high fiber stiffness, a large wall-to-cavity ratio, retains more lignin, and has strong fiber rigidity. A high proportion of BCTMP (40-50%) combined with a low freeness (15-25°SR) can construct a loose three-dimensional fiber network structure in the core layer, giving the paper high bulk and moderate compressibility, effectively reducing paper cohesion and Z-direction strength. At the same time, the large capillary channels formed by the coarse BCTMP fibers that run through the thickness direction of the paperboard can significantly improve cross-sectional air permeability, providing channels for the directional release of internal gases during lamination.
[0039] Rosin sizing agent is added to the core layer slurry, with the addition amount adjusted from the conventional 15 kg / t to 18-25 kg / t slurry, preferably 20 kg / t slurry. The addition of rosin allows hydrophobic rosin particles to adhere to the fiber surface, forming a hydrophobic film after drying. This improves the water resistance of the core layer and the airtightness of the paper edge, preventing the sterilizing solution from seeping into the paper edge during the subsequent hydrogen peroxide soaking and sterilization process.
[0040] The mechanism of action of increasing the dosage of rosin sizing agent in core layer slurry is as follows: Figure 2As shown, this invention, while reducing the core layer beating degree to ensure low Z-axis strength, appropriately increases the amount of rosin in the core layer (e.g., from 15 kg / t to 20 kg / t), forming a hydrophobic film on the fiber surface, improving the paper edge water resistance, and avoiding leakage problems during aseptic packaging sterilization processes (hydrogen peroxide immersion); it balances low Z-axis strength, interlayer bonding strength, and excellent leakage resistance. By reducing the core layer beating degree and increasing the core layer air permeability, the paper edge air tightness is reduced, solving the problems of filling delamination and blistering at the indentation line, while also preventing the leakage of sterilizing solution (hydrogen peroxide) into the paper edge during the immersion sterilization process.
[0041] Figure 3 This is a schematic diagram of the internal structure of the core layer of the present invention. By specifically controlling the fiber morphology of the core layer, a directional venting structure with synergistic effects of frontal sealing and sectional drainage is constructed. After improvement, for example, the path of gas escaping from the front side under the high temperature conditions of lamination is effectively blocked, and it is forced to be released directionally along the large capillary channels running through the core layer towards the sectional direction. Differentiated control of low air permeability on the front side and high air permeability on the sectional side is achieved, and the technical problem of indentation blistering caused by the inability of gas to be released directionally during the lamination process is solved from a structural level.
[0042] The freeness of the bleached softwood sulfate pulp in the core layer (18~24°SR) is lower than that in the top layer (24~27°SR) and the liner layer (23~26°SR), forming a decreasing freeness gradient from the top layer to the core layer. This gradient design causes the fiber weave density of the paper to gradually decrease from the top layer to the core layer. When indented, the external force is transmitted from the dense top layer to the loose core layer and is buffered step by step, avoiding stress concentration and bursting.
[0043] The beating degree of waste paper should be controlled at 30-40°SR. Appropriately increasing the beating degree of waste paper is beneficial to improving the fibrillation and bonding ability of waste paper fibers, while avoiding fiber damage caused by over-beating. Reusing waste paper not only reduces production costs but also promotes resource recycling.
[0044] The base slurry consists of the following components by weight percentage: 100% unbleached softwood sulfate pulp (USBKP) with a freeness controlled at 19~21°SR.
[0045] Unbleached softwood sulfate pulp retains the natural protective properties of lignin, resulting in high fiber strength and good folding endurance, providing excellent tensile strength, tear resistance, and compressive strength for paperboard. The bottom layer uses 100% unbleached softwood sulfate pulp with a low beating degree (19~21°SR), ensuring bottom layer strength while avoiding fiber damage caused by over-beating. When used for liquid packaging, the high-strength bottom layer effectively prevents packaging box breakage and leakage, while also helping to reduce warping and deformation of the paper base material.
[0046] Conventional wet-end chemical additives used in papermaking, such as cationic starch and rosin sizing agents, can be added to each layer of pulp as needed to improve pulp retention and paper water resistance. The types and amounts of these additives can be selected using conventional methods in the field.
[0047] In this invention, the freeness of the bleached softwood sulfate pulp in each layer of the pulp forms a specific decreasing gradient. The higher freeness of the surface layer allows for full fiber fibrillation and fine fiberization, forming a dense fiber interwoven network. This ensures high surface strength and good printability of the surface layer, while also creating a low-permeability front sealing layer. The lower freeness of the core layer retains the rigidity and stiffness of the fibers, and combined with a high proportion of BCTMP, forms a loose structure, giving the paper compressibility and high cross-sectional air permeability. This performance gradient from the outside to the inside ensures that the external force transmitted from the hard surface layer to the soft core layer during indentation is buffered step by step, avoiding stress concentration that could lead to bursting and cracking.
[0048] In a preferred embodiment of the liquid packaging paper of the present invention, the bleached hardwood sulfate pulp (LBKP) is Silverstar pulp; the bleached softwood sulfate pulp (NBKP) is Finya pulp; the bleached chemithermomechanical pulp (BCTMP) is cypress-maple pulp; the unbleached softwood sulfate pulp (USBKP) is Goldstar pulp; and the waste paper is recycled paper from liquid packaging paper production. All the above-mentioned raw materials of the present invention are commonly used commercial pulps in the papermaking industry, and their sources are not limited.
[0049] After each layer of pulp is prepared, it undergoes purification treatments such as sand removal and screening, and is then sent to the headbox of each layer of a multi-layer paper machine. The pulp is then sprayed onto the wire section for filtration and forming, followed by vacuum dewatering to create the wet paper web for each layer. The vacuum conditions for vacuum dewatering can range from -50 to 0 kPa.
[0050] During the wire forming process, the pulp-to-wire speed ratio of each layer of pulp sprayed onto the wire needs to be precisely controlled. The pulp-to-wire speed ratio refers to the ratio of the speed at which the pulp is ejected from the headbox to the running speed of the forming wire. The pulp-to-wire speed ratio affects the directional alignment of fibers on the wire and the uniformity of the paper structure.
[0051] In a preferred embodiment of the present invention, the pulp-to-mesh ratio of the surface layer slurry sprayed to the mesh is 0.950~0.960, the pulp-to-mesh ratio of the lining slurry sprayed to the mesh is 0.950~0.960, the pulp-to-mesh ratio of the core layer slurry sprayed to the mesh is 0.980~0.990, and the pulp-to-mesh ratio of the bottom layer slurry sprayed to the mesh is 0.980~0.990.
[0052] The resulting wet paper webs, consisting of the face layer, liner layer, core layer, and bottom layer, are laminated in the order of face layer-liner layer-core layer-bottom layer. During the lamination process, a reinforcing agent is applied between adjacent layers to form an interlayer reinforcing layer.
[0053] Specifically, starch is sprayed between the top layer and the liner to form a starch-reinforced layer. This starch-reinforced layer provides basic interlayer bonding strength.
[0054] A composite reinforcing layer is formed by spraying a mixture of starch and a microparticle polymer containing highly reactive aldehyde groups between the liner and the core layer, and between the core layer and the bottom layer. This provides strong compensation for interlayer bonding through chemical covalent bonds.
[0055] In the starch spraying process, the starch spraying amount between the surface layer and the lining layer can be 1.0~3.0 kg / t slurry, the starch spraying amount between the lining layer and the core layer can be 3.0~6.0 kg / t slurry, and the starch spraying amount between the core layer and the bottom layer can be 5.0~8.0 kg / t slurry. The starch spraying amount gradually increases from the surface lining layer to the core bottom layer, which matches the difficulty of interlayer bonding.
[0056] The amount of the microparticle polymer containing highly active aldehyde groups used per ton of paper dry-dry pulp can be 0.2~0.5 kg / t pulp, added after mixing with starch at a concentration of 2%.
[0057] Spraying can be carried out before or during the lamination of each layer of wet paper web. Preferably, just before the two layers of wet paper web are about to merge, the reinforcing agent is sprayed evenly onto the upper surface of the lower layer of wet paper web, and then the upper layer of wet paper web covers it. After lamination, the reinforcing agent is distributed at the interface between the two layers.
[0058] The microparticle polymer containing highly reactive aldehyde groups is the core component of the interlayer composite reinforcing agent. This substance refers to an insoluble microparticle dry strength agent formed by functionalizing and grafting highly reactive aldehyde groups (-CHO) onto a high molecular weight polyacrylamide (PAM) main chain. Its mechanism of action is as follows: the highly reactive aldehyde groups in the microparticle polymer structure can chemically react with the hydroxyl groups (-OH) on cellulose fibers to form stable chemical covalent bonds (such as hemiacetal structures). The bond energy of these chemical covalent bonds is much higher than that of the physical hydrogen bonds between fibers, which can significantly improve the bonding strength between fibers. Simultaneously, this polymer exists in the form of insoluble microparticles, which, compared to soluble polymers, are more easily trapped and retained by the fiber network, resulting in higher reinforcement efficiency.
[0059] In a preferred embodiment of the present invention, the particulate polymer containing highly active aldehyde groups can be glyoxal-modified polyacrylamide (GPAM) particles. Glyoxal-modified polyacrylamide is a polymer containing active aldehyde groups generated by the reaction of polyacrylamide and glyoxal, and Hercobond™ Plus series composite reinforcing agents (Hercobond Plus 800PB) can be used.
[0060] In this invention, a microparticle polymer containing highly reactive aldehyde groups is used in combination with starch, resulting in a synergistic reinforcing effect. Starch provides basic interlayer bonding through hydrogen bonds, while the microparticle polymer provides high-strength chemical bonding through covalent bonds. The hydroxyl groups of starch act as bridges, helping the microparticle polymer to disperse more uniformly on the fiber surface, while the covalent bonds of the microparticle polymer compensate for the decrease in strength of starch hydrogen bonds under wet conditions. This synergistic effect results in an increase in interlayer bonding strength even as the Z-axis strength decreases.
[0061] The composite wet paper web undergoes processes such as pressing, pre-drying, sizing, post-drying, and hard calendering to obtain the paper base layer.
[0062] The purpose of pressing is to remove some of the moisture from the wet paper web, while simultaneously increasing the density of the paper web and the interlayer bonding. In this invention, pressing includes ordinary pressing (first pressing), shoe pressing (second pressing), and light pressing (third pressing).
[0063] In a preferred embodiment of the present invention, the pressure of ordinary pressing is 120~180kN / m, the pressure of shoe pressing is 660~760kN / m, and the pressure of smooth pressing is 10~50kN / m.
[0064] The first press (or ordinary press) uses a relatively low linear pressure (120~180 kN / m), primarily to remove free water from the surface of the wet paper web while avoiding excessive compression of the core layer's loose structure under high pressure. The second press (or shoe press) uses a higher linear pressure (660~760 kN / m). The shoe press has a wider pressing zone, allowing for uniform removal of moisture from the paper web under higher pressure, while also improving the tightness of the bonding between layers. The third press (or finishing press) uses a relatively low linear pressure (10~50 kN / m), primarily to finish the paper web surface in preparation for subsequent drying.
[0065] It should be noted that the above pressing method and pressure parameters can be adjusted appropriately according to the specific configuration of the paper machine and product requirements.
[0066] Pre-drying involves heating and drying the wet paper web after pressing using a drying cylinder to remove most of the moisture. In a preferred embodiment of the invention, the pre-drying utilizes a two-stage temperature gradient drying process: a low-temperature stage at 60-100°C and a high-temperature stage at 90-160°C.
[0067] This invention first employs a low-temperature stage (60~100℃) for gentle drying, allowing free water in the paper web to evaporate slowly and preventing surface "shelling". Once the moisture content of the paper web has decreased to a certain level, a high-temperature stage (90~160℃) is used for intensive drying to quickly remove bound water. This stepped heating method not only improves drying efficiency but, more importantly, reduces residual stress within the paper, which is beneficial for reducing Z-axis strength. For core layers containing a high proportion of BCTMP, stepped heating drying can also avoid fiber keratinization and bulk loss caused by rapid high-temperature drying.
[0068] Preferably, the drying time in the low-temperature section accounts for 30% to 50% of the total pre-drying time, and the drying time in the high-temperature section accounts for 50% to 70% of the total pre-drying time. However, the present invention is not limited to this, and the specific time ratio can be appropriately adjusted according to factors such as paper machine speed, drying cylinder temperature, and paper web basis weight.
[0069] Sizing involves coating the surface and bottom layers of a paper substrate with starch raw material to improve the paper's surface strength and water resistance. In a preferred embodiment of the invention, sizing can be performed using film transfer sizing or impregnation sizing, with an application rate of 1.5~2.5 g / m² on the front side and 0.5~1.0 g / m² on the back side. The sizing starch can be a conventional surface-sizing starch, such as oxidized starch or enzyme-converted starch.
[0070] Post-drying involves further drying the sized paper web to remove moisture introduced during the sizing process. In a preferred embodiment of the invention, post-drying utilizes two temperature stages: Stage I (90-160°C) and Stage II (60-100°C). The post-drying employs a high-temperature-then-low-temperature drying curve, where the high-temperature stage rapidly removes moisture, and the low-temperature stage balances the paper web's moisture content, reducing curling and deformation.
[0071] Hard calendering is a process of calendering the dried paper base layer to improve the smoothness and gloss of the paper surface. In a preferred embodiment of the invention, the hard calendering pressure is 10~50 kN / m. Hard calendering uses a relatively low linear pressure (10~50 kN / m) to improve the smoothness of the paper surface while avoiding excessive compression of the loose core structure, thereby maintaining the paper's low Z-axis strength characteristics.
[0072] A coating is prepared on the surface and bottom layers of the paper base, and then soft calendering is performed to obtain the final liquid packaging paper.
[0073] The structure of the packaging paper of the present invention is as follows: Figure 4As shown, the paper base layer consists of a top layer, a backing layer, a core layer, and a bottom layer from the front to the back. The coating layer includes a back coating layer applied to the bottom layer and a base coating layer, a substrate coating layer, and a top coating layer applied to the top layer in sequence. There is also a top sizing layer between the top layer and the base coating layer, and a base sizing layer between the bottom layer and the back coating layer.
[0074] As a preferred embodiment of the present invention: The coatings for the primer and substrate each independently contain the following components in parts by weight: 10-20 parts latex, 93-100 parts calcium carbonate, and 0-7 parts calcined clay.
[0075] The coating material of the topcoat contains the following components in parts by weight: 15-20 parts latex, 70-90 parts calcium carbonate, and 10-30 parts kaolin.
[0076] The back coating contains starch, and a starch solution with a mass concentration of 8-12% can be used.
[0077] The calcined clay content in the primer and substrate coatings is extremely low (0-7 parts) or even zero, which is one of the important measures to control the front air permeability. Calcined clay has a flat, sheet-like structure, and excessive addition will clog the micropores of the surface layer, increasing the front air permeability resistance. This invention significantly reduces the calcined clay content in the primer and substrate coatings, and combines it with spherical calcium carbonate and latex to form a dense but uniform coating, effectively reducing the front air permeability.
[0078] The topcoat uses a combination of calcium carbonate and kaolin. Kaolin (porcelain clay) has excellent flaky structure and gloss, which helps improve the gloss and printability of the topcoat. Calcium carbonate provides good whiteness and hiding power. Latex acts as a binder, giving the coating strength and flexibility.
[0079] The coating may also contain conventional additives such as dispersants (e.g., sodium polyacrylate), water-resistant agents (e.g., polyamide epichlorohydrin resin), lubricants (e.g., calcium stearate), defoamers, pH adjusters (e.g., caustic soda), and bactericides, which can be selected in accordance with conventional methods in the field.
[0080] As a preferred embodiment of the present invention: Apply a primer coating of 8-12 g / m² (single-sided) to the top layer and dry to prepare the primer coating. Next, apply a substrate coating of 6-8 g / m² (single-sided) to the primer coating and dry to prepare the substrate coating. Then, apply a top coating of 5-9 g / m² (single-sided) to the substrate coating and dry to prepare the top coating. Finally, apply a back coating of 0.8-2.2 g / m² (single-sided) to the bottom layer and dry to prepare the back coating. The total coating weight is controlled at 23-26 g / m². The distribution of coating weight for each layer can be adjusted appropriately according to the paper's basis weight, whiteness requirements, and printability requirements.
[0081] The coating method can employ conventional coating equipment and methods in the art, such as metering bar coating, doctor blade coating, air knife coating, etc. Preferably, the primer can be applied using metering bar coating to accommodate the relatively rough surface of the base paper; the substrate and topcoat can be applied using doctor blade coating to obtain a smoother coating surface.
[0082] After coating, a soft calendering process is performed. The pressure of the soft calendering is 20~50kN / m. Soft calendering can be carried out using a soft calendering machine (such as a calendering machine with polyurethane or composite material soft rollers), which can achieve a good finishing effect under relatively low linear pressure.
[0083] In a preferred embodiment of the present invention, the total basis weight of the liquid packaging paper is 295~305g / m²; the basis weight of the surface layer of the paper base layer is 45~55g / m², the basis weight of the lining layer is 30~40g / m², and the basis weight of the bottom layer is 45~55g / m².
[0084] The quantitative control of each layer can be achieved by adjusting the slurry flow rate and concentration in each layer's headbox, and the specific methods are well known to those skilled in the art.
[0085] Figure 5 This is a complete production process flow diagram of the liquid packaging paper of the present invention. The top and backing layers are mainly formulated by mixing NBKP and LBKP, the core layer uses BCTMP, NBKP, and waste paper, and the bottom layer uses a single USBKP. These fiber raw materials of different grades and properties are respectively entered into their own independent pulping systems for pulping treatment, and then carried out pulping and forming processes according to their respective formulas, and finally transported to the corresponding headboxes. After the four layers of pulp are combined in the wire section of the paper machine, they enter the core wet end and drying end processes. First, the pulp is subjected to strong dewatering and forming at the vacuum couch roll. During the forming process, starch and "splitting starch + reinforcing agent" are sprayed between the paper layers to significantly improve the bonding strength between the paper layers and the overall physical properties of the paperboard. The demolded wet paper web is then subjected to pressing, pre-drying, sizing, post-drying, and hard calendering in sequence to give the paper excellent physical strength and water resistance. To achieve high-end printing standards, the paper web undergoes multiple precision coating processes, including base coating, interlayer coating, back coating, and top coating, to optimize whiteness, smoothness, and gloss. A soft calendering process further enhances the finished product's flatness. Finally, the formed paper rolls are wound, packaged, and stored. The entire process is highly automated, ensuring long-term stability of product quality under large-scale continuous production.
[0086] Through the above technical solutions, this invention achieves a balance between low Z-axis strength and interlayer bonding stability. It effectively reduces paper cohesion and Z-axis strength (≤400kPa), while achieving an interlayer bonding strength of ≥220J / m². A directional exhaust channel with low air permeability on the front side and high air permeability on the cut side is constructed. The combination of front-side sealing and cut-side conduction allows internal gas to be released directionally from the paperboard cut side during lamination, significantly reducing the bubbling rate of the crease lines. The paper structure is optimized through the synergistic control of the beating gradient and wire speed ratio. Gradient control of fiber arrangement is achieved. This structural gradient allows the paper to maintain surface strength and flatness while the core layer maintains high bulk and compressibility, comprehensively improving the paper's downstream processing performance.
[0087] Through the above comprehensive design, the liquid packaging paper prepared by the present invention exhibits excellent processing adaptability in the entire process of lamination, embossing, and filling, effectively solving problems such as embossing bursting, delamination, and bubbling in the prior art, and significantly improving product yield.
[0088] The liquid packaging paper and its preparation method provided by this invention can be widely used in the manufacturing of beverage cartons such as milk and juice. This invention effectively solves the technical problems of bubbling and delamination at the indentation points during the lamination and filling processes of existing liquid packaging papers through optimized design of a four-layer composite structure, innovative interlayer differential reinforcement system, and zoned control of air permeability. It has good industrial application prospects and economic benefits. This invention can be implemented on existing multi-layer paper machine production lines without large-scale equipment modifications, demonstrating good industrial applicability.
[0089] like Figure 6 As shown, Figure 6 A comparison of physical samples of conventional liquid packaging paper and the liquid packaging paper prepared according to the present invention shows that conventional liquid packaging paper before improvement is prone to defects such as delamination, crease lines, and bubbles during use, while the liquid packaging paper improved by the present invention does not produce delamination when made into a paper box, the crease lines are good, and the use effect is significantly improved.
[0090] To further illustrate the impact of the key components and dosages of this embodiment on the performance of liquid packaging paper, liquid packaging papers prepared in Examples 1 to 4 and Comparative Examples 1 to 4 are provided and tested.
[0091] Example 1
[0092] This embodiment provides a liquid packaging paper with high adhesion stability and low Z-axis strength and its preparation method, the specific steps of which are as follows.
[0093] I. Preparation of each layer of slurry
[0094] (1) Surface slurry: Bleached softwood sulfate pulp (NBKP, Fenya pulp) boards are broken down by a hydraulic pulper, then screened and polished to a freeness of 25°SR; bleached hardwood sulfate pulp (LBKP, Silver Star pulp) boards are broken down by a hydraulic pulper, then screened and polished to a freeness of 29°SR. NBKP and LBKP are mixed in a mass percentage ratio of 55% and 45% respectively, and cationic starch (addition amount 1.0 kg / t slurry) and rosin sizing agent (addition amount 15 kg / t slurry) are added to obtain the surface slurry.
[0095] (2) Lining slurry: NBKP (Fenya Pulp) slurry boards are broken down by a hydraulic pulper, then screened and milled to a freeness of 24°SR; LBKP (Silver Star Pulp) slurry boards are broken down by a hydraulic pulper, then screened and milled to a freeness of 29°SR. The slurry is prepared by mixing NBKP 55% and LBKP 45% by mass, and adding cationic starch (1.0 kg / t slurry) and rosin sizing agent (15 kg / t slurry) to obtain the lining slurry.
[0096] (3) Core Pulp: Bleached chemithermomechanical pulp (BCTMP, Tianbai Maple Pulp) is pulped in a hydrapulper, then screened and refinished to a freeness of 20°SR; NBKP (Finya Pulp) is pulped in a hydrapulper, then screened and refinished to a freeness of 21°SR; waste paper (recycled liquid packaging paper) is pulped in a hydrapulper, then screened and refinished to a freeness of 35°SR. The pulp is prepared by mixing BCTMP 45%, NBKP 35%, and waste paper 20% by mass, and adding cationic starch (0.5 kg / t pulp) and rosin sizing agent (20 kg / t pulp) to obtain the core pulp.
[0097] (4) Bottom layer slurry: After the unbleached softwood sulfate pulp (USBKP, Venus pulp) board is broken down by a hydraulic pulper, it is screened, milled and beaten to a freeness of 20°SR, and cationic starch (addition amount 1.0kg / t pulp) and rosin sizing agent (addition amount 15kg / t pulp) are added to obtain the bottom layer slurry.
[0098] II. Paper Machine Section
[0099] (1) Web forming and lamination: After removing sand from the above four layers of pulp, they are sprayed onto the wire section for filtration and forming, and then vacuum dewatered (vacuum degree -30~-10kPa) to obtain wet paper webs of surface layer, liner layer, core layer and bottom layer. Among them: the pulp-wire speed ratio of surface layer is 0.955, the pulp-wire speed ratio of liner layer is 0.955, the pulp-wire speed ratio of core layer is 0.985, and the pulp-wire speed ratio of bottom layer is 0.985.
[0100] Starch (1.5 kg / t pulp) is sprayed between the top and bottom layers; a mixture of starch (4.5 kg / t pulp) and a microparticle polymer containing highly active aldehyde groups (Hercobond Plus 800PB, 0.35 kg / t pulp per ton of dry paper, added at a concentration of 2% mixed with starch) is sprayed between the bottom and top layers; a mixture of starch (6.5 kg / t pulp) and a microparticle polymer containing highly active aldehyde groups (Hercobond Plus 800PB, 0.35 kg / t pulp per ton of dry paper, added at a concentration of 2% mixed with starch) is sprayed between the bottom and top layers. These four wet paper webs are then laminated to obtain a composite wet paper web.
[0101] (2) Pressing: Ordinary pressing (first press, pressure 150kN / m), shoe pressing (second press, pressure 710kN / m) and smooth pressing (third press, pressure 30kN / m) are carried out in sequence.
[0102] (3) Pre-drying: Step-by-step heating drying is adopted, with a low temperature section temperature of 80℃ and a high temperature section temperature of 120℃.
[0103] (4) Applying sizing: Apply sizing to the surface of the starch raw material coated on the front and back layers. The amount of sizing is 2.0 g / m² on the front and 0.8 g / m² on the back.
[0104] (5) Post-drying: Section I temperature 120℃, Section II temperature 80℃.
[0105] (6) Hard calendering: pressure 30kN / m, to obtain paper base layer.
[0106] (7) Coating: Apply a primer coating (10 g / m²) to the top layer and dry to prepare the primer coating; then apply a substrate coating (7 g / m²) to the primer coating and dry to prepare the substrate coating; then apply a topcoat coating (7 g / m²) to the substrate coating and dry to prepare the topcoat coating. Apply a back coating (1.5 g / m²) to the bottom layer and dry to prepare the backcoat coating. The total coating amount is controlled at 25 g / m².
[0107] The formulations of the primer and substrate coatings are as follows (parts by weight): 15 parts latex, 97 parts calcium carbonate, and 3 parts calcined clay. The formulation of the topcoat coating is as follows (parts by weight): 18 parts latex, 80 parts calcium carbonate, and 20 parts kaolin. The backcoat coating is a 10% starch solution.
[0108] (8) Soft calendering: pressure 35kN / m, to obtain liquid packaging paper.
[0109] The total basis weight of the resulting liquid packaging paper is 300 g / m², of which the basis weight of the top layer is 50 g / m², the basis weight of the liner layer is 35 g / m², and the basis weight of the bottom layer is 50 g / m².
[0110] Example 2
[0111] Other conditions are the same as in Example 1, except that: (1) Surface slurry: NBKP with a freeness of 27°SR and LBKP with a freeness of 31°SR, mixed at a mass percentage of 50% NBKP and 50% LBKP.
[0112] (2) Lining slurry: NBKP with a freeness of 26°SR and LBKP with a freeness of 31°SR, mixed at a mass percentage of 50% NBKP and 50% LBKP.
[0113] (3) Core pulp: BCTMP freeness 25°SR, NBKP freeness 24°SR, waste paper freeness 40°SR, mixed according to the mass percentage of BCTMP 40%, NBKP 30%, and waste paper 30%.
[0114] (4) Bottom layer slurry: USBKP slurry degree 21°SR.
[0115] (5) Spray starch (1.0 kg / t pulp) between the surface layer and the liner layer; spray a mixture of starch (4.0 kg / t pulp) and a microparticle polymer containing highly active aldehyde groups (Hercobond Plus 800PB, 0.2 kg / t pulp per ton of paper dry, mixed with starch at a concentration of 2%) between the liner layer and the core layer; spray a mixture of starch (6.0 kg / t pulp) and a microparticle polymer containing highly active aldehyde groups (Hercobond Plus 800PB, 0.2 kg / t pulp per ton of paper dry, mixed with starch at a concentration of 2%) between the core layer and the bottom layer. Lay the four wet paper webs together to obtain a composite wet paper web.
[0116] Example 3
[0117] Other conditions are the same as in Example 1, except that: (1) Surface slurry: NBKP with a freeness of 24°SR and LBKP with a freeness of 28°SR, mixed at a mass percentage of 60% NBKP and 40% LBKP.
[0118] (2) Lining slurry: NBKP with a freeness of 23°SR and LBKP with a freeness of 28°SR, mixed at a mass percentage of 60% NBKP and 40% LBKP.
[0119] (3) Core pulp: BCTMP freeness 15°SR, NBKP freeness 18°SR, waste paper freeness 30°SR, mixed with BCTMP 50%, NBKP 25% and waste paper 25% by mass percentage.
[0120] (4) Bottom layer slurry: USBKP slurry degree 19°SR.
[0121] (5) Spray starch (2.0 kg / t pulp) between the surface layer and the liner layer; spray a mixture of starch (5.0 kg / t pulp) and a micro-polymer containing highly active aldehyde groups (Hercobond Plus 800PB, 0.5 kg / t pulp per ton of paper dry, mixed with starch at a concentration of 2%) between the liner layer and the core layer; spray a mixture of starch (7.0 kg / t pulp) and a micro-polymer containing highly active aldehyde groups (Hercobond Plus 800PB, 0.5 kg / t pulp per ton of paper dry, mixed with starch at a concentration of 2%) between the core layer and the bottom layer. Lay the four wet paper webs together to obtain a composite wet paper web.
[0122] Example 4
[0123] Other conditions are the same as in Example 1, except that: (1) The formulation of the primer and substrate coating is as follows (parts by weight): 15 parts latex, 97 parts calcium carbonate, and 7 parts calcined clay.
[0124] Comparative Example 1
[0125] Other conditions are the same as in Example 1, except that: core pulp: BCTMP freeness 25°SR, NBKP freeness 26°SR, waste paper freeness 42°SR, mixed in a mass percentage of 50% BCTMP, 25% NBKP, and 25% waste paper.
[0126] Comparative Example 2
[0127] Other conditions are the same as in Example 1, except that: core pulp: BCTMP freeness 15°SR, NBKP freeness 16°SR, waste paper freeness 28°SR, mixed in a mass percentage of 50% BCTMP, 25% NBKP, and 25% waste paper.
[0128] Comparative Example 3
[0129] Other conditions were the same as in Example 1, except that only starch was sprayed between the top layer and the liner, between the liner and the core layer, and between the core layer and the bottom layer; no microparticle polymer containing highly active aldehyde groups was added. The starch spraying amounts for each layer were: 2.0 kg / t slurry between the top layer and the liner, 5 kg / t slurry between the liner and the core layer, and 6 kg / t slurry between the core layer and the bottom layer.
[0130] Comparative Example 4
[0131] Other conditions are the same as in Example 1, except that the formulations of the primer and substrate coatings are (parts by weight): 15 parts latex, 97 parts calcium carbonate, and 10 parts calcined clay.
[0132] Performance testing
[0133] The liquid packaging paper prepared in Examples 1-4 and Comparative Examples 1-4 was subjected to the following performance tests. All tests were conducted under standard constant temperature and humidity conditions (temperature 23±1℃, relative humidity 50±2%). The samples were equilibrated under these conditions for at least 4 hours before the tests.
[0134] (1) Z-direction strength: Determined according to GB / T 31110-2014 "Determination of Z-direction Tensile Strength of Paper and Paperboard". Cut the paper sample to length. Width is 5.0 Three samples were taken at three locations, each 5.0 cm in diameter, and the average of the three results was taken. (2) Interlayer bonding strength (internal bond strength): The test was conducted according to GB / T 26203-2023 "Determination of internal bond strength of paper and paperboard (Scott type)". The transverse paper sample was cut to length... Width is 12.7 Three samples were taken at 2.54 cm depth, and the average of the three results was taken. (3) Front air permeability: The test was conducted according to the Schubert method in GB / T 458-2008 "Determination of air permeability of paper and paperboard". The front of the sample was facing the airflow direction, and the average of the three samples was taken. (4) Cross-sectional air permeability: The test was conducted according to the Schubert method in GB / T 458-2008 "Determination of air permeability of paper and paperboard". The cross-section of the sample was oriented towards the airflow direction, and the gas permeated along the thickness direction of the paperboard. After the paper sample was coated, a circular cake was taken with a quantitative sampler, and then a circular cake with a radius of 3.0 cm was cut out from the center. The remaining circular ring was used as the test sample, and the average of the three sample results was taken. (5) Bubbling rate of crease line after lamination: After lamination, the paper is creased (the crease gap is 1.5 times the paper thickness and the pressure is 6kN). The proportion of bubbles appearing at the crease line is counted (100 samples per group).
[0135] Test Results
[0136] The test results for each embodiment and comparative example are shown in Table 1.
[0137] Table 1 Performance test results of Examples 1-4 and Comparative Examples 1-4
[0138] Data Analysis
[0139] The test results in Table 1 show that: Examples 1-4 all exhibit Z-direction strengths ≤400 kPa (361-396 kPa) and interlayer bonding forces ≥220 J / m² (224-243 J / m²), successfully achieving a balance between low Z-direction strength and high interlayer bonding stability. This indicates that the technical solution of this invention, which uses a high proportion of BCTMP in the core layer combined with a low beating degree design to impart moderate compressibility to the paper and reduce Z-direction strength, while simultaneously using a composite reinforcing layer of interlayer starch and microparticle polymers containing highly active aldehyde groups to compensate for interlayer bonding forces through chemical covalent bonds, is effective.
[0140] In Comparative Example 1, the core layer wasted NBKP freeness was 26°SR, and the paper freeness was 42°SR, both slightly high. The Z-axis strength increased to 419 kPa (exceeding 400 kPa), while the cross-sectional air permeability decreased to 1.781 mL / min, and the foaming rate was as high as 3.11%. Excessive freeness caused excessive fiber fibrillation and fine fiberization, increasing fiber interweaving density, enhancing paper cohesion, and increasing Z-axis strength. At the same time, the large capillary channels in the fiber network were blocked by fine fibers, reducing cross-sectional air permeability.
[0141] The NBKP freeness of the two core layers in the comparative example was 16°SR, and the freeness of the waste paper was 28°SR, both slightly low. Its interlayer bonding strength was only 206 J / m², still posing a risk of delamination during filling. The excessively low freeness leads to insufficient fibrillation of the waste paper fibers and a decrease in the bonding ability between fibers, which cannot be fully compensated for even with the addition of composite reinforcing agents.
[0142] Comparative Example 3, without the addition of microparticle polymers containing highly reactive aldehyde groups, showed an interlayer bonding strength of only 183 J / m², lower than 220 J / m², still posing a risk of delamination during filling. This indicates that the addition of microparticle polymers plays a crucial role in maintaining interlayer bonding strength under low freeness conditions. Microparticle polymers containing highly reactive aldehyde groups form chemical covalent bonds with the cellulose hydroxyl groups through their reactive aldehyde groups, compensating for the loss of cellulose hydrogen bonding strength due to reduced freeness.
[0143] In Examples 1-4, the front air permeability was ≤1.0 mL / min (0.81~0.96 mL / min), and the cross-sectional air permeability was ≥1.8 mL / min (1.809~1.835 mL / min), achieving differentiated control between low front air permeability and high cross-sectional air permeability. The high proportion of BCTMP (40~50%) coarse fibers in the core layer constructed large capillary channels throughout the thickness direction of the paperboard, significantly improving cross-sectional air permeability. The dense fiber interwoven network formed by the high proportion of LBKP (40~50%) in the surface and liner layers, combined with the sealing effect of low-calcined clay (0~7 parts) in the coating, kept the front air permeability at a low level.
[0144] The front air permeability of Comparative Example 4 was 1.18 mL / min, and the cross-sectional air permeability was 1.819 mL / min, but the foaming rate was as high as 2.28%. This indicates that when the front air permeability is too high, the internal gas generated during the lamination process will be released from the cross-section and overflow from the front, causing blistering of the indentation line.
[0145] As can be seen from the comparison of the above embodiments and comparative examples, the present invention, through the specific ratio and beating degree design of each layer of pulp, the differential composite reinforcement system between layers (the face liner is a starch reinforcement layer, and the core liner and the bottom core are starch and microparticle polymer composite reinforcement layers containing highly active aldehyde groups), and the synergistic effect of air permeability zone control (low air permeability on the front side + high air permeability on the cut side), enables the paper to simultaneously possess low Z-axis strength (≤400kPa) and interlayer bonding strength (≥220J / m²), and achieves directional gas release during the lamination process, effectively solving the technical problems of delamination during the back-end filling of existing liquid packaging paper and bubbling of the indentation line during lamination.
[0146] The above are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. Any equivalent structural transformations made using the contents of the present invention specification and drawings under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.
[0147] It should be noted that when numerical ranges are involved in this invention, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, preferred embodiments are described in order to avoid redundancy. Although preferred embodiments of this invention have been described, those skilled in the art can make other changes and modifications to these embodiments once they know the basic inventive concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of this invention.
[0148] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from the spirit and scope of this invention; if these modifications and variations of this invention fall within the scope of the claims of this invention and their equivalents, then this invention also intends to include these modifications and variations.
Claims
1. A liquid packaging paper with high adhesion stability and low Z-direction strength, comprising a paper base layer and a coating layer, wherein the paper base layer comprises, from front to back, a surface layer, a liner layer, a core layer, and a bottom layer, wherein the surface layer, liner layer, core layer, and bottom layer are respectively prepared from surface layer slurry, liner layer slurry, core layer slurry, and bottom layer slurry; characterized in that, The surface slurry is composed of the following components by mass percentage: 50-60% bleached softwood sulfate pulp and 40-50% bleached hardwood sulfate pulp; in the surface slurry, the freeness of the bleached softwood sulfate pulp is 24-27°SR and the freeness of the bleached hardwood sulfate pulp is 28-31°SR. The lining slurry is composed of the following components by mass percentage: 50-60% bleached softwood sulfate pulp and 40-50% bleached hardwood sulfate pulp; in the lining slurry, the freeness of the bleached softwood sulfate pulp is 23-26°SR, and the freeness of the bleached hardwood sulfate pulp is 28-31°SR. The core pulp is composed of the following components by mass percentage: 40-50% bleached chemithermomechanical pulp, 25-35% bleached softwood sulfate pulp, and 15-35% waste paper; in the core pulp, the freeness of the bleached chemithermomechanical pulp is 15-25°SR, the freeness of the bleached softwood sulfate pulp is 18-24°SR, and the freeness of the waste paper is 30-40°SR. The underlying slurry consists of the following components by mass percentage: 100% unbleached softwood sulfate pulp with a freeness of 19~21°SR; The beating degree of the bleached softwood sulfate pulp in the surface layer slurry, the beating degree of the bleached softwood sulfate pulp in the lining slurry, and the beating degree of the bleached softwood sulfate pulp in the core layer slurry decreases sequentially. A starch-reinforcing layer is provided between the surface layer and the liner, and a composite reinforcing layer is provided between the liner and the core layer and between the core layer and the bottom layer. The composite reinforcing layer contains starch and a microparticle polymer containing highly active aldehyde groups.
2. The liquid packaging paper according to claim 1, characterized in that, The liquid packaging paper has a front air permeability ≤1.0mL / min, a cross-sectional air permeability ≥1.8mL / min, a Z-direction strength ≤400kPa, and an interlayer bonding force ≥220J / m².
3. The liquid packaging paper according to claim 1, characterized in that, The total basis weight of the liquid packaging paper is 295~305g / m²; the basis weight of the surface layer of the paper base layer is 45~55g / m², the basis weight of the lining layer is 30~40g / m², and the basis weight of the bottom layer is 45~55g / m².
4. The liquid packaging paper according to claim 1, characterized in that, The coating layer includes a back coating layer applied to the bottom layer of the paper substrate and a base coating layer, a substrate coating layer, and a top coating layer applied sequentially to the top layer of the paper substrate; the coatings of the base coating layer and the substrate coating layer each independently contain the following components in parts by weight: 10-20 parts latex, 93-100 parts calcium carbonate, and 0-7 parts calcined clay; the coating of the top coating layer contains the following components in parts by weight: 15-20 parts latex, 70-90 parts calcium carbonate, and 10-30 parts kaolin.
5. The liquid packaging paper according to claim 1, characterized in that, The microparticle polymer containing highly active aldehyde groups is glyoxal-modified polyacrylamide microparticles.
6. The liquid packaging paper according to claim 1, characterized in that, The core layer slurry contains rosin sizing agent, with an addition amount of 18~25 kg / t slurry.
7. A method for preparing a liquid packaging paper with high adhesive stability and low Z-axis strength as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. The components of the surface slurry, lining slurry, core slurry and bottom slurry are crushed, deslag removed, impurity removed, milled and mixed to obtain the surface slurry, lining slurry, core slurry and bottom slurry respectively. S2. After removing sand from each layer of slurry obtained in step S1, spray them onto the wire section for filtration and shaping, and then vacuum dewater them to obtain a wet paper web consisting of a top layer, a liner layer, a core layer, and a bottom layer. Spray starch between the top layer and the liner layer, and spray a mixture of starch and a microparticle polymer containing highly active aldehyde groups between the liner layer and the core layer and between the core layer and the bottom layer. Composite the obtained wet paper webs consisting of the top layer, the liner layer, the core layer, and the bottom layer to obtain a composite wet paper web. S3. The composite wet paper web obtained in step S2 is dehydrated, pressed, pre-dried, sized, post-dried, and hard-calendered to obtain the paper base layer; S4. Prepare a coating on the surface and bottom layers of the paper base obtained in step S3, and then calender it to obtain liquid packaging paper.
8. The preparation method according to claim 7, characterized in that, In step S2, the vacuum conditions for vacuum dehydration are -50~0 kPa; in the sprayed starch, the amount of starch sprayed between the surface layer and the liner layer is 1.0~3.0 kg / t slurry, the amount of starch sprayed between the liner layer and the core layer is 3.0~6.0 kg / t slurry, and the amount of starch sprayed between the core layer and the bottom layer is 5.0~8.0 kg / t slurry; the amount of the microparticle polymer containing highly active aldehyde groups used per ton of paper for oven-drying is 0.2~0.5 kg / t slurry, which is added at a concentration of 2% mixed with starch.
9. The preparation method according to claim 7, characterized in that, In step S2, the slurry spraying speed ratio to the mesh section is 0.950~0.960, the slurry spraying speed ratio to the mesh section is 0.950~0.960, the slurry spraying speed ratio to the mesh section is 0.980~0.990, and the slurry spraying speed ratio to the mesh section is 0.980~0.
990.
10. The preparation method according to claim 7, characterized in that, In step S3, The pressing includes ordinary pressing, shoe pressing and smooth pressing; the pressure of ordinary pressing is 120~180kN / m, the pressure of shoe pressing is 660~760kN / m, and the pressure of smooth pressing is 10~50kN / m. The pre-drying process utilizes a two-stage stepped heating drying method, with the temperature of the low-temperature stage being 60~100℃ and the temperature of the high-temperature stage being 90~160℃. The post-drying process utilizes a first-stage temperature and a second-stage temperature, with the first-stage temperature being 90~160℃ and the second-stage temperature being 60~100℃. The pressure of the hard calendering is 10~50kN / m.
11. The preparation method according to claim 7, characterized in that, The preparation of coatings on the top and bottom layers of the paper substrate obtained in step S3 includes: applying a base coat of 8-12 g / m² to the top layer and drying it to prepare a base coat; then applying a substrate coat of 6-8 g / m² to the base coat and drying it to prepare a substrate coat; then applying a top coat of 5-9 g / m² to the substrate coat and drying it to prepare a top coat; and applying a back coat of 0.8-2.2 g / m² to the bottom layer and drying it to prepare a back coat.