A partial replacement and reinforcement method of a shear wall with a reserved thin layer on the outside of a high-rise building

By using a local replacement reinforcement method, including internal inspection and zoning, top support, directional chiseling, retention of thin layers, and high-strength material pouring, the problem of insufficient strength of the shear wall of the exterior wall of high-rise buildings was solved, achieving efficient and safe reinforcement and maintaining the integrity of the building facade.

CN123153569APending Publication Date: 2026-11-24SHAANXI ACAD OF ARCHITECTONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611636319.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The shear walls of high-rise buildings may suffer structural damage or collapse due to insufficient concrete strength. Existing reinforcement methods require damaging the facade and are costly, affecting user experience.

Method used

The method of local replacement reinforcement is adopted, which involves internal inspection and zoning, setting up top supports, directional chiseling of the internal side, retaining the thin layer on the outside, internal formwork and high-strength material pouring, avoiding external scaffolding and ensuring the integrity of the building facade.

Benefits of technology

It achieves efficient and safe shear wall reinforcement, reduces construction costs and impact on users, and improves the seismic performance and integrity of the structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153569A_ABST
    Figure CN123153569A_ABST
Patent Text Reader

Abstract

This invention discloses a method for partial replacement and reinforcement of the outer thin layer of shear wall in the exterior wall of a high-rise building. The method includes the following steps: 1. Inspection and zoning; 2. Temporary support and unloading; 3. Reinforcement marking; 4. Directional removal of inner concrete; 5. Reinforcement repair and reinforcement; 6. Interface treatment and inner formwork; 7. High-strength concrete pouring and curing; 8. Repeated construction; 9. Restoration of the interior surface layer, thus completing the partial replacement and reinforcement of the outer thin layer of shear wall in the exterior wall of a high-rise building. This invention, through dividing replacement units, setting top supports, directional removal of the inner side, retaining the complete outer thin concrete layer, inner formwork, and high-strength concrete pouring, completes the partial replacement and reinforcement of the outer thin layer of shear wall in the exterior wall of a high-rise building. The entire construction process is carried out only from the interior side, without the need for external scaffolding, and does not damage the external insulation layer, waterproof layer, or decorative surface layer. It avoids high-altitude operations and exterior wall repairs, significantly reducing the impact on normal user use and the building's appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of shear wall partial replacement and reinforcement technology, specifically relating to a method for partial replacement and reinforcement of shear walls in high-rise buildings, which retains the thin outer layer. Background Technology

[0002] Reinforced concrete shear walls are core components in high-rise buildings that bear vertical loads and resist horizontal seismic forces. Their concrete strength directly affects the overall structural safety and seismic performance. However, during actual construction, factors such as inadequate compaction, formwork leakage, and unstable concrete supply quality frequently lead to localized concrete strength issues in shear walls that fail to meet design requirements. When the concrete strength of the shear wall is severely insufficient, it can cause structural damage or even collapse, necessitating effective reinforcement measures. Generally, the exterior walls of a high-rise building are poured using the same batch of concrete. When quality problems are found in the exterior walls of a high-rise building, it usually indicates a problem with that batch of concrete, requiring reinforcement of the entire poured exterior wall.

[0003] Existing technologies typically employ the replacement concrete reinforcement method. This method fundamentally restores the load-bearing capacity of the structural member by removing inferior or damaged concrete and replacing it with high-strength, high-quality concrete. It is the primary technical means for addressing such problems. However, it requires the complete removal and re-pour of the entire wall, making construction cumbersome. Furthermore, the replacement construction of shear walls in high-rise buildings faces unique challenges: the exterior walls usually already have an external insulation layer or decorative finish. If the traditional double-sided removal and replacement method is used, it not only damages the building facade but also requires the erection of scaffolding on the exterior, resulting in high construction costs and significant disruption to users.

[0004] Therefore, there is a need for a method to locally replace and reinforce the outer thin layer of the shear wall in the exterior wall of a high-rise building. Summary of the Invention

[0005] The technical problem this invention aims to solve is to address the shortcomings of the prior art by providing a method for partial replacement and reinforcement of the outer thin layer of shear walls in the exterior walls of high-rise buildings. This method involves dividing the exterior walls into replacement units, setting up top supports, directional removal from the inside, preserving the intact outer thin concrete layer, supporting formwork on the inside, and pouring high-strength concrete. This completes the partial replacement and reinforcement of the outer thin layer of shear walls in the exterior walls of high-rise buildings. The entire construction process is carried out from the interior side, eliminating the need for external scaffolding, and does not damage the external insulation layer, waterproof layer, or decorative surface layer. The building facade remains intact, avoiding high-altitude work and exterior wall repairs, significantly reducing the impact on normal user use and the building's appearance.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for local replacement and reinforcement of shear walls in high-rise buildings, which retains the outer thin layer, the method comprising the following steps: Step 1, Inspection and Zoning: Rebound test and core sampling are carried out on the inner side of the shear wall in the exterior wall of the high-rise building. Areas whose strength does not meet the design requirements and specifications are identified as areas with insufficient strength. Then, the areas with insufficient strength are divided vertically into multiple replacement units. The construction sequence of each replacement unit is determined by the skip-fill method to obtain the shear wall to be constructed. Step 2, Temporary Support and Unloading: Top supports are installed at the floor level where the shear wall to be constructed is located and at the floor slab or connecting beam above it, obtained in Step 1, to obtain a shear wall with top supports; Step 3, Rebar Marking: Use a rebar scanner to scan the inside of the shear wall with top support obtained in Step 2 to obtain the location of the rebar and mark it; Step 4, Directional Removal of Inner Concrete: Following the construction sequence described in Step 1 and the location of the reinforcing bars described in Step 3, for the first group of replacement units that need to be constructed, use a water drill to drill into the shear wall in the non-reinforcing bar area with a depth of d-(40~60)mm, where d is the thickness of the shear wall in mm. Then, pry off the core sample and remove it. Then, use an electric hammer to remove the protruding section and the remaining gap concrete, leaving a thin layer of intact concrete on the outside of the shear wall. Finally, roughen the removed surface and remove dust and wet it to obtain the removed shear wall. Step 5, Reinforcement Repair and Strengthening: Remove rust and straighten the original reinforcement bars of the shear wall obtained in Step 4, and implant anti-crack tie bars into the thin concrete layer mentioned in Step 4 to obtain the reinforcement-repaired shear wall; Step 6, Interface Treatment and Inner Formwork: Apply interface agent and cement-based penetrating crystalline waterproofing agent to the chiseled surface of the steel reinforcement repair shear wall obtained in Step 5. Then, set up formwork and temporary support on the inner side of the shear wall, leaving pouring opening and vent hole to obtain the cavity to be poured. Step 7, High-strength material pouring and curing: The cavity to be poured obtained in Step 6 is poured in layers and vibrated to compact it. After pouring, it is moisturized and cured. After the design strength is reached, the inner template and temporary support are removed. Step 8: Repeat construction: Repeat steps 4 to 7 until each replacement unit is completed and a new shear wall is obtained; Step 9: Indoor surface layer restoration: Repair and level the newly poured shear wall obtained in Step 8, then restore the finishing layer, and complete the local replacement and reinforcement of the thin outer layer of the shear wall in the exterior wall of the high-rise building.

[0007] This invention utilizes the rebound method for rapid and non-destructive preliminary screening of large-area walls, while core sampling provides accurate strength data. The combination of these two methods ensures the reliability of the test results, avoiding the blind expansion or omission of areas with insufficient strength. By vertically segmenting areas with insufficient strength into multiple replacement units and determining the construction sequence of each replacement unit using a skip-pour method, the replacement units poured earlier can freely release shrinkage and temperature stresses in the early stages. Adjacent units are constructed only after their strength has increased sufficiently to resist subsequent stresses, effectively solving the stress lag problem in batch replacement and resulting in a more balanced stress distribution on the wall. Furthermore, the use of top supports replaces the traditional full-span scaffolding unloading scheme, requiring less construction space and making installation and dismantling easier. The invention is efficient because by simultaneously installing supports on the upper and lower floors of the wall to be replaced, a clear and stable load transfer path can be ensured, preventing structural deformation or damage due to local loss of load-bearing capacity during the removal process, thus ensuring construction safety. A rebar scanner can accurately identify the spacing and direction of the rebar within the wall, avoiding accidental damage to the original rebar during subsequent water drilling and electric hammer removal, protecting the integrity of the rebar skeleton and reducing unnecessary rebar repair work. The directional removal process, combining water drilling with electric hammer removal, allows for precise control of the removal depth, ensuring the integrity of the outer thin layer of concrete. This is the core feature that distinguishes this invention from traditional double-sided replacement; the preserved outer thin layer of concrete not only maintains the integrity of the building facade but also avoids the need for external scaffolding. The design, which also serves as a permanent outer formwork for newly poured concrete after the external insulation layer is damaged, simplifies the formwork process. Roughening the surface increases the mechanical bonding area between the old and new concrete. Dust removal and wetting provide a good base condition for applying the interface agent and cement-based penetrating crystalline waterproofing agent, as well as for pouring high-strength concrete. Rust removal and straightening ensure that the cross-sectional area and stress performance of the original steel reinforcement meet design requirements. Reinforcement measures guarantee the continuity of the steel reinforcement cage. Implanting crack-resistant tie bars in the thin-layer concrete effectively restrains the shrinkage deformation of the newly poured concrete, preventing cracks from forming under temperature changes and shrinkage. It also enhances the connection and anchorage between the old and new concrete, improving the interface crack resistance. Applying the interface agent and cement-based penetrating crystalline waterproofing agent... Waterproofing agents significantly improve the bond strength between new and old concrete. Cement-based penetrating crystalline waterproofing agents can also provide waterproofing for exterior walls, preventing water vapor penetration and steel corrosion. By setting up formwork and temporary supports on the inside of the shear wall, and leaving pouring ports and vents, a cavity is formed between the formwork, the remaining thin layer of concrete, and the shear walls on both sides that have not been removed, for pouring new shear walls. The pouring ports ensure smooth injection of the mortar, while the vents allow air to escape effectively, avoiding defects such as voids and honeycombs inside the poured body and ensuring the compactness of the pour. Layered pouring and vibration compaction ensure the uniformity and compactness of the poured body, and moisture curing provides the necessary conditions for the strength growth and volume stability of the newly poured concrete.By repeating the construction process until each replacement unit is completed, both construction efficiency and structural safety are balanced, achieving a streamlined replacement operation. Repair and leveling ensure the smoothness and aesthetics of the interior walls, and the restoration of the finishing layer minimizes the impact of reinforcement construction on users' daily lives. Since the entire construction process is carried out only on the interior side, the building facade remains intact, eliminating the need for outdoor high-altitude work and repair of the exterior finishing layer, significantly reducing overall construction costs and social impact.

[0008] The aforementioned method for local replacement and reinforcement of shear walls in high-rise buildings, which retains a thin outer layer, involves rebound testing and core sampling in step one, which comply with JGJ / T 23-2011, "Technical Specification for Testing Compressive Strength of Concrete by Rebound Method". This invention, by controlling the rebound testing and core sampling to meet the specified procedures, facilitates the generation of standardized reports, providing a basis for subsequent zoning, replacement, and project acceptance, thus achieving standardized construction.

[0009] The aforementioned method for local replacement and reinforcement of shear walls in high-rise buildings, which retains a thin outer layer, involves replacing units with a width not exceeding 0.6m in step one. This invention, by controlling the width of the replacement units, minimizes the scope of single-stage removal and replacement, resulting in less weakening of the original shear wall section and smoother transfer of upper loads. Furthermore, this method also minimizes shrinkage of the newly poured concrete, reduces the risk of cracking, is suitable for construction in confined indoor spaces, facilitates continuous pouring operations, and improves construction safety and flexibility.

[0010] In the aforementioned method for partial replacement and reinforcement of the outer thin layer of shear wall in the exterior wall of a high-rise building, the diameter of the water drill in step four is 70mm~100mm. In this invention, the reinforcing bars in the shear wall are distributed in a mesh pattern. By controlling the diameter of the water drill to match the common spacing of shear wall reinforcing bars, it is convenient to place holes in non-reinforced areas, allowing core drilling within the mesh of reinforcing bars, improving removal efficiency. Furthermore, the water drill produces round holes, has high core extraction efficiency, and causes minimal disturbance to the retained outer thin layer of concrete, reducing the impact of the electric hammer and accidental damage to the reinforcing bars, ensuring regular removal boundaries, and creating favorable conditions for subsequent reinforcing bar repair and formwork support.

[0011] The aforementioned method for partial replacement and reinforcement of shear walls in high-rise buildings, which retains a thin outer layer, involves adding reinforcing bars of the same specification and reliably connecting them to the original bars when the corrosion thickness of the original reinforcing bars exceeds 2mm or they are broken, as described in step five. This invention restores the effective cross-section and tensile bearing capacity of the original reinforcing bars, avoids insufficient stress due to localized weak sections, ensures the continuity of the reinforcing bar skeleton, enhances the synergistic working ability of new and old concrete, and improves the seismic performance and durability of the reinforced shear wall.

[0012] In the aforementioned method for partial replacement and reinforcement of the outer thin layer of the shear wall in the exterior wall of a high-rise building, the template mentioned in step six is ​​a lightweight steel formwork or a film-coated wooden formwork. The lightweight steel formwork and film-coated wooden formwork in this invention are lightweight, have good rigidity, and are flexible in assembly, making them suitable for formwork support in confined indoor spaces. They also offer good demolding effect, a smooth surface, and high turnover rate, reducing grout leakage, honeycombing, and pitting, and improving the appearance quality and density of freshly poured concrete.

[0013] The aforementioned method for partial replacement and reinforcement of the outer thin layer of the shear wall in the exterior wall of a high-rise building, wherein step seven involves layered pouring using high-strength, early-strength, micro-expansion concrete or Class IV cement-based grout. Both the high-strength, early-strength, micro-expansion concrete and Class IV cement-based grout used in this invention possess characteristics such as good fluidity, high early strength, and micro-expansion compensating for shrinkage, enabling them to fully fill narrow replacement spaces and rapidly form load-bearing capacity, thus shortening the construction cycle.

[0014] The aforementioned method for partial replacement and reinforcement of shear walls in high-rise buildings, which retains a thin outer layer, involves repeating steps four through seven in step eight. The next replacement unit is constructed only after the strength of the previously poured shear wall reaches at least 80% of its design value. This invention uses 80% of the design strength as a control indicator, ensuring that the load is gradually transferred to the newly poured wall only after the previously poured wall has sufficient load-bearing capacity. This avoids excessive stress on the previously poured wall due to premature construction of adjacent units. This control standard balances construction efficiency and structural safety, enabling a streamlined replacement process.

[0015] The above-mentioned method for local replacement and reinforcement of the outer thin layer of the shear wall in the exterior wall of a high-rise building includes, in step nine, a finishing layer comprising putty and paint.

[0016] Compared with the prior art, the present invention has the following advantages: 1. This invention achieves partial replacement and reinforcement of the outer thin layer of shear wall in the exterior wall of high-rise buildings by dividing the wall into replacement units, setting up top supports, directional chiseling on the inner side, preserving the complete thin layer of concrete on the outer side, supporting the inner side with formwork, and pouring high-strength materials. The entire construction process is carried out only from the indoor side, without the need to erect external scaffolding, without damaging the external insulation layer, waterproof layer, and decorative surface layer, keeping the building facade intact, avoiding high-altitude operations and exterior wall repairs, significantly reducing the impact on normal use by users and the building's appearance, and avoiding wall instability and sudden load changes during the reinforcement process, reducing disturbance to the original structure and reinforcing steel, ensuring the overall safety of the high-rise shear wall during partial replacement, and preventing structural deformation, collapse, and facade damage.

[0017] 2. This invention uses the skip-pour method to determine the construction sequence and requires that the strength of the previous newly poured wall reaches more than 80% of the design value before constructing the next unit. This can effectively solve the stress lag problem in batch replacement. By combining high-strength early-strength micro-expansion concrete or Class IV cement-based grouting material, crack-resistant tie bars and moisture-retaining curing, it can compensate for shrinkage, restrain cracks, make the stress of each batch of walls more balanced, and improve the integrity and seismic performance of the reinforced shear wall.

[0018] 3. This invention uses interface agents and cement-based penetrating crystalline waterproofing agents to improve adhesion and enhance the waterproofing of exterior walls. In addition, the high-strength early-strength micro-expansion concrete or Class IV cement-based grouting material has good fluidity and high early strength, and can fill narrow spaces. By using lightweight steel molds or film-coated wooden molds, pouring ports and venting holes, and layered vibration, the newly poured concrete is ensured to be dense and free of voids, forming a reliable new and old synergistic stress system.

[0019] 4. The rebound detection and core sampling detection in this invention are based on JGJ / T 23-2011, which can accurately delineate areas with insufficient strength; the position of the steel bars is marked by the steel bar scanner to avoid accidentally damaging the original bars; by adding reinforcing bars of the same specification and reliably connecting them to the steel bars with rust thickness exceeding 2mm or by chiseling the steel bars, and at the same time removing rust, straightening, and implanting crack-resistant tie bars, the continuity of the steel bar cross section and skeleton can be restored, ensuring the reinforcement bearing capacity and durability.

[0020] 5. This invention involves construction entirely from the interior side, eliminating the need for external scaffolding and damage to the external insulation and decorative layers; it employs small-unit, skip-construction assembly line operations and rapid load-bearing capacity of early-strength materials, which can shorten the construction period; furthermore, the interior surface layer only requires putty and paint restoration, making construction simple, cost-effective, and causing minimal disruption to users, while maintaining the integrity of the building facade, resulting in significant comprehensive economic and social benefits.

[0021] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0022] Figure 1 This is a schematic diagram of the construction sequence of each replacement unit in Embodiment 1 of the present invention.

[0023] Figure 2 This is a schematic diagram of the construction sequence of each replacement unit in Embodiment 2 of the present invention.

[0024] Figure 3 This is a schematic diagram of the construction sequence of each replacement unit in Embodiment 3 of the present invention.

[0025] Figure 4 This is a schematic diagram of the construction sequence of each replacement unit in Embodiment 4 of the present invention. Detailed Implementation

[0026] Example 1 This embodiment includes the following steps: Step 1: Testing and Zoning: Rebound and core sampling tests are performed on the inner side of the shear walls in the exterior walls of high-rise buildings. Areas where the strength does not meet design and specification requirements are identified as insufficient strength areas. These insufficient strength areas are then vertically segmented into 11 replacement units, each 0.6m wide. The construction sequence of each replacement unit is determined using the skip-construction method, resulting in the shear walls to be constructed. The rebound and core sampling tests comply with JGJ / T 23-2011 "Technical Specification for Testing Compressive Strength of Concrete by Rebound Method". The construction sequence is as follows: Figure 1 , Figure 1 The first two pieces in the first group are constructed together, then the second two pieces in the second group are constructed together, the third two pieces in the third group are constructed together, the fourth two pieces in the fourth group are constructed together, the fifth two pieces in the fifth group are constructed together, and so on until the sixth group is constructed. Step 2, Temporary Support and Unloading: Top supports are installed at the floor level where the shear wall to be constructed is located and at the floor slab or connecting beam above it, obtained in Step 1, to obtain a shear wall with top supports; Step 3, Rebar Marking: Use a rebar scanner to scan the inside of the shear wall with top support obtained in Step 2 to obtain the location of the rebar and mark it; Step 4: Directional Removal of Inner Concrete: Following the construction sequence described in Step 1 and the location of the reinforcing bars described in Step 3, for the first replacement unit to be constructed, use an 80mm diameter water drill to drill 150mm into the shear wall in the non-reinforcing bar area. The thickness of the shear wall is 200mm. Then, pry off the core sample and remove it. Then, use an electric hammer to remove the protruding section and the remaining gap concrete, leaving a complete thin layer of concrete on the outside of the shear wall. Finally, roughen the removed surface, remove dust and moisten it to obtain the removed shear wall. Step 5, Reinforcing steel repair and reinforcement: Remove rust and straighten the original reinforcing steel obtained in Step 4 for chiseling out the shear wall. If the rust thickness of the original reinforcing steel exceeds 2mm or it is broken, add reinforcing steel of the same specification and reliably connect it with the original steel. Also, implant anti-crack tie bars in the thin concrete layer mentioned in Step 4 to obtain the reinforcing steel repair shear wall. Step 6, Interface Treatment and Inner Formwork: Apply interface agent and cement-based penetrating crystalline waterproofing agent to the chiseled surface of the steel reinforcement repair shear wall obtained in Step 5. Then, set up a lightweight steel formwork and temporary support on the inner side of the shear wall, leaving a pouring port and vent hole to obtain the cavity to be poured. Step 7, High-strength material pouring and curing: High-strength early-strength micro-expansion concrete is used to pour the cavity to be poured in layers and vibrate it to make it dense. After pouring, it is moisturized and cured. After the design strength is reached, the inner formwork and temporary support are removed. Step 8: Repeat steps 4 to 7, and after the strength of the previous newly poured shear wall reaches more than 80% of the design value, proceed with the construction of the next replacement unit until each replacement unit is completed and a new poured shear wall is obtained. Step 9: Interior surface layer restoration: Repair and level the newly poured shear wall obtained in Step 8, then restore the putty and paint finishing layer, and complete the local replacement and reinforcement of the thin outer layer of the shear wall in the exterior wall of the high-rise building.

[0027] Example 2 This embodiment includes the following steps: Step 1: Testing and Zoning: Rebound and core sampling tests are performed on the inner side of the shear walls in the exterior walls of high-rise buildings. Areas where the strength does not meet the design and specification requirements are identified as insufficient strength areas. These insufficient strength areas are then vertically divided into four replacement units, each 0.5m wide. The construction sequence of each replacement unit is determined using the skip-construction method, resulting in the shear walls to be constructed. The rebound and core sampling tests comply with JGJ / T 23-2011 "Technical Specification for Testing Compressive Strength of Concrete by Rebound Method". The construction sequence is as follows: Figure 2 , Figure 2 The first two pieces in the first group were constructed together, and then the second two pieces in the second group were constructed together. Step 2, Temporary Support and Unloading: Top supports are installed at the floor level where the shear wall to be constructed is located and at the floor slab or connecting beam above it, obtained in Step 1, to obtain a shear wall with top supports; Step 3, Rebar Marking: Use a rebar scanner to scan the inside of the shear wall with top support obtained in Step 2 to obtain the location of the rebar and mark it; Step 4: Directional Removal of Inner Concrete: Following the construction sequence described in Step 1 and the location of the reinforcing bars described in Step 3, for the first replacement unit to be constructed, use a 100mm diameter water drill to drill 190mm into the shear wall in the non-reinforcing bar area. The thickness of the shear wall is 250mm. Then, pry off the core sample and remove it. Then, use an electric hammer to remove the protruding section and the remaining gap concrete, leaving a complete thin layer of concrete on the outside of the shear wall. Finally, roughen the removed surface and remove dust and wet it to obtain the removed shear wall. Step 5, Reinforcing steel repair and reinforcement: Remove rust and straighten the original reinforcing steel obtained in Step 4 for chiseling out the shear wall. If the rust thickness of the original reinforcing steel exceeds 2mm or it is broken, add reinforcing steel of the same specification and reliably connect it with the original steel. Also, implant anti-crack tie bars in the thin concrete layer mentioned in Step 4 to obtain the reinforcing steel repair shear wall. Step 6, Interface Treatment and Inner Formwork: Apply interface agent and cement-based penetrating crystalline waterproofing agent to the chiseled surface of the steel reinforcement repair shear wall obtained in Step 5. Then, set up a film-covered wooden formwork and temporary support on the inner side of the shear wall, leaving a pouring port and vent hole to obtain the cavity to be poured. Step 7, High-strength material pouring and curing: High-strength early-strength micro-expansion concrete is used to pour the cavity to be poured in layers and vibrate it to make it dense. After pouring, it is moisturized and cured. After the design strength is reached, the inner formwork and temporary support are removed. Step 8: Repeat steps 4 to 7, and after the strength of the previous newly poured shear wall reaches more than 80% of the design value, proceed with the construction of the next replacement unit until each replacement unit is completed and a new poured shear wall is obtained. Step 9: Interior surface layer restoration: Repair and level the newly poured shear wall obtained in Step 8, then restore the putty and paint finishing layer, and complete the local replacement and reinforcement of the thin outer layer of the shear wall in the exterior wall of the high-rise building.

[0028] Example 3 This embodiment includes the following steps: Step 1: Testing and Zoning: Rebound and core sampling tests are performed on the inner side of the shear walls in the exterior walls of high-rise buildings. Areas where the strength does not meet the design and specification requirements are identified as insufficient strength areas. These insufficient strength areas are then vertically divided into 13 replacement units, each 0.4m wide. The construction sequence of each replacement unit is determined using the skip-construction method, resulting in the shear walls to be constructed. The rebound and core sampling tests comply with JGJ / T 23-2011 "Technical Specification for Testing Compressive Strength of Concrete by Rebound Method". The construction sequence is as follows: Figure 3 , Figure 3 The first two pieces in the first group are constructed together, then the second two pieces in the second group are constructed together, then the third two pieces in the third group are constructed together, then the fourth group is constructed together, then the fifth group is constructed together, then the sixth group is constructed together, and finally the seventh group is constructed together. Step 2, Temporary Support and Unloading: Top supports are installed at the floor level where the shear wall to be constructed is located and at the floor slab or connecting beam above it, obtained in Step 1, to obtain a shear wall with top supports; Step 3, Rebar Marking: Use a rebar scanner to scan the inside of the shear wall with top support obtained in Step 2 to obtain the location of the rebar and mark it; Step 4: Directional Removal of Inner Concrete: Following the construction sequence described in Step 1 and the location of the reinforcing bars described in Step 3, for the first replacement unit to be constructed, use a 70mm diameter water drill to drill 160mm into the shear wall in the non-reinforcing bar area. The thickness of the shear wall is 200mm. Then, pry off the core sample and remove it. Use an electric hammer to remove the protruding section and the remaining gap concrete, leaving a complete thin layer of concrete on the outside of the shear wall. Finally, roughen the removed surface, remove dust and moisten it to obtain the removed shear wall. Step 5, Reinforcing steel repair and reinforcement: Remove rust and straighten the original reinforcing steel obtained in Step 4 for chiseling out the shear wall. If the rust thickness of the original reinforcing steel exceeds 2mm or it is broken, add reinforcing steel of the same specification and reliably connect it with the original steel. Also, implant anti-crack tie bars in the thin concrete layer mentioned in Step 4 to obtain the reinforcing steel repair shear wall. Step 6, Interface Treatment and Inner Formwork: Apply interface agent and cement-based penetrating crystalline waterproofing agent to the chiseled surface of the steel reinforcement repair shear wall obtained in Step 5. Then, set up a lightweight steel formwork and temporary support on the inner side of the shear wall, leaving a pouring port and vent hole to obtain the cavity to be poured. Step 7, High-strength material pouring and curing: The cavity to be poured obtained in Step 6 is poured in layers and compacted by vibration using Class IV cement-based grout. After pouring, it is kept moist and cured. After reaching the design strength, the inner formwork and temporary support are removed. Step 8: Repeat steps 4 to 7, and after the strength of the previous newly poured shear wall reaches more than 80% of the design value, proceed with the construction of the next replacement unit until each replacement unit is completed and a new poured shear wall is obtained. Step 9: Interior surface layer restoration: Repair and level the newly poured shear wall obtained in Step 8, then restore the putty and paint finishing layer, and complete the local replacement and reinforcement of the thin outer layer of the shear wall in the exterior wall of the high-rise building.

[0029] Example 4 This embodiment includes the following steps: Step 1: Testing and Zoning: Rebound and core sampling tests are performed on the inner side of the shear walls in the exterior walls of high-rise buildings. Areas where the strength does not meet design and specification requirements are identified as insufficient strength areas. These insufficient strength areas are then vertically segmented into 14 replacement units, each 0.3m wide. The construction sequence of each replacement unit is determined using the skip-construction method, resulting in the shear walls to be constructed. The rebound and core sampling tests comply with JGJ / T 23-2011 "Technical Specification for Testing Compressive Strength of Concrete by Rebound Method". The construction sequence is as follows: Figure 4 , Figure 4 The first two pieces of the first group are constructed together, then the second two pieces of the second group are constructed together, the third two pieces of the third group are constructed together, and so on, until the seventh group of two pieces are constructed together. Step 2, Temporary Support and Unloading: Top supports are installed at the floor level where the shear wall to be constructed is located and at the floor slab or connecting beam above it, obtained in Step 1, to obtain a shear wall with top supports; Step 3, Rebar Marking: Use a rebar scanner to scan the inside of the shear wall with top support obtained in Step 2 to obtain the location of the rebar and mark it; Step 4: Directional Removal of Inner Concrete: Following the construction sequence described in Step 1 and the location of the reinforcing bars described in Step 3, for the first replacement unit to be constructed, use a 90mm diameter water drill to drill 150mm into the shear wall in the non-reinforcing bar area. The thickness of the shear wall is 200mm. Then, pry off the core sample and remove it. Then, use an electric hammer to remove the protruding section and the remaining gap concrete, leaving a complete thin layer of concrete on the outside of the shear wall. Finally, roughen the removed surface and remove dust and wet it to obtain the removed shear wall. Step 5, Reinforcing steel repair and reinforcement: Remove rust and straighten the original reinforcing steel obtained in Step 4 for chiseling out the shear wall. If the rust thickness of the original reinforcing steel exceeds 2mm or it is broken, add reinforcing steel of the same specification and reliably connect it with the original steel. Also, implant anti-crack tie bars in the thin concrete layer mentioned in Step 4 to obtain the reinforcing steel repair shear wall. Step 6, Interface Treatment and Inner Formwork: Apply interface agent and cement-based penetrating crystalline waterproofing agent to the chiseled surface of the steel reinforcement repair shear wall obtained in Step 5. Then, set up a lightweight steel formwork and temporary support on the inner side of the shear wall, leaving a pouring port and vent hole to obtain the cavity to be poured. Step 7, High-strength material pouring and curing: High-strength early-strength micro-expansion concrete is used to pour the cavity to be poured in layers and vibrate it to make it dense. After pouring, it is moisturized and cured. After the design strength is reached, the inner formwork and temporary support are removed. Step 8: Repeat steps 4 to 7, and after the strength of the previous newly poured shear wall reaches more than 80% of the design value, proceed with the construction of the next replacement unit until each replacement unit is completed and a new poured shear wall is obtained. Step 9: Interior surface layer restoration: Repair and level the newly poured shear wall obtained in Step 8, then restore the putty and paint finishing layer, and complete the local replacement and reinforcement of the thin outer layer of the shear wall in the exterior wall of the high-rise building.

[0030] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the inventive essence shall still fall within the protection scope of the present invention.

Claims

1. A method for local replacement and reinforcement of shear walls in high-rise buildings, retaining the thin outer layer, characterized in that... The method includes the following steps: Step 1, Inspection and Zoning: Rebound test and core sampling are carried out on the inner side of the shear wall in the exterior wall of the high-rise building. Areas whose strength does not meet the design requirements and specifications are identified as areas with insufficient strength. Then, the areas with insufficient strength are divided vertically into multiple replacement units. The construction sequence of each replacement unit is determined by the skip-fill method to obtain the shear wall to be constructed. Step 2, Temporary Support and Unloading: Top supports are installed at the floor level where the shear wall to be constructed is located and at the floor slab or connecting beam above it, obtained in Step 1, to obtain a shear wall with top supports; Step 3, Rebar Marking: Use a rebar scanner to scan the inside of the shear wall with top support obtained in Step 2 to obtain the location of the rebar and mark it; Step 4, Directional Removal of Inner Concrete: Following the construction sequence described in Step 1 and the location of the reinforcing bars described in Step 3, for the first group of replacement units that need to be constructed, use a water drill to drill into the shear wall in the non-reinforcing bar area with a depth of d-(40~60)mm, where d is the thickness of the shear wall in mm. Then, pry off the core sample and remove it. Then, use an electric hammer to remove the protruding section and the remaining gap concrete, leaving a complete thin layer of concrete on the outside of the shear wall. Finally, roughen the removed surface and remove dust and wet it to obtain the removed shear wall. Step 5, Reinforcement Repair and Strengthening: Remove rust and straighten the original reinforcement bars of the shear wall obtained in Step 4, and implant anti-crack tie bars into the thin concrete layer mentioned in Step 4 to obtain the reinforcement-repaired shear wall; Step 6, Interface Treatment and Inner Formwork: Apply interface agent and cement-based penetrating crystalline waterproofing agent to the chiseled surface of the steel reinforcement repair shear wall obtained in Step 5. Then, set up formwork and temporary support on the inner side of the shear wall, leaving pouring opening and vent hole to obtain the cavity to be poured. Step 7, High-strength material pouring and curing: The cavity to be poured obtained in Step 6 is poured in layers and vibrated to compact it. After pouring, it is moisturized and cured. After the design strength is reached, the inner template and temporary support are removed. Step 8: Repeat construction: Repeat steps 4 to 7 until each replacement unit is completed and a new shear wall is obtained; Step 9: Indoor surface layer restoration: Repair and level the newly poured shear wall obtained in Step 8, then restore the finishing layer, and complete the local replacement and reinforcement of the thin outer layer of the shear wall in the exterior wall of the high-rise building.

2. The method for local replacement and reinforcement of the outer thin layer of the shear wall in the exterior wall of a high-rise building according to claim 1, characterized in that, The rebound test and core sampling test described in step one meet the requirements of JGJ / T 23-2011 "Technical Specification for Testing Compressive Strength of Concrete by Rebound Method".

3. The method for local replacement and reinforcement of the outer thin layer of the shear wall in the exterior wall of a high-rise building according to claim 1, characterized in that, The width of the replacement unit mentioned in step one is no greater than 0.6m.

4. A method for local replacement and reinforcement of a shear wall retaining a thin outer layer in the exterior wall of a high-rise building according to claim 1, characterized in that, The diameter of the water drill mentioned in step four is 70mm~100mm.

5. A method for local replacement and reinforcement of a shear wall retaining a thin outer layer in the exterior wall of a high-rise building according to claim 1, characterized in that, If the original steel reinforcement has a rust thickness exceeding 2mm or is broken as described in step five, reinforcing steel reinforcement of the same specification shall be added and reliably connected to the original reinforcement.

6. A method for local replacement and reinforcement of a shear wall retaining a thin outer layer in the exterior wall of a high-rise building according to claim 1, characterized in that, The template mentioned in step six is ​​a lightweight steel mold or a film-coated wooden mold.

7. A method for local replacement and reinforcement of a shear wall retaining a thin outer layer in the exterior wall of a high-rise building according to claim 1, characterized in that, The layered pouring described in step seven uses high-strength, early-strength, micro-expansion concrete or Class IV cement-based grouting material.

8. A method for local replacement and reinforcement of a shear wall retaining a thin outer layer in the exterior wall of a high-rise building according to claim 1, characterized in that, In step eight, during the process of repeating steps four through seven, after the strength of the previously newly poured shear wall reaches more than 80% of the design value, the construction of the next replacement unit will proceed.

9. A method for local replacement and reinforcement of a shear wall retaining a thin outer layer in the exterior wall of a high-rise building according to claim 1, characterized in that, The finishing layer described in step nine includes putty and paint.