A multi-layer composite pipe for subsea oil and gas transportation and a method for manufacturing the same
By setting a prefabricated slip-limiting interlocking strip between the compressive armor layer and the inner tensile armor layer, and utilizing the mechanical interlocking of the discrete protrusions and grooves on both sides of the strip, the abnormal slippage problem of the non-bonded flexible tube under dynamic bending conditions is solved. This achieves selective slip limitation, which prevents interference during normal sliding and only interferes during abnormal sliding, reducing fretting wear and fatigue risks, and ensuring the flexibility and wear resistance of the tube body.
Patent Information
- Application Number
- CN202611668231.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-27
- Publication Date
- 2026-11-24
AI Technical Summary
Under dynamic bending conditions, the abnormal relative slippage between the compressive armor layer and the inner tensile armor layer of existing non-bonded flexible tubes cannot be effectively limited, resulting in fretting wear and shortened fatigue life. Existing technologies fail to simultaneously ensure tube bending flexibility and interlayer slippage control.
A prefabricated anti-slip interlocking strip is set between the compressive armor layer and the inner tensile armor layer. The strip uses discrete protrusions on both sides of the strip and the pre-machined grooves of the adjacent steel layer for disengageable mechanical interlocking. By setting matching grooves and protrusion arrays on the outer surface of the compressive armor layer and the inner surface of the inner tensile armor layer, free sliding during normal sliding and limiting during abnormal sliding can be achieved.
It effectively limits the abnormal slippage amplitude between the compressive armor layer and the inner tensile armor layer, reduces the risk of fretting wear and fretting fatigue, maintains the bending flexibility of the tube body, and provides a graded response mechanism of friction damping and rigid limiting through biomimetic protrusions, thereby improving the wear resistance and fatigue life of the tube body.
Smart Images

Figure CN123154196A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite pipe technology, and more specifically, to a multi-layer composite pipe for subsea oil and gas transportation and its preparation method. Background Technology
[0002] Non-bonded flexible pipes are composed of an extruded polymer layer and a spiral metal reinforcement layer. Each layer can slide relative to the other when the pipe is bent, thus combining high axial / radial stiffness with excellent bending flexibility. This type of pipe is the mainstream pipe for deep-sea oil and gas transportation.
[0003] A typical existing non-bonded flexible tube structure comprises, from the inside out: a skeleton layer, a polymer inner liner, a compression armor layer, an inner tensile armor layer, an outer tensile armor layer, a buckling-resistance layer, and an outer sheath. The compression armor layer is a Z-shaped interlocking carbon steel strip with a near-circumferential winding angle, resisting circumferential stress from the internal pressure. The inner and outer tensile armor layers are double-layered, counter-winding carbon steel flat wires, balancing axial tension and torque.
[0004] The flexibility of unbonded flexible tubes stems from the "allowable relative slippage" between their layers. However, under dynamic bending conditions, repeated relative slippage occurs between the compressive armor layer and the inner tensile armor layer. If the two steel armor layers are in direct contact, the contact stress is significant, easily leading to fretting wear and fretting fatigue. Existing solutions typically use a smooth polymer anti-wear strip between the two layers, but this strip only passively isolates the two metal layers and cannot limit the amplitude of abnormal slippage. Once the anti-wear strip fails due to wear or creep, the compressive armor layer and the inner tensile armor layer will be in direct contact, drastically shortening the fatigue life.
[0005] In the prior art, Chinese patent CN113531235B discloses an X-shaped profile and a pressure-resistant armor layer for marine composite hoses. The profiles are connected by interlocking winding, with gaps between the interlocking structures allowing for relative sliding. However, the interlocking and gaps in this patent are limited to the profiles within the pressure-resistant armor layer itself. Its technical purpose is to prevent slippage between adjacent steel strips of the pressure-resistant armor layer, and it does not address interlayer slippage control between the pressure-resistant armor layer and the inner tensile armor layer.
[0006] Chinese patent application CN122429299A discloses a biomimetic micro-anchoring intercalation layer, a composite tube, and its preparation method. This biomimetic micro-anchoring intercalation layer includes a matrix with a fibrous mesh structure or a nonwoven fabric structure. The surface and / or interior of the matrix are provided with micron-sized fiber protrusions (10–2000 μm in length and 0.5–20 μm in diameter), which extend into three-dimensional space to achieve mechanical interlocking. This biomimetic micro-anchoring intercalation layer achieves interlocking by embedding micron-fibers into the upper and lower matrix layers or resin. It is suitable for composite tube applications requiring complete interlayer anchoring, but not for applications where metal layers in non-bonded flexible tubes need to maintain relative sliding space.
[0007] None of the aforementioned existing technologies simultaneously solve the technical challenge of "actively limiting abnormal relative slippage between the compressive armor layer and the inner tensile armor layer while ensuring the bending flexibility of the pipe body". Summary of the Invention
[0008] The purpose of this invention is to overcome the shortcomings of the prior art and provide a multi-layer composite pipe for subsea oil and gas transportation and its preparation method. While maintaining the basic layer structure of the non-bonded flexible pipe, a prefabricated anti-slip interlocking strip is set between the pressure-resistant armor layer and the inner tensile armor layer. The strip utilizes the detachable mechanical interlocking of discrete protrusions on both sides of the strip with pre-machined grooves in the adjacent steel layers to allow normal bending and slip while limiting abnormal slip amplitude, thereby solving the problem of interlayer fretting wear.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: A multi-layer composite pipe for subsea oil and gas transportation comprises, from the inside out, a skeleton layer, a polymer inner liner, a pressure-resistant armor layer, an inner tensile armor layer, an outer tensile armor layer, a buckling-resistance layer, and an outer sheath. A prefabricated slip-limiting interlocking strip is provided between the pressure-resistant armor layer and the inner tensile armor layer. The prefabricated slip-limiting interlocking strip includes a continuous strip-shaped substrate, with discrete tooth arrays on both its inner and outer surfaces. The outer surface of the pressure-resistant armor layer is machined with a groove array A matching the discrete tooth array on the inner surface, and the inner surface of the inner tensile armor layer is machined with a groove array B matching the discrete tooth array on the outer surface. The prefabricated slip-limiting interlocking strip spirally wraps around the outer surface of the pressure-resistant armor layer, with the discrete teeth on the inner surface embedded in groove array A and the discrete teeth on the outer surface embedded in groove array B. The discrete protrusions have an initial circumferential gap of 0.05–0.2 mm between their sides and the corresponding groove sidewalls in the direction around the tube axis, and an initial radial gap of 0.1–0.5 mm between their tops and the bottoms of the grooves. When the relative slip between layers is less than or equal to the initial circumferential gap, the discrete protrusions can slide freely within the grooves to maintain the flexibility of the tube. When the relative slip between layers is greater than the initial circumferential gap, the sides of the discrete protrusions abut against the sidewalls of the grooves to limit further slippage.
[0010] Furthermore, the tooth height of the discrete convex teeth is 0.2–2 mm, and the pitch between adjacent discrete convex teeth in the length direction of the strip matrix is 0.5–5 mm; the tooth shape of the discrete convex teeth is one or a combination of trapezoidal, triangular, and arc-shaped, and the tooth tip width is 1 / 3–2 / 3 of the pitch; the discrete convex tooth array on the inner side of the strip matrix corresponds one-to-one with the discrete convex tooth array on the outer side of the strip matrix in the thickness direction of the strip matrix.
[0011] Furthermore, the tooth tip surface of the discrete protrusion is provided with biomimetic protrusions, which are columnar or branched, with a height of 50–500 μm, a root diameter of 5–100 μm, and a surface density of 10. 4 ~10 6 pcs / cm 2 The spacing between adjacent biomimetic protrusions is 10–200 μm; the biomimetic protrusions provide frictional damping when the relative slip between layers is less than or equal to the initial circumferential gap, and the discrete protrusions provide rigid restraint when the relative slip between layers is greater than the initial circumferential gap.
[0012] Furthermore, the material of the strip matrix is thermoplastic polyurethane or polyetheretherketone, with a width of 50-300 mm and a thickness of 1-5 mm; the strip matrix is incorporating a hybrid reinforcing phase of chopped carbon fibers and aramid fibers, with a mass ratio of carbon fibers to aramid fibers of (1-3):1 and a fiber length of 50-500 μm.
[0013] Furthermore, the groove depth of groove array A is 0.2–2.5 mm and does not exceed 15% of the thickness of the steel strip constituting the compressive armor layer; the groove depth of groove array B is 0.2–2.5 mm and does not exceed 15% of the radial thickness of the steel wire in the inner tensile armor layer; the spiral winding angle of the prefabricated limited-slip interlocking belt is 5°–15°; when the prefabricated limited-slip interlocking belt is spirally wound, a gap of 0.5–3 mm is reserved between adjacent turns, the width of the gap is smaller than the spacing of the discrete protrusions in the width direction of the strip matrix, and the gap is filled with thermoplastic elastomer or silicone rubber.
[0014] Furthermore, the skeleton layer is an S-shaped interlocking stainless steel strip; the polymer inner liner is made of PVDF or PA12 with a thickness of 6–15 mm; the compression armor layer is a Z-shaped interlocking carbon steel strip; both the inner and outer tensile armor layers are made of carbon steel flat wire; the buckling-resistant layer is made of aramid or glass fiber reinforced polymer tape; the outer sheath is made of HDPE, PA, or PVDF; the winding angle of the compression armor layer is 82°–88°, the winding angle of the inner tensile armor layer is +30°–+35°, and the winding angle of the outer tensile armor layer is -35°–-30°.
[0015] In this invention, the above-mentioned further technical solutions can be implemented individually or in any combination without conflict.
[0016] The present invention also provides a method for preparing the above-mentioned multilayer composite pipe, comprising the following steps: S1: Spiral winding of S-shaped interlocking stainless steel strip on the core mold to form the skeleton layer; S2: Extrusion molding of polymer inner liner on the skeleton layer; S3: A Z-shaped interlocking carbon steel strip is wound around the polymer inner liner at a winding angle of 82° to 88° to form a pressure-resistant armor layer; S4: Groove array A is machined on the outer surface of the pressure-resistant armor layer; S5: Prefabricated limited-slip interlocking belt: Extruded thermoplastic polyurethane or polyetheretherketone continuous belt, with discrete tooth arrays formed on the inner and outer sides of the belt respectively. S6: The prefabricated limited-slip interlocking belt obtained in step S5 is wound around the outer surface of the pressure-resistant armor layer with a helical angle of 5° to 15°, so that the discrete protrusions on the inner side of the belt are embedded in the groove array A. By controlling the processing size of the discrete protrusions and the processing size of the groove array A, the discrete protrusions are embedded in the groove array A to form an initial circumferential gap of 0.05 to 0.2 mm and an initial radial gap of 0.1 to 0.5 mm. S7: The inner surface of the carbon steel flat wire is processed to form a groove structure that matches the discrete tooth array on the inner surface of the carbon steel flat wire; then the carbon steel flat wire is wound around the outer surface of the prefabricated limited slip interlocking strip obtained in step S6 at a winding angle of +30° to +35° to form an inner tensile armor layer. The groove structure forms a groove array B on the inner surface of the inner tensile armor layer. During the winding process, the discrete teeth on the outer side of the strip are embedded in the groove array B. By controlling the processing size of the discrete teeth and the processing size of the groove array B, the discrete teeth are embedded in the groove array B to form an initial circumferential gap of 0.05 to 0.2 mm and an initial radial gap of 0.1 to 0.5 mm. S8: The outer tensile armor layer is formed by reverse winding at a winding angle of -35° to -30°; S9: Wrapped anti-buckling layer; S10: Extruded outer sheath, assembly end connector; In steps S6 and S7, the embedding rate of discrete protrusions into the corresponding grooves is not less than 90% by controlling the winding tension. The embedding rate is defined as the percentage of the number of protrusions that are actually embedded into the corresponding grooves in each turn of the prefabricated limited-slip interlocking belt, with an initial circumferential gap of 0.05 to 0.2 mm and an initial radial gap of 0.1 to 0.5 mm, relative to the total number of protrusions on the corresponding side in that turn. The corresponding side is the inner side in step S6 and the outer side in step S7.
[0017] Further, in step S5, during the extrusion of the continuous strip, a hybrid reinforcing phase of chopped carbon fibers and aramid fibers is incorporated into the matrix of the strip at a mass ratio of (1-3):1, with a fiber length of 50-500 μm; during the forming of the discrete tooth array, the tooth tip surface of the discrete teeth is formed into a columnar or branched shape, with a protrusion height of 50-500 μm, a root diameter of 5-100 μm, and an areal density of 10. 4 ~10 6 pcs / cm 2The biomimetic protrusions are made, and the spacing between adjacent biomimetic protrusions is controlled at 10-200μm; in step S6, during winding, a gap of 0.5-3mm is reserved between adjacent turns, and thermoplastic elastomer or silicone rubber is filled in the gap.
[0018] Further, in step S4, the groove array A is processed by laser etching or roll forming, and the groove depth is controlled to be 0.2-2.5 mm and not more than 15% of the thickness of the steel strip constituting the pressure-resistant armor layer; in step S7, the groove structure is processed on the inner surface of the carbon steel flat wire by laser etching or roll forming, and the groove depth is controlled to be 0.2-2.5 mm and not more than 15% of the radial thickness of the carbon steel flat wire.
[0019] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention establishes a prefabricated slip-limiting interlocking strip between the compressive armor layer and the inner tensile armor layer. Discrete protrusions on both sides of the strip are embedded in the groove array A on the outer surface of the compressive armor layer and the groove array B on the inner surface of the inner tensile armor layer, forming a cross-layer mechanical interlock. During normal bending of the tube, the protrusions can slide freely within the grooves to maintain the tube's flexibility. When the relative slippage between the layers exceeds the initial circumferential gap, the sides of the protrusions abut against the groove sidewalls, limiting further slippage. This achieves selective slip limitation, where "normal slippage does not interfere, and abnormal slippage only interferes." This mechanism effectively limits the abnormal slippage amplitude between the compressive armor layer and the inner tensile armor layer, reducing the risk of fretting wear and fretting fatigue.
[0020] 2. The discrete protrusions of the prefabricated limited-slip interlocking belt have biomimetic protrusions on their tooth tip surfaces. During the small slip stage (when the slip amount is less than or equal to the initial circumferential clearance), the biomimetic protrusions provide frictional damping, reducing direct metal-to-metal contact wear. During the large slip stage (when the slip amount is greater than the initial circumferential clearance), the discrete protrusions provide rigid restraint. The two work together at different slip scales to form a two-stage graded response mechanism of "micro-protrusion frictional damping in the small slip segment and macro-tooth rigid restraint in the over-threshold segment".
[0021] 3. A hybrid reinforcing phase of chopped carbon fiber and aramid fiber is incorporated into the strip matrix. The carbon fiber provides stiffness and shear strength to resist the deformation and wear of the protrusions in the grooves, while the aramid provides toughness and fatigue resistance to withstand repeated bending and slip loads. The synergistic effect of the two makes the belt have both creep resistance and wear resistance, avoiding the problem of insufficient stiffness or toughness of single fiber solutions, and ensuring that the belt does not fail before the limited slip function under repeated slip conditions.
[0022] 4. When the prefabricated anti-slip interlocking belt is spirally wound, a gap is reserved between adjacent turns so that the anti-slip function is achieved by the "meshing of the teeth and grooves" rather than by the rigid constraint formed by the overlap of the belt material, thus avoiding the belt material itself becoming a bottleneck in the anti-slip function and affecting the flexibility of the pipe body.
[0023] 5. The preparation method of the present invention controls the processing dimensions of discrete protrusions and the processing dimensions of the groove array A / B, so that the protrusions are embedded in the grooves to form a preset circumferential initial gap and radial initial gap; by controlling the winding tension, the embedding rate is not less than 90%, ensuring that each protrusion can participate in the limited slip function and guaranteeing the consistency of the preparation quality. Attached Figure Description
[0024] Figure 1 This is a schematic cross-sectional view of the prefabricated limited-slip interlocking belt of the present invention; Figure 2 This is a magnified view showing the detailed interaction between the discrete convex teeth and the groove array A and groove array B of the present invention. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of protection of this invention.
[0026] I. Overall Structure of Multi-Layer Composite Pipes This invention provides a multi-layer composite pipe for submarine oil and gas transportation, comprising, from the inside out: a skeleton layer, a polymer inner lining layer, a pressure-resistant armor layer, a prefabricated slip-limiting interlocking band, an inner tensile armor layer, an outer tensile armor layer, a buckling-resistant layer, and an outer sheath.
[0027] The skeleton layer is an S-shaped interlocking stainless steel strip, made of corrosion-resistant materials such as 304L, 316L, or duplex stainless steel, and formed by continuous spiral winding and interlocking. The skeleton layer is used to resist external pressure, prevent the inner lining layer from being crushed, and provide radial stiffness.
[0028] The polymer liner is placed outside the skeleton layer and is extruded from thermoplastic polymers such as PVDF or PA12, with a thickness of 6–15 mm. The liner serves to form a fluid sealing barrier to prevent internal fluid leakage.
[0029] The pressure-resistant armor layer is located outside the polymer inner liner and is formed by interlocking Z-shaped carbon steel strips spirally wound at a winding angle of 82° to 88°. The pressure-resistant armor layer is used to withstand the circumferential stress generated by the pressure inside the pipe and to provide radial stiffness.
[0030] The prefabricated limited-slip interlocking strip is installed between the compressive armor layer and the inner tensile armor layer. The specific structure of the prefabricated limited-slip interlocking strip will be described in detail below.
[0031] The inner tensile armor layer is located outside the prefabricated limited-slip interlocking strip and is formed by spirally winding carbon steel flat wire at a winding angle of +30° to +35°. The outer tensile armor layer is located outside the inner tensile armor layer and is formed by spirally winding carbon steel flat wire in the opposite direction at a winding angle of -35° to -30°. The inner and outer tensile armor layers are wound in opposite directions to achieve torque balance and jointly bear the axial tensile load.
[0032] The buckling-resistant layer is placed on the outside of the outer tensile armor layer and is wrapped with aramid or glass fiber reinforced polymer tape to prevent radial buckling of the tensile armor layer.
[0033] The outer sheath is placed outside the buckling-resistant layer and is made of polymers such as HDPE, PA or PVDF through extrusion molding to prevent seawater corrosion and mechanical damage.
[0034] II. Detailed Structure of Prefabricated Limited-Slip Interlocking Belt Please see Figure 1 The prefabricated limited-slip interlocking belt includes a continuous strip-shaped substrate, and discrete convex tooth arrays are provided on both the inner and outer sides of the strip-shaped substrate.
[0035] Strip matrix: The strip matrix is made of thermoplastic polyurethane (TPU) or polyetheretherketone (PEEK). TPU combines elasticity and fatigue resistance, making it suitable for general working conditions; PEEK has excellent high-temperature performance and chemical corrosion resistance, making it suitable for high-temperature or highly corrosive working conditions. The strip width is 50–300 mm, preferably 100–200 mm; the strip thickness is 1–5 mm, preferably 2–3 mm. A hybrid reinforcing phase of chopped carbon fibers and aramid fibers is incorporated into the strip matrix. Carbon fibers provide stiffness and shear strength to resist deformation and wear of the protrusions in the grooves; aramid fibers provide toughness and fatigue resistance to withstand repeated bending and sliding loads. The mass ratio of carbon fibers to aramid fibers is (1–3):1, preferably 2:1; the fiber length is 50–500 μm, preferably 100–300 μm.
[0036] When the mass ratio of carbon fiber to aramid fiber is less than 1:1, the belt stiffness is insufficient, and the protrusions are prone to deformation in the grooves; when the mass ratio is greater than 3:1, the belt toughness is insufficient, and fatigue fracture is likely to occur under repeated slip conditions. When the fiber length is less than 50 μm, the reinforcing effect is limited; when the fiber length is greater than 500 μm, the fibers are unevenly dispersed in the matrix, affecting the forming accuracy of the protrusions. Therefore, the above-mentioned ratio and length range are the preferred ranges that balance stiffness, toughness, and forming accuracy.
[0037] It should be noted that the synergistic effect of the hybrid fibers is mainly reflected in creep resistance and abrasion resistance. The addition of carbon fiber improves the tensile modulus and shear strength of the belt, while the addition of aramid fiber improves the toughness and fatigue resistance of the belt. After the two are mixed, the belt achieves complementary properties in terms of creep resistance and abrasion resistance.
[0038] Discrete tooth array: Discrete tooth arrays are provided on both the inner and outer surfaces of the strip substrate. The tooth height of the discrete teeth is 0.2–2 mm, preferably 0.5–1.5 mm; the pitch between adjacent discrete teeth along the length of the strip substrate is 0.5–5 mm, preferably 1–3 mm; the tooth shape of the discrete teeth is one or a combination of trapezoidal, triangular, and arc-shaped, preferably trapezoidal, to facilitate demolding and uniform stress; the tooth tip width is 1 / 3–2 / 3 of the pitch. The discrete tooth arrays on the inner and outer surfaces of the strip substrate correspond one-to-one in the thickness direction of the strip substrate, ensuring uniform stress transmission along the thickness direction and preventing buckling under eccentric loads. It is worth mentioning that… Figure 1 and Figure 2 The convex teeth and grooves are drawn as trapezoids in the figure, which is only an example and does not constitute a limitation of the present invention.
[0039] It should be noted that the steel strip that constitutes the compressive armor layer is a Z-shaped interlocking carbon steel strip, and the steel wire that constitutes the inner tensile armor layer is a carbon steel flat wire.
[0040] Bionic protrusions: The tooth tip surface of the discrete protrusions is provided with bionic protrusions. These protrusions are columnar or branched, with a height of 50–500 μm, a root diameter of 5–100 μm, and a surface density of 10. 4 ~10 6 pcs / cm 2 The spacing between adjacent biomimetic protrusions ranges from 10 to 200 μm. These protrusions can be integrally formed onto the tooth tip surface using processes such as molding, laser etching, or 3D printing, eliminating the need for additional bonding or assembly. The biomimetic protrusions and the macroscopic discrete teeth form a dual-scale interlocking structure: "macroscopic tooth-groove mechanical interlock + microscopic tooth tip biomimetic protrusion friction enhancement." During the small slip phase (when the slip is less than or equal to the initial circumferential clearance), the biomimetic protrusion makes microscopic contact with the bottom / side surface of the groove, providing continuous frictional damping through its high areal density. During the large slip phase (when the slip is greater than the initial circumferential clearance), the side surface of the macroscopic discrete teeth abuts against the groove sidewall, providing rigid restraint. The two structures have clearly defined functions and do not interfere with each other. During the large slip phase, the bionic protrusions do not participate in the main load-bearing. Even if some bionic protrusions are flattened due to contact stress, their roots remain on the tooth tip surface, which does not affect the rigid limiting function of the macroscopic tooth. Furthermore, during the large slip phase, the limiting function is mainly achieved by the contact between the side of the macroscopic tooth and the groove sidewall, without relying on the integrity of the bionic protrusions.
[0041] If only macroscopic discrete teeth are provided without biomimetic protrusions, during the small slip stage (when the slip amount is less than or equal to the initial circumferential clearance), the teeth and grooves are in direct metal-polymer contact, resulting in a low coefficient of friction and limited wear reduction. Conversely, if only biomimetic protrusions are provided without macroscopic discrete teeth, during the large slip stage (when the slip amount is greater than the initial circumferential clearance), the biomimetic protrusions cannot provide sufficient rigid restraint, and the teeth may dislodge from the grooves. Therefore, a dual-scale fit between macroscopic teeth and biomimetic protrusions is necessary.
[0042] III. Setting and Coordination Relationship of Trench Array A / B Please see Figure 2 The outer surface of the pressure-resistant armor layer is machined with a groove array A that matches the discrete tooth array on the inner surface of the strip-shaped substrate. The groove depth of the groove array A is 0.2–2.5 mm and does not exceed 15% of the thickness of the steel strip constituting the pressure-resistant armor layer. The groove array A can be processed by laser etching or roll forming. Laser etching has high precision and is suitable for small batches or high precision requirements; roll forming has high efficiency and is suitable for mass production.
[0043] The inner surface of the inner tensile armor layer is machined with a groove array B that matches the discrete tooth array on the outer surface of the strip-shaped substrate. The groove depth of the groove array B is 0.2 to 2.5 mm and does not exceed 15% of the radial thickness of the steel wire in the inner tensile armor layer. Specifically, the inner surface of the carbon steel flat wire is first machined to form a groove structure that matches the discrete tooth array on the inner surface of the carbon steel flat wire; then, the carbon steel flat wire is wound around the outer surface of the prefabricated limited-slip interlocking strip at a winding angle of +30° to +35° to form the inner tensile armor layer. The groove structure forms the groove array B on the inner surface of the inner tensile armor layer.
[0044] The prefabricated anti-slip interlocking strip is spirally wrapped around the outer surface of the pressure-resistant armor layer. Discrete protrusions on the inner side are embedded in groove array A, and discrete protrusions on the outer side are embedded in groove array B. The spiral winding angle of the prefabricated anti-slip interlocking strip is 5°–15°, preferably 8°–12°. A gap of 0.5–3 mm is reserved between adjacent turns during spiral winding. The width of the gap is smaller than the spacing of the discrete protrusions in the width direction of the strip matrix. The gap is filled with thermoplastic elastomer (TPE) or silicone rubber. The filling material is used to form a secondary buffer and seal, preventing seawater or media from intruding into the interface, while also preventing the strip itself from becoming a bottleneck in the anti-slip process.
[0045] The gap width between adjacent turns is smaller than the spacing between adjacent discrete teeth in the same turn in the width direction of the strip matrix, thereby ensuring that the limited slip function is provided by the meshing of the teeth and the groove, rather than by the rigid constraint formed by the overlap between strip turns.
[0046] It should be noted that the groove array B is only formed on the inner surface of the carbon steel flat wire (i.e., the side facing the prefabricated anti-slip interlocking strip), and does not affect the tensile strength of the outer surface of the wire. The groove depth does not exceed 15% of the radial thickness of the wire, and has a limited weakening effect on the main load-bearing section of the wire, and will not significantly affect the axial load-bearing capacity of the inner tensile armor layer.
[0047] IV. Tiered Response Slip Limiting Mechanism This invention achieves a graded response limiting slip mechanism that "does not interfere during normal sliding and only interferes during abnormal sliding" by coordinating the circumferential initial clearance and the radial initial clearance.
[0048] The initial circumferential clearance is the tangential gap between the side of the protruding tooth and the sidewall of the groove along the pipe axis. The pipe axis direction refers to the direction of relative tangential displacement between the compression-resistant armor layer and the inner tensile armor layer when the pipe body is subjected to axial tension, compression, or bending. Since the winding angles of the compression-resistant armor layer (82°~88°), the prefabricated limited-slip interlocking belt (5°~15°), and the inner tensile armor layer (+30°~+35°) are all different, and the differences in the three helix angles are significant, the initial circumferential clearance is defined with the pipe axis as a unified reference system. Specifically, the initial circumferential clearance is the distance between the side of the protruding tooth and the sidewall of the groove measured tangentially along the pipe axis within the pipe body cross-section (the plane perpendicular to the pipe axis). Because the protruding tooth and the sidewall of the groove are parallel, the initial circumferential clearance is uniform along the pipe axis throughout the entire mating section between the protruding tooth and the groove. The initial circumferential clearance is 0.05~0.2mm.
[0049] The initial radial clearance is the gap between the top of the tooth and the bottom of the groove along the pipe diameter (the top of the tooth refers to the top of the tooth body, excluding the biomimetic protrusions on the tooth tip surface). The initial radial clearance is 0.1–0.5 mm.
[0050] During normal bending of the tube, relative slippage occurs between the compressive armor layer and the inner tensile armor layer. When the relative slippage is less than or equal to the initial circumferential gap, the discrete protrusions can slide freely within the groove, and the tube maintains the bending flexibility expected of an unbonded flexible tube. When the relative slippage exceeds the initial circumferential gap, the sides of the discrete protrusions abut against the sidewalls of the groove, limiting further slippage. At this point, the discrete protrusions and the strip-shaped matrix undergo elastic deformation or limited plastic deformation, dissipating energy and suppressing fretting wear and impact.
[0051] In addition, the interlocking of the double-sided protrusions and grooves forms a circumferential constraint at the interface between the compressive armor layer and the inner tensile armor layer, which inhibits the radial buckling of the tensile armor wire and the expansion of birdcage instability.
[0052] In contrast, if the prefabricated anti-slip interlocking strip is removed and a steel rigid interlocking strip (zero-gap fit) is used, there is no relative slippage between layers, the bending stiffness of the tube increases, the flexibility decreases, and the fatigue life is reduced. If a fully anchored biomimetic micro-anchoring interlayer is set between the two metal layers, quantitative gap control cannot be achieved, and there is no clear threshold response for interlayer slippage. The prefabricated anti-slip interlocking strip of this invention achieves selective anti-slip by pre-setting a dual gap threshold, while ensuring bending flexibility, thus taking into account both the requirements of maintaining flexibility and limiting interlayer slippage.
[0053] V. Definition and Calculation of Embedding Rate During the fabrication process, the winding tension is controlled to ensure that the embedding rate of discrete protrusions into the corresponding grooves is not less than 90%. The embedding rate is defined as the percentage of the total number of protrusions on the corresponding side of each turn of the prefabricated limited-slip interlocking belt that are actually embedded in the corresponding groove, with an initial circumferential gap of 0.05–0.2 mm and an initial radial gap of 0.1–0.5 mm. The embedding rates for the inner and outer sides are calculated in the same manner.
[0054] Specifically, the embedding rate is calculated as follows: For each turn of the prefabricated limited-slip interlocking belt, the total number of protrusions on the inner and outer sides of the turn is counted. Then, it is checked whether each protrusion is actually embedded in the corresponding groove array A or groove array B, and whether the initial circumferential gap between the protrusion and the corresponding groove is within the range of 0.05-0.2 mm and the initial radial gap is within the range of 0.1-0.5 mm. The number of protrusions on the same side that simultaneously meet the above conditions is divided by the total number of protrusions on that side in the turn, which is the embedding rate of that side of the turn. For example, in a turn of the prefabricated limited-slip interlocking belt, the inner side contains 200 protrusions, of which 185 protrusions are actually embedded in groove array A, and the initial circumferential gap between them and groove array A is within the range of 0.05-0.2 mm and the initial radial gap is within the range of 0.1-0.5 mm. Then, the embedding rate of the inner side of the turn is 185 / 200 = 92.5%; the outer side is calculated in the same way. The embedding rate was calculated separately for the inner and outer surfaces, and both were not less than 90%.
[0055] An embedding rate of not less than 90% ensures that the anti-slip function is evenly distributed in the circumferential and axial directions of the tube, which helps to avoid local stress concentration and thus improve the fatigue life of the tube.
[0056] VI. Preparation Method The present invention also provides a method for preparing the above-mentioned multilayer composite pipe, comprising the following steps: S1: Spiral winding of S-shaped interlocking stainless steel strips onto the core mold to form the skeleton layer.
[0057] A rotatable mandrel is provided, and S-shaped interlocking stainless steel strip is wound spirally around the surface of the mandrel. Adjacent turns are interlocked by an S-shaped cross section to form a skeleton layer. The winding angle can be determined according to the pipe diameter and design requirements.
[0058] S2: Extruding a polymer liner onto the skeleton layer.
[0059] A polymer inner liner with a thickness of 6 to 15 mm is formed by extruding thermoplastic polymers such as PVDF or PA12 on the outside of the skeleton layer through an extruder at an extrusion temperature of 220 to 250°C.
[0060] S3: A Z-shaped interlocking carbon steel strip is wound around the polymer liner at a winding angle of 82° to 88° to form a pressure-resistant armor layer.
[0061] Z-shaped interlocking carbon steel strips are spirally wound around the outside of the polymer inner liner at a winding angle of 82° to 88°, and adjacent steel strips are interlocked through the Z-shaped cross section to form a pressure-resistant armor layer.
[0062] S4: Groove array A is machined on the outer surface of the pressure-resistant armor layer.
[0063] The groove array A is machined on the outer surface of the pressure-resistant armor layer by laser etching or roll forming. During machining, the groove depth is controlled to be 0.2–2.5 mm and does not exceed 15% of the thickness of the steel strip constituting the pressure-resistant armor layer. The pitch and shape of the grooves are matched with the discrete tooth array on the inner side of the prefabricated limited-slip interlocking belt.
[0064] S5: Prefabricated limited-slip interlock belt.
[0065] Extruded continuous thermoplastic polyurethane or polyetheretherketone (PEEK) tapes are produced. During extrusion, a hybrid reinforcing phase of chopped carbon fibers and aramid fibers is incorporated into the tape matrix at a mass ratio of (1–3):1, with fiber lengths ranging from 50 to 500 μm. Discrete tooth arrays are formed on both the inner and outer surfaces of the tape. When forming the discrete tooth arrays, the tooth tip surfaces are shaped into columnar or branched forms with a protrusion height of 50–500 μm, a root diameter of 5–100 μm, and an areal density of 10. 4 ~10 6 pcs / cm 2 The biomimetic protrusions are designed, and the spacing between adjacent biomimetic protrusions is controlled between 10 and 200 μm.
[0066] S6: Wrap prefabricated limited-slip interlocking belt.
[0067] The prefabricated limited-slip interlocking tape obtained in step S5 is wound around the outer surface of the compression-resistant armor layer at a helical angle of 5° to 15°, so that the discrete protrusions on the inner side of the tape are embedded in the groove array A. By controlling the processing dimensions of the discrete protrusions and the groove array A, an initial circumferential gap of 0.05 to 0.2 mm and a radial initial gap of 0.1 to 0.5 mm are formed after the discrete protrusions are embedded in the groove array A. During winding, a gap of 0.5 to 3 mm is reserved between adjacent turns, and thermoplastic elastomer or silicone rubber is filled in the gap. The winding tension is controlled so that the embedding rate of the discrete protrusions on the inner side into the groove array A is not less than 90%.
[0068] S7: Molded internal tensile armor layer.
[0069] The inner surface of the carbon steel flat wire is machined to form a groove structure that matches the discrete tooth array. The machining method can be laser etching or roll forming. During machining, the groove depth is controlled to be 0.2–2.5 mm and does not exceed 15% of the radial thickness of the carbon steel flat wire. Then, the carbon steel flat wire is wound around the outer surface of the prefabricated anti-slip interlocking strip obtained in step S6 at a winding angle of +30°–+35° to form an inner tensile armor layer. The groove structure forms a groove array B on the inner surface of the inner tensile armor layer. During the winding process, the discrete teeth on the outer side of the strip are embedded into the groove array B. By controlling the machining dimensions of the discrete teeth and the groove array B, an initial circumferential gap of 0.05–0.2 mm and a radial initial gap of 0.1–0.5 mm are formed after the discrete teeth are embedded into the groove array B. By controlling the winding tension, the embedding rate of the discrete teeth on the outer side into the groove array B is not less than 90%.
[0070] S8: Molded external tensile armor layer.
[0071] Carbon steel flat wire is wound in the opposite direction at a winding angle of -35° to -30° to form an outer tensile armor layer, which forms a torque balance with the inner tensile armor layer.
[0072] S9: Wrapped anti-buckling layer.
[0073] Aramid or glass fiber reinforced polymer tape is wrapped around the outside of the outer tensile armor layer to form a buckling-resistant layer.
[0074] S10: Extruded outer sheath, assembly end connector.
[0075] The outermost layer is formed by extruding polymers such as HDPE, PA, or PVDF through an extruder.
[0076] VII. Specific Structural Examples and Parameter Verification Example 1 A specific structural example of the pipe of the present invention is as follows: A multi-layer composite pipe for subsea oil and gas transportation, the structure of which, from the inside out, consists of: Skeleton layer: S-type interlocking 316L stainless steel strip; Polymer inner liner: PVDF; Compression-resistant armor layer: Z-shaped interlocking carbon steel strip, steel strip thickness 9mm; Prefabricated limited-slip interlocking belt: TPU matrix, 150mm wide and 2.5mm thick; short-cut carbon fiber and aramid fiber hybrid reinforcement phase are incorporated into the belt matrix at a mass ratio of 2:1, with a fiber length of 200μm; trapezoidal discrete protrusions (tooth height 1.0mm, pitch 2mm, tooth top width 1.2mm, tooth bottom width 1.6mm) are provided on both the inner and outer surfaces, and columnar biomimetic protrusions (height 200μm, root diameter 50μm) are provided on the tooth top surface; the spiral winding angle is 10°; there is a 0.1mm circumferential initial gap and a 0.3mm radial initial gap between the discrete protrusions and the groove array A / B; Trench array A / B: The trench depth is 1.3mm, the top width is 1.8mm, and the bottom width is 1.28mm; wherein, the top width is the width at the opening of the trench (i.e., the side facing the prefabricated limited slip interlocking strip), and the bottom width is the width at the deepest point of the trench. Inner tensile armor layer: carbon steel flat wire; External tensile armor layer: carbon steel flat wire; Anti-buckling layer: Aramid-reinforced polymer tape; Outer sheath: HDPE.
[0077] Parameter verification To verify the critical effects of the aforementioned initial circumferential and radial clearance ranges, a finite element method (FEM) simulation analysis was employed. A simulation model was established based on the structural parameters of Example 1, with boundary conditions and material parameters set according to ISO 13628 standard. Simulation conditions were: temperature 25℃, artificial seawater as the medium, loading frequency 0.5Hz, slip amplitude ±2mm, bending radius 5 times the pipe diameter, and 10 cycles. 4 Second, axial tensile load of 50% of the tube's yield strength.
[0078] Using the initial circumferential clearance of 0.1 mm in Example 1 as a benchmark, five sets of clearances (0.03 mm, 0.05 mm, 0.1 mm, 0.2 mm, and 0.3 mm) within the range of 0.03–0.3 mm were selected for simulation comparison (where 0.1 mm is the benchmark value of Example 1). The results show that when the initial circumferential clearance is less than 0.05 mm, the protruding teeth frequently contact the sidewall of the groove, resulting in false positioning and a decrease in positioning accuracy; when the initial circumferential clearance is greater than 0.2 mm, the positioning function lags behind, and the interlayer slippage increases; within the range of 0.05–0.2 mm, the bending flexibility retention rate is ≥96%, the positioning accuracy exceedance rate is ≤15%, and the overall performance is optimal.
[0079] Using the initial radial clearance of 0.3 mm in Example 1 as a baseline, five sets of clearances (0.05 mm, 0.1 mm, 0.3 mm, 0.5 mm, and 0.6 mm) were selected within the range of 0.05–0.6 mm for simulation comparison (where 0.3 mm is the baseline value of Example 1). The results show that when the initial radial clearance is less than 0.1 mm, the top of the protrusion frequently contacts the bottom of the groove, and the bionic protrusion experiences interference compression with the bottom of the groove, affecting the floating of the protrusion within the groove and the integrity of the bionic protrusion; when the initial radial clearance is greater than 0.5 mm, the distance between the top of the protrusion and the bottom of the groove is too large, resulting in a delayed limiting response; the overall performance is optimal within the range of 0.1–0.5 mm.
[0080] The simulation results above verify that the circumferential initial gap (0.05-0.2 mm) and radial initial gap (0.1-0.5 mm) ranges defined by the present invention have a critical effect. Gap values outside this range cannot simultaneously take into account bending flexibility and positioning accuracy.
[0081] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Various changes made within the scope of knowledge possessed by those skilled in the art without departing from the concept of the present invention still fall within the scope of protection of the present invention.
Claims
1. A multi-layer composite pipe for subsea oil and gas transportation, comprising, from the inside out, a skeleton layer, a polymer inner lining layer, a pressure-resistant armor layer, an inner tensile armor layer, an outer tensile armor layer, a buckling-resistant layer, and an outer sheath, characterized in that: A prefabricated slip-limiting interlocking strip is provided between the compressive armor layer and the inner tensile armor layer; The prefabricated limited-slip interlocking strip includes a strip-shaped base, and discrete tooth arrays are provided on both the inner and outer sides of the strip-shaped base. The outer surface of the compressive armor layer is machined with a groove array A that matches the discrete tooth array on the inner side of the strip-shaped substrate, and the inner surface of the inner tensile armor layer is machined with a groove array B that matches the discrete tooth array on the outer side of the strip-shaped substrate. The prefabricated limited-slip interlocking strip is spirally wrapped around the outer surface of the pressure-resistant armor layer. The discrete protrusions on the inner side of the strip-shaped substrate are embedded in the groove array A, and the discrete protrusions on the outer side of the strip-shaped substrate are embedded in the groove array B. The discrete protrusions have an initial circumferential gap of 0.05–0.2 mm between their sides and the corresponding groove sidewalls in the direction around the tube axis, and an initial radial gap of 0.1–0.5 mm between their tops and the bottoms of the corresponding grooves. When the relative slippage between layers is less than or equal to the initial circumferential gap, the discrete protrusions can slide freely within the corresponding grooves to maintain the flexibility of the tube body. When the relative slippage between layers is greater than the initial circumferential gap, the sides of the discrete protrusions abut against the sidewalls of the corresponding grooves to limit further slippage.
2. The multi-layer composite pipe for subsea oil and gas transportation according to claim 1, characterized in that, The discrete protrusions have a tooth height of 0.2–2 mm, and the pitch between adjacent discrete protrusions in the length direction of the strip-shaped substrate is 0.5–5 mm. The tooth shape of the discrete protrusions is one or a combination of trapezoidal, triangular, and arc-shaped, and the tooth tip width is 1 / 3 to 2 / 3 of the pitch. The discrete protrusion array on the inner side of the strip-shaped substrate corresponds one-to-one with the discrete protrusion array on the outer side in the thickness direction of the strip-shaped substrate.
3. The multi-layer composite pipe for subsea oil and gas transportation according to claim 1, characterized in that, The discrete convex teeth have biomimetic protrusions on their tip surfaces. These protrusions are columnar or branched, with a height of 50–500 μm, a root diameter of 5–100 μm, and a surface density of 10. 4 ~10 6 pcs / cm 2 The spacing between adjacent biomimetic protrusions is 10–200 μm; the biomimetic protrusions provide frictional damping when the relative slippage between layers is less than or equal to the initial circumferential gap, and the discrete protrusions provide rigid restraint when the relative slippage between layers is greater than the initial circumferential gap.
4. The multi-layer composite pipe for subsea oil and gas transportation according to claim 1, characterized in that, The strip matrix is made of thermoplastic polyurethane or polyetheretherketone, with a width of 50-300 mm and a thickness of 1-5 mm. The strip matrix contains a hybrid reinforcing phase of chopped carbon fibers and aramid fibers, with a mass ratio of carbon fibers to aramid fibers of (1-3):1 and a fiber length of 50-500 μm.
5. The multi-layer composite pipe for subsea oil and gas transportation according to claim 1, characterized in that, The groove depth of groove array A is 0.2–2.5 mm and does not exceed 15% of the thickness of the steel strip constituting the compressive armor layer; the groove depth of groove array B is 0.2–2.5 mm and does not exceed 15% of the radial thickness of the steel wire in the inner tensile armor layer; the spiral winding angle of the prefabricated limited-slip interlocking strip is 5°–15°; when the prefabricated limited-slip interlocking strip is spirally wound, a gap of 0.5–3 mm is reserved between adjacent turns, the width of the gap is smaller than the spacing of the discrete protrusions in the width direction of the strip matrix, and the gap is filled with thermoplastic elastomer or silicone rubber.
6. The multi-layer composite pipe for subsea oil and gas transportation according to claim 1, characterized in that, The skeleton layer is an S-shaped interlocking stainless steel strip; the polymer inner liner is made of PVDF or PA12 with a thickness of 6-15mm; the compression armor layer is a Z-shaped interlocking carbon steel strip; both the inner and outer tensile armor layers are made of carbon steel flat wire; the buckling-resistant layer is an aramid or glass fiber reinforced polymer tape; the outer sheath is made of HDPE, PA, or PVDF; the winding angle of the compression armor layer is 82°-88°, the winding angle of the inner tensile armor layer is +30°-+35°, and the winding angle of the outer tensile armor layer is -35°--30°.
7. A method for preparing a multi-layer composite pipe for subsea oil and gas transportation according to any one of claims 1 to 6, characterized in that, The steps are as follows: S1: Spiral winding of S-shaped interlocking stainless steel strip on the core mold to form the skeleton layer; S2: Extruding a polymer liner layer onto the skeleton layer; S3: Wrap a Z-shaped interlocking carbon steel strip around the polymer liner at a winding angle of 82° to 88° to form a pressure-resistant armor layer; S4: Process groove array A on the outer surface of the pressure-resistant armor layer; S5: Prefabricated limited-slip interlocking belt: Extruded thermoplastic polyurethane or polyetheretherketone continuous belt, with discrete tooth arrays formed on the inner and outer sides of the belt respectively. S6: The prefabricated limited-slip interlocking strip obtained in step S5 is wound around the outer surface of the pressure-resistant armor layer with a helical angle of 5° to 15°, so that the discrete protrusions on the inner side of the strip are embedded in the groove array A. By controlling the processing size of the discrete protrusions and the processing size of the groove array A, the discrete protrusions are embedded in the groove array A to form an initial circumferential gap of 0.05 to 0.2 mm and an initial radial gap of 0.1 to 0.5 mm. S7: The inner surface of the carbon steel flat wire is processed to form a groove structure that matches the discrete tooth array on the inner surface of the carbon steel flat wire; then the carbon steel flat wire is wound around the outer surface of the prefabricated limited slip interlocking strip obtained in step S6 at a winding angle of +30° to +35° to form an inner tensile armor layer. The groove structure forms a groove array B on the inner surface of the inner tensile armor layer. During the winding process, the discrete teeth on the outer side of the strip are embedded in the groove array B. By controlling the processing size of the discrete teeth and the processing size of the groove array B, the discrete teeth are embedded in the groove array B to form an initial circumferential gap of 0.05 to 0.2 mm and an initial radial gap of 0.1 to 0.5 mm. S8: The outer tensile armor layer is formed by reverse winding at a winding angle of -35° to -30°; S9: Wrapped anti-buckling layer; S10: Extruded outer sheath, assembly end connector; In steps S6 and S7, the embedding rate of the discrete protrusions into the corresponding grooves is not less than 90% by controlling the winding tension. The embedding rate is defined as the percentage of the number of protrusions that are actually embedded in the corresponding grooves in each turn of the prefabricated limited-slip interlocking belt, with an initial circumferential gap of 0.05 to 0.2 mm and an initial radial gap of 0.1 to 0.5 mm between them and the corresponding grooves, relative to the total number of protrusions on the corresponding side of the turn. The corresponding side is the inner side in step S6 and the outer side in step S7.
8. The preparation method according to claim 7, characterized in that, In step S5, during the extrusion of the continuous strip, a hybrid reinforcing phase of chopped carbon fibers and aramid fibers is incorporated into the matrix of the strip at a mass ratio of (1-3):1, with a fiber length of 50-500 μm. During the forming of the discrete tooth array, the tooth tip surface is formed into a columnar or branched shape, with a protrusion height of 50-500 μm, a root diameter of 5-100 μm, and an areal density of 10. 4 ~10 6 pcs / cm 2 The biomimetic protrusions are made, and the spacing between adjacent biomimetic protrusions is controlled at 10-200μm; in step S6, during winding, a gap of 0.5-3mm is reserved between adjacent turns, and thermoplastic elastomer or silicone rubber is filled in the gap.
9. The preparation method according to claim 7, characterized in that, In step S4, the groove array A is processed by laser etching or roll forming. During processing, the groove depth is controlled to be 0.2-2.5 mm and does not exceed 15% of the thickness of the Z-shaped interlocking carbon steel strip. In step S7, the groove structure is processed on the inner surface of the carbon steel flat wire by laser etching or roll forming. During processing, the groove depth is controlled to be 0.2-2.5 mm and does not exceed 15% of the radial thickness of the carbon steel flat wire.
Citation Information
Patent Citations
An X-shaped profile and pressure-resistant armor layer for marine composite hoses
CN113531235B
Bionic micro-anchoring intercalation, composite pipe and preparation method of composite pipe
CN122429299A