By performing carbonitriding surface strengthening treatment on the valve seat and valve core of the steam trap, the problem of sealing failure of the steam trap in high-temperature condensate medium was solved, resulting in extended service life, reduced cost, and improved sealing reliability.
Patent Information
- Application Number
- CN202611060652.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-16
- Publication Date
- 2026-11-24
AI Technical Summary
Existing steam traps suffer from sealing failure due to cavitation, erosion, and corrosion in high-temperature condensate media, resulting in short service life. Current technical solutions are costly and complex.
The carbonitriding surface strengthening process is used to carbonitride the sealing surfaces of the valve seat and valve core to form a high-hardness surface strengthening film. Combined with a low-carbon or low-alloy steel substrate and a filter assembly, the sealing surface is protected. The preparation process includes pretreatment, gas carbonitriding, quenching, cleaning, and tempering.
It significantly extends the service life of steam traps, improves sealing reliability, reduces manufacturing costs, and effectively filters impurities, avoiding additional leakage points.
Smart Images

Figure CN123154239A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of steam trap technology, and in particular to a steam trap with carbonitriding surface strengthening treatment and its manufacturing process. Background Technology
[0002] Steam traps are crucial energy-saving devices in steam pipeline systems. Their basic function is to promptly discharge condensate, air, and carbon dioxide from the steam system while automatically preventing steam leakage to the greatest extent possible. However, the operating conditions of steam traps are extremely harsh: the valve interior contains a mixture of condensate and steam at high temperatures, large pressure differentials, and high flow rates. Condensate is prone to flash evaporation and cavitation after pressure reduction. Under these conditions, core sealing components such as the valve core and seat are subjected to a combination of cavitation, erosion, and corrosion over a long period. The sealing surfaces are easily impacted, forming honeycomb-like pores, leading to valve leakage and a significantly shortened service life.
[0003] Currently, the industry mostly uses solid stainless steel to manufacture steam traps to address corrosion issues. However, simply upgrading the material is insufficient to solve the problems of high-frequency wear and cavitation damage on the sealing surface. Some steam traps employ localized reinforcement methods such as hard alloy overlay welding, but these methods have drawbacks such as complex processes, high costs, and weak areas at the interface between dissimilar materials.
[0004] Carbonitriding, as a mature chemical heat treatment method, can form a high-hardness carbonitrided layer on the surface of a workpiece, combining the high hardness of a carburized layer with the corrosion resistance and anti-adhesion advantages of a nitrided layer. It has been successfully applied in wear-resistant parts such as automotive gears and valve sleeves. However, there are currently no reports of applying carbonitriding technology to the core components of steam traps.
[0005] Content of the invention
[0006] (1) Technical problems to be solved
[0007] The purpose of this invention is to address the challenges posed by existing steam traps, which operate in harsh environments with a mixture of condensate and steam at high temperatures, large pressure differentials, and high flow rates. These environments cause flashing and cavitation phenomena in the condensate after pressure reduction. The invention aims to solve the problems of sealing failure and leakage in the valve core, seat, and other core components of existing steam traps due to cavitation, erosion, and corrosion in high-temperature condensate media. Existing processing techniques for these components are costly and complex. Therefore, this invention proposes a carbonitriding surface-strengthened steam trap and its manufacturing process, successfully solving the problems of high processing costs and cumbersome procedures, and extending the service life of the steam trap.
[0008] (2) Technical solution
[0009] To solve the above-mentioned technical problems, the present invention discloses a steam trap with carbonitriding surface strengthening treatment, including a valve body, a valve seat, a valve core and a valve cover. The valve seat is fixed at the inner flow channel of the valve body. The valve core is provided above the valve seat. The valve cover is installed at the top opening of the valve body. An automatic venting valve is installed on the valve cover. A filter assembly is installed inside the inlet flow channel of the valve body.
[0010] The sealing surfaces of at least one of the valve seat and the valve core are treated with carbonitriding to form a surface-strengthening film.
[0011] Preferably, the valve cover is fastened to the top flange surface of the valve body by bolts and nuts, and a gasket is also sandwiched between the valve cover and the valve body;
[0012] Both the medium inlet and medium outlet ends of the valve body are connected to welded flanges.
[0013] Preferably, the filter assembly is a detachable filter screen located in the inlet flow channel of the valve body, used to intercept impurities such as rust and welding slag in the pipeline, and to prevent impurities from scratching the sealing working surface after carbonitriding treatment. The inner side of the valve body is provided with a filter screen mounting groove for installing the filter screen.
[0014] Preferably, an adjusting screw plug is installed on the valve seat, and a screw plug is also installed on the valve seat next to the adjusting screw plug.
[0015] Preferably, the valve core is a float-type valve core; the base material of the valve core and valve seat is low-carbon or low-alloy steel.
[0016] Preferably, the sealing working surface of the valve seat is treated with carbonitriding to form a surface-strengthening film, or;
[0017] The sealing working surface of the valve core is treated with carbonitriding to form a surface-strengthening film, or;
[0018] Both the sealing working surface of the valve seat and the sealing working surface of the valve core are treated with carbonitriding to form a surface strengthening film.
[0019] Preferably, the sealing pair between the valve seat and the valve core is a conical surface fit, the sealing working surface of the valve core is a conical surface, and the sealing working surface of the valve seat is a matching conical hole.
[0020] This invention also provides a process for preparing the above-mentioned carbonitriding surface-strengthened steam trap, comprising the following steps:
[0021] I. Preprocessing:
[0022] The valve seat blank and / or valve core blank are subjected to stress-relief annealing, heated in the furnace to 540~560℃, held for 120~180 minutes, and then air-cooled to room temperature after being taken out of the furnace.
[0023] II. Gas carbonitriding:
[0024] The pretreated workpiece is placed in a gas carburizing and nitriding furnace. The furnace temperature is raised to 840~880℃ and held for 90~180 minutes. Carburizing medium and ammonia are introduced into the furnace. The carbon potential is controlled at 0.8%~0.9% and the ammonia gas fraction is controlled at 5%~15%. After carbonitriding treatment, the sealing working surfaces of the valve seat and / or valve core form a high-hardness, wear-resistant sealing pair.
[0025] III. Quenching treatment:
[0026] After the gas carbonitriding operation is completed, the furnace is cooled to 820~850℃, and the workpiece is immersed in quenching oil for rapid cooling. The quenching oil temperature is controlled at 40~80℃, and the cooling time is 15~30 minutes.
[0027] IV. Cleaning and Drying:
[0028] After quenching, the workpiece is soaked and cleaned with a metal cleaning agent solution, then sprayed with rust-preventive water and drained.
[0029] V. Low-temperature tempering treatment:
[0030] After cleaning and drying, place the workpiece in a tempering furnace and keep it at 160~280℃ for 120~180 minutes, then air cool to room temperature.
[0031] VI. Assembly:
[0032] Assemble the valve seat and valve core processed in step five with other purchased components to form a steam trap.
[0033] Preferably, the gas carbonitriding temperature in step two is in the range of 840~880℃, which can ensure sufficient carbon and nitrogen atom diffusion rate and avoid excessive austenite grain growth; a carbon potential range of 0.8%~0.9% can obtain a suitable carburized layer depth and surface carbon concentration; the ammonia gas integral number is controlled at 5%~15% to appropriately introduce nitrogen elements on the basis of carburizing, which can improve surface hardness and anti-adhesion performance while controlling the brittleness of the carburized layer.
[0034] Preferably, in step two, the gas carbonitriding temperature is set to 855~865℃, the holding time is 90 minutes, the carbon potential is controlled at 0.85%, and the ammonia gas integral is controlled at 8%~12%.
[0035] Preferably, after the gas carbonitriding treatment in step two is completed, the surface hardness of the sealing working surface of the valve seat and / or valve core reaches 58~64HRC, the effective hardened layer depth is 0.2~0.8mm, and the residual compressive stress in the carbonitrided layer improves the fatigue strength of the workpiece.
[0036] Preferably, the base material of the valve seat and valve core is 20CrMnTi steel or 20Cr steel, because low-carbon or low-alloy steel has good hardenability, and carbon and nitrogen atoms can easily diffuse, so as to obtain an ideal diffusion layer depth; at the same time, the cost of this type of steel is much lower than that of stainless steel, thus taking into account economic efficiency.
[0037] Preferably, the valve body is cast from ductile iron QT600-3, and the inner wall of the valve body flow channel is coated with a corrosion-resistant protective coating. Ductile iron has excellent casting performance and sufficient strength, and the inner wall protective coating can control manufacturing costs while ensuring the overall structural reliability.
[0038] Preferably, the tempering temperature of 160~280℃ in step five can eliminate quenching stress while maintaining high surface hardness.
[0039] Preferably, the tempering temperature in step five is set between 250 and 270°C to obtain the best match between hardness and toughness.
[0040] Preferably, the sealing pair between the valve seat and the valve core is designed as a conical mating structure, with the valve core sealing surface being a conical surface and the valve seat sealing surface being a matching conical hole. The two are then combined through carbonitriding to form a high-hardness, wear-resistant sealing pair.
[0041] Preferably, the valve body is equipped with an opening and closing drive assembly, which is a thermostatic drive mechanism including a bimetallic strip or a thermally sensitive telescopic element, and automatically controls the opening and closing of the valve core according to the change of condensate temperature.
[0042] (3) Beneficial effects
[0043] Compared with the prior art, the present invention has the following advantages:
[0044] This invention can significantly extend the service life of core components: the sealing surfaces of valve seats and valve cores are strengthened by carbonitriding treatment, resulting in a significant increase in surface hardness and enhanced resistance to cavitation and erosion. The dense nitride layer in the co-diffusion layer also improves corrosion resistance and effectively resists the weak acid corrosion of high-temperature condensate.
[0045] This invention can effectively improve the reliability of the seal: the sealing working surfaces of the valve seat and valve core treated by carbonitriding form a high-hardness sealing pair, which improves the holding force of the valve core when it is closed, the sealing working surface is not easily deformed and worn, and the steam leakage rate can be controlled at an extremely low level.
[0046] This invention can effectively reduce manufacturing costs: the valve seat and valve core adopt a low carbon or low alloy steel matrix combined with carbonitriding surface strengthening treatment, and the performance is comparable to or even surpasses the overall stainless steel or hard alloy welding solution, while the material cost and processing cost are significantly reduced.
[0047] This invention can effectively filter impurities and extend service life: by setting up a filter component, the carbonitriding sealing surface is protected from the source, avoiding the pipeline complexity and additional leakage points caused by adding an external filter. Attached Figure Description
[0048] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0049] Figure 1 This is a cross-sectional view of the structure of a steam trap valve with carbonitriding surface strengthening treatment according to the present invention.
[0050] In the attached diagram, the components represented by each number are as follows:
[0051] 1 - Valve seat, 2 - Valve core, 3 - Automatic vent valve, 4 - Valve cover, 5 - Filter assembly, 6 - Welded flange, 7 - Valve body, 8 - Adjusting screw plug, 9 - Screw plug. Detailed Implementation
[0052] The present invention will be described in detail below using different manufacturing processes. The examples listed will enable those skilled in the art to better understand the present invention, but will not limit the present invention in any way. For example, the present invention can be extended to the production of friction plates or similar products in other fields.
[0053] Example 1:
[0054] Please see Figure 1 This invention provides a steam trap with carbonitriding surface strengthening treatment, including a valve body 7, a valve seat 1, a valve core 2, and a valve cover 4. The valve seat 1 is fixed at the inner flow channel opening of the valve body 7. The valve core 2 is disposed above the valve seat 1. The valve core 2 is a float valve core. The valve cover 4 is installed at the top opening of the valve body 7. An automatic venting valve 3 is installed on the valve cover 4. A filter assembly 5 is installed inside the inlet flow channel of the valve body 7. The filter assembly 5 is a detachable filter screen opened in the inlet flow channel of the valve body 7. The inner side of the valve body 7 is provided with a filter screen mounting groove for installing the filter screen.
[0055] At least one of the sealing surfaces of the valve seat 1 and the valve core 2 is subjected to carbonitriding treatment to form a surface strengthening film. Specifically, it can be divided into the following three types: ① The sealing surface of the valve seat 1 is subjected to carbonitriding treatment to form a surface strengthening film; ② The sealing surface of the valve core 2 is subjected to carbonitriding treatment to form a surface strengthening film; ③ Both the sealing surfaces of the valve seat 1 and the valve core 2 are subjected to carbonitriding treatment to form a surface strengthening film.
[0056] The valve cover 4 is fastened to the top flange surface of the valve body 7 by bolts and nuts, and a gasket is also sandwiched between the valve cover 4 and the valve body 7; a welded flange 6 is connected to both the medium inlet end and the medium outlet end of the valve body 7; an adjusting screw plug 8 is installed on the valve seat 1, and a screw plug 9 is also installed on the valve seat 1 next to the adjusting screw plug 8.
[0057] To reduce production costs, it is advisable to improve hardenability, and the base material of the valve core 2 and valve seat 1 is low-carbon or low-alloy steel.
[0058] To achieve an effective sealing fit, the sealing pair between the valve seat 1 and the valve core 2 is a conical surface fit, the sealing working surface of the valve core 2 is a conical surface, and the sealing working surface of the valve seat 1 is a matching conical hole.
[0059] Example 2:
[0060] The fabrication process of a steam trap with carbonitriding surface strengthening treatment includes the following steps:
[0061] I. Preprocessing:
[0062] The valve seat blank and / or valve core blank are subjected to stress-relief annealing, heated in the furnace to 540~560℃, held for 120~180 minutes, and then air-cooled to room temperature after being taken out of the furnace.
[0063] II. Gas carbonitriding:
[0064] The pretreated workpiece is placed in a gas carburizing and nitriding furnace. The furnace temperature is raised to 855℃ and held for 90 minutes. Carburizing medium and ammonia are introduced into the furnace. The carbon potential is controlled at 0.85% and the ammonia gas integral is controlled at 8%. After carbonitriding treatment, the sealing working surfaces of the valve seat and / or valve core form a high-hardness and wear-resistant sealing pair.
[0065] III. Quenching treatment:
[0066] After the carbonitriding operation with gas is completed, the furnace temperature is lowered to 830°C, and the workpiece is immersed in quenching oil for rapid cooling. The quenching oil temperature is controlled at 60°C and the cooling time is 20 minutes.
[0067] IV. Cleaning and Drying:
[0068] After quenching, the workpiece is soaked and cleaned with a metal cleaning agent solution, then sprayed with rust-preventive water and drained.
[0069] V. Low-temperature tempering treatment:
[0070] After cleaning and drying, the workpiece is placed in a tempering furnace and kept at 250°C for 180 minutes, then air-cooled to room temperature.
[0071] VI. Assembly:
[0072] Assemble the valve seat and valve core processed in step five with other purchased components to form a steam trap.
[0073] After the gas carbonitriding treatment in step two is completed, the surface hardness of the sealing working surface of the valve seat and / or valve core reaches 60 HRC, and the effective hardened layer depth is 0.25 mm.
[0074] Example 3:
[0075] The fabrication process of a steam trap with carbonitriding surface strengthening treatment includes the following steps:
[0076] I. Preprocessing:
[0077] The valve seat blank and / or valve core blank are subjected to stress-relief annealing, heated in the furnace to 540~560℃, held for 120~180 minutes, and then air-cooled to room temperature after being taken out of the furnace.
[0078] II. Gas carbonitriding:
[0079] The pretreated workpiece is placed in a gas carburizing and nitriding furnace. The furnace temperature is raised to 865℃ and held for 120 minutes. Carburizing medium and ammonia are introduced into the furnace. The carbon potential is controlled at 0.88% and the ammonia gas integral is controlled at 12%. After carbonitriding treatment, the sealing working surfaces of the valve seat and / or valve core form a high-hardness and wear-resistant sealing pair.
[0080] III. Quenching treatment:
[0081] After the carbonitriding operation with gas is completed, the furnace temperature is lowered to 820°C, and the workpiece is immersed in quenching oil for rapid cooling. The quenching oil temperature is controlled at 80°C and the cooling time is 30 minutes.
[0082] IV. Cleaning and Drying:
[0083] After quenching, the workpiece is soaked and cleaned with a metal cleaning agent solution, then sprayed with rust-preventive water and drained.
[0084] V. Low-temperature tempering treatment:
[0085] After cleaning and drying, the workpiece is placed in a tempering furnace and kept at 270℃ for 150 minutes, then air-cooled to room temperature.
[0086] VI. Assembly:
[0087] Assemble the valve seat and valve core processed in step five with other purchased components to form a steam trap.
[0088] After the gas carbonitriding treatment in step two is completed, the surface hardness of the sealing working surface of the valve seat and / or valve core reaches 62 HRC, and the effective hardened layer depth is 0.5 mm.
[0089] Example 4:
[0090] The fabrication process of a steam trap with carbonitriding surface strengthening treatment includes the following steps:
[0091] I. Preprocessing:
[0092] The valve seat blank and / or valve core blank are subjected to stress-relief annealing, heated in the furnace to 540~560℃, held for 120~180 minutes, and then air-cooled to room temperature after being taken out of the furnace.
[0093] II. Gas carbonitriding:
[0094] The pretreated workpiece is placed in a gas carburizing and nitriding furnace. The furnace temperature is raised to 880℃ and held for 180 minutes. Carburizing medium and ammonia are introduced into the furnace. The carbon potential is controlled at 0.86% and the ammonia gas integral is controlled at 15%. After carbonitriding treatment, the sealing working surfaces of the valve seat and / or valve core form a high-hardness and wear-resistant sealing pair.
[0095] III. Quenching treatment:
[0096] After the carbonitriding operation with gas is completed, the furnace temperature is lowered to 840°C, and the workpiece is immersed in quenching oil for rapid cooling. The quenching oil temperature is controlled at 40°C and the cooling time is 18 minutes.
[0097] IV. Cleaning and Drying:
[0098] After quenching, the workpiece is soaked and cleaned with a metal cleaning agent solution, then sprayed with rust-preventive water and drained.
[0099] V. Low-temperature tempering treatment:
[0100] After cleaning and drying, place the workpiece in a tempering furnace and hold it at 160℃ for 120 minutes, then air cool it to room temperature.
[0101] VI. Assembly:
[0102] Assemble the valve seat and valve core processed in step five with other purchased components to form a steam trap.
[0103] After the gas carbonitriding treatment in step two is completed, the surface hardness of the sealing working surface of the valve seat and / or valve core reaches 59 HRC, and the effective hardened layer depth is 0.4 mm.
[0104] Example 5:
[0105] The fabrication process of a steam trap with carbonitriding surface strengthening treatment includes the following steps:
[0106] I. Preprocessing:
[0107] The valve seat blank and / or valve core blank are subjected to stress-relief annealing, heated in the furnace to 540~560℃, held for 120~180 minutes, and then air-cooled to room temperature after being taken out of the furnace.
[0108] II. Gas carbonitriding:
[0109] The pretreated workpiece is placed in a gas carburizing and nitriding furnace. The furnace temperature is raised to 840℃ and held for 150 minutes. Carburizing medium and ammonia are introduced into the furnace. The carbon potential is controlled at 0.9% and the ammonia gas integral is controlled at 13%. After carbonitriding treatment, the sealing working surfaces of the valve seat and / or valve core form a high-hardness and wear-resistant sealing pair.
[0110] III. Quenching treatment:
[0111] After the carbonitriding operation with gas is completed, the furnace temperature is lowered to 850°C, and the workpiece is immersed in quenching oil for rapid cooling. The quenching oil temperature is controlled at 70°C and the cooling time is 25 minutes.
[0112] IV. Cleaning and Drying:
[0113] After quenching, the workpiece is soaked and cleaned with a metal cleaning agent solution, then sprayed with rust-preventive water and drained.
[0114] V. Low-temperature tempering treatment:
[0115] After cleaning and drying, the workpiece is placed in a tempering furnace and kept at 280℃ for 145 minutes, then air-cooled to room temperature.
[0116] VI. Assembly:
[0117] Assemble the valve seat and valve core processed in step five with other purchased components to form a steam trap.
[0118] After the gas carbonitriding treatment in step two is completed, the surface hardness of the sealing working surface of the valve seat and / or valve core reaches 63 HRC, and the effective hardened layer depth is 0.55 m.
[0119] The data above show that the surface hardness of the treated sealing working surface can reach 59~63 HRC, and the effective hardened layer depth is 0.25~0.55 mm. This combination of parameters achieves better core toughness in exchange for lower hardness and a slightly shallower seepage layer, making it suitable for steam pipeline systems subjected to large impact loads.
[0120] In addition, a commercially available stainless steel valve seat and valve core steam trap was used as a comparative example. Under the same operating conditions as the embodiment in this solution, steam leakage occurred after 3 months of operation. Upon disassembly and inspection, obvious honeycomb-shaped cavitation pits were found on the valve core sealing surface, and the sealing performance had significantly decreased. However, the steam trap using this solution did not experience steam leakage after 3 months. After disassembly and inspection, the sealing surface performance was good, and the sealing performance was not significantly changed.
[0121] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should be included in the scope of the present invention.
Claims
1. A steam trap with carbonitriding surface strengthening treatment, characterized in that: The valve body (7), valve seat (1), valve core (2) and valve cover (4) are included. The valve seat (1) is fixed at the inner flow channel opening of the valve body (7). The valve core (2) is provided above the valve seat (1). The valve cover (4) is installed at the top opening of the valve body (7). An automatic venting valve (3) is installed on the valve cover (4). A filter assembly (5) is installed inside the inlet flow channel of the valve body (7). At least one of the sealing working surfaces of the valve seat (1) and the valve core (2) is treated with carbonitriding to form a surface-strengthening film.
2. A steam trap with carbonitriding surface strengthening treatment according to claim 1, characterized in that: The valve cover (4) is fastened to the top flange surface of the valve body (7) by bolts and nuts, and a gasket is also sandwiched between the valve cover (4) and the valve body (7); Welded flanges (6) are connected to both the medium inlet end and the medium outlet end of the valve body (7).
3. A steam trap with carbonitriding surface strengthening treatment according to claim 1, characterized in that: The filter assembly (5) is a detachable filter screen opened in the inlet flow channel of the valve body (7), and the inner side of the valve body (7) is provided with a filter screen mounting groove for installing the filter screen.
4. A steam trap with carbonitriding surface strengthening treatment according to claim 1, characterized in that: An adjusting screw plug (8) is installed on the valve seat (1), and a screw plug (9) is also installed on the valve seat (1) next to the adjusting screw plug (8).
5. A steam trap with carbonitriding surface strengthening treatment according to claim 1, characterized in that: The valve core (2) is a float valve core; The base material of the valve core (2) and valve seat (1) is low carbon or low alloy steel.
6. A steam trap with carbonitriding surface strengthening treatment according to claim 1, characterized in that: The sealing working surface of the valve seat (1) is treated with carbonitriding and a surface strengthening film is formed, or; The sealing working surface of the valve core (2) is treated with carbonitriding to form a surface strengthening film, or; The sealing working surface of the valve seat (1) and the sealing working surface of the valve core (2) are both treated with carbonitriding to form a surface strengthening film.
7. A steam trap with carbonitriding surface strengthening treatment according to claim 6, characterized in that: The sealing pair between the valve seat (1) and the valve core (2) is a conical surface fit, the sealing working surface of the valve core (2) is a conical surface, and the sealing working surface of the valve seat (1) is a matching conical hole.
8. The manufacturing process of a steam trap with carbonitriding surface strengthening treatment according to any one of claims 1-7, characterized in that: Includes the following steps: I. Preprocessing: The valve seat blank and / or valve core blank are subjected to stress-relief annealing, heated in the furnace to 540~560℃, held for 120~180 minutes, and then air-cooled to room temperature after being taken out of the furnace. II. Gas carbonitriding: The pretreated workpiece is placed in a gas carburizing and nitriding furnace. The furnace temperature is raised to 840~880℃ and held for 90~180 minutes. Carburizing medium and ammonia are introduced into the furnace. The carbon potential is controlled at 0.8%~0.9% and the ammonia gas fraction is controlled at 5%~15%. After carbonitriding treatment, the sealing working surfaces of the valve seat and / or valve core form a high-hardness, wear-resistant sealing pair. III. Quenching treatment: After the gas carbonitriding operation is completed, the furnace is cooled to 820~850℃, and the workpiece is immersed in quenching oil for rapid cooling. The quenching oil temperature is controlled at 40~80℃, and the cooling time is 15~30 minutes. IV. Cleaning and Drying: After quenching, the workpiece is soaked and cleaned with a metal cleaning agent solution, then sprayed with rust-preventive water and drained. V. Low-temperature tempering treatment: After cleaning and drying, place the workpiece in a tempering furnace and keep it at 160~280℃ for 120~180 minutes, then air cool to room temperature. VI. Assembly: Assemble the valve seat and valve core processed in step five with other purchased components to form a steam trap.
9. The manufacturing process of a steam trap with carbonitriding surface strengthening treatment according to claim 8, characterized in that: In step two, the gas carbonitriding temperature is set to 855~865℃, the holding time is 90 minutes, the carbon potential is controlled at 0.85%, and the ammonia gas integral is controlled at 8%~12%.
10. The manufacturing process of a steam trap with carbonitriding surface strengthening treatment according to claim 9, characterized in that: After the gas carbonitriding treatment in step two is completed, the surface hardness of the sealing working surface of the valve seat and / or valve core reaches 58~64HRC, and the effective hardened layer depth is 0.2~0.8mm.