A method of firing a continuous refining furnace

By using a combination of U-tube heat exchanger to preheat the purging medium and ash removal spray gun in a continuous refining furnace, the problems of uneven temperature caused by charcoal ash accumulation and prolonged furnace drying cycle were solved. This achieved a stable transition of furnace temperature, reduced fuel consumption and equipment damage, and improved furnace drying efficiency and equipment stability.

CN123154648APending Publication Date: 2026-11-24DAYE NONFERROUS METALS
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611453429.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the existing technology, continuous refining furnaces have problems such as uneven furnace lining temperature caused by charcoal ash accumulation, prolonged furnace drying cycle, increased fuel consumption, and thermal stress damage to the furnace lining during the furnace drying process. In addition, thermal shock caused by ambient temperature compressed air purging and bag filter clogging problems can lead to furnace drying interruptions.

Method used

A U-tube heat exchanger is used to preheat the purging medium. By preheating the purging medium to 150-200℃ at the end of the early stage of furnace drying, combined with the ash removal spray gun and stepped flow control, charcoal ash is removed. In the later stage of furnace drying, low-pressure air is switched to regulate the temperature, so as to achieve a smooth transition of furnace temperature.

Benefits of technology

It effectively solved the problems of uneven furnace lining temperature and prolonged furnace drying cycle caused by charcoal ash accumulation, reduced fuel consumption, avoided thermal shock and bag filter clogging, shortened furnace drying time, and improved the service life of furnace lining and the operational stability of equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123154648A_ABST
    Figure CN123154648A_ABST
Patent Text Reader

Abstract

This invention discloses a method for baking a continuous refining furnace, specifically including the following steps: S1. Setting up a heat exchange purging structure; S2. Performing a wood-fired baking stage in the early stage of baking; S3. Preheating the purging medium; S4. Purging the charcoal ash generated in step S2; S5. Performing a burner baking stage in the later stage of baking; S6. Baking completed. This invention provides a method for baking a continuous refining furnace, effectively solving a series of problems such as prolonged baking cycle, increased fuel consumption, and thermal stress damage to the furnace lining caused by charcoal ash accumulation at the end of the early stage of baking. It achieves a rapid and stable temperature transition from the early stage to the later stage of baking, avoiding a sudden drop in furnace temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of recycled copper refining technology, and in particular to a method for drying a continuous refining furnace. Background Technology

[0002] The patented technology, "A Continuous Refining Furnace and a Process for Refining Recycled Copper Using the Continuous Refining Furnace" (CN 108754176B), describes the continuous refining furnace as the core equipment for recycled copper production. Its lining is constructed of magnesia refractory material. After overhaul, the furnace lining contains a large amount of free water and crystal water. If directly put into production, the steam pressure generated by the rapid vaporization of moisture in the lining at an operating temperature of 1200℃ can cause the lining to crack, peel, or even explode, severely shortening the service life of the continuous refining furnace lining. Therefore, after overhaul, the furnace must be baked according to a strict heating curve. The core technical requirement is uniform and uninterrupted heating, especially avoiding sudden rises and falls in furnace temperature.

[0003] The initial 3-4 days of continuous refining furnace baking is a low-temperature baking stage. The core task during this stage is to slowly remove free water from the furnace lining. It is crucial to strictly avoid excessive temperature differences between different areas of the furnace to prevent excessive local heat concentration, which could lead to rapid vaporization of moisture within the lining and subsequent steam pressure damage to the lining structure. The continuous refining furnace is equipped with a natural gas burner. Among fuels commonly used in the recycled copper industry, natural gas has the gentlest combustion heat. However, based on actual results during the initial baking stage, natural gas burners still exhibit localized overheating issues. Practice shows that adding firewood to the furnace remains the best method for the initial baking stage of the continuous refining furnace due to its low flame temperature, low heat flux density, and minimal thermal shock to the furnace lining; the combustion process is easily controlled manually, allowing for real-time fuel adjustments based on lining temperature feedback; and the flame coverage can be flexibly adjusted, ensuring uniform heat distribution and minimizing localized overheating.

[0004] The furnace drying process after a major overhaul of the continuous refining furnace adopts a two-stage approach: initial drying with firewood followed by drying with natural gas burners. However, the inventors discovered through long-term production practice that this traditional method has a technical defect that has not yet been fully recognized: 1. Deterioration of the drying effect due to the accumulation of charcoal ash. In the early stages of furnace drying, firewood is continuously added to the furnace chamber in a "small amount at first, then larger amount" manner. As the early drying phase ends and the process transitions to the later stages, a large amount of charcoal ash remaining after the firewood burns accumulates at the bottom of the furnace and partially covers the furnace walls. This charcoal ash is 300-600 mm thick, loosely textured, and possesses excellent heat insulation properties.

[0005] When the natural gas burner is started for later heating, the accumulated charcoal ash effectively blocks the heat transfer from the burner flame to the furnace lining below the charcoal ash-covered area (hereinafter referred to as the "ash-covered zone"), making it difficult for the temperature of the "ash-covered zone" to rise. Actual measurements show that the temperature difference between the furnace lining of the "ash-covered zone" and the area without charcoal ash coverage (hereinafter referred to as the "ash-free zone") can reach 200℃. This leads to a series of chain reactions: First, the furnace drying cycle is prolonged. The furnace lining temperature in the "ash-covered zone" is far lower than the set temperature, causing the continuous refining furnace heating curve to deviate significantly from the design curve, thus forcing a prolonged overall furnace drying cycle.

[0006] Second, increased fuel consumption. To compensate for the insufficient temperature in the "ash-covered zone," it is necessary to increase the firepower output of the natural gas burner, resulting in a significant increase in natural gas consumption.

[0007] 3. Thermal stress damage to the furnace lining. The significant temperature gradient between the "ash-covered zone" and the "ash-free zone" causes uneven thermal expansion of the furnace lining, inducing thermal stress damage and severely shortening the service life of the furnace lining.

[0008] 2. Secondary problems caused by compressed air purging To solve the problem of charcoal ash accumulation, the inventors attempted to purge the furnace chamber by inserting a compressed air pipe through the working door at the end of the early stage of furnace drying, blowing the charcoal ash into the flue, and starting the exhaust fan to draw the dust-laden flue gas into the bag filter for particulate matter collection. However, this improvement scheme generated the following three interrelated secondary problems: (1) Thermal shock problem: The temperature of the compressed air is about 30°C, while the surface temperature of the "ash-free zone" of the furnace bottom lining during purging has reached 550-600°C. During the purging process, the low-temperature high-speed airflow (wind speed 15-25m / s) impacts the high-temperature furnace lining. The measured local temperature of the furnace bottom drops by 120-150°C within 30 minutes, which is essentially a rapid forced cooling of the furnace bottom lining, seriously violating the basic principle of "uniform heating and avoiding sudden rises and falls in furnace temperature" during the furnace drying process, and adversely affecting the service life of the furnace lining.

[0009] (2) Bag clogging problem in bag filters: The temperature of the flue gas after purging is low, resulting in the inlet flue gas temperature of the bag filter being lower than 50°C and containing a large amount of water vapor. The water vapor condenses into water on the surface of the filter bag, and the dust in the flue gas combines with it to form a mud-like substance, which blocks the pores on the surface of the filter bag, preventing airflow from passing through the filter bag. The filter bag has to be scrapped, causing significant economic losses, i.e., a bag clogging accident.

[0010] (3) Interruption of furnace drying: When the bag filter becomes clogged, it must be shut down immediately to replace the filter bags, a process that takes 24 to 36 hours. During this period, the continuous refining furnace cannot start its natural gas burner for subsequent furnace drying, resulting in an interruption of the drying process for 24 to 36 hours and a drop in furnace temperature of 180 to 240°C. This seriously violates the basic requirements of "no interruption" and "avoiding sudden rises and falls in furnace temperature" in the furnace drying process, and the damage to the furnace lining is even greater than the sum of other problems.

[0011] Due to the extremely serious consequences, the method of using compressed air to purge charcoal ash had to be discontinued, and the consequences of prolonged furnace drying cycle, increased fuel consumption, and thermal stress damage to the furnace lining caused by the accumulation of charcoal ash after the initial drying phase had to be accepted.

[0012] 3. Limitations in industry knowledge The inventors discovered through long-term technical practice that although the aforementioned technical defects objectively exist, they have not received sufficient attention from engineering and technical personnel in the industry.

[0013] Given the series of problems caused by charcoal ash purging, such as "thermal shock," "bag clogging," and "furnace drying interruption," existing technologies typically regard the charcoal ash accumulation problem after the initial stage of furnace drying as an "unavoidable normal phenomenon," and the problems caused by charcoal ash accumulation, such as prolonged furnace drying cycle, increased fuel consumption, and thermal stress damage to the furnace lining, as "a necessary price to pay." This technological bias is precisely the key breakthrough that this invention aims to overcome.

[0014] Through a systematic analysis of the above-mentioned technical problems, it was recognized that the following deep-seated contradictions exist in the existing technology: Contradiction 1: Charcoal ash must be removed, otherwise it will lead to uneven furnace lining temperature, prolonged furnace drying cycle, and increased fuel consumption.

[0015] The second contradiction is that while using room temperature compressed air to purge can remove charcoal ash, it will cause thermal shock to the high-temperature furnace lining and lead to the "bag clogging" problem in the bag filter, which in turn will cause serious consequences such as interruption of the furnace drying process.

[0016] The third contradiction is that the existence of the above contradictions is not due to improper operation, but rather to the structural defects of the existing furnace drying process itself—the lack of a technical means to remove charcoal ash without causing thermal shock to the furnace lining, without causing "bag clogging" problems, and without interrupting the furnace drying process.

[0017] Therefore, it is essential to develop a technical solution that can effectively remove charcoal ash, protect the furnace lining, and prevent bag clogging and furnace drying interruptions. Summary of the Invention

[0018] The purpose of this invention is to provide a method for drying a continuous refining furnace in response to the above-mentioned situation.

[0019] The specific solution of the present invention is: a method for drying a continuous refining furnace, which specifically includes the following steps: S1. Setting up a heat exchange and purging structure: A U-tube heat exchanger is installed in the flue of the continuous refining furnace. The heat exchange tubes of the U-tube heat exchanger are placed inside the flue. The inlet end of the U-tube heat exchanger is connected to both the purging medium cold pipe and the blower for introducing the purging medium or low-pressure air. The outlet end of the U-tube heat exchanger is connected to both the purging medium heat pipe and the preheating air pipe. The end of the purging medium heat pipe is connected to the cleaning spray gun installed on the furnace head end wall. The above structure is set up and ready for use. S2. The wood drying stage before furnace drying: According to the predetermined heating curve, wood is added into the furnace of the continuous refining furnace for low-temperature drying for 3 to 4 days to remove free water from the furnace lining. S3. Preheating of purge medium: At the end of the early stage of oven drying, start the exhaust fan and open the purge medium cold pipe at the same time to introduce purge medium into the U-tube heat exchanger. The flow rate is controlled at 200-800 Nm³ / h. When the purge medium flows through the heat exchange tubes of the U-tube heat exchanger, it exchanges heat with the high-temperature flue gas in contact with the outer wall of the tube and is preheated to 150-200℃. S4. Blow away the charcoal ash produced in step S2: turn on the blowing medium heat pipe and close the preheating air pipe. Spray the preheated blowing medium from the furnace head cleaning spray gun into the furnace to blow away the charcoal ash accumulated on the furnace bottom and furnace wall. The blowing time is controlled at 30 to 60 minutes until there is no obvious ash accumulation on the furnace bottom. During blowing, the working door is closed. S5. Perform the later stage of furnace drying, i.e., the burner furnace drying stage: After the charcoal ash is purged, start the natural gas burner and enter the later stage of furnace drying and heating; close the purging medium heat pipe and open the preheating air pipe; at the same time, close the purging medium cold pipe and start the blower to switch the medium introduced into the heat exchange tube of the U-tube heat exchanger to low-pressure air, and control the low-pressure air flow rate at 4000~8000Nm³ / h; S6. After the furnace drying is completed according to the predetermined heating curve, the continuous refining furnace will be put into normal production.

[0020] Furthermore, the purging medium in step S3 of this invention is any one of nitrogen, oxygen, or compressed air.

[0021] Furthermore, the ash removal spray guns described in this invention are heat-resistant steel pipes, numbered 1 to 4, with a diameter of 20 to 100 mm, and are pre-embedded in the furnace head end wall masonry; the ash removal spray guns are tilted 15 to 45° towards the furnace, and their outlet direction is aimed at the area of ​​accumulated charcoal ash at the bottom of the furnace.

[0022] Furthermore, the purging medium described in this invention is injected into the furnace at a speed of 10-30 m / s through a cleaning spray gun.

[0023] Furthermore, the heat exchange tube of the U-tube heat exchanger described in this invention is made of 316L stainless steel, and the heat exchange area is 20-50m².

[0024] Furthermore, the flow control mode of the purging medium in this invention is a step-by-step control: a large flow rate of 500-800 Nm³ / h is used in the initial stage of purging, and a small flow rate of 200-500 Nm³ / h is used in the later stage of purging.

[0025] This invention provides a method for drying a continuous refining furnace, which effectively solves a series of problems such as prolonged drying cycle, increased fuel consumption, and thermal stress damage to the furnace lining caused by charcoal ash accumulation at the end of the early stage of drying. It achieves a rapid and stable temperature transition from the early stage to the later stage of drying, avoiding a sudden drop in furnace temperature.

[0026] The application of this invention upgrades the furnace drying process after a major overhaul of a continuous refining furnace from the traditional two-stage process of "early wood drying → later natural gas burner drying" to a three-stage process of "early wood drying → preheating medium purging → later natural gas burner drying". The core value of this process upgrade lies in transforming the traditional model of "passively bearing" the problem of charcoal ash accumulation into an innovative model of "actively removing and smoothly transitioning".

[0027] Compared with the prior art, the present invention has the following technical effects: 1. It solves the problem of thermal shock to the furnace lining caused by purging charcoal ash. Traditional technology uses compressed air at around 30°C to purge the high-temperature furnace lining at 550-600°C. This results in an instantaneous temperature difference of up to 600°C, causing the furnace lining to cool down rapidly during purging, with a drop of 120-150°C. This seriously violates the principle of "avoiding sudden temperature rises and falls" in furnace baking.

[0028] This invention uses nitrogen gas preheated to 150-200°C for purging, reducing the temperature difference between the nitrogen and the furnace lining to 300-400°C. Combined with a stepped flow control mode of "large flow first, then small flow," the temperature drop of the furnace lining during purging is more gradual. Actual measurements show that the temperature drop on the furnace lining surface is controlled within 20-30°C, meeting the technical requirements of "uniform heating and avoiding sudden temperature increases and decreases" in furnace baking. This effect is something that those skilled in the art could not have foreseen using existing technology.

[0029] 2. Completely eliminated the risk of "bag clogging" in baghouse dust collectors. In existing technologies, ambient temperature purging causes the inlet flue gas temperature of the bag filter to drop below 50°C, resulting in water vapor condensing into water on the surface of the filter bags, causing a "bag clogging" accident, which leads to the scrapping of the filter bags and the interruption of the drying furnace.

[0030] This invention raises the inlet flue gas temperature of the bag filter to 60-70°C by preheating the purging medium, while simultaneously diluting the water vapor concentration in the flue gas, resulting in a dew point temperature lower than the actual operating temperature, thus preventing water vapor from condensing on the filter bag surface. Actual operation shows that after adopting this method, the pressure differential of the bag filter stabilizes within the normal range of 1200-1500 Pa, and "bag clogging" accidents no longer occur. This effect also exceeded the expectations of those skilled in the art.

[0031] 3. It realizes the "dual-purpose" function of the heat exchanger, reducing equipment investment. This invention creatively utilizes the same heat exchanger for both preheating the purging medium (at the end of the early stage of furnace drying) and cooling the flue gas (at the end of the later stage of furnace drying), achieving functional reuse of a single device in two different process stages. Compared to the conventional approach of setting up separate preheating and cooling devices, this invention significantly reduces equipment investment and floor space. This design concept has not been found to offer any technological inspiration in the prior art.

[0032] 4. Overcame technical biases within the industry. For a long time, the industry has generally believed that the following technical bias exists: "The use of firewood for the initial drying of the furnace, the accumulation of charcoal ash, and the resulting problems of prolonged drying cycle, increased fuel consumption, and thermal stress damage to the furnace lining are unavoidable and must be accepted costs." This invention, through systematic mechanism analysis and innovative technical solutions, creatively provides a solution that is scientific, economical, and reliable, breaking through the aforementioned technical biases.

[0033] Therefore, this invention completely solves the problem of charcoal ash accumulation caused by wood-fired ovens, which leads to uneven furnace lining temperature, prolonged oven drying cycle, and increased fuel consumption. At the same time, in the process of removing charcoal ash, it also creatively solves the problems of furnace lining thermal shock, bag filter clogging, and oven drying interruption.

[0034] 5. High-efficiency utilization of low-grade waste heat has been achieved. This invention overcomes another common prejudice among those skilled in the art from the very beginning of its engineering design: "The flue gas temperature is low and fluctuates greatly in the early stage of furnace drying, and it does not have the value of waste heat recovery." Traditionally, it has been believed that only high-temperature flue gas with a temperature >800℃ and stable output is worth installing heat exchangers for waste heat recovery, while fluctuating flue gas with temperatures of 400-600℃ produced in the early stages of furnace drying is considered "waste heat" and has long been neglected. This invention, through the compact design of a U-tube heat exchanger and a media switching strategy, successfully demonstrates that low-grade, variable-temperature flue gas can also be efficiently utilized through a specially designed heat exchange system.

[0035] This technological approach provides a replicable paradigm for the recycling and utilization of other low-temperature waste heat resources (such as anode furnace flue gas and baking waste heat) in the recycled copper smelting industry, and has broad application value.

[0036] Furthermore, the present invention has produced the following unexpected technical effects: 1. It significantly shortens the furnace baking cycle and reduces fuel consumption. Because the charcoal ash is completely removed, the burner flame can act evenly on the furnace lining surface, eliminating the problem of uneven local temperature caused by charcoal ash coverage. Actual production data shows that, after adopting the method of this invention, the later stage heating time of the furnace is shortened by approximately 12-36% compared to the design value, and natural gas consumption is reduced by approximately 10-30% compared to the design value. This technical effect is the result of the overall synergistic effect of the technical solution of this invention. The furnace drying effect is significantly improved, and the furnace drying cycle and fuel consumption are significantly reduced—technical effects that the inventors did not expect in their technical practice.

[0037] 2. Eliminated environmental risks associated with the soot blowing process. Traditional soot blowing methods have the following problems: Soot blowing is carried out through a compressed air pipe at the working door, which is limited by the position and size of the working door, resulting in a limited blowing angle, low blowing efficiency, long blowing time, and exacerbating the cooling of the furnace lining during the soot blowing process. The working door must be opened during soot blowing, and the dust-laden flue gas overflows directly from the working door, causing environmental pollution.

[0038] This invention achieves the following improvements by installing a dedicated ash-cleaning spray gun on the furnace head end wall: the blowing angle is not restricted by the working door, it can fully cover the bottom of the furnace, the blowing efficiency is high and the time is short, and it avoids the significant cooling of the furnace lining after fuel combustion is stopped during ash-cleaning, ensuring thorough ash removal. The working door is closed throughout the ash-cleaning process, preventing charcoal ash from being blown out of the furnace, fundamentally avoiding environmental pollution caused by smoke and dust overflow. Attached Figure Description

[0039] Figure 1 This is a schematic diagram of the main cross-section of the present invention; Figure 2 yes Figure 1 Schematic diagram of the structure in the AA direction; Figure 3 This is a schematic diagram of the main section structure of a traditional continuous refining furnace; Figure 4 This is a schematic diagram of the cross-sectional structure of the furnace in Comparative Example 1; Figure 5 This is a schematic diagram of the cross-sectional structure of the furnace in Comparative Example 2.

[0040] In the diagram: 1—Natural gas burner, 2—Charcoal ash, 3—Purge medium heat pipe, 4—Cleaning spray gun, 5—Furnace head end wall, 6—Blower, 7—Purge medium cold pipe, 8—U-tube heat exchanger, 9—Preheating air duct, 10—Flue, 11—Bag filter, 12—Exhaust fan, 13—Working door panel, 14—Working door, 15—Continuous refining furnace, 16—Compressed air duct. Detailed Implementation

[0041] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention. In the description of the present invention, it should be noted that the terms "upper," "lower," "inner," "outer," etc., indicating orientation or positional relationship are based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product of the invention is in use. They are only for the convenience of describing the present invention or simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed or operated in a specific orientation, and therefore should not be construed as a limitation of the present invention.

[0042] In the description of this invention, it should also be noted that, unless otherwise explicitly specified and limited, the terms "set," "install," and "connect" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal communication between two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0043] See Figure 1 , Figure 2 This invention is a method for drying a continuous refining furnace, specifically including the following steps: S1. Setting up a heat exchange purging structure: A U-tube heat exchanger 8 is set up in the flue of the continuous refining furnace. The heat exchange tubes of the U-tube heat exchanger are placed inside the flue 10. The inlet end of the U-tube heat exchanger is connected to the purging medium cold pipe 7 and the blower 6 for introducing the purging medium or low-pressure air. The outlet end of the U-tube heat exchanger 8 is connected to the purging medium heat pipe 3 and the preheating air pipe 9 respectively. The end of the purging medium heat pipe 3 is connected to the cleaning spray gun 4 set on the furnace head end wall 5. The above structure is set up and ready for use. Further, the heat exchange tube of the U-tube heat exchanger in this invention is made of 316L stainless steel and the heat exchange area is 20-50m². S2. The wood drying stage before furnace drying: According to the predetermined heating curve, wood is added into the furnace of the continuous refining furnace for low-temperature drying for 3 to 4 days to remove free water from the furnace lining. S3. Preheating of the purge medium: At the end of the initial stage of oven drying, start the exhaust fan and simultaneously open the purge medium cold pipe to introduce the purge medium into the U-tube heat exchanger. The flow rate is controlled at 200-800 Nm³ / h. When the purge medium flows through the heat exchange tubes of the U-tube heat exchanger, it exchanges heat with the high-temperature flue gas in contact with the outer wall of the tube and is preheated to 150-200°C. Further, the purge medium in step S3 of this invention is any one of nitrogen, oxygen or compressed air. S4. Purging the charcoal ash generated in step S2: Turn on the purging medium heat pipe 3 and close the preheating air pipe 9. Spray the preheated purging medium from the furnace head cleaning spray gun 4 into the furnace to purge the charcoal ash 2 accumulated on the furnace bottom and furnace wall. The purging time is controlled at 30 to 60 minutes until there is no obvious ash accumulation on the furnace bottom. During purging, the working door plate 13 is closed. Further, the cleaning spray gun 4 in this invention is a heat-resistant steel pipe, with a quantity of 1 to 4 pipes and a diameter of 20 to 100 mm, which is embedded in the furnace head end wall masonry. The cleaning spray gun is tilted 15 to 45 degrees into the furnace, and its outlet direction is aimed at the area of ​​charcoal ash accumulated on the furnace bottom. Further, the purging medium in this invention is sprayed into the furnace through the cleaning spray gun at a speed of 10 to 30 m / s. S5. Perform the later stage of furnace drying, i.e., the burner furnace drying stage: After the charcoal ash is purged, start the natural gas burner 1 to enter the later stage of furnace drying and heating; close the purging medium heat pipe and open the preheating air pipe; at the same time, close the purging medium cold pipe and start the blower to switch the medium introduced into the heat exchange tube of the U-tube heat exchanger to low-pressure air, and control the low-pressure air flow rate at 4000~8000Nm³ / h; S6. After the furnace drying is completed according to the predetermined heating curve, the continuous refining furnace will be put into normal production.

[0044] Furthermore, the flow control mode of the purging medium in this invention is a step-by-step control: a large flow rate of 500-800 Nm³ / h is used in the initial stage of purging, and a small flow rate of 200-500 Nm³ / h is used in the later stage of purging.

[0045] Further comparative studies on the purging media show that nitrogen is the preferred purging medium, and its effectiveness is more clearly demonstrated in specific embodiments. Using nitrogen has the following significant advantages over using compressed air or oxygen, as shown in the table below: This invention provides a method for drying a continuous refining furnace, which effectively solves a series of problems such as prolonged drying cycle, increased fuel consumption, and thermal stress damage to the furnace lining caused by charcoal ash accumulation at the end of the early stage of drying. It achieves a rapid and stable temperature transition from the early stage to the later stage of drying, avoiding a sudden drop in furnace temperature.

[0046] The technical solution of the present invention will be further described below with reference to the accompanying drawings. Example 1

[0047] A U-tube heat exchanger is installed inside the flue of the continuous refining furnace. The heat exchange tubes of the U-tube heat exchanger are made of 316L stainless steel, and the heat exchange area is 40m². The heat exchange tubes are placed inside the flue, and their inlets are connected to the purge medium cold pipe and the blower, respectively, for introducing the purge medium or low-pressure air. The outer wall of the heat exchange tubes exchanges heat with the high-temperature flue gas discharged from the continuous refining furnace to preheat the purge medium or low-pressure air inside the tubes. The outlet of the heat exchange tubes is connected to the purge medium heat pipe and the preheating air pipe, respectively. The end of the purge medium heat pipe is connected to the cleaning spray gun installed on the end wall of the furnace head.

[0048] Both the purging medium heat pipe and the preheating air duct are covered with an aluminum silicate fiber insulation layer to reduce heat loss after preheating. The purging medium is compressed air with a pressure of 600 kPa and a supply air volume of 600 Nm³. 3 / h. The blower has a total pressure of 10 kPa and a blower volume of 6000 Nm³. 3 / h. The cleaning spray gun is a heat-resistant steel pipe, two in number, with a diameter of 80mm, pre-embedded in the masonry of the furnace head end wall; the cleaning spray gun is tilted 30° towards the furnace, and its outlet direction is aimed at the area of ​​accumulated charcoal ash at the bottom of the furnace. The compressed air is injected into the furnace through the cleaning spray gun at a speed of 10-30m / s to blow away the accumulated charcoal ash.

[0049] The specific oven drying steps are as follows: Step 1: Early stage of furnace drying (firewood drying stage) According to the predetermined heating curve, firewood is added to the furnace chamber of the continuous refining furnace for low-temperature drying for 4 days to remove free water from the furnace lining.

[0050] Step 2: Preheating of the purging medium: At the end of the initial stage of furnace baking, start the exhaust fan; at the same time, turn on the cold pipe of the purging medium and introduce compressed air into the heat exchange tube, with the flow rate controlled at 600 Nm³ / h; when the compressed air flows through the heat exchange tube, it exchanges heat with the high-temperature flue gas (temperature of about 550-650℃) in contact with the outer wall of the tube and is preheated to 150-200℃.

[0051] Step 3: Charcoal Ash Purging: Turn on the purging medium heat pipe and close the preheating air pipe. Spray preheated compressed air into the furnace from the furnace head cleaning gun to purge the charcoal ash accumulated on the furnace bottom and walls. The purging time should be controlled at 20-30 minutes until there is no obvious ash accumulation on the furnace bottom. During purging, the working door should be closed.

[0052] Step Four: Late Stage of Furnace Drying (Burner Drying Stage): After the charcoal ash is purged, the natural gas burner is started, entering the late stage of furnace drying and heating. The purging medium heat pipe is closed, and the preheating air pipe is opened. Simultaneously, the purging medium cold pipe is closed, and the blower is started to switch the medium flowing into the heat exchange tubes to low-pressure air, with the low-pressure air flow rate controlled at 6000 Nm³ / h. The low-pressure air absorbs heat from the flue gas in the heat exchange tubes, cooling the flue gas from the continuous refining furnace, so that the temperature of the flue gas entering the bag filter is controlled at 70–120℃. The heated air is used for other purposes, including but not limited to heating the denitrification solution, insulating the bag filter, and providing combustion air, achieving cascade recovery and utilization of waste heat from the flue gas.

[0053] Step 5: Furnace drying completed. After the furnace drying is completed according to the predetermined heating curve, the continuous refining furnace is put into normal production.

[0054] When compressed air was used to purge charcoal ash, the bag filter operated normally without bag clogging. The working door remained closed throughout the purging process, preventing charcoal ash from being blown out of the furnace and avoiding environmental pollution caused by flue gas spillage. The surface temperature of the continuous refining furnace lining decreased by 30-40°C. The heating time in the later stages of furnace drying was shortened by 25%, and natural gas consumption was reduced by 20% compared to the design value. Example 2

[0055] A U-tube heat exchanger is installed inside the flue of the continuous refining furnace. The heat exchange tubes are made of 316L stainless steel and have a heat exchange area of ​​40m². The heat exchange tubes are placed inside the flue, and their inlets are connected to the purge medium cold pipe and the blower, respectively, for introducing the purge medium or low-pressure air. The outer wall of the heat exchange tubes exchanges heat with the high-temperature flue gas discharged from the continuous refining furnace to preheat the purge medium or low-pressure air inside the tubes. The outlet of the heat exchange tubes is connected to the purge medium heat pipe and the preheating air pipe, respectively. The end of the purge medium heat pipe is connected to the cleaning spray gun installed on the furnace head end wall.

[0056] Both the purging medium heat pipe and the preheating air duct are covered with an aluminum silicate fiber insulation layer to reduce heat loss after preheating. The purging medium is oxygen, with a pressure of 200 kPa and a supply air volume of 600 Nm³. 3 / h. The blower has a total pressure of 10 kPa and a blower volume of 6000 Nm³. 3 / h. The cleaning spray gun is a heat-resistant steel pipe, two in number, with a diameter of 80mm, pre-embedded in the masonry of the furnace head end wall; the cleaning spray gun is tilted 30° towards the furnace, and its outlet direction is aimed at the area of ​​accumulated charcoal ash at the bottom of the furnace. The oxygen is injected into the furnace through the cleaning spray gun at a speed of 10-30m / s to blow away the accumulated charcoal ash.

[0057] The specific oven drying steps are as follows: Step 1: Early stage of furnace drying (firewood drying stage) According to the predetermined heating curve, firewood is added to the furnace chamber of the continuous refining furnace for low-temperature drying for 4 days to remove free water from the furnace lining.

[0058] Step 2: Preheating of the purge medium: At the end of the initial stage of furnace baking, start the exhaust fan; at the same time, turn on the purge medium cold pipe and introduce oxygen into the heat exchange tube, with the flow rate controlled at 600 Nm³ / h; when the purge medium flows through the heat exchange tube, it exchanges heat with the high-temperature flue gas (temperature about 550-650℃) in contact with the outer wall of the tube and is preheated to 150-200℃.

[0059] Step 3: Charcoal Ash Purging: Turn on the purging medium heat pipe and close the preheating air pipe. Inject preheated oxygen into the furnace from the furnace head cleaning gun to purge the charcoal ash accumulated on the furnace bottom and walls. The purging time should be controlled at 30-40 minutes until there is no obvious ash accumulation on the furnace bottom. During purging, the working door should be closed.

[0060] Step Four: Late Stage of Furnace Drying (Burner Drying Stage): After the charcoal ash is purged, the natural gas burner is started, entering the late stage of furnace drying and heating. The purging medium heat pipe is closed, and the preheating air pipe is opened. Simultaneously, the purging medium cold pipe is closed, and the blower is started to switch the medium introduced into the heat exchange tubes to low-pressure air, with the low-pressure air flow rate controlled at 6000 Nm³ / h. The low-pressure air absorbs heat from the flue gas in the heat exchange tubes, cooling the flue gas from the continuous refining furnace, so that the temperature of the flue gas entering the bag filter is controlled at 70–120℃. The heated air is used for other purposes, including but not limited to heating the denitrification solution, insulating the bag filter, and providing combustion air, achieving the cascade recovery and utilization of waste heat from the flue gas.

[0061] Step 5: Furnace drying completed. After the furnace drying is completed according to the predetermined heating curve, the continuous refining furnace is put into normal production.

[0062] During oxygen purging of charcoal ash, the bag filter operated normally without bag clogging. The working door remained closed throughout the purging process, preventing charcoal ash from being blown out of the furnace and avoiding environmental pollution caused by flue gas spillage. The surface temperature of the continuous refining furnace lining decreased by 35–45°C. The heating time in the later stages of furnace drying was shortened by 23%, and natural gas consumption was reduced by 19% compared to the design value. Example 3

[0063] A U-tube heat exchanger is installed inside the flue of the continuous refining furnace. The heat exchange tubes are made of 316L stainless steel and have a heat exchange area of ​​40m². The heat exchange tubes are placed inside the flue, and their inlets are connected to the purge medium cold pipe and the blower, respectively, for introducing the purge medium or low-pressure air. The outer wall of the heat exchange tubes exchanges heat with the high-temperature flue gas discharged from the continuous refining furnace to preheat the purge medium or low-pressure air inside the tubes. The outlet of the heat exchange tubes is connected to the purge medium heat pipe and the preheating air pipe, respectively. The end of the purge medium heat pipe is connected to the cleaning spray gun installed on the furnace head end wall.

[0064] The heat pipe for the purging medium and the preheating air duct are both covered with an aluminum silicate fiber insulation layer to reduce heat loss after preheating. The purging medium is nitrogen gas at a pressure of 300 kPa and a supply air volume of 200–800 Nm³ / h. The blower has a total pressure of 10 kPa and a blower volume of 6000 Nm³ / h. 3 / h. The cleaning spray gun is a heat-resistant steel pipe, two in number, with a diameter of 80mm, pre-embedded in the masonry of the furnace head end wall; the cleaning spray gun is tilted 30° towards the furnace, and its outlet direction is aimed at the area of ​​accumulated charcoal ash at the bottom of the furnace. The nitrogen gas is injected into the furnace through the cleaning spray gun at a speed of 10-30m / s to purge the accumulated charcoal ash.

[0065] The specific oven drying steps are as follows: Step 1: Early stage of furnace drying (firewood drying stage) According to the predetermined heating curve, firewood is added to the furnace chamber of the continuous refining furnace for low-temperature drying for 4 days to remove free water from the furnace lining.

[0066] Step 2: Preheating of the purge medium: At the end of the initial stage of furnace baking, start the exhaust fan; at the same time, turn on the purge medium cold pipe and introduce nitrogen into the heat exchange tube, with the flow rate controlled at 200-800 Nm³ / h; when the purge medium flows through the heat exchange tube, it exchanges heat with the high-temperature flue gas (temperature about 550-650℃) in contact with the outer wall of the tube and is preheated to 150-200℃.

[0067] Step 3: Charcoal Ash Purging: Turn on the purging medium heat pipe and close the preheating air pipe. Inject preheated nitrogen gas into the furnace from the furnace head cleaning gun to purge the charcoal ash accumulated on the furnace bottom and walls. The purging time should be controlled at 15-20 minutes until there is no obvious ash accumulation on the furnace bottom. During purging, the working door should be closed.

[0068] The flow control mode of the purging medium nitrogen is a step-by-step control of "large flow first, small flow later": a larger flow rate (500-800 Nm³ / h) is used in the initial stage of purging (first 10-15 min) to quickly purge the main body of accumulated charcoal ash; a smaller flow rate (200-500 Nm³ / h) is used in the later stage of purging (remaining 5-10 min) to remove residual charcoal ash and avoid a significant drop in furnace lining temperature.

[0069] Step Four: Late Stage of Furnace Drying (Burner Drying Stage): After the charcoal ash is purged, the natural gas burner is started, entering the late stage of furnace drying and heating. The purging medium heat pipe is closed, and the preheating air pipe is opened. Simultaneously, the purging medium cold pipe is closed, and the blower is started to switch the medium flowing into the heat exchange tubes to low-pressure air, with the low-pressure air flow rate controlled at 6000 Nm³ / h. The low-pressure air absorbs heat from the flue gas in the heat exchange tubes, cooling the flue gas from the continuous refining furnace, so that the temperature of the flue gas entering the bag filter is controlled at 70–120℃. The heated air is used for other purposes, including but not limited to heating the denitrification solution, insulating the bag filter, and providing combustion air, achieving cascade recovery and utilization of waste heat from the flue gas.

[0070] Step 5: Furnace drying completed. After the furnace drying is completed according to the predetermined heating curve, the continuous refining furnace is put into normal production.

[0071] During nitrogen purging of charcoal ash, the bag filter operated normally without bag clogging. The working door remained closed throughout the purging process, preventing charcoal ash from being blown out of the furnace and avoiding environmental pollution caused by flue gas spillage. The surface temperature of the continuous refining furnace lining decreased by 20-30°C. The heating time in the later stages of furnace drying was shortened by 28%, and natural gas consumption was reduced by 24% compared to the design value.

[0072] Comparative Example 1 (see Figure 3 and Figure 4 ) After the continuous refining furnace is overhauled, it is dried using conventional methods. After the initial drying phase, the charcoal ash is not removed.

[0073] Step 1: Early stage of furnace drying (firewood drying stage) According to the predetermined heating curve, firewood is added to the furnace of the continuous refining furnace for low-temperature drying for 3 to 4 days to remove free water from the furnace lining.

[0074] Step 2: Late stage of furnace drying (burner drying stage): Start the natural gas burner and enter the late stage of furnace drying and heating. Step 3: Furnace drying completed. After the furnace drying is completed according to the predetermined heating curve, the continuous refining furnace is put into normal production.

[0075] At the end of the initial furnace drying phase, due to the fire-insulating effect of charcoal ash, the temperature difference between the "ash-covered zone" and the "ashless zone" of the furnace lining can reach 200℃. This temperature gradient leads to thermal stress damage to the furnace lining. To avoid this problem, two methods are employed: first, increasing the firepower of the natural gas burner; and second, maintaining a constant temperature for 1-2 hours after every 3-4 hours of heating. This aims to raise the temperature in the "ash-covered zone" while preventing the "ashless zone" from heating up faster and thus increasing the temperature gradient. The direct consequence is that the heating curve deviates significantly from the design curve, and the heating time is extended by 24-35 hours compared to the design time, with natural gas consumption increasing by 28-40% compared to the design value.

[0076] Comparative Example 2 (see Figure 3and Figure 5 ) After the continuous refining furnace is overhauled, it is dried using conventional methods. After the initial drying phase, compressed air is used to blow away and remove charcoal ash.

[0077] Direct air blowing mode: Step 1: Early stage of furnace drying (firewood drying stage) According to the predetermined heating curve, firewood is added to the furnace of the continuous refining furnace for low-temperature drying for 3 to 4 days to remove free water from the furnace lining.

[0078] Step Two: At the end of the initial stage of furnace drying, open the working door and insert compressed air pipe 16 through the working door to purge the furnace chamber, blowing the charcoal ash into the flue. Then, start the exhaust fan to draw the dust-laden flue gas into the bag filter for particulate matter collection. Continue until there is no obvious ash accumulation at the bottom of the furnace. The purging time is 20–40 minutes.

[0079] Step 3: Late stage of furnace drying (burner drying stage): After the charcoal ash is purged, the natural gas burner is started to enter the late stage of furnace drying and heating. Step 4: Furnace drying completed. After the furnace drying is completed according to the predetermined heating curve, the continuous refining furnace is put into normal production.

[0080] During charcoal ash blowing, a low-temperature, high-speed airflow (15-25 m / s) impacts the high-temperature furnace lining. Actual measurements show that the local temperature at the furnace bottom drops by 120-150°C within 30 minutes. This effectively subjects the furnace lining to a rapid and forced cooling, severely violating the fundamental principle of "uniform heating and avoiding sudden temperature fluctuations" during furnace drying, thus adversely affecting the service life of the furnace lining. To mitigate the damage caused by ash blowing, a lower heat output and slower heating rate are used after starting the natural gas burner, resulting in a significant deviation of the heating curve from the design curve. Simultaneously, the heating time is extended by 12-24 hours compared to the design time, and natural gas consumption increases by 15-30% compared to the design.

[0081] During charcoal ash purging, the bag filter sometimes experiences "bag clogging," forcing a shutdown to replace the filter bags at a cost exceeding 100,000 yuan. Replacing the filter bags takes 24-36 hours. During this period, the exhaust fan is shut down, and the continuous refining furnace cannot start its natural gas burner for furnace drying, resulting in a 24-36 hour interruption in the drying process and a drop in furnace temperature of 180-240°C. This severely violates the basic requirements of "no interruption" and "avoiding sudden rises and falls in furnace temperature" during the drying process. After replacing the filter bags, restarting the natural gas drying process requires an additional 24-48 hours to compensate for the lost temperature, increasing natural gas consumption by 30-60% compared to the design value.

Claims

1. A method for drying a continuous refining furnace, characterized in that, Specifically, the following steps are included: S1. Setting up a heat exchange and purging structure: A U-tube heat exchanger is installed in the flue of the continuous refining furnace. The heat exchange tubes of the U-tube heat exchanger are placed inside the flue. The inlet end of the U-tube heat exchanger is connected to both the purging medium cold pipe and the blower for introducing the purging medium or low-pressure air. The outlet end of the U-tube heat exchanger is connected to both the purging medium heat pipe and the preheating air pipe. The end of the purging medium heat pipe is connected to the cleaning spray gun installed on the furnace head end wall. The above structure is set up and ready for use. S2. The wood drying stage before furnace drying: According to the predetermined heating curve, wood is added into the furnace of the continuous refining furnace for low-temperature drying for 3 to 4 days to remove free water from the furnace lining. S3. Preheating of purge medium: At the end of the early stage of oven drying, start the exhaust fan and open the purge medium cold pipe at the same time to introduce purge medium into the U-tube heat exchanger. The flow rate is controlled at 200-800 Nm³ / h. When the purge medium flows through the heat exchange tubes of the U-tube heat exchanger, it exchanges heat with the high-temperature flue gas in contact with the outer wall of the tube and is preheated to 150-200℃. S4. Blow away the charcoal ash produced in step S2: turn on the blowing medium heat pipe and close the preheating air pipe. Spray the preheated blowing medium from the furnace head cleaning spray gun into the furnace to blow away the charcoal ash accumulated on the furnace bottom and furnace wall. The blowing time is controlled at 30 to 60 minutes until there is no obvious ash accumulation on the furnace bottom. During blowing, the working door is closed. S5. Perform the later stage of furnace drying, i.e., the burner furnace drying stage: After the charcoal ash is purged, start the natural gas burner and enter the later stage of furnace drying and heating; close the purging medium heat pipe and open the preheating air pipe; at the same time, close the purging medium cold pipe and start the blower to switch the medium introduced into the heat exchange tube of the U-tube heat exchanger to low-pressure air, and control the low-pressure air flow rate at 4000~8000Nm³ / h; S6. After the furnace drying is completed according to the predetermined heating curve, the continuous refining furnace will be put into normal production.

2. The method for drying a continuous refining furnace according to claim 1, characterized in that, The purging medium in step S3 is any one of nitrogen, oxygen, or compressed air.

3. The method for drying a continuous refining furnace according to claim 1, characterized in that, The cleaning spray gun is a heat-resistant steel pipe, numbered 1 to 4, with a diameter of 20 to 100 mm, and is pre-embedded in the masonry of the furnace head end wall; the cleaning spray gun is tilted 15 to 45 degrees into the furnace, and its outlet direction is aimed at the area of ​​accumulated charcoal ash at the bottom of the furnace.

4. The method for drying a continuous refining furnace according to claim 1, characterized in that, The purging medium is injected into the furnace through a cleaning spray gun at a speed of 10-30 m / s.

5. The method for drying a continuous refining furnace according to claim 1, characterized in that, The heat exchange tubes of the U-tube heat exchanger are made of 316L stainless steel, and the heat exchange area is 20-50m².

6. The method for drying a continuous refining furnace according to claim 1, characterized in that, The flow control mode of the purging medium is a step-by-step control: a large flow rate of 500-800 Nm³ / h is used in the initial stage of purging, and a small flow rate of 200-500 Nm³ / h is used in the later stage of purging.

Citation Information

Patent Citations

  • A continuous refining furnace and a process for refining recycled copper using the continuous refining furnace.