A system and method for the cascade utilization of waste heat in the preparation of ultrafine metakaolin from sea mud
By using a closed-loop system of marine mud pre-drying, calcination, and steam kinetic mill, and utilizing the waste heat from calcination flue gas to prepare medium-temperature superheated steam, the problems of low resource utilization rate and high energy consumption of marine mud are solved. This achieves efficient preparation and green utilization of ultrafine metakaolin, and improves the performance of cement-based materials.
Patent Information
- Application Number
- CN202611562619.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies suffer from low utilization rates of marine mud resources, high preparation costs, strong corrosiveness and poor applicability of traditional alkali activation processes, waste of waste heat from calcination flue gas, high energy consumption in the pretreatment and drying of wet marine mud, cumbersome process flow, and a lack of a waste heat cascade utilization system.
By using a closed-loop system of pre-drying, calcination, and steam kinetic mill, the waste heat from calcination flue gas is used to prepare medium-temperature superheated steam, which drives grinding and pre-drying, thus achieving the preparation of ultrafine metakaolin, avoiding chemical alkali activators, and constructing a waste heat cascade utilization system.
It has enabled the high-value, large-scale, and green utilization of marine mud, reduced cement consumption and carbon emissions in the building materials industry, enhanced the activity of powder pozzolanics, and improved the density and mechanical properties of cement-based materials.
Smart Images

Figure CN123154651A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of solid waste resource utilization, industrial waste heat recovery and powder deep processing technology, and in particular to a waste heat cascade utilization system and method for preparing ultrafine metakaolin from marine mud calcination. Background Technology
[0002] Dredged marine mud is a major solid waste problem that hinders ecological restoration and engineering construction in coastal areas. Its large volume, the difficulty of centralized disposal, the large land occupation caused by open-air storage, and its high risk of water siltation, soil salinization, and secondary pollution all contribute to its challenges. Currently, the mainstream disposal methods for dredged marine mud are deep-sea dumping, landfilling, low-value brick making, and simple solidification backfilling. These methods result in extremely low resource utilization rates, leading to significant potential resource waste and increasing the burden on ecological and environmental governance.
[0003] The dredged marine mud has a stable mineral composition, mainly enriched in kaolinite-type aluminosilicate minerals, with a total silicon and aluminum oxide content exceeding 80%. Its mineral structure is highly similar to natural kaolin, providing a natural raw material basis for the thermal activation and preparation of highly reactive metakaolin. Metakaolin is a high-quality amorphous volcanic ash active admixture, characterized by a large specific surface area, abundant active sites, and strong hydration reactivity. When incorporated into a cement system, it effectively consumes the cement hydration product calcium hydroxide, continuously generating cementitious products such as hydrated calcium silicate and hydrated calcium aluminate, filling the internal pores of the matrix and significantly improving the density, mechanical strength, and durability of cement-based materials.
[0004] The preparation of metakaolin through calcination activation can achieve high-value resource utilization of dredged marine mud. However, metakaolin powder prepared by a single calcination activation process has a large particle size and insufficient exposure of surface active sites, resulting in limited pozzolanic activity and low cement substitution dosage, making it difficult to improve the added value of marine mud resource utilization. Currently, the preparation of highly active metakaolin mostly relies on chemical alkali activators such as sodium hydroxide and water glass: some technologies use NaOH as a single activator to compound cement to prepare alkali-activated metakaolin materials; others compound diatomaceous earth, metakaolin, and NaOH to prepare metakaolin-based polymer cementitious materials; still others use kaolin tailings, coal gangue, and silt mixed and calcined, followed by the addition of composite chemical admixtures for activation modification. The above-mentioned traditional activation processes generally have drawbacks such as high production costs, strong corrosiveness during construction, easy initiation of alkali-aggregate reactions, and difficulty in large-scale industrial promotion.
[0005] The existing process for preparing metakaolin by calcining solid waste has two major technical pain points: First, the high-temperature flue gas produced by the 700℃ calcination kiln is directly vented into the atmosphere. This flue gas has a high waste heat grade and suffers from significant heat loss, resulting in high overall energy consumption of the system. At the same time, the initial moisture content of the solid waste is high, requiring a separate hot air drying system for the calcination pretreatment stage, which increases fuel consumption and equipment investment, making the process lengthy and the operating cost high. Second, there is currently no waste heat recovery and utilization system specifically designed for the solid waste calcination process, and a green industrialized complete set of processes integrating calcination activation, waste heat utilization, ultrafine mechanical activation, and alkali-free high-admixture modification has not yet been formed. Summary of the Invention
[0006] The purpose of this invention is to provide a waste heat cascade utilization system and method for preparing ultrafine metakaolin from marine mud calcination, so as to overcome the multiple technical defects of the prior art, such as low resource utilization rate of marine mud, high cost of natural metakaolin preparation, strong corrosiveness and poor scalability of traditional alkali activation process, waste of waste heat from calcination flue gas, high energy consumption of wet marine mud pretreatment and drying, and complicated process flow.
[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution: One of the technical solutions of this invention provides a method for the cascade utilization of waste heat from the calcination of marine mud to prepare ultrafine metakaolin, comprising the following steps: (1) The marine mud raw material is fed into a pre-drying equipment for pre-drying treatment to obtain pre-dried marine mud; (2) The pre-dried sea mud is fed into a calcining kiln for calcination to obtain metakaolin clinker; (3) The metakaolin clinker is fed into a steam kinetic energy mill for grinding to obtain ultrafine metakaolin; In step (2), the calcination flue gas generated by the calcination kiln is sent to the waste heat boiler for heat exchange; the waste heat boiler uses the waste heat of the calcination flue gas to produce medium-temperature superheated steam. The medium-temperature superheated steam is fed into the steam kinetic energy mill in step (3) as a power medium; In step (3), the steam kinetic energy mill discharges low-temperature exhaust steam; the low-temperature exhaust steam is sent to the pre-drying equipment in step (1) as a heat source to pre-dry the marine mud raw material.
[0008] The second technical solution of the present invention provides a waste heat cascade utilization system for the preparation of ultrafine metakaolin by calcining marine mud, including a pre-drying machine, a calcining kiln, a waste heat boiler and a steam kinetic energy mill; The material discharge end of the pre-drying machine is connected to the feed end of the calcining kiln; the material discharge end of the calcining kiln is connected to the feed end of the steam kinetic mill; the flue gas outlet of the calcining kiln is connected to the flue gas inlet of the waste heat boiler through an insulated pipe; the steam outlet of the waste heat boiler is connected to the air inlet of the steam kinetic mill; and the exhaust steam outlet of the steam kinetic mill is connected to the heat exchange inlet of the pre-drying machine, forming a closed-loop system for the cascade utilization of materials and waste heat.
[0009] The third technical solution of the present invention provides a composite cementitious powder, comprising ultrafine metakaolin prepared by the above method and cement; wherein the mass fraction of ultrafine metakaolin in the composite cementitious powder is 15~25%, and the mass fraction of cement is 75~85%.
[0010] Compared with the prior art, the present invention has the following beneficial effects: (1) Based on the physicochemical properties, thermal activation mechanism, and mechanochemical activation mechanism of dredged marine mud, this invention innovatively constructs a cascade utilization system for waste heat from calcination flue gas. It utilizes the waste heat from high-temperature calcination flue gas to prepare medium-temperature superheated steam, which drives a steam-powered mill to achieve ultrafine grinding and mechanical activation of metakaolin. No chemical alkali activators are required throughout the process, significantly increasing the cement substitution content of marine mud-based metakaolin. This invention, by optimizing the calcination process and powder blending ratio, develops a low-carbon, low-cost, and high-performance process for preparing marine mud-modified cementitious materials. This enables the high-value, large-scale, and green utilization of marine solid waste, effectively reducing cement consumption and carbon emissions from the building materials industry.
[0011] (2) This invention relies on a calcining kiln to prepare metakaolin from marine mud. The entire process relies on the waste heat of calcining flue gas to achieve reasonable energy gradient matching in the whole process of steam generation, ultrafine grinding and raw material pre-drying, with no energy waste. This invention activates metakaolin through superheated steam supersonic mechanical grinding, which greatly improves the activity of powder volcanic ash. The entire process does not require chemical alkali activators such as sodium hydroxide and water glass, avoiding the defects of traditional processes such as strong corrosion, high risk of alkali-aggregate reaction and high construction difficulty. At the same time, it can give full play to the hydration activity of volcanic ash and the filling effect of micro-aggregates, significantly improving the density, mechanical properties and long-term durability of cement-based materials. Attached Figure Description
[0012] Figure 1 This is a schematic diagram of the waste heat cascade utilization system for preparing ultrafine metakaolin from marine mud calcination according to the present invention. Figure 2 XRD patterns of the ultrafine metakaolin prepared in Examples 1-3; Figure 3 The infrared spectra of the ultrafine metakaolin prepared in Examples 1-3 are shown. Detailed Implementation
[0013] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0014] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0015] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0016] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be obvious to those skilled in the art. This application specification and embodiments are merely exemplary.
[0017] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0018] All raw materials used in this invention can be obtained commercially or prepared using existing technologies.
[0019] This invention uses dredged marine mud as raw material, which is pre-dried and then calcined at a constant temperature in a calcining kiln to prepare metakaolin clinker. The high-temperature flue gas from the calcination is collected and sent to a waste heat boiler to generate medium-temperature superheated steam. Using this superheated steam as the power medium, the metakaolin clinker is ultra-finely ground through a steam kinetic energy mill. After heat exchange during grinding, low-temperature exhaust steam is produced. This low-temperature exhaust steam is used as a heat source to pre-dry the wet marine mud, constructing a production process that utilizes waste heat in a cascade manner and features a dual closed-loop system for material and energy. This invention eliminates the need for external heating, effectively solving the problems of waste heat waste, high energy consumption, and cumbersome processes in traditional marine mud metakaolin preparation. The ground metakaolin exhibits excellent activity and uniform particle size. Furthermore, the highly active metakaolin is compounded with ordinary silicate cement to prepare high-performance composite cementitious powder, which can significantly improve the density and mechanical properties of cement-based materials, achieving low-carbon, high-value, and large-scale utilization of marine solid waste, resulting in significant energy-saving, efficiency-enhancing, and environmental benefits.
[0020] This invention provides a method for the cascade utilization of waste heat from the calcination of marine mud to prepare ultrafine metakaolin, comprising the following steps: (1) The marine mud raw material is fed into a pre-drying equipment for pre-drying treatment to obtain pre-dried marine mud; (2) The pre-dried sea mud is fed into a calcining kiln for calcination to obtain metakaolin clinker; (3) The metakaolin clinker is fed into a steam kinetic energy mill for grinding to obtain ultrafine metakaolin; In step (2), the calcination flue gas generated by the calcination kiln is sent to the waste heat boiler for heat exchange; the waste heat boiler uses the waste heat of the calcination flue gas to produce medium-temperature superheated steam. The medium-temperature superheated steam is fed into the steam kinetic energy mill in step (3) as a power medium; In step (3), the steam kinetic energy mill discharges low-temperature exhaust steam; the low-temperature exhaust steam is sent to the pre-drying equipment in step (1) as a heat source to pre-dry the marine mud raw material.
[0021] The marine mud raw material of this invention needs to be naturally dehydrated, mechanically crushed, and passed through a 60-mesh standard sieve before pre-drying, and then undergoes pre-drying treatment at the school.
[0022] In a preferred embodiment of the present invention, the marine mud raw material is derived from dredged marine mud from the South China Sea coast of Shenzhen, Guangdong.
[0023] Step (2) of this invention is to send the pre-dried sea mud into a calcining kiln for constant temperature calcination to obtain metakaolin clinker. The calcining kiln continuously discharges high-temperature flue gas, and all the flue gas is collected and sent to a waste heat boiler for heat exchange. The waste heat boiler uses the waste heat of the calcining flue gas to produce medium-temperature superheated steam.
[0024] In this invention, the calcination temperature is 690~760℃, for example, it can be 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 750℃ or 760℃, etc., and the time is 1~2h, for example, it can be 1h, 1.5h or 2h.
[0025] In this invention, the temperature of the medium-temperature superheated steam is 260~280℃, for example, 260℃, 270℃ or 280℃, and the pressure is 1.2~1.5MPa, for example, 1.2MPa, 1.3MPa, 1.4MPa or 1.5MPa.
[0026] Step (3) of this invention is to send medium-temperature superheated steam into the steam kinetic mill as the power medium, and send the calcined metakaolin clinker into the steam kinetic mill to achieve ultrafine grinding and uniform mixing of the material. During the grinding process, the low-temperature exhaust steam with a stable discharge temperature is maintained.
[0027] In this invention, the flow velocity of the steam at the outlet of the steam kinetic energy mill nozzle is 900~1000m / s, for example, it can be 900m / s, 920m / s, 940m / s, 950m / s, 960m / s, 980m / s or 1000m / s, etc.
[0028] In this invention, the particle size D50 of the ultrafine metakaolin is ≤5μm.
[0029] In this invention, the temperature of the low-temperature exhaust steam is 140°C.
[0030] In a preferred embodiment of the present invention, all the low-temperature exhaust steam discharged from the steam kinetic energy mill is sent to a pre-drying device as the sole heat source to pre-dry the wet marine mud with high moisture content before it enters the kiln, thereby realizing the cascade utilization of calcination waste heat and the closed-loop circulation of materials and energy.
[0031] The present invention also provides a waste heat cascade utilization system for the preparation of ultrafine metakaolin by calcining marine mud, including a pre-drying machine, a calcining kiln, a waste heat boiler and a steam kinetic energy mill; The material discharge end of the pre-drying machine is connected to the feed end of the calcining kiln; the material discharge end of the calcining kiln is connected to the feed end of the steam kinetic mill; the flue gas outlet of the calcining kiln is connected to the flue gas inlet of the waste heat boiler through an insulated pipe; the steam outlet of the waste heat boiler is connected to the air inlet of the steam kinetic mill; and the exhaust steam outlet of the steam kinetic mill is connected to the heat exchange inlet of the pre-drying machine, forming a closed-loop system for the cascade utilization of materials and waste heat.
[0032] The present invention also provides a composite cementitious powder comprising ultrafine metakaolin prepared by the above method and cement; wherein the mass fraction of ultrafine metakaolin in the composite cementitious powder is 15-25%, for example, it can be 15%, 18%, 20%, 22% or 25%, etc., and the mass fraction of cement is 75-85%, for example, it can be 75%, 80% or 85%, etc.
[0033] In a preferred embodiment of the present invention, the cement is preferably P.O42.5 ordinary Portland cement.
[0034] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0035] This invention utilizes dredged marine mud from the South China Sea coast of Shenzhen, Guangdong Province, and P.O42.5 ordinary Portland cement as the cementitious substrate. The chemical compositions of the marine mud and cement are shown in the table below: Table 1 Chemical composition (wt%) of marine mud and cement
[0036] Example 1 (1) The dredged marine mud is naturally dehydrated, mechanically crushed, passed through a 60-mesh standard sieve, and dried to obtain pre-treated marine mud raw material.
[0037] (2) The dried and pretreated marine mud raw material is sent into the calcining kiln, the kiln temperature is stably controlled at 700±10℃, and constant temperature calcination is carried out for 1 hour. The calcining kiln continuously discharges high temperature flue gas, and all flue gas is collected and sent to the waste heat boiler for heat exchange. (3) The waste heat boiler utilizes the waste heat of calcination flue gas to stably produce medium-temperature superheated steam; the medium-temperature superheated steam at 270℃ and 1.3MPa is sent into the steam kinetic energy mill, and the steam flow rate at the nozzle outlet is controlled at 950m / s. After grinding, the ultrafine highly active metakaolin powder with D50≤5μm is collected in stages; after grinding and heat exchange, the low-temperature exhaust steam at 140℃ is stably discharged. (4) Closed-loop pre-drying of wet marine mud: All the low-temperature exhaust steam at 140℃ is sent into the indirect dryer to dry the wet marine mud to be calcined with an initial moisture content of 40%. After drying, the marine mud is sent into the calcining kiln.
[0038] Example 2 (1) The pretreatment process for marine mud is the same as in Example 1; (2) The pretreated marine mud is sent into the calcining kiln, the kiln temperature is stably controlled at 750±10℃, and constant temperature calcination is carried out for 1 hour. The calcining kiln continuously discharges high temperature flue gas, and all flue gas is collected and sent to the waste heat boiler for heat exchange. (3) The waste heat boiler utilizes the waste heat of calcination flue gas to stably produce medium-temperature superheated steam; the 1.5MPa, 280℃ medium-temperature superheated steam is sent into the steam kinetic energy mill, and the steam flow rate at the nozzle outlet is controlled at 1000m / s. After grinding, the ultrafine highly active metakaolin powder with D50≤5μm is collected in stages; after grinding and heat exchange, the low-temperature exhaust steam at 140℃ is stably discharged. (4) Closed-loop pre-drying of wet marine mud: All the low-temperature exhaust steam at 140℃ is sent into the indirect dryer to dry the wet marine mud to be calcined with an initial moisture content of 40%. After drying, the marine mud is sent into the calcining kiln.
[0039] Example 3 (1) The pretreatment process for marine mud is the same as in Example 1; (2) The pretreated marine mud is sent into the calcining kiln, the kiln temperature is stably controlled at 720±10℃, and constant temperature calcination is carried out for 2 hours. The calcining kiln continuously discharges high temperature flue gas, and all flue gas is collected and sent to the waste heat boiler for heat exchange. (3) The waste heat boiler utilizes the waste heat of calcination flue gas to stably produce medium-temperature superheated steam; the 1.2MPa, 260℃ medium-temperature superheated steam is sent into the steam kinetic energy mill, and the steam flow rate at the nozzle outlet is controlled to be 900m / s. After grinding, the ultrafine highly active metakaolin powder with D50≤5μm is collected in stages; after grinding and heat exchange, the low-temperature exhaust steam at 140℃ is stably discharged. (4) Closed-loop pre-drying of wet marine mud: All the low-temperature exhaust steam at 140℃ is sent into the indirect dryer to dry the wet marine mud with an initial moisture content of 40% to be calcined. After drying, the marine mud is sent into the calcining kiln.
[0040] Comparative Example 1 The preparation process of metakaolin based on marine mud adopted industry standard: constant temperature calcination in a calcining kiln combined with dry grinding in a traditional ball mill, without waste heat recovery, steam heat exchange, or closed-loop drying system for exhaust steam. The experimental raw materials, marine mud pretreatment method, calcination temperature, calcination time, gelling ratio, water-cement ratio, molding and curing conditions were completely consistent with those in Example 1, only the grinding equipment was changed and all waste heat utilization steps were eliminated.
[0041] (1) The same batch of dredged marine mud was naturally dehydrated, mechanically crushed, screened with a 60-mesh sieve, and dried to obtain the same dry pretreated marine mud raw material.
[0042] (2) The dried marine mud is fed into the calcining kiln and calcined at a constant temperature of 700±10℃ for 1 hour. The high-temperature flue gas from the calcination is directly discharged into the air without waste heat recovery or heat exchange.
[0043] (3) After calcination, the marine mud clinker was dry-ground for 30 minutes using a traditional ball mill to obtain ordinary marine mud metakaolin powder.
[0044] (4) The wet marine mud with an initial moisture content of 40% is dried independently using an external electric heating device, relying entirely on external energy consumption and without utilizing process waste heat.
[0045] Application Example 1 The ultrafine marine mud-based metakaolin prepared in Example 1 was uniformly mixed with ordinary silicate cement at a mass ratio of 20%:80% to prepare composite cementitious powder; the water-cement ratio was fixed at 0.4, water was added and stirred evenly, and then the mixture was placed into a 40mm×40mm×160mm mortar mold and vibrated to compact it; after being left to cure at room temperature for 1 day, the mold was removed and then transferred to a standard curing box for curing for 28 days.
[0046] The test results show that the alkali-free modified cement-based mortar prepared in this embodiment has a 28-day compressive strength of 43.82 MPa and a 28-day flexural strength of 9.22 MPa.
[0047] Application Example 2 The ultrafine marine mud-based metakaolin prepared in Example 2 was uniformly mixed with ordinary silicate cement at a mass ratio of 25%:75% to prepare composite cementitious powder. The water-cement ratio was fixed at 0.4. After adding water and stirring evenly, the mixture was placed into a 40mm×40mm×160mm mortar mold and vibrated to compact it. After being left to cure at room temperature for 1 day, the mold was removed and then transferred to a standard curing box for curing for 28 days.
[0048] The test results show that the alkali-free modified cement-based mortar prepared in this embodiment has a 28-day compressive strength of 41.45 MPa and a 28-day flexural strength of 9.06 MPa.
[0049] Application Example 3 The ultrafine marine mud-based metakaolin prepared in Example 3 was uniformly mixed with ordinary silicate cement at a mass ratio of 15%:85% to prepare composite cementitious powder. The water-cement ratio was fixed at 0.4. After adding water and stirring evenly, the mixture was placed into a 40mm×40mm×160mm mortar mold and vibrated to compact it. After being left to cure at room temperature for 1 day, the mold was removed and then transferred to a standard curing box for curing for 28 days.
[0050] The test results show that the alkali-free modified cement-based mortar prepared in this embodiment has a 28-day compressive strength of 42.89 MPa and a 28-day flexural strength of 9.13 MPa.
[0051] Application Example 4 The finely ground marine mud-based metakaolin prepared in Comparative Example 1 was uniformly mixed with ordinary silicate cement at a mass ratio of 20%:80% to prepare composite cementitious powder. The water-cement ratio was fixed at 0.4. After adding water and stirring evenly, the powder was placed into a 40mm×40mm×160mm mortar mold and vibrated to compact it. After being cured at room temperature for 1 day, the powder was demolded and then transferred to a standard curing box for curing for 28 days.
[0052] The test results show that the alkali-free modified cement-based mortar prepared in this embodiment has a 28-day compressive strength of 39.1 MPa and a 28-day flexural strength of 8.24 MPa.
[0053] (1) Comparison of waste heat utilization rate: The overall waste heat utilization rate of the waste heat cascade utilization process of the present invention can reach 82.7%; the traditional calcination + ball mill process in Comparative Example 1 has no waste heat recovery measures and the waste heat utilization rate is 0%.
[0054] (2) Effect of reducing flue gas temperature: The flue gas temperature directly discharged in Comparative Example 1 is about 600℃; after the waste heat is utilized in stages, the final flue gas temperature of this invention is reduced to 180-200℃, which is more than 400℃ lower than the flue gas temperature of the traditional process.
[0055] (3) Heat consumption rate reduction effect: The comprehensive heat consumption of a unit product in Comparative Example 1 is 1350kJ / kg; the comprehensive heat consumption of a unit product in this invention is only 420kJ / kg, which is about 70% lower than that of traditional process.
[0056] (4) Carbon emission reduction effect: Comparative Example 1 relies on external electric heating, independent heating and high energy consumption ball milling, resulting in high carbon emissions; This invention replaces external energy consumption with waste heat closed loop, and CO2 emissions can be reduced by 0.4t per ton of metakaolin powder, with a carbon emission reduction rate of 64% compared with the traditional calcination + ball mill process.
[0057] Compared to the traditional "calcining kiln + ball mill" process, this invention utilizes a tiered utilization system that combines waste heat from calcination flue gas to generate steam, steam kinetic energy for ultrafine grinding, and low-temperature exhaust steam closed-loop pre-drying. This system achieves ultrafine powder production and enhanced powder activity, significantly improving the compressive and flexural mechanical properties of cement-based mortar. Furthermore, it substantially recovers process waste heat, reduces flue gas heat loss, and decreases overall system energy consumption and carbon emissions. This addresses the technical shortcomings of traditional processes, such as severe waste of waste heat, high grinding energy consumption, poor powder activity, low mechanical properties of finished products, and high carbon emissions.
[0058] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for the cascade utilization of waste heat from the calcination of marine mud to prepare ultrafine metakaolin, characterized in that, Includes the following steps: (1) The marine mud raw material is fed into a pre-drying equipment for pre-drying treatment to obtain pre-dried marine mud; (2) The pre-dried sea mud is fed into a calcining kiln for calcination to obtain metakaolin clinker; (3) The metakaolin clinker is fed into a steam kinetic energy mill for grinding to obtain ultrafine metakaolin; In step (2), the calcination flue gas generated by the calcination kiln is sent to the waste heat boiler for heat exchange; the waste heat boiler uses the waste heat of the calcination flue gas to produce medium-temperature superheated steam. The medium-temperature superheated steam is fed into the steam kinetic energy mill in step (3) as a power medium; In step (3), the steam kinetic energy mill discharges low-temperature exhaust steam; the low-temperature exhaust steam is sent to the pre-drying equipment in step (1) as a heat source to pre-dry the marine mud raw material.
2. The method for the cascade utilization of waste heat from the calcination of marine mud to prepare ultrafine metakaolin, as described in claim 1, is characterized in that... The calcination temperature is 690~760℃, and the time is 1~2h.
3. The method for the cascade utilization of waste heat from the calcination of marine mud to prepare ultrafine metakaolin, as described in claim 1, is characterized in that... The temperature of the medium-temperature superheated steam is 260~280℃, and the pressure is 1.2~1.5MPa.
4. The method for the cascade utilization of waste heat from the calcination of marine mud to prepare ultrafine metakaolin, as described in claim 1, is characterized in that... The steam velocity at the nozzle outlet of the steam kinetic energy mill is 900~1000m / s.
5. The method for the cascade utilization of waste heat from the calcination of marine mud to prepare ultrafine metakaolin, as described in claim 1, is characterized in that... The particle size D50 of the ultrafine metakaolin is ≤5μm.
6. The method for the cascade utilization of waste heat from the calcination of marine mud to prepare ultrafine metakaolin, as described in claim 1, is characterized in that... The temperature of the low-temperature exhaust steam is 140°C.
7. A waste heat cascade utilization system for the preparation of ultrafine metakaolin from marine mud calcination, characterized in that, This includes pre-drying machines, calcining kilns, waste heat boilers, and steam kinetic energy mills; The material discharge end of the pre-drying machine is connected to the feed end of the calcining kiln; the material discharge end of the calcining kiln is connected to the feed end of the steam kinetic mill; the flue gas outlet of the calcining kiln is connected to the flue gas inlet of the waste heat boiler through an insulated pipe; the steam outlet of the waste heat boiler is connected to the air inlet of the steam kinetic mill; and the exhaust steam outlet of the steam kinetic mill is connected to the heat exchange inlet of the pre-drying machine, forming a closed-loop system for the cascade utilization of materials and waste heat.
8. A composite gelling powder, characterized in that, The composite cementitious powder comprises ultrafine metakaolin prepared by any one of claims 1 to 6 and cement; wherein the mass fraction of ultrafine metakaolin in the composite cementitious powder is 15 to 25%, and the mass fraction of cement is 75 to 85%.