Titanium slag electric furnace collapse pre-pressure relief coordinated regulation method

By combining zoned controllable gas injection and slag viscosity detection with electric furnace power regulation, the safety issues caused by pressure buildup in the material layer during titanium slag electric furnace smelting were resolved, achieving stable furnace pressure control and equipment protection throughout the process.

CN123154657APending Publication Date: 2026-11-24PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611576529.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the process of titanium slag electric furnace smelting, the increase in material layer thickness leads to an increase in internal pressure, which can easily cause material collapse and instantaneous release of high-pressure gas, resulting in safety and environmental problems such as flue gas leakage and furnace cover impact. Existing technologies cannot effectively prevent these issues, and fixed parameter injection leads to equipment wear and tear.

Method used

The technology of zoned controllable gas injection is adopted. The injection points and pressures are set at different stages according to the material accumulation characteristics in the furnace. Combined with slag viscosity detection and electric furnace power control, segmented injection and full-area enhanced injection are carried out, and the injection parameters are dynamically adjusted to achieve orderly release of gas in the material layer and improve slag fluidity.

Benefits of technology

It significantly smooths out furnace pressure fluctuations throughout the entire smelting cycle, avoids instantaneous overpressure and flue gas leakage caused by material collapse, reduces equipment wear, and achieves stable production throughout the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123154657A_ABST
    Figure CN123154657A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of titanium slag electric arc furnace (EAF) smelting process control technology. It discloses a collaborative control method for pre-pressure relief of titanium slag EAF material collapse. Based on a collaborative system of zoned controllable gas injection in the furnace cover, integrated molten slag viscosity detection, and adaptive EAF power control, the method sequentially completes the configuration and location of zoned injection system parameters, pre-pressure relief in the early stage of smelting, pressure stabilization and control in the middle stage of smelting, and pre-pressure relief before slag removal in the later stage of smelting. Simultaneously, molten slag viscosity detection and adaptive EAF power adjustment are carried out throughout the entire smelting cycle. This method eliminates the potential for gas accumulation and pressure buildup in the material layer through segmented active injection, and combines molten slag state monitoring and dynamic power matching to clear gas escape channels, thus preventing sudden increases in furnace pressure and flue gas leakage caused by material collapse from the source.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium slag electric furnace smelting process control technology, specifically relating to a method for coordinated control of pre-pressure relief in titanium slag electric furnace smelting. Background Technology

[0002] Titanium slag electric arc furnaces generally employ a closed-loop continuous feeding smelting process. During smelting, materials continuously accumulate inside the furnace, easily forming an elevated, bulging structure that traps large amounts of reactive gases such as CO and CO2. As the material layer thickness increases, the internal pressure rises continuously. In the event of a large-scale collapse, the instantaneous release of high-pressure gases can cause a sudden surge in furnace pressure, leading to safety and environmental problems such as flue gas leakage and furnace cover impact. Traditional production methods primarily rely on passive pressure relief after a collapse, failing to address the underlying gas accumulation hazard and resulting in delayed prevention and control.

[0003] Existing in-furnace injection or pressure relief technologies mostly employ uniformly arranged injection points and fixed pressure parameters. They fail to consider the differences in material layer thickness and slag agglomeration at different smelting stages of titanium slag electric furnaces, resulting in insufficient targeted control of the thick central material layer and slag around the electrodes. This makes it difficult to effectively break down the deep, suspended gas storage structure, leading to limited overall pressure relief. Furthermore, injection with fixed parameters easily causes airflow erosion and loss between the electrodes and the furnace lining, affecting equipment lifespan.

[0004] Slag viscosity is a key parameter affecting the rate of gas escape from the furnace, directly related to the degree of gas accumulation in the material bed and the risk of material collapse. Existing control methods lack a coordinated linkage mechanism between slag viscosity, electric furnace power, and injection pressure relief process, making it impossible to dynamically adjust smelting conditions according to slag fluidity. Gas escape channels are easily blocked due to excessively high slag viscosity, making it difficult to achieve stable furnace pressure control throughout the entire smelting cycle. Summary of the Invention

[0005] To address the aforementioned problems, this invention provides a method for coordinated control of pre-pressure relief in titanium slag electric furnace collapse, comprising the following steps: Based on the furnace type, capacity, feeding structure and material accumulation characteristics inside the furnace, inter-phase injection points are arranged on the furnace cover, directly facing the central thick layer of material accumulation area, and edge injection points are arranged close to the electrodes. The gas injection pressure is set respectively, and the inter-phase injection pressure is higher than the edge injection base pressure. After continuous feeding in the early stage of smelting, feeding is stopped, and inter-phase injection and edge injection are started simultaneously to break up the initial suspended material and disperse the surface accumulated powder, release the accumulated gas, and resume feeding after the injection is completed. During the middle of smelting, feeding was stopped again, and intermittent multi-round segmented blowing was carried out to penetrate the thickened central material layer and break up the slag and agglomeration around the electrodes. The interval between rounds was dynamically adjusted according to the furnace pressure feedback, and the deep-accumulated gas was released in layers. After all the materials have been added, stop adding materials and carry out full-area enhanced injection. After the injection is completed, allow a buffer period and wait for the gas to escape steadily and the furnace pressure to be stable before slag removal. Simultaneously, in-situ sampling and temperature measurement of molten slag are carried out throughout the entire smelting cycle. The viscosity of the sample is detected at the measured temperature. Based on the measured molten slag viscosity, if the molten slag temperature is too low, the fluidity is poor, and the gas escape channel is blocked, the electric furnace power is automatically increased to improve the molten pool temperature and the fluidity of the molten slag, and to clear the gas escape channel. This is coordinated with the segmented blowing to regulate the furnace working conditions.

[0006] Preferably, the arrangement of the injection points includes: retaining the original central feeding point on the furnace cover and the corresponding circumferential main feeding point of the electrode, and arranging the intermittent injection points at the gap position between adjacent circumferential main feeding points; arranging the edge injection points according to the furnace type and capacity, with small and medium-sized electric furnaces arranging edge injection points on one side of each electrode, and large electric furnaces arranging edge injection points symmetrically on the left and right sides of each electrode.

[0007] Preferably, both the interphase injection points and the edge injection points are injection pipes that extend into the inside of the furnace cover. Anti-clogging atomizing nozzles are configured at the ends of the injection pipes, and the vertical height of the injection pipes is dynamically adjusted according to the real-time material level to avoid the nozzles being buried and blocked, and to prevent the injection airflow from scouring the furnace lining and electrodes.

[0008] Preferably, the setting of the gas injection pressure includes: using independent pressure stabilization for the interphase injection pipeline and the edge injection pipeline respectively, setting the interphase injection working pressure to penetrate the central thick material layer, and setting the edge injection working pressure to be independently adjustable, thereby increasing the edge injection pressure under abnormal operating conditions to enhance the injection effect.

[0009] Preferably, the pre-smelting injection includes: immediately after stopping feeding, simultaneously starting interphase injection and edge injection, using the high-pressure airflow of interphase injection to impact the central material layer and penetrate the initially formed slightly suspended material structure, releasing the carbon monoxide and carbon dioxide reaction gases accumulated in the material layer in advance; using edge injection to disperse the accumulated powder around the electrodes and on the furnace wall surface to avoid local suspension; and resuming normal feeding after completing the initial pre-depressurization.

[0010] Preferably, the intermittent multi-stage segmented blowing during the smelting process includes: maintaining the interphase blowing working pressure to continuously penetrate the thickened central material layer and release the deep-accumulated gas in layers; increasing the edge blowing pressure according to the degree of slag and agglomeration around the electrode to strengthen crushing and clean the slag and floating material around the electrode; setting an interval that is dynamically adjusted according to the furnace pressure feedback between adjacent cycles, and gradually dissipating the gas accumulation in the material layer through multiple intermittent blowing cycles to avoid a sudden rise in furnace pressure caused by concentrated gas release.

[0011] Preferably, the full-area enhanced injection and slag removal includes: simultaneously activating all interphase injection points and edge injection points to break the residual overhead gas storage layer and release the trapped gas trapped in the layer; after the injection is completed, allowing the gas to escape smoothly and the furnace pressure to drop back to a stable range during the buffer period; and starting the slag removal operation after confirming that the buffer period has ended and the furnace pressure is stable without fluctuations.

[0012] Preferably, the in-situ sampling, temperature measurement, and viscosity detection of the molten slag includes: obtaining a sample of the molten slag inside the furnace through a sampling hole independently set on the furnace cover and not interfering with the electrode hole and the charging hole; simultaneously acquiring the actual temperature of the molten pool using a thermal imaging device during the sampling process; and performing a viscosity test on the obtained molten slag sample at the actual temperature of the molten pool to obtain the measured viscosity of the molten slag.

[0013] Preferably, the electric furnace power control includes: presetting a standard slag viscosity adaptation range for titanium slag smelting; when the measured slag viscosity is in the viscosity range that characterizes low slag temperature and poor fluidity, it is determined that the gas escape channel is obstructed, and the electric furnace working power is increased based on the electric furnace benchmark working power before adjustment. The slag fluidity is improved by increasing the molten pool temperature, so that the slag viscosity is stabilized within the standard slag viscosity adaptation range, and the reaction gas is released smoothly by segmented injection.

[0014] Preferably, the titanium slag electric furnace is a large titanium slag electric furnace, with a dedicated sampling and testing hole independently set on its furnace cover as the sampling hole, and a sealing lifting mechanism configured for the dedicated sampling and testing hole.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: Targeting the characteristics of the material layer and gas storage features in the pre-smelting, middle-smelting, and late-stage processes, we adopted full-area injection, intermittent segmented injection, and full-area enhanced injection modes, respectively, combined with differential pressure parameters between phases and edges, to precisely break up the overhead material and slag agglomerates at different levels, release the accumulated gas in a layered and orderly manner, significantly smooth out furnace pressure fluctuations throughout the smelting cycle, and avoid instantaneous overpressure and flue gas leakage caused by concentrated material collapse.

[0016] By using in-situ sampling and temperature measurement to match viscosity detection, the true fluidity of the molten slag is accurately reflected. Combined with adaptive adjustment of the electric furnace power within the viscosity range, the molten pool temperature is increased to improve the molten slag condition, clear the gas escape channels, and form a synergistic effect with the segmented injection and depressurization process, thus stabilizing the furnace conditions from both the material state and process operation aspects.

[0017] The number and layout of injection points are designed for large, medium and small titanium slag electric furnaces, and the corresponding working pressure and injection duration are matched. The height of the injection pipe can be dynamically adjusted according to the material surface. While ensuring the pressure relief effect, it reduces the scouring and loss of the airflow on the electrodes and furnace lining, and adapts to the continuous and stable production needs of electric furnaces of different capacities. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0019] Figure 1 This is the overall flow of the method of the present invention. Detailed Implementation

[0020] The present invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention. The present invention relates to a coordinated control method for pre-decompression of titanium slag electric furnace material collapse. This method is based on a coordinated system of controllable gas injection in furnace cover zones, integrated molten slag viscosity detection, and adaptive control of electric furnace power. It takes active injection and decompression in stages throughout the smelting cycle as the core, combined with real-time monitoring of molten slag status and dynamic power matching, to preemptively eliminate the hidden dangers of gas accumulation and pressure buildup in the material layer, and avoid sudden rise in furnace pressure and flue gas leakage caused by material collapse from the source.

[0021] The method sequentially executes the following steps according to the smelting time sequence: pre-setting of the injection system, pre-pressure relief in the early stage of smelting, pressure stabilization and control in the middle stage of smelting, and pre-pressure relief before slag discharge in the later stage of smelting. Simultaneously, slag viscosity detection and adaptive linkage adjustment of electric furnace power are carried out throughout the entire smelting cycle, forming a closed-loop active control process of pre-pressure relief, operating condition monitoring, and parameter adaptation.

[0022] refer to Figure 1 The specific control steps of the method are as follows: Step 1: Configure and deploy the parameters of the zoned jet purging system. This step is the preparatory stage for pre-pressure relief control. Based on the furnace type, capacity, charging structure, and material accumulation characteristics of the titanium slag electric furnace, zoned controllable gas injection components are installed on the furnace cover and operating parameters are set. The specific configuration is as follows: Point layout: The furnace cover retains the original 1 central charging point and 3 corresponding circular main charging points for the electrodes; 3 alternating blowing points are arranged in the gaps between adjacent main charging points, directly facing the thick layer of material accumulation area in the center of the furnace; edge blowing points are arranged on both sides of the electrodes, totaling 3 to 6, arranged close to the electrodes. Among them, small and medium-sized electric furnaces use 1 point on each side of each electrode, for a total of 3 edge blowing points, while large electric furnaces use symmetrically arranged edge blowing points on both sides of each electrode, for a total of 6 edge blowing points.

[0023] Structural parameters: All injection pipes extend 5 to 10 cm inside the furnace cover, with anti-clogging atomizing nozzles at the ends to prevent blockage by high-temperature dust inside the furnace; the vertical height of the injection pipes can be dynamically adjusted according to the real-time material level to avoid nozzle clogging and airflow scouring of the furnace lining and electrodes. The interphase injection pipes and the edge injection pipes adopt two independent pressure-stabilized gas supply lines.

[0024] Operating parameters preset: The interphase blowing working pressure is preset to 0.6 to 0.8 MPa, which is used to penetrate the thick central material layer; the edge blowing working pressure is preset to 0.3 to 0.5 MPa, and the pressure is independently adjustable. Under abnormal working conditions, the pressure can be increased to enhance the blowing effect; the duration of a single uniform blowing is controlled to 20 to 40 seconds.

[0025] Step 2, Pre-pressure relief control during the early stage of smelting: After continuous feeding and smelting for 3 to 4 hours, feeding should be stopped, and differentiated injection operations should be started immediately to break up the slight overhang of materials in the early stage of smelting and release the accumulated gas in advance. The specific operation is as follows: Simultaneous start of interphase injection and edge injection: Interphase injection uses a high-pressure airflow of 0.6 to 0.8 MPa to impact the central material layer, penetrate the slightly open material structure formed in the early stage of smelting, release the CO and CO2 reaction gases accumulated in the material layer in advance, and avoid the continuous accumulation of materials to form a closed gas cavity. Edge blowing uses a pressure of 0.3 to 0.5 MPa to blow the floating material around the electrode and on the surface of the furnace wall, breaking up the powder accumulated on the surface and avoiding local voids; The duration of a single injection is controlled to be 20 to 40 seconds. After the initial pre-pressure relief is completed, normal feeding is resumed to stabilize the furnace pressure conditions in the initial stage of smelting.

[0026] Step 3, Mid-term pressure stabilization and control during smelting: After 6 to 7 hours of continuous smelting, feeding is stopped again, and intermittent, segmented blowing is implemented to gradually break up the thickened material layer and slag agglomerates, release accumulated gas evenly, and stabilize furnace pressure fluctuations. The specific operation is as follows: The intermittent multi-round segmented injection mode is adopted, with each round of injection lasting 20 to 40 seconds, and the interval between rounds is dynamically adjusted according to furnace pressure feedback; The intermittent injection maintains a working pressure of 0.6 to 0.8 MPa, continuously penetrating the central material layer that continues to thicken during the smelting process, and releasing the gas accumulated deep inside the furnace in layers; Edge blowing can appropriately increase the pressure according to the degree of slag and agglomeration around the electrode to enhance the crushing and blowing effect and clean up the slag and floating material around the electrode; By gradually dissipating the gas buildup in the material layer through multiple rounds of intermittent injection, the sudden increase in furnace pressure caused by concentrated release is avoided, thereby reducing the pressure fluctuation amplitude throughout the smelting cycle.

[0027] Step 4: Pressure relief and regulation before slag removal in the later stage of smelting: After all feeding is completed, feeding is stopped, and a final pre-blowing is carried out across the entire area. A buffer is reserved to allow the gas to escape smoothly before slag discharge, thus preventing material collapse and explosive surging during the slag discharge stage from the root. The specific operation is as follows: At the same time, all interphase injection points and edge injection points are activated to carry out full-area enhanced injection, completely break the residual overhead gas storage material layer in the furnace, and fully release the trapped gas trapped in the material layer. After the injection operation is completed, allow a buffer period of 20 to 30 minutes to allow the gas trapped inside the furnace to escape fully and smoothly, and for the furnace pressure to drop back to a stable range. After confirming that the buffer period has ended and the furnace pressure is stable and without fluctuations, the slag removal operation can be started to avoid large-scale instantaneous material collapse and high-pressure gas explosion caused by slag removal disturbance.

[0028] The method of this invention performs full-cycle slag viscosity detection and adaptive power control: Throughout the entire smelting cycle, in-situ sampling, temperature measurement, and viscosity testing of the molten slag are performed simultaneously. Based on the test results, the electric furnace power is adaptively adjusted to improve the molten slag fluidity. This, combined with a segmented pressure relief process, achieves coordinated and stable operating conditions. The specific operations are as follows: Integrated sampling and temperature measurement: In-situ molten slag sampling inside the furnace is completed through a sampling hole independently set on the furnace cover. This sampling hole does not interfere with functional holes such as electrode holes and charging holes. During the sampling process, thermal imaging equipment is used to collect the real temperature of the molten pool to ensure that the temperature of the sampled molten slag is completely consistent with the actual working conditions inside the furnace.

[0029] Viscosity testing: The obtained slag sample was subjected to viscosity testing at the above-mentioned measured temperature to obtain the measured slag viscosity. This avoids viscosity measurement deviations caused by temperature differences.

[0030] Viscosity Standard and Judgment: The system presets the standard viscosity range for titanium slag smelting as follows:

[0031] This refers to the standard slag viscosity for titanium slag smelting, expressed in millipascals per second (mPa). s). When the measured viscosity of the molten slag At 120–200 mPa When the temperature is in the s range, it is determined that the slag temperature is too low, the fluidity is poor, and the gas escape channel is not smooth.

[0032] Power adaptive adjustment: The system automatically increases the working power of the electric furnace by 10% to 20%, and the adjusted furnace power meets the following requirements:

[0033] The adjusted working power of the electric furnace is expressed in kilowatts (kW). The reference operating power of the electric furnace before adjustment is expressed in kilowatts (kW). This is the power enhancement factor, ranging from 10% to 20%.

[0034] Synergistic control logic: By increasing the power of the electric furnace to raise the temperature of the molten pool, improve the fluidity of the molten slag, clear the gas escape channels in the furnace, ensure the stable release of reaction gases, and stabilize the viscosity of the molten slag within the standard range, it works in synergy with the segmented injection and depressurization process to jointly stabilize the working conditions inside the furnace.

[0035] Example 1: This example is for a 25000kVA small-to-medium-sized titanium slag electric arc furnace, which has the characteristics of thin material layer, light slag buildup, and small fluctuations in operating conditions. The control is implemented according to the above steps, and the specific parameters are as follows: Step 1 parameter configuration: Set up 3 interphase blowing points and 3 edge blowing points, and set 1 edge blowing point on one side of each electrode; the interphase blowing working pressure is 0.7MPa, and the edge blowing base pressure is 0.4MPa; the blowing pipe extends 7cm out of the inside of the furnace cover, and the nozzle can be vertically raised and lowered; the duration of a single blowing is 30s.

[0036] Step 2: Pre-smelting control: After continuous feeding for 3.5 hours, stop feeding and start full-area blowing for 30 seconds to disperse the surface powder and break up the initial slight gas accumulation.

[0037] Step 3 Mid-term smelting control: After 6.5 hours of continuous smelting, stop feeding and adopt intermittent segmented spraying with an interval of 1-2 times. If the furnace condition is abnormal, such as frequent collapse, it is recommended to stop feeding and spraying to break up the thickened material layer and slight slag agglomeration, and release the accumulated gas evenly to stabilize the furnace pressure.

[0038] Step 4: Post-smelting control: After all the materials have been added, carry out full-area pre-injection. After the injection is completed, allow a 25-minute buffer period. After the furnace gas has been released stably, proceed with the slag removal operation.

[0039] Linked control: The furnace cover has a dedicated viscosity probe mounting hole, equipped with a sealing lifting sleeve; thermal imaging equipment is used simultaneously to collect the actual temperature of the molten pool, and viscosity detection is performed based on the temperature; the preset standard range for molten slag viscosity is 80 to 120 mPa. s, when the measured viscosity is greater than 150 mPa When the time reaches s, the power of the electric furnace is automatically increased.

[0040] This embodiment can achieve uniform pre-collapse of the furnace charge and orderly gas release in layers, reducing furnace pressure fluctuations compared to traditional processes, ensuring stable furnace pressure throughout the smelting process, eliminating sudden increases in furnace pressure and flue gas overflow during slag discharge, and reducing electrode and furnace lining erosion losses.

[0041] Example 2: This example is for a 35000kVA large titanium slag electric arc furnace, which has the characteristics of thick material layer, severe slag agglomeration, large gas storage capacity in the furnace, and drastic furnace pressure fluctuations. The control is implemented according to the above steps, and the specific parameters are as follows: Step 1 parameter configuration: Set up 3 interphase injection points and 6 edge injection points, with edge injection points symmetrically arranged on both sides of each electrode; increase the working pressure of interphase injection to 0.8MPa, and the basic pressure of edge injection to 0.5MPa, which can be flexibly increased according to the slag adhesion situation; extend the injection pipe 8cm inside the furnace cover, and increase the lifting stroke of the nozzle; the duration of a single injection is 35s.

[0042] Step 2: Pre-smelting control: After continuous feeding for 3 to 4 hours, stop feeding, start full-area blowing, quickly disperse the thick surface material, break up the initial suspended material, and avoid rapid gas accumulation to form high-pressure cavities.

[0043] Step 3 Mid-term control of smelting: After smelting for 6 to 7 hours, stop feeding and use high-frequency intermittent segmented injection to gradually break up and thicken the central material layer and heavy slag agglomerates, and release the accumulated high-pressure gas in a balanced and slow manner to suppress violent furnace pressure fluctuations.

[0044] Step 4: Post-smelting control: After the feeding is completed, carry out full-area enhanced pre-injection to completely eliminate the deep overhead gas storage layer; after the injection is completed, reserve a buffer time of 25 to 30 minutes, and start the slag removal operation after the gas in the furnace has fully and steadily escaped.

[0045] Linked control: The furnace cover is equipped with a dedicated sampling and testing hole, and a large-stroke sealing lifting mechanism; high-precision thermal imaging equipment is used simultaneously to collect the actual temperature of the molten pool, and viscosity testing is performed according to the temperature; the preset standard range for molten slag viscosity is 80 to 120 mPa. s, when the measured viscosity is greater than 180 mPa When the time reaches s, the power of the electric furnace is automatically increased.

[0046] This embodiment can achieve uniform pre-collapse of thick material layers, complete removal of slag agglomeration, no instantaneous overpressure peaks, no concentrated material collapse, no sudden rise in furnace pressure, and continuous compliance of flue gas emissions, making it suitable for the high-load continuous production needs of large titanium slag electric furnaces.

Claims

1. A method for collaborative regulation of pre-discharge pressure of collapsed material of a titanium slag electric furnace, characterized in that, Includes the following steps: Based on the furnace type, capacity, feeding structure and material accumulation characteristics inside the furnace, inter-phase injection points are arranged on the furnace cover, directly facing the central thick layer of material accumulation area, and edge injection points are arranged close to the electrodes. The gas injection pressure is set respectively, and the inter-phase injection pressure is higher than the edge injection base pressure. After continuous feeding in the early stage of smelting, feeding is stopped, and inter-phase injection and edge injection are started simultaneously to break up the initial suspended material and disperse the surface accumulated powder, release the accumulated gas, and resume feeding after the injection is completed. During the middle of smelting, feeding was stopped again, and intermittent multi-round segmented blowing was carried out to penetrate the thickened central material layer and break up the slag and agglomeration around the electrodes. The interval between rounds was dynamically adjusted according to the furnace pressure feedback, and the deep-accumulated gas was released in layers. After all the materials have been added, stop adding materials and carry out full-area enhanced injection. After the injection is completed, allow a buffer period and wait for the gas to escape steadily and the furnace pressure to be stable before slag removal. Simultaneously, in-situ sampling and temperature measurement of molten slag are carried out throughout the entire smelting cycle. The viscosity of the sample is detected at the measured temperature. Based on the measured molten slag viscosity, if the molten slag temperature is too low, the fluidity is poor, and the gas escape channel is blocked, the electric furnace power is automatically increased to improve the molten pool temperature and the fluidity of the molten slag, and to clear the gas escape channel. This is coordinated with the segmented blowing to regulate the furnace working conditions.

2. The method according to claim 1, characterized in that, The arrangement of the injection points includes: retaining the original central feeding point on the furnace cover and the corresponding circumferential main feeding point of the electrode, and arranging the inter-phase injection points at the gap position between adjacent circumferential main feeding points; arranging the edge injection points according to the furnace type and capacity, with small and medium-sized electric furnaces arranging edge injection points on one side of each electrode, and large electric furnaces arranging edge injection points symmetrically on the left and right sides of each electrode.

3. The method according to claim 1, characterized in that, Both the interphase injection points and the edge injection points adopt injection pipes that extend into the inside of the furnace cover. Anti-clogging atomizing nozzles are configured at the ends of the injection pipes, and the vertical height of the injection pipes is dynamically adjusted according to the real-time material level to avoid the nozzles being buried and blocked, and to prevent the injection airflow from scouring the furnace lining and electrodes.

4. The method according to claim 1, characterized in that, The setting of the gas injection pressure includes: using independent pressure stabilization for the interphase injection pipeline and the edge injection pipeline respectively; setting the interphase injection working pressure to penetrate the central thick material layer; and setting the edge injection working pressure to be independently adjustable, thereby increasing the edge injection pressure under abnormal operating conditions to enhance the injection effect.

5. The method according to claim 1, wherein, The pre-smelting injection includes: immediately after stopping feeding, simultaneously starting interphase injection and edge injection; the high-pressure airflow of interphase injection impacts the central material layer and penetrates the initially formed slightly suspended material structure, releasing the carbon monoxide and carbon dioxide reaction gases accumulated in the material layer in advance; the edge injection disperses the accumulated powder around the electrodes and on the furnace wall surface to avoid local suspension; and normal feeding resumes after the initial pre-depressurization is completed.

6. The method according to claim 1, wherein, The intermittent multi-stage segmented blowing during the smelting process includes: maintaining the interphase blowing working pressure to continuously penetrate the thickened central material layer and release the deep-accumulated gas in layers; increasing the edge blowing pressure according to the degree of slag and agglomeration around the electrode to strengthen crushing and clean the slag and floating material around the electrode; setting an interval that is dynamically adjusted according to the furnace pressure feedback between adjacent cycles, and gradually dissipating the gas accumulation in the material layer through multiple intermittent blowing cycles to avoid a sudden rise in furnace pressure caused by concentrated gas release.

7. The method for coordinated control of pre-pressure relief in titanium slag electric furnace collapse according to claim 1, characterized in that, The full-area enhanced injection and slag removal includes: simultaneously activating all interphase injection points and edge injection points to break the residual overhead gas storage layer and release the trapped gas trapped in the layer; after the injection is completed, allowing the gas to escape smoothly and the furnace pressure to drop back to a stable range during the buffer period; and starting the slag removal operation after confirming that the buffer period has ended and the furnace pressure is stable without fluctuations.

8. The method for coordinated control of pre-pressure relief in titanium slag electric furnace collapse according to claim 1, characterized in that, The in-situ sampling, temperature measurement, and viscosity detection of the molten slag include: obtaining molten slag samples from inside the furnace through sampling holes independently set on the furnace cover and not interfering with the electrode holes and charging holes; simultaneously acquiring the actual temperature of the molten pool using thermal imaging equipment during the sampling process; and conducting viscosity tests on the obtained molten slag samples at the actual temperature of the molten pool to obtain the measured molten slag viscosity.

9. The method for coordinated control of pre-pressure relief in titanium slag electric furnace collapse according to claim 1, characterized in that, The electric furnace power control includes: pre-setting a standard slag viscosity adaptation range for titanium slag smelting; when the measured slag viscosity is in the viscosity range that characterizes low slag temperature and poor fluidity, it is determined that the gas escape channel is obstructed, and the electric furnace working power is increased based on the electric furnace benchmark working power before adjustment. The slag fluidity is improved by increasing the molten pool temperature, so that the slag viscosity is stabilized within the standard slag viscosity adaptation range, and the reaction gas is released smoothly by segmented injection.

10. The method for coordinated control of pre-pressure relief in titanium slag electric furnace collapse according to claim 8, characterized in that, The titanium slag electric furnace is a large titanium slag electric furnace, with a dedicated sampling and testing hole independently set on its furnace cover as the sampling hole, and a sealing lifting mechanism configured for the dedicated sampling and testing hole.