Aramid / carbon fiber blended core rope TFP continuous laying bulletproof helmet and its forming process
By using the TFP continuous laying process of aramid/carbon fiber blended core rope, the material gradient distribution and fiber continuity of the bulletproof helmet in different areas are achieved, which solves the problems of weak edge protection and fiber discontinuity in traditional bulletproof helmets, improves shear resistance and impact resistance, and has the advantage of lightweight.
Patent Information
- Application Number
- CN202611157112.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-24
AI Technical Summary
Existing bulletproof helmets suffer from weak edge protection and fiber discontinuity when dealing with high-speed fragments and high-energy projectile impacts, making it difficult to meet the protection requirements of both rigidity and flexibility. Traditional multi-layer composite structures are prone to delamination and failure, and the overall process is complex and costly.
The TFP continuous laying process of aramid/carbon fiber blended core rope is adopted. By adjusting the blending ratio, laying density and laying layers of aramid and carbon fiber in different areas of the helmet, a gradient distribution of fiber preform is formed. Combined with Archimedes spiral or spatial grid topology path for laying, a seamless bulletproof helmet shell is produced.
It achieves material matching in different areas of the bulletproof helmet, improves shear resistance and structural stiffness, enhances fiber continuity and load transfer efficiency, and solves the problems of insufficient edge protection and poor resistance to multiple impacts in traditional bulletproof helmets. It has excellent impact resistance and lightweight characteristics.
Smart Images

Figure CN123154705A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of fiber-reinforced composite material molding technology, and in particular to a ballistic helmet with aramid / carbon fiber blended core rope TFP continuous laying and its molding process. Background Technology
[0002] Currently, most mainstream bulletproof helmets are made of 2D / 2.5D woven or non-woven fabrics made of high-strength fibers such as aramid or ultra-high molecular weight polyethylene, which are laminated and molded. Although this technology is mature, it still has the following inherent structural defects when dealing with high-speed fragments and high-energy projectile impacts on the modern battlefield: (1) Weak edge protection and prominent fiber discontinuity issues: Traditional lamination process requires cutting flat fabrics to adapt to the hyperboloid geometry of the helmet, resulting in a large number of fiber cross sections at the helmet edge and openings. This not only destroys the continuity of fibers and weakens the shear resistance of the edge area, but also makes it easy for interlayer peeling and edge curling to occur when impacted, seriously affecting the utilization rate of the protective area. (2) A single material system is difficult to meet the protection requirements of "rigidity and flexibility". Pure aramid material has good toughness but insufficient rigidity. After impact, it is easy to produce excessive back feature depth, causing serious blunt trauma to the head; while pure carbon fiber has high modulus and high strength, but is brittle and is prone to fragmentation when subjected to high-energy impacts, and cannot effectively absorb impact energy. Therefore, there is an irreconcilable contradiction between "penetration resistance" and "dent resistance" in traditional single-layer homogeneous structures.
[0003] To address the aforementioned issues, various improvements have emerged in existing technologies. For example, patent CN116222307B discloses a triple-protection structure consisting of an outer shell layer, a buffer energy-absorbing layer, and an inner shell layer. This structure attempts to utilize high-rigidity outer materials to resist penetration and high-toughness inner materials to absorb energy through macroscopic material stacking. However, this type of multi-layered composite structure is essentially still a physical superposition. The interlayer interfaces are highly susceptible to becoming channels for crack propagation under continuous high-intensity impacts, leading to delamination failure. Furthermore, this solution does not address the fundamental problem of discontinuous edge fibers, and the shear resistance of the sidewalls remains limited. Patent CN119433815A achieves continuous spatial interweaving of fibers through a three-dimensional woven prefabricated structure. While this technology effectively eliminates the risk of interlayer delamination and solves the wrinkling problem during curved surface forming, its global material homogeneity makes it difficult to achieve differentiated customization of local functions. Moreover, the overall three-dimensional weaving process is complex, lacks flexibility, and has high manufacturing costs, making it difficult to meet the needs of large-scale industrial production.
[0004] In view of this, it is necessary to design an improved aramid / carbon fiber blended core rope TFP continuous laying bulletproof helmet and its molding process to solve the above problems. Summary of the Invention
[0005] The purpose of this invention is to provide a ballistic helmet with aramid / carbon fiber blended core rope TFP continuous laying and its molding process.
[0006] To achieve the above-mentioned objectives, in a first aspect, the present invention provides a ballistic helmet with aramid / carbon fiber blended core rope TFP continuous laying, comprising: a fiber reinforced composite shell, which is formed by continuously laying aramid / carbon fiber blended core rope with a predetermined mixing ratio through TFP to form a fiber preform, impregnating it with resin, and then molding and curing it.
[0007] The fiber preform exhibits a gradient distribution of decreasing aramid fiber content and increasing carbon fiber content along the height direction from the top of the helmet to the brim. The area near the center of the top of the helmet is rich in aramid fibers, while the area near the brim is rich in carbon fibers.
[0008] In the height direction, the mass ratio of aramid fiber to carbon fiber in the fiber preform is 20:80 to 80:20.
[0009] Preferably, the fiber preform, in the height direction from the top of the helmet to the brim, consists of an aramid enrichment zone, a first transition zone, a second transition zone, and a carbon fiber enrichment zone in sequence; the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the aramid enrichment zone is 80:20, the mass ratio of aramid fiber to carbon fiber in the first transition zone is 60:40, the mass ratio of aramid fiber to carbon fiber in the second transition zone is 40:60, and the mass ratio of aramid fiber to carbon fiber in the carbon fiber enrichment zone is 20:80.
[0010] Secondly, the present invention provides a molding process for a bulletproof helmet, comprising the following steps:
[0011] A TFP continuous layup device is used to continuously lay up aramid / carbon fiber blended core ropes with a predetermined mixing ratio. The blended core ropes are composed of aramid fiber bundles and carbon fiber bundles arranged side by side and bound together by wrapping yarn. The layup path starts from the center of the helmet top and follows the trajectory of an Archimedean spiral r=a+bθ and / or a spatial grid topology trajectory to sequentially form an aramid enrichment zone, a first transition zone, a second transition zone, and a carbon fiber enrichment zone, thus producing a fiber preform. In the equation r=a+bθ, r is the radial distance from any point on the layup trajectory to the center of the helmet top, in mm; θ is the polar angle, representing the angle of rotation of the layup trajectory around the helmet center; and a is the initial radius of the spiral, in mm.
[0012] After weaving, the resulting fiber preform is immersed in a resin matrix and then cured by hot pressing to obtain a seamless bulletproof helmet.
[0013] Preferably, when laid out according to the trajectory of the Archimedean spiral r=a+bθ, the aramid enrichment region satisfies the following conditions: the initial spiral region 0≤r<35mm, 0°≤θ<1300°; the first transition region satisfies 35mm≤r<70mm, 1300°≤θ<2200°; the second transition region satisfies 70mm≤r<100mm, 2200°≤θ<3000°; and the carbon fiber enrichment region satisfies 100mm≤r≤R, 3000°≤θ<3600°, where R is the maximum laying radius of the helmet edge.
[0014] Preferably, during the laying of the aramid / carbon fiber blend core rope, the laying speed is 150 mm / s, the core rope tension is 15 N, the stitch pitch is 2.2 mm, the row spacing is 1.5 mm, the overlap rate of adjacent laying paths is 15-25%, the minimum laying turning radius is not less than 8 mm, the laying speed is controlled at 120-180 mm / s, the core rope tension is controlled at 8-15 N, the stitch pitch is 1.8-2.5 mm, and the row spacing is 1.2-1.8 mm.
[0015] Preferably, the aramid enrichment zone has a layup density of 0.80-0.90 fibers / mm, a layup spacing of 1.1-1.3mm, and 10-12 layers, with a corresponding thickness of approximately 8.0mm; the first transition zone has a layup density of 0.75-0.80 fibers / mm, 8-10 layers, and a thickness of approximately 7.0mm; the second transition zone has a layup density of 0.70-0.75 fibers / mm, 7-8 layers, and a thickness of approximately 6.2mm; and the carbon fiber enrichment zone has a layup density of 0.65-0.70 fibers / mm, 6-7 layers, and a thickness of approximately 5.5mm.
[0016] Preferably, the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the aramid enrichment zone is 80:20; the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the first transition zone is 60:40; the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the second transition zone is 40:60; and the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the carbon fiber enrichment zone is 20:80.
[0017] Preferably, the impregnation process of the fiber preform in the resin matrix is carried out under vacuum conditions, with a vacuum degree of -0.095 MPa and an impregnation time of 30 min.
[0018] Preferably, the curing temperature is 150°C and the curing time is 180 min.
[0019] Preferably, the resin matrix is at least one of epoxy resin, vinyl ester resin, bismaleimide resin, and phenolic resin.
[0020] The beneficial effects of this invention are:
[0021] 1. The bulletproof helmet molding process provided by this invention first uses customized fiber layup (TFP) technology to obtain a fiber preform, then impregnates it with resin, and finally produces a continuous, seamless bulletproof helmet. During the fiber preform preparation process, a dual-gradient design combining thickness gradient and material ratio gradient is adopted. The mixing ratio, layup density, and number of layup layers of aramid and carbon fiber are adjusted in different areas of the helmet (such as the top, sidewalls, and edges) to ensure that the material distribution is highly matched with the actual stress state of the helmet (high energy absorption is required for the top under impact, and high stiffness is required for the sidewalls / edges under shear). The high proportion of aramid fiber in the top area can improve the impact energy absorption capacity and reduce the depth of the back indentation. At the same time, the carbon fiber enrichment area of the brim and edges utilizes the extremely high tensile modulus and compressive strength of carbon fiber to significantly improve the shear resistance and structural stiffness of the area, preventing edge cracking and curling under bullet shear or impact loads. This fundamentally solves the defects of "contradiction between energy absorption and stiffness" and "insufficient edge protection" in traditional bulletproof helmets, and achieves synergistic optimization of protective performance and lightweight.
[0022] 2. The molding process provided by this invention, by employing a spatially continuous and uninterrupted topological laying path (Archimedean spiral, spatial grid topological line, or a combination thereof) using TFP technology, replaces the traditional two-dimensional fabric piece splicing structure, constructing an integral fiber prefabricated body without cutting or overlapping seams, effectively reducing a large number of broken fiber ends and splicing gaps at the edges. Secondly, the aforementioned weaving method significantly improves fiber continuity, allowing loads to be evenly distributed along the continuous fiber path, avoiding the "stress concentration" problem in traditional 2D / 2.5D structures. Simultaneously, the continuous and seamless integral molding method greatly improves load transfer efficiency, enhancing the structural integrity of the helmet under multi-directional impacts and the damage tolerance after multiple impacts, effectively solving the defects of traditional bulletproof fabrics such as "discontinuous edge fibers" and "poor resistance to multiple impacts."
[0023] 3. The molding process provided by this invention optimizes the resin impregnation process of the fiber preform by using an aramid / carbon fiber blended core rope to weave the fiber preform. Compared with traditional coarse fiber bundles, the blended core rope has richer resin permeation channels and a suitable internal pore structure. In the vacuum-assisted impregnation process, the resin fluid can achieve rapid and thorough capillary penetration along the axial and radial directions of the core rope, which helps to reduce porosity and reduce the generation of dry spot defects. At the same time, the close contact and complementarity of aramid and carbon fiber at the microscale optimizes the interfacial bonding state between the fiber and the resin matrix, effectively alleviating the interfacial delamination problem caused by the surface inertness of single carbon fiber and the insufficient compressibility of single aramid fiber. Thus, at the microscopic level, it achieves efficient resin coating and stress transfer of reinforcing fibers, improving the helmet's energy absorption performance, structural stiffness, and overall impact resistance. Attached Figure Description
[0024] Figure 1 A schematic diagram of the structure of the fiber preform for the bulletproof helmet provided by the present invention;
[0025] Figure 2 for Figure 1 Sectional view of AA;
[0026] Figure 3 A schematic diagram of the aramid / carbon fiber blend core rope used in the preparation of the fiber preform of the present invention;
[0027] Figure 4 A schematic diagram of the TFP continuous laying integral molding process for the bulletproof helmet provided by the present invention;
[0028] Figure 5 A schematic diagram comparing the fiber preform provided by this invention with the structure of traditional 2D / 2.5D preforms;
[0029] Figure 6 This is a photograph of the fiber preform obtained in Example 2 of the present invention.
[0030] The attached figures are labeled as follows:
[0031] 1. Helmet shell; 2. Center point of helmet top; 3. Inner lining buffer layer; 12. TFP continuous laying device; 13. Resin impregnation device; 14. Molding and curing device; 20. Fiber preform; 21. Aramid enrichment zone; 22. First transition zone; 23. Second transition zone; 24. Carbon fiber enrichment zone; 31. Aramid / carbon fiber blended core rope; 32. Aramid fiber bundle; 33. Carbon fiber bundle; 34. Outer covering yarn. Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0033] It should also be noted that, in order to avoid obscuring the present invention with unnecessary details, only the structures and / or processing steps closely related to the present invention are shown in the accompanying drawings, while other details that are not closely related to the present invention are omitted.
[0034] Additionally, it should be noted that the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0035] Terminology Explanation:
[0036] Continuous laying: refers to the continuous connection of Archimedes spiral trajectory, Bezier transition trajectory and spatial grid topology trajectory in terms of geometric path and load transfer relationship, while the continuous transition of material composition is achieved by the overlapping and stitching between adjacent specification blended core ropes.
[0037] Seamless: This means that the helmet shell does not use the traditional two-dimensional fabric cutting, splicing and multi-piece prefabricated assembly method, and there is no macroscopic through seam formed by splicing the edges of fabric pieces.
[0038] Please see Figure 1 As shown, the present invention provides a ballistic helmet with aramid / carbon fiber blended core rope TFP continuous laying, including a fiber reinforced composite shell. The shell is formed by continuously laying aramid fiber / carbon fiber blended core rope with a predetermined mixing ratio through TFP to form a fiber preform, impregnating it with resin, and then molding and curing it.
[0039] Specifically, along the height direction from the top of the helmet to the brim, the mass ratio of aramid fiber to carbon fiber in the fiber preform is 20:80 to 80:20, exhibiting a gradient distribution with decreasing aramid fiber content and increasing carbon fiber content. The area near the center of the helmet top is rich in aramid fibers, while the area near the brim is rich in carbon fibers. More specifically, along the height direction from the top of the helmet to the brim, the fiber preform consists of, in sequence, an aramid-rich area, a first transition area, a second transition area, and a carbon fiber-rich area.
[0040] Further, please refer to Figure 4 As shown, the present invention also provides a molding process for the above-mentioned bulletproof helmet, which specifically includes the following steps:
[0041] A TFP continuous layup device is used to continuously lay up aramid / carbon fiber blended core ropes with a predetermined mixing ratio. The blended core ropes are composed of aramid fiber bundles and carbon fiber bundles arranged side by side in different mass ratios and bound together by wrapping yarn. The layup path is centered on the top center of the helmet and follows the trajectory of an Archimedean spiral r=a+bθ and / or a spatial grid topology trajectory to sequentially form an aramid enrichment zone, a first transition zone, a second transition zone, and a carbon fiber enrichment zone, thus producing a fiber preform. In the equation r=a+bθ, r is the radial distance from any point on the layup trajectory to the top center of the helmet, in mm; θ is the polar angle, representing the angle of rotation of the layup trajectory around the center of the helmet; and a is the initial radius of the spiral, in mm.
[0042] After weaving, the resulting fiber preform is immersed in a resin matrix and then cured by hot pressing to obtain a seamless bulletproof helmet.
[0043] Specifically, in some other embodiments, when using a spatial grid topology path for laying, a parametric surface coordinate system is established based on the helmet surface, and a longitudinal and latitudinal spatial grid is generated according to the helmet shape. The spatial grid consists of multiple intersecting continuous laying units, each grid unit preferably having an approximately rhomboid structure, with its major axis arranged along the longitudinal direction of the helmet and its minor axis arranged along the latitudinal direction of the helmet. Among them, the high aramid ratio region (8) corresponds to the main impact bearing area on the top of the helmet. In order to improve the local fiber coverage and energy absorption capacity, the grid size of this region is preferably set to 8 mm × 8 mm, and a higher laying density is used for continuous laying.
[0044] The first transition region (10) is located between the high aramid ratio region and the second transition region. To ensure the smooth transmission of impact loads, the grid size of this region is preferably set to 10 mm × 10 mm. The second transition region (11) is located between the first transition region and the high carbon fiber ratio region. Its grid size is further adjusted to 12 mm × 12 mm to gradually increase the structural stiffness while avoiding local stress concentration caused by abrupt changes in material properties. The high carbon fiber ratio region (9) corresponds to the helmet sidewall and edge region. This region mainly bears shear loads, bending loads, and edge deformation. To balance overall stiffness, shear resistance, and lightweight requirements, its grid size is preferably set to 15 mm × 15 mm.
[0045] By continuously varying the grid size from small to large, the spatial grid topology is kept consistent with the aramid / carbon fiber gradient distribution, achieving synchronous gradient changes in fiber coverage density, material composition, and structural stiffness, thereby improving the overall impact resistance and structural stability of the helmet. Furthermore, regardless of whether an Archimedes spiral path or a spatial grid topology path is used, the same four functional gradient regions (high aramid ratio region, first transition region, second transition region, and high carbon fiber ratio region) are employed. The only difference lies in the geometry of the continuous laying path, while the material gradient design principles remain consistent.
[0046] In some embodiments, the mass ratio (hybridization ratio) of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the aramid-rich region is 80:20; the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the first transition region is 60:40; the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the second transition region is 40:60; and the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the carbon fiber-rich region is 20:80. Through the gradient design of the aramid / carbon fiber ratio, different areas of the helmet possess mechanical properties that match the actual stress state. Specifically, the top area of the helmet uses a high-proportion aramid fiber blend core rope. Utilizing the high breaking elongation, excellent toughness, and energy absorption capacity of aramid fibers, it can absorb a large amount of impact energy during the initial contact phase of the projectile through fiber stretching, pull-out, and breakage processes, effectively reducing the rate at which the impact load is transmitted to the interior of the helmet, thereby reducing the depth of the indentation on the back. As the impact load diffuses along the helmet structure towards the sidewalls and edges, the proportion of carbon fiber in the blended core rope gradually increases. Due to the high elastic modulus and excellent axial load-bearing capacity of carbon fiber, it enhances load transfer efficiency and structural stiffness in the transition region, preventing localized deformation concentration caused by residual load absorbed in the top area. Simultaneously, the high proportion of carbon fiber reinforcement in the edge region effectively resists shear deformation, bending deformation, and edge curling failure during impact, improving the overall impact resistance and stability of the helmet.
[0047] More specifically, the aramid-enriched region has a layup density of 0.90 fibers / mm, a layup spacing of 1.3mm, and 11 layers, with a corresponding thickness of approximately 8.0mm; the first transition region has a layup density of 0.75 fibers / mm, a layup spacing of 1.45mm, an overlap rate of 20% between adjacent layup paths, 10 layers, and a thickness of approximately 7.0mm; the second transition region has a layup density of 0.70 fibers / mm, a layup spacing of 1.55mm, an overlap rate of 18% between adjacent layup paths, 8 layers, and a thickness of approximately 6.2mm; and the edge carbon fiber-enriched region has a layup density of 0.65 fibers / mm, a layup spacing of 1.70mm, an overlap rate of 15% between adjacent layup paths, 6 layers, and a thickness of approximately 5.5mm. The laying density, laying spacing, overlap rate of adjacent laying paths, number of laying layers and structural thickness of each of the above regions are determined according to the stress characteristics of different regions of the helmet, and are used to construct a gradient reinforcement structure that changes continuously from the top to the edge; the above parameters are structural design parameters of the helmet, and can be set separately for different regions according to protection requirements.
[0048] Throughout the continuous TFP laying process, the equipment operating parameters remain consistent. To ensure the continuous and stable laying of the blended core rope, these parameters are kept constant. Specifically, the laying speed is preferably 150 mm / s, the core rope tension is preferably 15 N, the stitch pitch is preferably 2.2 mm, the minimum turning radius of the laying path is controlled at 8-30 mm, preferably 10-15 mm, more preferably 10 mm, and the maximum turning radius is preferably 40 mm. These operating parameters are primarily used to ensure the stability of the laying process and are not adjusted according to changes in the gradient structure of different areas. The laying speed, core rope tension, stitch pitch, and turning radius of the laying path are TFP equipment operating parameters, which are kept consistent throughout the continuous laying process to ensure laying quality and process stability. By controlling the process parameters within the above ranges, the blended core rope is ensured to maintain a stable fit to the helmet surface during continuous laying, avoiding fiber bundle bending, wrinkling, or localized stress concentration due to excessively small curvature. In this step, by using a blended core rope composed of aramid fiber and carbon fiber as a continuous laying unit, the two reinforcing fibers are synergistically reinforced in the same structure. The high energy absorption characteristics of aramid fiber and the high stiffness characteristics of carbon fiber complement each other. Combined with the continuous and seamless laying method, the impact load can be evenly diffused along the continuous fiber path, which greatly improves the isotropic protection performance and anti-rolling ability of the helmet under multi-directional impact.
[0049] In the aforementioned technical solution, a dual-gradient synergistic mechanism of "continuous fiber path diffusion load" and "aramid energy absorption - carbon fiber load bearing" enables the projectile impact energy to undergo a gradual dissipation process within the helmet, from the impact point to the peripheral area, and from absorption in high-toughness areas to transmission in high-stiffness areas. On one hand, the aramid-rich region reduces the peak energy at the moment of impact, minimizing back-side indentation; on the other hand, the high carbon fiber region enhances structural load-bearing capacity, delays crack propagation and localized failure, thereby improving the helmet's ballistic protection capability and overall structural stability while ensuring lightweight design. By jointly controlling the layup density, layup spacing, and number of layup layers, the fiber volume fraction and local structural thickness in different areas are adjusted, achieving an optimized match between helmet protective performance and weight.
[0050] In some embodiments, the impregnation process of the fiber preform in the resin matrix is carried out under vacuum conditions, with a vacuum degree of -0.095 MPa and an impregnation time of 30 min.
[0051] In some embodiments, the hot-press curing temperature is 150°C, the time is 180 min, and the pressure is 2-5 MPa, preferably 3 MPa. When the molding pressure is below 2 MPa, the fiber layer is not sufficiently compacted, which easily leads to pores and interlayer defects; when the molding pressure is above 5 MPa, it is easy to cause excessive resin extrusion, reduce the resin content, and may affect the structural integrity of the fiber preform.
[0052] In some embodiments, the resin matrix is a thermosetting resin, including but not limited to epoxy resin, vinyl ester resin, bismaleimide resin or phenolic resin, preferably epoxy resin.
[0053] In the above technical solution, by using a continuous Archimedean spiral, spatial grid topology, or a combination thereof starting from the center of the helmet top for integral laying, a large number of broken fiber ends at the edges can be eliminated, improving fiber continuity and load transfer efficiency. Simultaneously, this continuous, seamless integral laying method can form a near-isotropic reinforcing structure, allowing impact loads to be uniformly diffused along the continuous fiber path, improving the helmet's overall ballistic performance, structural integrity, and damage tolerance after multiple impacts.
[0054] The following specific embodiments further illustrate the aramid / carbon fiber blend core rope TFP continuous laying bulletproof helmet and its molding process provided by the present invention:
[0055] Example 1
[0056] Please see Figure 1 As shown, this embodiment provides a ballistic helmet with aramid / carbon fiber blend core rope TFP continuous laying, which includes:
[0057] The shell 1 is made by continuously laying aramid fiber / carbon fiber blend core rope with a predetermined mixing ratio through TFP to form a fiber preform 20, impregnating it with resin, and then molding and curing it.
[0058] The inner lining buffer layer 3 is disposed on the inner side wall of the housing 1.
[0059] Specifically, please refer to Figure 2 As shown, the fiber preform 20, from its top center to its edge, consists of an aramid enrichment zone 21, a first transition zone 22, a second transition zone 23, and a carbon fiber enrichment zone 24, in sequence. The four zones exhibit a gradient distribution with decreasing aramid fiber content and increasing carbon fiber content. Specifically, the mixing ratio of aramid fiber / carbon fiber blended core rope used to prepare the aramid enrichment zone 21 is 80:20, the mixing ratio of aramid fiber / carbon fiber blended core rope used in the first transition zone 22 is 60:40, the mixing ratio of aramid fiber / carbon fiber blended core rope used in the second transition zone 23 is 40:60, and the mixing ratio of aramid fiber / carbon fiber blended core rope used in the carbon fiber enrichment zone 24 is 20:80.
[0060] The specific structural diagram of the aramid fiber / carbon fiber blend core rope 31 is as follows: Figure 3 As shown, it is a partitioned bundled structure. Specifically, the aramid fiber / carbon fiber blended core rope 31 is mainly composed of two sets of fiber bundles arranged in parallel: several parallel aramid fiber bundles 32 are concentrated on one side of the core rope, and several parallel carbon fiber bundles 33 are concentrated on the other side; all the aramid fiber bundles 32 and carbon fiber bundles 33 are wrapped together by the outer covering yarn 34, thereby forming a structurally stable fiber bundle, which is conducive to subsequent stable laying. In this embodiment, the outer covering yarn 34 is specifically polyester filament with a linear density of 167 dtex (approximately 150D). It is uniformly wrapped around the outside of the aramid fiber bundles 32 and carbon fiber bundles 33 by spiral winding, with a covering pitch of 4.0 mm and a covering coverage of 25%. The aramid fiber bundle 32 is specifically a continuous para-aramid filament with a linear density of 1100 dtex, and the carbon fiber bundle 33 is specifically a 12K high-strength carbon fiber bundle with a linear density of 800 tex. In the specific preparation process, the number of fibers used is determined based on the mass ratio of aramid fiber to carbon fiber in the blended core rope used in each region, and then the fibers are spirally wound. The aramid fiber / carbon fiber blended core rope 31 has a diameter of 0.90 mm and a unit length mass of 1.95 g / m.
[0061] Example 2
[0062] Please see Figure 4 As shown, this embodiment provides a molding process for a ballistic helmet with a continuous TFP (Telematics Particulate Fiber) core rope of aramid / carbon fiber. The structural limitations of the ballistic helmet are described in Embodiment 1. The specific molding process includes the following steps:
[0063] First, based on the mass ratio of aramid fiber bundles to carbon fiber bundles in the aramid / carbon fiber blended core rope 31 used in each region of the fiber preform of shell 1, four types of aramid / carbon fiber blended core ropes 31 with different mass ratios are prepared. The blended core ropes used in the aramid enrichment region 21, the first transition region 22, the second transition region 23, and the carbon fiber enrichment region 24 are blended core rope A, blended core rope B, blended core rope C, and blended core rope D, respectively.
[0064] The TFP continuous laying device 12 is used to automatically lay the aramid / carbon fiber blend core rope with a predetermined mixing ratio. First, the blend core rope A is loaded, and the laying starts from the center point 2 of the helmet top. It is continuously woven according to the Archimedean spiral r=a+bθ and laid outward along the Archimedean spiral trajectory to complete the laying of the aramid-rich area on the top of the helmet. During the laying process, when the laying trajectory reaches the first preset radius boundary, the TFP device stops the supply of core rope A and switches to blend core rope B, and keeps the laying trajectory continuously extended. Then, blend core rope C and blend core rope D are switched in sequence to finally complete the continuous gradient laying from the top to the edge and obtain the fiber preform. Each time the switch is made, the end of the previous core rope and the beginning of the next core rope are laid overlapping, with an overlap length of 20-30mm, to avoid local fiber discontinuity caused by core rope replacement.
[0065] In the formula r = a + bθ, r is the radial distance from any point on the laying trajectory to the center point of the helmet top, in mm; θ is the polar angle, representing the angle by which the laying trajectory rotates around the helmet center; a is the initial radius of the helix, in this embodiment a = 0 mm, meaning laying begins from the center of the helmet top; b is the pitch control coefficient, used to control the radial spacing between adjacent spiral coils, its value is determined based on the core rope width and overlap rate, in this embodiment b = 1.4 mm / rad. During the laying process, as θ continuously increases, the laying trajectory gradually expands from the top of the helmet outwards, maintaining a center distance of approximately 1.5 mm between adjacent spiral coils, meeting the set laying density requirements; laying terminates when the laying trajectory reaches the helmet edge contour, i.e., r ≥ R. r ≥R, where R is the maximum radial dimension corresponding to the outer contour of the helmet. In this embodiment, R=145 mm (corresponding to the outer contour of size M helmet). At this time, the corresponding polar angle is approximately θ≈104rad, which means that approximately 16.5 consecutive lay-up circles are completed.
[0066] The automatic layup process for the blended core cord has a layup speed of 150 mm / s, a core cord tension of 15 N, a needle pitch of 2.2 mm, a row spacing of 1.5 mm, and an overlap rate of 20% between adjacent layup paths. This ensures a 20% width overlap between adjacent core cord layup paths, preventing excessive overlap that could lead to localized thickness increases and resin impregnation difficulties. The minimum layup turning radius is no less than 8 mm. The aramid enrichment zone satisfies the initial spiral region condition of 0 ≤ r < 35 mm and 0° ≤ θ < 1300°. The mass ratio of aramid fiber to carbon fiber in the aramid / carbon fiber blended core cord used is 80:20. The first transition zone satisfies the condition of 35 mm ≤ r < 70 mm. The first transition zone satisfies 1300°≤θ<2200°, and the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used is 60:40; the second transition zone satisfies 70mm≤r<100mm, 2200°≤θ<3000°, and the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used is 40:60; the carbon fiber enrichment zone satisfies 100mm≤r≤R, 3000°≤θ<3600°, where R is the maximum laying radius of the helmet edge, and the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used is 60:40. The carbon fiber mass ratio is 20:80; the aramid-rich zone has a layup density of 0.90 fibers / mm, a layup spacing of 1.3mm, and 11 layers, with a corresponding thickness of approximately 8.0mm; the first transition zone has a layup density of 0.75 fibers / mm, 10 layers, and a thickness of approximately 7.0mm; the second transition zone has a layup density of 0.70 fibers / mm, 8 layers, and a thickness of approximately 6.2mm; and the edge carbon fiber-rich zone has a layup density of 0.65 fibers / mm, 6 layers, and a thickness of approximately 5.5mm.
[0067] After the fiber preform is laid, it is immersed in the resin matrix and impregnated under a vacuum of -0.095 MPa for 30 min. Then, it is hot-pressed and cured at 150℃ and 3 MPa for 180 min to complete the cross-linking and curing of the resin matrix, thus obtaining the desired fiber preform. Figure 6The example shown is a seamless bulletproof helmet. The resin matrix is a mixture of 100 parts by weight of epoxy resin E-51, 80 parts by weight of methyltetrahydrophthalic anhydride, and 1.0 part by weight of curing accelerator 2,4,6-tris(dimethylaminomethyl)phenol. The system has a viscosity of 300-500 mPa·s at 25 °C. Before impregnating the fiber preform into the resin matrix, it needs to be preheated at 60 °C to reduce its viscosity to a suitable range for vacuum impregnation. It should be noted that in this embodiment, the resin impregnation process is carried out in the resin impregnation device 13, and the hot-press curing process is carried out in the molding curing device 14. The resin impregnation device 13, the molding curing device 14, and the TFP continuous layup device 12 all adopt conventional structures known in the art, and their specific construction is not the focus of this invention and will not be described in detail here.
[0068] The bulletproof helmet manufactured in this embodiment, under standard 9mm full metal jacket bullet impact conditions, showed a back feature indentation depth of 11.6mm, with no penetration damage and the overall structure remaining intact. Under the same testing conditions, the back indentation depth of a traditional pure aramid 2D bulletproof helmet was 15.2mm, representing a reduction of approximately 23.7% in this embodiment. This embodiment features a continuously laid fiber prefabricated structure and a traditional 2D woven structure, as shown in the example... Figure 5 As shown, the traditional 2D / 2.5D fabric structure on the left uses a splicing and laying process, which has obvious problems of multiple cross sections and stress concentration, resulting in a decrease in impact resistance. In contrast, the continuous laying structure on the right achieves seamless integrated molding, has the significant advantage of continuous fibers, can achieve uniform load transfer, and ultimately effectively improves the overall impact resistance.
[0069] In the V50 ballistic maximum velocity test, the V50 value measured in this embodiment was 652 m / s, while the corresponding V50 value of the traditional aramid bulletproof helmet was 571 m / s, an improvement of about 14.2%, indicating that the structure of the present invention has a higher resistance to high-speed impact.
[0070] In the drop hammer impact test (impact energy set at 50J), the maximum indentation depth of the sample in this embodiment was 8.4mm, and the peak impact load was 6.2kN; compared with the conventional aramid bulletproof helmet, the maximum indentation depth was 10.3mm and the peak load was 7.1kN, indicating that this embodiment has better energy absorption and load dispersion capabilities.
[0071] In the edge impact resistance test, the maximum bending deformation of the edge area of this embodiment under the same impact conditions was 4.1 mm, while that of the aramid bulletproof helmet was 5.6 mm. The edge deformation resistance was significantly improved, indicating that the carbon fiber enrichment area effectively improved the local stiffness.
[0072] Regarding overall areal density, the areal density of the bulletproof helmet in this embodiment is 5.82 kg / m³. 2 Traditional aramid bulletproof helmets weigh 6.35 kg / m². 2 While improving protective performance, it also achieves a lightweight optimization of approximately 8.4%.
[0073] The above conclusions demonstrate that by employing a continuous seamless TFP layup structure and a gradient synergistic design of aramid / carbon fiber, impact loads can be continuously diffused and dissipated within the structure, thereby significantly improving the ballistic limit velocity and overall structural stability while reducing back-side indentation. The use of a continuous seamless TFP layup structure avoids the localized weak connection areas caused by cutting, splicing, and fiber breakage found in traditional two-dimensional or two-and-a-half-dimensional fabric structures. In traditional bulletproof helmets, reinforcing fibers are typically formed by stacking multiple layers of fabric pieces. The cut edges expose a large number of fiber ends, making it easy for stress concentration to occur in the splicing areas and fiber ends under impact loads, leading to premature local fiber breakage and reducing the overall load transfer efficiency of the structure.
[0074] This embodiment employs the TFP (Transformer Photopolymerization) process, starting from the center of the helmet's top and using an Archimedes spiral continuous laying path to form a continuous reinforcement network of aramid / carbon fiber blend core fibers along the helmet's curved surface. Because the reinforcing fibers remain continuous throughout the helmet, the transient load generated by projectile impact can be rapidly transferred to surrounding areas along the continuous fiber path, transforming the impact energy from a locally concentrated state to a widely diffused state. This reduces the local stress peak in the impact area and minimizes damage propagation caused by fiber breakage. Simultaneously, the seamless structure improves the continuity of load transfer between different areas, enabling the helmet to maintain high structural integrity even under multi-directional impacts.
[0075] Example 3
[0076] The only difference between this embodiment and Embodiment 2 is that the aramid enrichment area has a laying density of 1.0 strands / mm and 14 layers. At the same time, a 30% overlap laying method is used in the carbon fiber enrichment area at the edge of the helmet, that is, a 30% width overlap is maintained between the laying paths of adjacent carbon fiber blend core ropes to improve the fiber continuity and local load-bearing capacity of the edge area. The overlap laying method here only changes the local laying density and does not change the spatial range and height of the carbon fiber enrichment area. All other experimental parameters are the same as in Embodiment 2 and will not be repeated here.
[0077] Test results show that, in a comparative test with a traditional pure aramid bulletproof helmet, the back feature depth (BFS) of the helmet in this embodiment was measured to be 10.8 mm, while that of the traditional structure was 15.2 mm, a reduction of approximately 28.9%.
[0078] In ballistic limit performance testing, the V50 value of this embodiment was measured to be 675 m / s, while that of the traditional aramid bulletproof helmet was 571 m / s, representing an improvement of approximately 18.2%, indicating a significant enhancement in its resistance to high-speed impacts.
[0079] In the drop hammer impact test (impact energy 50J), the maximum indentation depth of this embodiment was 7.9mm and the peak impact load was 5.8kN, while the corresponding values for the traditional structure were 10.3mm and 7.1kN, respectively, indicating that this embodiment has better energy absorption and load dispersion capabilities.
[0080] Regarding structural integrity, this embodiment did not exhibit significant through-crack propagation after multi-point impact testing, while traditional structures showed localized fiber breakage and interlaminar debonding under the same conditions, indicating that the structure of this invention has higher resistance to damage propagation. Furthermore, the areal density of the helmet in this embodiment was measured to be 5.95 kg / m³. 2 While improving performance, it still maintains excellent lightweight characteristics.
[0081] The above conclusions indicate that by increasing the top layer density and optimizing the edge overlap structure, impact loads can be more evenly diffused and dissipated within the helmet structure, thereby significantly improving the overall ballistic performance, impact resistance, and structural stability of the helmet.
[0082] Example 4
[0083] The difference between this embodiment and Embodiment 2 is that the fiber preform is prepared using a TFP hybrid continuous placement method that combines Archimedean spiral trajectory and spatial grid topology trajectory. Specifically, the top aramid-rich region of the fiber preform is laid using an Archimedean spiral trajectory, and a Bezier transition section is set in the first transition region to convert the Archimedean spiral trajectory to the spatial grid topology trajectory. The remaining parts of the first transition region, the second transition region, and the carbon fiber-rich region are laid using the spatial grid topology trajectory. To adapt to the load transfer characteristics of the above hybrid trajectory, this embodiment re-sets the radial boundaries, grid size, and trajectory switching positions of each functional region. The specific preparation method is as follows:
[0084] Using the center point of the helmet top as the starting point for laying, and the horizontal projection distance from this point to the helmet edge as the radial position parameter, corresponding to a helmet mold with a maximum horizontal projection radius of approximately 145 mm, the fiber preform is divided from top to edge into an aramid enrichment zone, a first transition zone, a second transition zone, and a carbon fiber enrichment zone. Specifically, the region with a projection radius of 0-45 mm is the aramid enrichment zone, using a blended core rope with an aramid fiber to carbon fiber mass ratio of 80:20; the region with a projection radius of 45-75 mm is the first transition zone, using a blended core rope with a mass ratio of 60:40; the region with a projection radius of 75-105 mm is the second transition zone, using a blended core rope with a mass ratio of 40:60; and the region with a projection radius of 105-145 mm is the carbon fiber enrichment zone, using a blended core rope with a mass ratio of 20:80.
[0085] When the laying trajectory reaches the boundaries of the preset material regions with projection radii of 45 mm, 75 mm, and 105 mm, respectively, the blended core ropes of adjacent specifications are switched. At the projection radius of 45 mm, the end position of the helical main path and the beginning position of the first transition zone are adjacent, so this position involves both the switching of the blended core rope composition and the transformation of the laying trajectory from the helical main path to the Bezier transition path. At the projection radii of 75 mm and 105 mm, only the blended core rope specifications and corresponding structural parameters are switched, and the spatial grid topology path continues to extend continuously.
[0086] The top area of the helmet is continuously laid out according to the Archimedes spiral path, which satisfies r = a + bθ in the horizontal projection plane of the helmet mold. , Its plane parametric equation is , The spiral trajectory unfolds continuously outward within a projection radius of 0-45 mm. When the spiral trajectory reaches a projection radius of 45 mm, this position is set as the termination position of the main spiral path, and from there, the transition segment from the spiral trajectory to the spatial grid topology trajectory begins. The trajectory transition segment is set within a projection radius of 45-60 mm, still within the first transition zone. A cubic Bézier curve is used to achieve tangential continuity between the Archimedean spiral trajectory and the spatial grid topology trajectory. The starting point of the cubic Bézier curve is the termination point of the main spiral path, and the ending point is the entry point of the spatial grid path. The first control point is located in the tangential extension direction of the spiral termination point, and the second control point is located in the reverse extension direction of the tangent of the grid entry point. The distance between the two control points and their corresponding endpoints is 15 mm. Through the above control point settings, the spiral trajectory, the Bézier transition trajectory, and the spatial grid trajectory maintain positional continuity and tangential direction continuity. Starting from a projection radius of 60 mm, the laying trajectory is completely converted into a spatial grid topology trajectory, continuously covering the remaining part of the first transition zone, the second transition zone, and the carbon fiber enrichment zone.
[0087] The transition curve satisfies ,in, This is the endpoint of the spiral path. This is the entry point for the spatial grid path. Located in the tangential direction at the end of the spiral, Located in the opposite direction to the tangent at the starting point of the grid path; and Between and and The distances between them are all 15 mm to ensure tangential continuity between the spiral trajectory, transition trajectory, and grid trajectory. The minimum turning radius of the transition trajectory is not less than 10 mm to prevent bending, kinking, or local accumulation of the blended core rope; the spatial grid topology path is formed within the helmet's horizontal projection plane by... and The system consists of two intersecting paths, with an angle of 90° between the two paths and a 45° angle with the helmet's reference axis.
[0088] Two sets of paths are projected onto the helmet surface along the mold normal, forming a spatial grid structure covering the helmet sidewalls and edge areas. The first transition zone uses a 10 mm × 10 mm grid size, the second transition zone uses a 12 mm × 12 mm grid size, and the carbon fiber enrichment zone uses a 15 mm × 15 mm grid size. The ends of each grid path are reversed using arcs or cubic Bézier curves, with a reversal radius of not less than 10 mm. At the boundaries of different material gradient regions, the end of the aramid / carbon fiber blend core rope of the previous specification is overlapped with the starting end of the blend core rope of the next specification by 20 mm along the laying direction and secured together with TFP stitching to ensure the laying path remains continuous and does not form structural breaks through the shell. During the mixed laying process, the laying speed is 150 mm / s, the core rope tension is 15 N, the stitch pitch is 2.2 mm, and the minimum turning radius is 10 mm. Before entering the Bézier transition zone and the reversal zone at the end of the grid path, the laying speed is reduced to 110 mm / s. mm / s, after completing the reversal, it returns to 150 mm / s. The adjacent path overlap rates of the aramid enrichment zone, the first transition zone, the second transition zone and the carbon fiber enrichment zone are 25%, 20%, 18% and 15%, respectively, and the number of layers laid are 11, 10, 8 and 6, respectively.
[0089] After all the fiber preforms were laid out, the resulting fiber preforms were placed in a vacuum-assisted resin impregnation device. A resin system consisting of E-51 bisphenol A epoxy resin, methyltetrahydrophthalic anhydride curing agent and DMP-30 accelerator was used, with a mass ratio of 100:80:1. The preforms were impregnated for 30 min under a vacuum of -0.095 MPa to allow the resin to fully penetrate the blended core rope and interlayer pores. Subsequently, the impregnated preforms were placed in a molding and curing device (14) and cured for 180 min under a molding pressure of 3 MPa and a temperature of 150°C. After curing, the preforms were cooled to below 60°C and then depressurized to obtain a seamless aramid / carbon fiber composite bulletproof helmet with material composition and structural parameters that change gradient from the top to the edge.
[0090] Test results show that the combined use of the Archimedes spiral path and the spatial grid topology path can construct a multi-scale load transfer network extending continuously from the top impact zone to the sidewalls and edge regions inside the helmet shell. The two laying paths complement each other in terms of impact load diffusion direction, fiber stress mode, and crack suppression mechanism, thus producing a synergistic enhancement effect superior to a single laying path. When a projectile impacts the top of the helmet, the impact load first acts on the aramid-rich area laid using the Archimedes spiral path. Since the spiral path continuously unfolds around the top center, and adjacent spirals maintain a continuous and uniform radial spacing, the local impact load can propagate outward synchronously along the spiral tangentially and radially. Compared with a single ring or straight laying path, the Archimedes spiral path does not have obvious laying start and end points, allowing multiple turns of the blended core rope to participate in tensile, bending, and interfacial shear deformation sequentially, transforming the high-amplitude load concentrated near the impact point into tensile loads and interlaminar shear loads distributed along a longer spiral path. At the same time, the high aramid content, laying density and number of layers in the top region enable the fiber bundle to absorb impact energy through stretching deformation, fiber pull-out, interface debonding and resin microcracks, thereby reducing the local stress peak and back bulge near the impact point.
[0091] As the impact stress wave propagates from the top to the sidewalls, the load is smoothly transferred to the spatial grid topology region via the Bezier transition trajectory. This transition trajectory maintains tangential continuity between the helical path and the grid path, avoiding fiber bending, abrupt stiffness changes, and interface stress concentration caused by abrupt trajectory changes. This allows the impact load to gradually transition from the radial diffusion state of the helical path to the multidirectional distribution state of the spatial grid path. Therefore, this transition region not only serves as a geometric trajectory switching function but also forms a load conversion zone with continuously changing mechanical properties, preventing impact energy reflection or local accumulation at the termination position of the helical structure.
[0092] The spatial grid topology consists of two sets of cross-laid blended core fibers, forming multiple interconnected load-bearing nodes in the helmet's sidewalls and edges. When loads transmitted from the top enter the grid area, they are decomposed and redistributed to fiber paths in different directions at each cross node, transforming the originally radially-oriented impact load into a multi-directional load propagating circumferentially, radially, and obliquely. Fiber bundles in the cross grid bear tensile, shear, and bending loads respectively, while the grid nodes, through the resin matrix and stitching, provide local constraints, limiting the relative slippage of adjacent fiber bundles, thereby increasing the in-plane shear stiffness and load diffusion area of the shell. Especially in the sidewalls and edges, the higher proportion of carbon fiber provides greater axial stiffness and shear resistance, suppressing edge opening, curling, and local buckling.
[0093] When the two trajectories are used in combination, the Archimedes spiral path is mainly responsible for energy absorption and radial diffusion in the initial stage of impact, while the spatial grid topology path is mainly responsible for multi-directional flow splitting, lateral constraint, and edge bearing in the later stage of impact propagation. The former reduces the local impact stress peak and extends the impact load transmission path; the latter expands the effective bearing area and hinders the rapid propagation of cracks in a single direction through intersection nodes. After the two are connected by a continuous transition trajectory, a composite force transmission mechanism is formed, which transforms from "linear continuous diffusion" to "networked distributed bearing". This causes the load to undergo multiple directional changes, interface transmission, and energy attenuation in the shell, increasing energy dissipation processes such as fiber stretching, resin cracking, interface debonding, fiber pull-out, and grid node shearing, thereby improving the impact energy absorption capacity per unit mass of the structure.
[0094] Furthermore, while the Archimedes spiral path avoids a significant weak point in the top region due to the unidirectional fiber orientation, its ability to constrain circumferential shear loads in the sidewalls and edges is relatively limited. Although the spatial grid topology has good multi-directional load-bearing capacity, if used alone in the top impact zone, it is prone to local stiffness abrupt changes and stress concentrations near the intersection nodes. By arranging the spiral path in the high-energy-absorbing area at the top and the spatial grid path in the high-stiffness areas of the sidewalls and edges, with a continuous transition trajectory between the two, the advantages of both structures can be leveraged while mitigating their limitations when used alone. This synergistic effect allows the helmet shell to undergo controlled deformation during impact to absorb energy while maintaining sufficient overall stiffness and edge constraint, thus achieving a balance between low back bulge, high penetration resistance, and good post-impact structural integrity.
[0095] Based on the above mechanism, the hybrid layup structure, upon impact, sequentially undergoes local deformation energy absorption in the top aramid-rich region, radial continuous diffusion along the helical path, smooth load transfer in the gradient transition region, multi-directional load diversion in the grid region, and rigid constraint in the high-carbon fiber edge region, forming a step-by-step protection mechanism of "energy absorption—diffusion—load diversion—constraint". Therefore, this hybrid layup structure outperforms structures using either the Archimedes helical path or the spatial grid topology path alone in terms of impact resistance, edge shear resistance, crack propagation suppression, and post-impact structural integrity, indicating a significant synergistic structural enhancement effect between the two layup trajectories.
[0096] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention.
Claims
1. An aramid / carbon fiber blend core rope TFP continuous lay ballistic helmet, characterized by, include: The fiber-reinforced composite shell is made by continuously laying aramid fiber / carbon fiber blend core rope with a predetermined mixing ratio through TFP to form a fiber preform, impregnating it with resin, and then molding and curing it. The fiber preform exhibits a gradient distribution of decreasing aramid fiber content and increasing carbon fiber content along the height direction from the top of the helmet to the brim. The area near the center of the top of the helmet is rich in aramid fibers, while the area near the brim is rich in carbon fibers. In the height direction, the mass ratio of aramid fiber to carbon fiber in the fiber preform is 20:80 to 80:
20.
2. The ballistic helmet of claim 1, wherein, The fiber preform, in the height direction from the top of the helmet to the brim, consists of an aramid enrichment zone, a first transition zone, a second transition zone, and a carbon fiber enrichment zone in sequence. The mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the aramid enrichment zone is 80:20, the mass ratio of aramid fiber to carbon fiber in the first transition zone is 60:40, the mass ratio of aramid fiber to carbon fiber in the second transition zone is 40:60, and the mass ratio of aramid fiber to carbon fiber in the carbon fiber enrichment zone is 20:
80.
3. A forming process for a ballistic helmet as claimed in claim 2, characterised in that, Includes the following steps: A TFP continuous layup device is used to continuously lay up aramid / carbon fiber blended core ropes with a predetermined mixing ratio. The blended core ropes are composed of aramid fiber bundles and carbon fiber bundles arranged side by side and bound together by wrapping yarn. The layup path starts from the center of the helmet top and follows the trajectory of an Archimedean spiral r=a+bθ and / or a spatial grid topology trajectory to sequentially form an aramid enrichment zone, a first transition zone, a second transition zone, and a carbon fiber enrichment zone, thus producing a fiber preform. In the equation r=a+bθ, r is the radial distance from any point on the layup trajectory to the center of the helmet top, in mm; θ is the polar angle, representing the angle of rotation of the layup trajectory around the helmet center; and a is the initial radius of the spiral, in mm. After weaving, the resulting fiber preform is immersed in a resin matrix and then cured by hot pressing to obtain a seamless bulletproof helmet.
4. The forming process of claim 3, wherein, When laid out according to the Archimedean spiral trajectory r=a+bθ, the aramid enrichment region satisfies the following conditions: the initial spiral region 0≤r<35mm, 0°≤θ<1300°; the first transition region satisfies 35mm≤r<70mm, 1300°≤θ<2200°; the second transition region satisfies 70mm≤r<100mm, 2200°≤θ<3000°; and the carbon fiber enrichment region satisfies 100mm≤r≤R, 3000°≤θ<3600°, where R is the maximum laying radius at the helmet edge.
5. The forming process of claim 4, wherein, During the laying of the aramid / carbon fiber blend core rope, the laying speed is 150mm / s, the core rope tension is 15N, the stitch pitch is 2.2mm, the row spacing is 1.5mm, the overlap rate of adjacent laying paths is 15-25%, the minimum laying turning radius is not less than 8mm, the laying speed is controlled at 120-180mm / s, the core rope tension is controlled at 8-15N, the stitch pitch is 1.8-2.5mm, and the row spacing is 1.2-1.8mm.
6. The forming process of claim 5, wherein, The aramid enrichment zone has a layup density of 0.80-0.90 fibers / mm, a layup spacing of 1.1-1.3mm, and 10-12 layers, with a corresponding thickness of approximately 8.0mm. The first transition zone has a layup density of 0.75-0.80 fibers / mm, 8-10 layers, and a thickness of approximately 7.0mm. The second transition zone has a layup density of 0.70-0.75 fibers / mm, 7-8 layers, and a thickness of approximately 6.2mm. The carbon fiber enrichment zone has a layup density of 0.65-0.70 fibers / mm, 6-7 layers, and a thickness of approximately 5.5mm.
7. A forming process according to claim 6, characterised in that, The mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the aramid enrichment zone is 80:20; the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the first transition zone is 60:40; the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the second transition zone is 40:60; and the mass ratio of aramid fiber to carbon fiber in the aramid fiber / carbon fiber blend core rope used to prepare the carbon fiber enrichment zone is 20:
80.
8. A forming process according to claim 7, characterised in that, The impregnation process of the fiber preform in the resin matrix was carried out under vacuum conditions, with a vacuum degree of -0.095 MPa and an impregnation time of 30 min.
9. The forming process of claim 8, wherein, The curing temperature is 150℃ and the curing time is 180 minutes.
10. The forming process of claim 9, wherein, The resin matrix is at least one of epoxy resin, vinyl ester resin, bismaleimide resin, and phenolic resin.
Citation Information
Patent Citations
Three-dimensional woven preform containing curable resin and bulletproof helmet
CN119433815A