A composite stabilizer for determining phosphorus content and a determination method

By using a composite stabilizer formulated with HEDP and KNO₃, the problems of Fe³⁺ interference and phosphate adsorption in high-pressure lithium iron phosphate materials were solved, achieving accuracy and reproducibility in phosphorus content determination and meeting the analytical requirements of high-end materials.

CN123155277APending Publication Date: 2026-11-24CHANGZHOU LIYUAN NEW ENERGY TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610904274.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies for determining phosphorus content in high-pressure lithium iron phosphate materials suffer from interference from high-concentration Fe³⁺ and phosphate adsorption losses, making it difficult to meet the accuracy and reproducibility requirements of high-end material research and development and quality control.

Method used

A composite stabilizer was formulated using hydroxyethylidene diphosphonic acid (HEDP) and potassium nitrate (KNO₃). HEDP complexes Fe³⁺ through multiple phosphonic acid groups, while KNO₃ provides high ionic strength and common ion effect, avoiding phosphate adsorption and promoting the precipitation of quinoline phosphomolybdate.

Benefits of technology

It effectively eliminates interference from high-concentration Fe³⁺, avoids phosphate adsorption loss, improves the accuracy and reproducibility of measurement results, and meets the analytical requirements of high-end materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123155277A_ABST
    Figure CN123155277A_ABST
Patent Text Reader

Abstract

This invention discloses a composite stabilizer and a method for determining phosphorus content. The composite stabilizer comprises the following components in molar concentrations: 0.1-0.2 mol / L hydroxyethylidene diphosphonic acid, 1.0-2.0 mol / L potassium nitrate, and the remainder being water. The determination method includes the following steps: (1) weighing a lithium iron phosphate sample and dissolving it in acid to obtain a phosphorus-containing test solution; (2) adding the composite stabilizer to the phosphorus-containing test solution to obtain a mixed solution; (3) heating the mixed solution to a slight boil, adding quinomolybdate reagent, cooling and aging to obtain a precipitate; (4) filtering, washing, drying, weighing, and calculating the phosphorus content of the precipitate. This invention couples the strong chemical masking effect of hydroxyethylidene diphosphonic acid with the high-strength physical shielding effect of potassium nitrate to reduce the high concentration of Fe in the phosphorus-containing test solution. 3+ It forms a stable water-soluble complex, preventing it from competing with phosphorus during the quinomolybdate reagent treatment process and improving the accuracy of the assay.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a stabilizer and a method for determining phosphorus content, and more particularly to a composite stabilizer for determining phosphorus content and a method for determining phosphorus content in lithium iron phosphate. Background Technology

[0002] The phosphomolybdicone gravimetric method (quinomolybdicone method) is a classic method for determining total phosphorus. In an acidic medium, phosphate ions react with quinomolybdicone reagent to form a yellow quinoline phosphomolybdate precipitate. After filtration, washing, drying, and weighing the precipitate, the phosphorus content is calculated. This method has the advantages of high accuracy and low equipment requirements.

[0003] However, in the analysis of high compaction (compacted density > 2.6 g / cm³) 3 When using lithium iron phosphate (LiFePO4) cathode materials, after the sample is digested with a strong acid (such as aqua regia), the test solution contains an extremely high concentration of iron ions (Fe2+). 3+ (typically >1000 mg / L), and possesses high ionic strength. High concentrations of Fe 3+ It strongly complexes with citric acid in quinomolybdate, competitively consuming the active ingredient, leading to incomplete or no precipitation of the target product, quinoline phosphomolybdate, resulting in a significant negative error. Simultaneously, phosphate ions readily adsorb onto the surface of acidic glassware, causing transfer loss and further affecting the accuracy of the results. Existing techniques typically improve this by increasing the amount of masking agent, repeated washing, or extending the aging time. For example, CN107037036A discloses a method for determining phosphorus content in lithium iron phosphate, using tannic acid, citric acid, or KCN as masking agents. However, the effect is limited and cannot fundamentally solve the problem of high-concentration Fe... 3+ Interference and phosphorus adsorption losses make it difficult to meet the accuracy and reproducibility requirements of high-end material research and development and quality control. Summary of the Invention

[0004] Purpose of the invention: The purpose of this invention is to provide a method for effectively masking Fe in the determination of phosphorus content in high-pressure lithium iron phosphate materials. 3+ The second objective of this invention is to provide a method for determining the phosphorus content in lithium iron phosphate using the aforementioned composite stabilizer, which also avoids the loss of phosphate ions due to adsorption on the surface of glassware.

[0005] Technical solution: The composite stabilizer for determining phosphorus content of the present invention comprises the following components in molar concentrations: 0.1~0.2 mol / L hydroxyethylidene diphosphonic acid, 1.0~2.0 mol / L potassium nitrate, and the balance being water.

[0006] Hydroxyethylidene diphosphonic acid (HEDP) is acidic, and its concentration is directly related to the pH of the composite stabilizer. When HEDP is within this concentration range, the pH of the stabilizer is 1~1.5. If the amount of HEDP is too small, the pH of the composite stabilizer will be too high (>1.5), causing ferric phosphate to precipitate and affecting the measurement results. If the amount of HEDP is too large, the pH of the composite stabilizer will be too low (<1), which will inhibit the complexation ability of citric acid in the quinomolybdate reagent to molybdate ions during the subsequent treatment process, affecting the formation of quinoline phosphomolybdate precipitate.

[0007] Hydroxyethylidene diphosphonic acid (HEDP) contains multiple phosphonic acid groups (-PO3H2) in its molecule, which can be fully protonated in water to maximize the complexation of Fe. 3+ Furthermore, it remains stable even under strongly acidic conditions, maintaining a high level of protonation and high complexing activity. Moreover, HEDP possesses significant steric hindrance, which can enhance its ability to bind Fe... 3+ Forming a "cage-like" enclosure, effectively blocking Fe 3+ Contact with citric acid from phosphate or quinomolybdate-limonene reagents prevents the formation of ferric phosphate or heteropolyacid precipitates (such as ferric phosphomolybdate) at the source. Furthermore, HEDP is stable in high-temperature environments and does not easily decompose under heating conditions, avoiding the introduction of additional interference.

[0008] Preferably, the aforementioned composite stabilizer is prepared using a 60% HEDP aqueous solution.

[0009] Preferably, the water is deionized water.

[0010] Potassium nitrate (KNO3) completely dissociates in water, acting as an ionic strength modifier and providing a common ion effect. The potassium ions (K+) released from KNO3 dissociate... + It provides extremely high ionic strength, effectively compressing the electric double layer of phosphate ions, neutralizing the electrostatic adsorption of phosphate ions on the glass surface, and preventing phosphorus loss caused by phosphate adsorption on the glass surface; while nitrate (NO3) - With high steric hindrance and solvation degree, it hardly forms sparingly soluble salts with metal ions, avoiding the introduction of additional precipitation interference. Furthermore, it has weak corrosiveness to glass and metal equipment, facilitating experimental operation and glassware maintenance. Meanwhile, K... + It is the balancing cation required for the formation of quinoline phosphomolybdate precipitate during the subsequent quinoline phosphomolybdate treatment, promoting the precipitation of quinoline phosphomolybdate precipitate and making its crystal structure more compact, which is convenient for filtration and washing.

[0011] The method for determining the phosphorus content in lithium iron phosphate according to the present invention includes the following steps:

[0012] (1) Weigh the lithium iron phosphate sample and dissolve it in acid to obtain a phosphorus-containing test solution;

[0013] (2) Add a composite stabilizer for determining phosphorus content to the phosphorus-containing test solution to obtain a mixed solution;

[0014] (3) After heating the mixed solution to a gentle boil, add the quinomolybdate reagent, cool and age to obtain a precipitate;

[0015] (4) Filter, wash, and dry the precipitate, weigh it and calculate the phosphorus content.

[0016] In step (1), the acid is one of aqua regia and a nitric acid-perchloric acid mixed solution, which is highly acidic and can completely dissolve the lithium iron phosphate sample.

[0017] Preferably, in step (1), the volume ratio of nitric acid to perchloric acid in the nitric acid-perchloric acid mixed solution is (3~5):1.

[0018] Preferably, in step (1), the amount of acid used is 5 to 10 times the mass of the lithium iron phosphate sample to ensure that the sample is completely dissolved and leaves no residue.

[0019] Preferably, in step (1), the dissolution process is heated to promote the dissolution of the lithium iron phosphate sample.

[0020] In step (1), the pH of the phosphorus-containing test solution is ≤1 to prevent Fe 3+ Hydrolysis and loss due to the formation of colloids or precipitates from phosphates.

[0021] In step (2), the amount of composite stabilizer used is 20-30 mL per 1 g of lithium iron phosphate sample, ensuring sufficient Fe in the composite stabilizer and phosphorus-containing test solution. 3+ Reaction, efficient complexation of Fe 3+ At this point, due to the dissociation of KNO3 in the composite stabilizer, K... + It has a certain degree of weak alkalinity, which can slightly neutralize phosphorus-containing test solutions, raising the pH of the mixed solution to 1~1.5, thus preventing the citric acid in the quinomolybdate reagent from being deactivated during subsequent quinomolybdate reagent treatment.

[0022] In step (2), the mixed solution is diluted with water to 1.8 to 2.7 times its original volume to ensure that the composite stabilizer is within the effective ionic strength range, providing the optimal liquid phase space for the full growth of quinoline phosphomolybdate crystals.

[0023] In step (3), the slight boiling is at 95~100℃, at which point the solution maintains a slight boil, with a small number of bubbles continuously escaping from the surface but not violently churning. The slight boiling state provides sufficient heat energy to the system, ensuring the rapid formation of quinoline phosphomolybdate precipitate; at the same time, the gentle thermal convection helps to form large, uniform crystals, avoiding precipitate splashing loss or decomposition of quinoline phosphomolybdate reagent caused by violent boiling.

[0024] Preferably, in step (3), the solution is continuously stirred during heating and adding of the quinomolybdate reagent to ensure that the solution is fully heated and the quinomolybdate reagent is uniformly dispersed in the solution.

[0025] Preferably, in step (3), the amount of quinomolybdate reagent added is 1.5 to 2.0 times the theoretical molar amount of phosphorus in lithium iron phosphate, to ensure that the phosphorus in the mixed solution reacts fully with the quinomolybdate reagent to generate quinoline phosphomolybdate.

[0026] In step (3), after adding the quinomolybdate reagent, maintain a gentle boil for 1-2 minutes to avoid violent boiling that could cause precipitate splashing or solution turbulence, so that the precipitate can coat the unreacted mother liquor or Fe during the growth process. 3+ Impurities.

[0027] In step (3), the cooling and aging temperature is 70-80℃, and the time is 30-60 min. Aging is used to dissolve and recrystallize the microcrystals onto the surface of large crystals, generating coarse, uniform, and dense crystals. This process significantly reduces the specific surface area of ​​the precipitate, reduces impurity adsorption, and greatly improves the performance of subsequent filtration and washing, ensuring the accuracy and reproducibility of the measurement results. If the aging time is too long, it will cause the quinoline phosphomolybdate precipitate to age excessively, making filtration difficult, or it will cause the quinoline phosphomolybdate precipitate to form a loose structure with a high specific surface area, significantly increasing the filtration efficiency of unreacted mother liquor or Fe. 3+ The adsorption and encapsulation of impurities, nitrates, and organic decomposition products lead to an increase in the precipitate mass and introduce errors.

[0028] In step (4), the phosphorus content is calculated in the following way:

[0029] ,

[0030] in, m sinking The total mass of the filter paper and crucible containing the precipitate. m empty For the quality of filter paper and crucible, m-type The mass of the lithium iron phosphate sample in step (1) is denoted as 0.1401. 0.1401 is the conversion factor for quinoline phosphomolybdate to phosphorus, calculated based on the fixed molecular composition of the quinoline phosphomolybdate precipitate ((C9H7N)3[H3PO4·12MoO3]), and is a well-known factor for converting quinoline phosphomolybdate to elemental phosphorus.

[0031] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) A composite stabilizer synergistically formulated with hydroxyethylidene diphosphonic acid (HEDP) and potassium nitrate (KNO3) is prepared, which couples the strong chemical masking effect of HEDP with the high-strength physical shielding effect of KNO3. HEDP preferentially reacts with the high concentration of Fe in the phosphorus-containing test solution. 3+This forms a stable water-soluble complex, preventing it from competing with phosphorus during treatment with quinomolybdate-limonene reagent, thus fundamentally solving the problem of high-concentration Fe. 3+ Interference; simultaneously, KNO3 creates a high ionic strength environment, which shields Fe already complexed with HEDP. 3+ The complex activity is reduced, and the activity of ions in the solution, including phosphate, molybdate, and quinoline ions, is decreased, and this is achieved through K... + The common ion effect specifically reduces the solubility of quinoline phosphomolybdate precipitate, and promotes the selective and rapid formation of the target precipitate while suppressing interference; (2) The high ionic strength of KNO3 effectively compresses the double electric layer of phosphate ions, neutralizes the electrostatic adsorption of phosphate ions on the surface of glassware, avoids phosphorus loss caused by phosphate adsorption on the surface of glassware, and solves the physical and equilibrium contradiction between "phosphate adsorption loss" and "precipitation condition optimization". Attached Figure Description

[0032] Figure 1 This is a photograph of the conical flask after the reaction in Example 1 of the present invention has ended;

[0033] Figure 2 This is a photograph of the conical flask after the reaction in Comparative Example 2 of this invention has ended. Detailed Implementation

[0034] The technical solution of the present invention will be further described below with reference to the embodiments and comparative examples. Unless otherwise stated, all reagents used are commercially available and are used directly without purification.

[0035] Example 1

[0036] 1. Formulation of composite stabilizers

[0037] The specific steps for preparing a composite stabilizer stock solution (pH≈1.0) with a concentration of 0.10 mol / L hydroxyethylidene diphosphonic acid (HEDP) and 1.0 mol / L potassium nitrate (KNO3) are as follows:

[0038] In a 50 mL beaker, precisely add 2.37 mL of 60% HEDP aqueous solution and 20 mL of deionized water, and stir to mix well. Then, add 10.11 g of potassium nitrate solid (AR) in batches, stirring until completely dissolved. Transfer the resulting solution to a 100 mL volumetric flask, wash the beaker with deionized water and dilute to the mark, shake well, and obtain the composite stabilizer for determining phosphorus content.

[0039] 2. Determination of phosphorus content in high-pressure lithium iron phosphate samples

[0040] (1) Sample digestion: Accurately weigh 1.000 g of standard high-pressure lithium iron phosphate sample into a polytetrafluoroethylene beaker, add 10 mL of aqua regia, and heat on a hot plate until the solution is clear. After cooling, quantitatively transfer the solution to a 250 mL volumetric flask, dilute with dilute nitric acid (volume ratio 1:9) and make up to the mark, shake well to obtain a phosphorus-containing test solution with a pH ≤ 1.

[0041] (2) Pre-precipitation treatment: Accurately transfer 15.00 mL of phosphorus-containing test solution into a 500 mL Erlenmeyer flask. Add 20.0 mL of the aforementioned composite stabilizer and rinse the flask wall with a small amount of deionized water. Then, place the Erlenmeyer flask in an ultrasonic cleaner and sonicate for 2 minutes to desorb any phosphate ions that may adhere to the flask wall.

[0042] (3) Precipitation and Aging: Remove the conical flask and dilute with water to approximately 80 mL. Heat on a hot plate to 95°C, bringing the solution to a gentle boil. With magnetic stirring, slowly and evenly add 50 mL of quinomolybdate reagent using a dispenser. Continue to maintain a gentle boil for 2 minutes. Then transfer the conical flask to a 70°C constant temperature water bath and age for 45 minutes to ensure complete precipitation and maturation. The conical flask after the reaction is complete is as follows: Figure 1 As shown.

[0043] (4) Filtration, drying, and weighing: Filter using a G4 glass frit crucible pre-dried to constant weight at 180℃. Place the crucible in an oven and dry at 180℃ for 1 hour. After drying, remove it and place it in a desiccator to cool to room temperature, then weigh accurately. Calculate the phosphorus content using the following formula:

[0044] ,

[0045] in, m sinking The total mass of the filter paper and crucible containing the precipitate. m empty For the quality of filter paper and crucible, m-type 0.1401 is the mass of the lithium iron phosphate sample in step (1), and 0.1401 is the conversion factor of quinoline phosphomolybdate to phosphorus.

[0046] To ensure the accuracy and precision of this method, at least two parallel determinations should be performed, with resampling for each parallel determination. The result deviation (i.e., the ratio of the difference between the maximum and minimum measured values ​​to the arithmetic mean of all measured values) should not exceed ±0.3%. If the result deviation exceeds this range, resampling and determination should be performed. In this embodiment, two parallel determinations were performed, and the arithmetic mean of the two measurements was used as the final test result, yielding a phosphorus content of 19.47% in the sample.

[0047] 3. Verification

[0048] To verify the accuracy of the method, inductively coupled plasma optical emission spectrometry (ICP-OES) was used as a control method to measure the same sample, and the result was 19.49%, with a relative deviation of 0.02%. The results of the method of this invention are highly consistent with those of the ICP-OES method, with minimal difference, which fully demonstrates that the composite stabilizer and determination method provided by this invention can completely eliminate high concentrations of Fe. 3+ Interference and phosphorus adsorption losses were minimized, achieving accuracy and precision approaching that of instrumental analysis, fully meeting the stringent requirements for phosphorus content determination in high-pressure lithium iron phosphate materials; simultaneously, by Figure 1 It can be seen that no obvious adsorption was observed on the surface of the glassware used in the experiment, indicating that the addition of composite stabilizer can significantly reduce the adsorption loss on the surface of the glassware.

[0049] Example 2

[0050] 1. Formulation of composite stabilizers

[0051] Using the same preparation method as in Example 1, 3.6 mL of 60% HEDP aqueous solution was accurately measured, and 15.16 g of potassium nitrate was accurately weighed to prepare a composite stabilizer stock solution with a concentration of 0.15 mol / L hydroxyethylidene diphosphonic acid (HEDP) and 1.5 mol / L potassium nitrate (KNO3) (pH≈1.0).

[0052] 2. Determination of phosphorus content in high-pressure lithium iron phosphate samples

[0053] (1) Sample digestion: Accurately weigh 1.000 g of standard high-pressure lithium iron phosphate sample into a polytetrafluoroethylene beaker, add 10 mL of nitric acid-perchloric acid mixed solution (volume ratio of nitric acid to perchloric acid is 4:1), and heat on a hot plate to digest until the solution is clear. After cooling, quantitatively transfer the solution to a 250 mL volumetric flask, dilute with dilute nitric acid (volume ratio 1:9) and make up to the mark, shake well to obtain a phosphorus-containing test solution with a pH ≤ 1. The volume ratio of nitric acid to perchloric acid can be selected from (3~5):1, all of which can achieve similar results.

[0054] (2) Pre-precipitation treatment: Accurately transfer 10.00 mL of phosphorus-containing test solution into a 500 mL Erlenmeyer flask. Add 30.00 mL of the aforementioned composite stabilizer and rinse the flask wall with a small amount of deionized water. Then, place the Erlenmeyer flask in an ultrasonic cleaner and sonicate for 2 minutes to desorb any phosphate ions that may adhere to the flask wall.

[0055] (3) Precipitation and aging: Take out the conical flask and dilute it with water to a total volume of about 80 mL. Place it on a hot plate and heat it to 97°C to bring the solution to a gentle boil. With magnetic stirring, slowly and evenly add 50 mL of quinomolybdate reagent using a dispenser. Continue to maintain a gentle boil for 1.5 minutes. Then transfer the conical flask to an 80°C constant temperature water bath and age it for 30 minutes to allow the precipitation to be complete and mature.

[0056] (4) Filtration, drying and weighing: The sample was filtered, dried and weighed in the same way as in Example 1 and two parallel measurements were performed. The arithmetic mean of the two measurements was taken as the final test result. The phosphorus content in the sample was calculated to be 19.39%, and compared with the ICP-OES result (19.45%), the relative deviation was 0.06%, which was still within the acceptable range (the relative deviation between the calculated phosphorus content in the sample and the ICP-OES result was ≤0.3%). No obvious residue was observed on the surface of the glassware used in the experiment.

[0057] Meanwhile, it was observed that the precipitate particles were slightly larger, resulting in a slight increase in filtration speed, but the viscosity of the stabilizer solution itself increased. This indicates that the phosphorus precipitation reaction can still be quantitatively completed at this high concentration ratio, proving that the present invention has a certain degree of concentration redundancy and operational tolerance. However, a higher HEDP concentration may slightly introduce the risk of blank values ​​due to phosphorus impurities in the reagent itself, and reaching a KNO3 concentration of 1.5 mol / L does not provide significant additional benefits but instead increases reagent costs. Therefore, although this formulation is feasible, it is not the most economically optimal choice.

[0058] Example 3

[0059] 1. Formulation of composite stabilizers

[0060] Using the same preparation method as in Example 1, 4.8 mL of 60% HEDP solution was accurately measured, and 20.22 g of potassium nitrate was accurately weighed to prepare a composite stabilizer stock solution with a concentration of 0.2 mol / L hydroxyethylidene diphosphonic acid (HEDP) and 2.0 mol / L potassium nitrate (KNO3) (pH≈1.0).

[0061] 2. Determination of phosphorus content in high-pressure lithium iron phosphate samples

[0062] (1) Sample digestion: Accurately weigh 1.000 g of standard high-pressure lithium iron phosphate sample into a polytetrafluoroethylene beaker, add 10 mL of aqua regia, and heat on a hot plate until the solution is clear. After cooling, quantitatively transfer the solution to a 250 mL volumetric flask, dilute with dilute nitric acid (volume ratio 1:9) and make up to the mark, shake well to obtain a phosphorus-containing test solution with a pH ≤ 1.

[0063] (2) Pre-precipitation treatment: Accurately transfer 10.00 mL of the above test solution into a 500 mL Erlenmeyer flask. Add 20.0 mL of the aforementioned composite stabilizer and rinse the flask wall with a small amount of deionized water. Then, place the Erlenmeyer flask in an ultrasonic cleaner and sonicate for 2 minutes to desorb any phosphate ions that may adhere to the flask wall.

[0064] (3) Precipitation and aging: Take out the conical flask and dilute it with water to a total volume of about 80 mL. Place it on a hot plate and heat it to 100°C to bring the solution to a gentle boil. With magnetic stirring, slowly and evenly add 50 mL of quinomolybdate reagent using a dispenser. Continue to maintain a gentle boil for 1 minute. Then transfer the conical flask to a 75°C constant temperature water bath and age it for 60 minutes to allow the precipitation to be complete and mature.

[0065] (4) Filtration, drying and weighing: The sample was filtered, dried and weighed in the same way as in Example 1 and two parallel measurements were performed. The arithmetic mean of the two measurements was used as the final test result. The phosphorus content in the sample was calculated to be 19.35%. Compared with the ICP-OES result (19.43%), the relative deviation was 0.08%, which was still within the acceptable range. No obvious residue was observed on the surface of the glassware used in the experiment.

[0066] Meanwhile, the precipitate particles were slightly larger, resulting in a slight increase in filtration speed, but the viscosity of the stabilizer solution itself increased. Transferring and mixing required longer times, and although the deviation remained within acceptable limits, it was the lowest among the three examples. Furthermore, the high concentration of salts may introduce a slight tendency for crystallization. This indicates that the upper limit concentration ratio still ensures quantitative precipitation of phosphorus, verifying that the concentration boundary of the present invention is safe and effective. However, its measurement accuracy is slightly lower than in Examples 1 and 2, its operational convenience is reduced, its reagent cost is the highest, and there is a potential risk of interference introduced by reagent impurities. This ratio is mainly suitable for verifying the robustness of the method; in practical applications, Example 1 (optimal ratio) is the preferred option.

[0067] Example 4

[0068] Four parallel measurements were performed using Example 1, and the results of each parallel measurement are shown in Table 1.

[0069] Table 1. Results of phosphorus content determination in lithium iron phosphate in Example 4

[0070] As shown in Table 1, the deviation between the four detection results and the ICP-OES results is small, indicating that the method of the present invention has good detection stability.

[0071] Comparative Example 1

[0072] The difference from Example 1 is that no composite stabilizer was added; otherwise, it was the same as Example 1. The calculated phosphorus content in the sample deviated from the ICP-OES result by approximately 1.41%, and insufficient yellow quinoline phosphomolybdate precipitate could not be formed, with severe adhesion to the sample walls. This indicates that without the composite stabilizer, the high concentration of Fe in the high-pressure compaction lithium iron phosphate sample... 3+ It cannot be adequately masked, and it severely interferes with the results of phosphorus content testing.

[0073] Comparative Example 2

[0074] The difference from Example 1 is that KNO3 was not added when preparing the composite stabilizer, and the stabilizer only contained 0.10 mol / L HEDP. Everything else was the same as in Example 1. The conical flask after the reaction was completed was as follows: Figure 2 As shown. The calculated phosphorus content in the sample deviates from that obtained by ICP-OES by approximately 0.33%, but due to... Figure 2 It can be seen that the precipitate on the glassware has obvious adhesion, the filtration speed is slow, and the precision of phosphorus content determination decreases, proving that KNO3 is essential for preventing adsorption and ensuring precision.

[0075] Comparative Example 3

[0076] The difference from Example 1 is that HEDP was not added when preparing the composite stabilizer; the stabilizer only contained 1.0 mol / L KNO3 solution, otherwise it was the same as Example 1. The calculated phosphorus content in the sample deviated from the ICP-OES result by approximately 0.44%, and the quinoline phosphomolybdate precipitation was incomplete, resulting in a turbid solution, proving that the absence of HEDP prevented the elimination of Fe. 3+ Chemical interference.

[0077] Comparison Column 4

[0078] The difference from Example 1 is that the concentrations of each component in the composite stabilizer preparation were HEDP 0.05 mol / L, KNO3 0.5 mol / L, and the stabilizer pH ≈ 1.0; the rest was the same as in Example 1. The calculated phosphorus content in the sample deviated from the ICP-OES result by approximately 0.32%, indicating a significant systematic error. The obtained quinoline phosphomolybdate precipitate was yellowish, indicating that Fe... 3+ The shielding was incomplete, with signs of residue or co-precipitation, and the amount of adhering residue on the reactor wall was significantly increased.

[0079] This indicates that at this low concentration ratio, the insufficient HEDP concentration prevents it from completely complexing the high concentration of Fe in the phosphorus-containing test solution. 3+ Unmasked Fe 3+It will compete with molybdate for reaction, inhibiting the quantitative formation of the target phosphomolybdate quinoline. Simultaneously, insufficient KNO3 concentration weakens its "salt effect," increasing the solubility of the precipitate while reducing its effectiveness in preventing the adsorption of phosphate and the precipitate on the glass surface. Therefore, this formulation cannot guarantee the accuracy of the determination and carries a clear risk.

[0080] Comparative Example 5

[0081] The difference from Example 1 is that an equal amount of citric acid was used instead of HEDP, and the stabilizer pH≈1.0 was used. Everything else was the same as in Example 1. The calculated phosphorus content in the sample deviated from the ICP-OES result by approximately 1.25%. During the experiment, very little quinoline phosphomolybdate precipitate was formed. The solution turned a turbid orange-yellow color after the addition of quinoline phosphomolybdate reagent, and sufficient, pure yellow quinoline phosphomolybdate precipitate could not be obtained by filtration. This demonstrates that under strongly acidic conditions of pH 1-1.5, citric acid is almost unable to complex high concentrations of Fe. 3+ This leads to Fe 3+ Chemical interference was severe, and the precipitation reaction of quinoline phosphomolybdate was significantly inhibited.

[0082] Comparative Example 6

[0083] The difference from Example 1 is that an equal amount of tannic acid was used instead of HEDP; otherwise, the results were the same as in Example 1. The calculated phosphorus content in the sample deviated from the ICP-OES result by approximately -1.06%. During the experiment, after adding the composite stabilizer, a large amount of brown flocculent precipitate immediately formed in the solution. After adding the quinomolybdate reagent, the system turned into a dark turbid liquid, and no clear yellow precipitate could be observed. The filtered solid was a mixture of discolored substances. This indicates that most tannic acid molecules exist in the form of undissociated phenolic hydroxyl groups, and their coordination ability is further suppressed. Furthermore, under strongly acidic conditions of pH 1-1.5, the solubility of tannic acid itself decreases sharply, easily resulting in brown flocculent precipitates or colloids. These precipitates cannot be uniformly dispersed in the test solution to provide a masking effect and instead introduce solid impurities that encapsulate the analyte. Moreover, even if some Fe... 3+ Temporarily chelated, tannic acid cannot prevent the remaining Fe 3+ It reacts with phosphate to form ferric phosphate precipitates or colloids, and unlike HEDP, it cannot react with Fe through phosphonic acid groups. 3+ It forms a "cage-like" enclosure, thus making it impossible to eliminate Fe. 3+ Competitive interference with the precipitation reaction of quinoline phosphomolybdate.

[0084] Comparative Example 7

[0085] The difference from Example 1 is that an equal amount of HNO3 was used instead of KNO3; otherwise, it was the same as Example 1. The calculated phosphorus content in the sample deviated from that of ICP-OES by approximately 0.8%. Experiments showed that the final precipitate particles were extremely fine and slurry-like, forming a dense, difficult-to-transfer layer on the glass vessel wall, resulting in slow filtration and significant losses. This indicates that providing only HNO3... + The lack of KNO3 ionic strength prevents the formation of large crystals and instead worsens the physical morphology of the precipitate, resulting in significant transfer losses.

[0086] Comparative Example 8

[0087] The difference from Example 1 is that an equal amount of NaNO3 was used instead of KNO3; otherwise, the results were the same as in Example 1. The calculated phosphorus content in the sample deviated from the ICP-OES result by approximately -0.36%, and the precipitation process was accompanied by a slight milky white turbidity. This may be due to the presence of Na... + The introduction of [a substance] forms slightly soluble sodium salt impurities with molybdate or phosphate in the system. The co-precipitation of these impurities leads to a slight increase in the measured total mass.

[0088] Comparative Example 9

[0089] The difference from Example 1 is that an equal amount of KCl was used instead of KNO3; otherwise, it was the same as Example 1. The calculated phosphorus content in the sample deviated from the ICP-OES result by approximately 0.52%. During the experiment, the solution abnormally darkened in color (yellowish-brown) after heating, and the resulting precipitate was dark in color. This indicates that Cl... - As a ligand, with Fe 3+ A stable yellow ferric chloride complex ion was formed, which competitively consumed Fe. 3+ It interferes with the formation of phosphomolybdic acid heteropolyacids, altering the composition of the precipitate. Meanwhile, Cl... - It has the potential to corrode equipment.

Claims

1. A complex stabilizer for determining phosphorus content, characterized by, The components include the following molar concentrations: 0.1~0.2 mol / L hydroxyethylidene diphosphonic acid, 1.0~2.0 mol / L potassium nitrate, and the balance being water.

2. A method for determining the phosphorus content in lithium iron phosphate, characterized by, Includes the following steps: (1) Weigh the lithium iron phosphate sample and dissolve it in acid to obtain a phosphorus-containing test solution; (2) Add a composite stabilizer for determining phosphorus content to the phosphorus-containing test solution to obtain a mixed solution; (3) After heating the mixed solution to a gentle boil, add the quinomolybdate reagent, cool and age to obtain a precipitate; (4) Filter, wash, and dry the precipitate, weigh it and calculate the phosphorus content.

3. The assay method according to claim 2, characterized in that, In step (1), the acid is either aqua regia or a nitric acid-perchloric acid mixed solution.

4. The assay method according to claim 2, characterized by, In step (1), the pH of the phosphorus-containing test solution is ≤1.

5. The assay method according to claim 2, characterized by, In step (2), the amount of composite stabilizer used is 20-30 mL per 1 g of lithium iron phosphate sample.

6. The assay method according to claim 2, characterized by, In step (2), the mixed solution is diluted with water to 1.8 to 2.7 times its original volume.

7. The determination method according to claim 2, characterized in that, In step (3), the micro-boiling temperature is 95~100℃.

8. The determination method according to claim 2, characterized in that, In step (3), after adding the quinomolybdate reagent, maintain a gentle boil for 1-2 minutes.

9. The determination method according to claim 2, characterized in that, In step (3), the cooling and aging temperature is 70~80℃ and the time is 30~60min.

10. The determination method according to claim 2, characterized in that, In step (4), the phosphorus content is calculated in the following way: , in, m sinking The total mass of the filter paper and crucible containing the precipitate. m empty For the quality of filter paper and crucible, m-type The mass of the lithium iron phosphate sample in step (1) is the mass of the sample.

Citation Information

Patent Citations

  • Measuring method of phosphorus content in lithium iron phosphate

    CN107037036A