A method for detecting the impact strength of titanium dioxide in PC resin
By optimizing the processing temperature, drying conditions, and the use of lubricants, a method for testing the impact strength of titanium dioxide in PC resin suitable for small laboratory equipment was established. This method solves the problems of high testing cost, long cycle, and inaccurate results in the existing technology, and achieves rapid and accurate testing results.
Patent Information
- Application Number
- CN202611098560.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies cannot quickly and accurately detect the impact strength of titanium dioxide in PC resin using small laboratory equipment, resulting in high testing costs, long testing cycles, and inaccurate results.
By optimizing the processing temperature, sample drying conditions, and notch forming conditions, an impact strength testing method suitable for titanium dioxide samples in the kilogram range was established. The method includes four steps: color particle preparation, sample preparation, condition adjustment, and impact strength testing. Pentaerythritol stearate was used as a lubricant to ensure uniform dispersion of titanium dioxide in PC resin.
It enables rapid and low-cost impact strength testing of titanium dioxide samples in the kilogram range. The test results are accurate, reliable, and reproducible, significantly reducing sample consumption and testing time, making it suitable for batch screening in laboratory pilot-scale tests.
Smart Images

Figure CN123155278A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of titanium dioxide application performance testing technology, and more specifically, to a method for testing the impact strength of titanium dioxide in PC resin. Background Technology
[0002] Polycarbonate (PC) is a high molecular polymer containing carbonate groups in its molecular chain. It has high light transmittance and excellent impact resistance, and is widely used in electronics, automobiles, construction and other fields.
[0003] Adding titanium dioxide to PC resin can improve the whiteness and hiding power of PC products. At the same time, titanium dioxide can absorb and scatter ultraviolet rays, which can enhance the weather resistance of PC products and slow down the aging rate of PC under light. In addition, adding an appropriate amount of titanium dioxide can also improve the heat resistance of PC, enhance the stability during high-temperature processing, reduce deformation problems caused by temperature changes, and thus improve the processing performance of PC.
[0004] However, the addition of titanium dioxide can also bring negative effects. On the one hand, titanium dioxide has a certain catalytic degradation effect, which may accelerate the degradation of PC molecular chains during high-temperature processing; on the other hand, titanium dioxide has poor interfacial compatibility with PC resin, easily leading to insufficient dispersibility. All of these factors can significantly reduce the impact resistance of PC products. Therefore, in the research and development of PC-specific titanium dioxide, accurately testing the impact strength of titanium dioxide / PC composites under specific processing conditions is of great significance for evaluating the application performance of titanium dioxide.
[0005] Currently, the impact strength testing of titanium dioxide in PC resin mainly relies on large-scale production lines, requiring tens or even more kilograms of titanium dioxide samples. This results in long testing cycles and high costs, failing to meet the rapid testing needs of laboratory-scale titanium dioxide samples weighing less than one kilogram. Furthermore, laboratory-grade small twin-screw extruders and injection molding machines differ significantly from large-scale production equipment in terms of processing temperature, sample moisture control, and titanium dioxide dispersion conditions. Directly applying testing methods from large-scale production makes it difficult to obtain accurate and reproducible results.
[0006] Therefore, there is an urgent need to establish a PC resin impact strength testing method that is applicable to titanium dioxide samples in the kilogram range and has a short testing cycle, low cost, and accurate and reliable results. Summary of the Invention
[0007] The purpose of this invention is to overcome the relatively poor dispersion conditions of laboratory-grade small twin-screw extruders and injection molding machines by optimizing key process parameters such as processing temperature, sample drying conditions, and notch forming conditions, and to establish a rapid method for testing the impact strength of titanium dioxide in PC resin at kilogram levels or below.
[0008] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: According to an aspect of the present invention, a method for testing the impact strength of titanium dioxide in PC resin is provided, comprising the following steps: Color particle preparation: Titanium dioxide and PC resin are mixed, melt extruded, cooled, and granulated to obtain color particles; Sample preparation: The color particles are dried and then injection molded to obtain the sample. Spline conditioning: The spline is conditioned in a constant temperature and humidity environment; Impact strength test: The impact strength of the spline after condition adjustment is tested.
[0009] In one embodiment of the present invention, in the step of preparing the colored particles, the amount of titanium dioxide added is 5%-15% of the mass of PC resin.
[0010] In one embodiment of the present invention, in the step of preparing colored particles, pentaerythritol stearate is added, wherein the amount of pentaerythritol stearate added is not higher than 0.5% of the mass of PC resin.
[0011] In one embodiment of the present invention, in the step of preparing colored particles, the maximum processing temperature of melt extrusion is 250°C-290°C; the cooling method is water cooling.
[0012] In one embodiment of the present invention, in the sample preparation step, the drying temperature of the color particles is 120℃±2℃, and the drying time is 1-4 hours.
[0013] In one embodiment of the present invention, in the sample preparation step, the color particles are laid flat in an enamel or stainless steel tray with a thickness of ≤1cm.
[0014] In one embodiment of the present invention, the maximum processing temperature for injection molding in the sample preparation step is 250°C-290°C.
[0015] In one embodiment of the present invention, in the step of spline state conditioning, the temperature of the constant temperature and humidity environment is 23℃±2℃, the relative humidity is 50%±5%, and the state conditioning time is at least 16 hours.
[0016] In one embodiment of the present invention, in the step of spline state adjustment, the number of splines is 5 parallel splines.
[0017] In one embodiment of the present invention, in the step of preparing the sample strip, the injection molding is carried out in accordance with the GB / T 1843 / A standard; in the step of impact strength testing, the impact strength testing is carried out in accordance with the GB / T 1843 / 8.2 standard.
[0018] By adopting the above technical solution, the present invention has the following advantages compared with the prior art: (1) This invention provides a rapid test method for the impact strength of titanium dioxide in PC resin at a level of less than one kilogram. It has the advantages of requiring less sample and not needing to use tens of kilograms of titanium dioxide sample at a time; short test cycle, saving 2-3 hours of test time at a time; and low test cost.
[0019] (2) The method of the present invention only requires a titanium dioxide sample of less than one kilogram to complete the impact strength test, while the existing large production line testing method requires tens of kilograms or even more titanium dioxide samples, which greatly reduces the sample quantity requirements in the titanium dioxide research and development test stage.
[0020] (3) By optimizing process parameters such as drying time and processing temperature, the present invention can save 2-3 hours per detection cycle compared with existing methods, which significantly improves detection efficiency.
[0021] (4) This invention reduces the detection cost in many ways, such as reducing the amount of titanium dioxide sample used, reducing the power consumption of detection, and shortening the detection time, and is suitable for batch rapid screening in the laboratory pilot stage.
[0022] (5) This invention is designed for the characteristics of laboratory small twin-screw extruders and injection molding machines. It systematically optimizes key parameters such as processing temperature, drying conditions and cooling methods, overcomes the disadvantage of poor dispersion conditions in laboratory small equipment, and the test results have good reproducibility (the difference in impact strength between parallel samples is <10kJ / m²), which can truly reflect the impact performance of titanium dioxide in PC resin. Attached Figure Description
[0023] Figure 1 A schematic flowchart of a method for testing the impact strength of titanium dioxide in PC resin provided in an embodiment of the present invention is shown. Figure 2 The following diagram illustrates the influence of different formulations and sample preparation conditions on the impact strength of PC in Examples 1-8 of this invention. Detailed Implementation
[0024] It should be understood that the embodiments of the invention shown in the exemplary embodiments are merely illustrative. Although only a few embodiments have been described in detail in this invention, those skilled in the art will readily recognize that various modifications are possible without substantially departing from the teachings of the invention. Accordingly, all such modifications should be included within the scope of the invention. Other substitutions, modifications, variations, and deletions can be made to the design, operating conditions, and parameters of the following exemplary embodiments without departing from the spirit of the invention.
[0025] Figure 1 A schematic flowchart of a method for testing the impact strength of titanium dioxide in PC resin according to an embodiment of the present invention is shown. Figure 1 As shown, a method for testing the impact strength of titanium dioxide in PC resin includes the following steps: S1. Preparation of colored particles: Titanium dioxide and PC resin are mixed, melt extruded, cooled, and granulated to obtain colored particles; S2. Sample preparation: The color particles are dried and then injection molded to obtain the sample; S3. Spline conditioning: Condition the spline under constant temperature and humidity. S4. Impact strength test: Perform impact strength test on the spline after condition adjustment.
[0026] This invention optimizes the design of laboratory-scale twin-screw extruders and injection molding machines, establishing a complete impact strength testing process for titanium dioxide samples in the sub-kilogram range. This solves the technical challenge that large-scale production testing methods are unsuitable for laboratory pilot-scale testing. The overall four-step approach—"color particle preparation → sample preparation → state conditioning → impact testing"—makes the entire testing process compact and orderly, providing a methodological basis for optimizing specific process parameters in subsequent steps and filling the technical gap in impact strength testing of sub-kilogram titanium dioxide in PC resin.
[0027] In the above embodiments, in step S1, the amount of titanium dioxide added is 5%-15% of the mass of PC resin. Preferably, it is 6%, 10% or 15%.
[0028] In this embodiment, if the amount of titanium dioxide added is too small (<5%), the whiteness and hiding power of the PC product will not be improved sufficiently, and the change in impact strength will be too small, making it difficult to distinguish the performance differences between different titanium dioxide samples and resulting in insufficient detection sensitivity. If the amount of titanium dioxide added is too large (>15%), the catalytic degradation effect of titanium dioxide and poor interfacial compatibility with PC resin will lead to insufficient dispersibility, causing the impact strength of the PC product to drop sharply, exceeding the effective range of the impact strength testing equipment. At the same time, the difficulty in dispersion will also lead to large deviations in the test results.
[0029] This invention controls the amount of titanium dioxide added within the range of 5%-15%, which not only ensures that the impact strength test results are sufficiently sensitive to changes in the application performance of titanium dioxide, but also ensures the processing fluidity and dispersion uniformity of the sample during injection molding, thus guaranteeing the validity and distinguishability of the test results.
[0030] In the above embodiments, in step S1, pentaerythritol stearate (PETS) is selectively added, and the amount of pentaerythritol stearate added is 0-0.5% of the mass of PC resin. Preferably, it is not added (0%), added at 0.3%, or added at 0.4%.
[0031] In this embodiment, PETS, as an internal and external lubricant, can improve the interfacial compatibility between titanium dioxide and PC resin, and enhance the dispersion uniformity of titanium dioxide in the PC matrix, thereby reducing the abnormal decrease in impact strength caused by poor dispersion and making the test results closer to the true performance of the material.
[0032] On the other hand, more PETS is not necessarily better. When the amount of PETS exceeds 0.5% of the PC resin mass, the excess lubricant will form low-molecular-weight precipitates in the PC matrix, which will reduce the bonding force between PC molecular chains and cause the impact strength to decrease instead of increase. This invention controls the amount of PETS added to 0-0.5%, which can give full play to the dispersing and promoting effect of PETS while avoiding the negative effects caused by excessive addition.
[0033] Meanwhile, the limitation of "selective addition" (addition amount of 0-0.5%) allows this technical solution to cover both the "no PETS added" and "PETS added" scenarios, providing users with flexibility to choose the formula according to actual needs and expanding the scope of application of this invention.
[0034] In the above embodiments, in step S1, the maximum processing temperature of melt extrusion is 250℃-290℃; the cooling method is water cooling. Preferably, the maximum processing temperature is 260℃±2℃ or 270℃±2℃.
[0035] In this embodiment, the present invention defines the key conditions for the preparation of color particles from two aspects: processing temperature and cooling method, which has the following synergistic technical effects: (1) Regarding the extrusion temperature of 250℃-290℃: The melt extrusion temperature is a key parameter affecting the dispersion of titanium dioxide in PC resin. If the temperature is too low (<250℃), the PC resin will not melt sufficiently and the melt viscosity will be too high, which is not conducive to the uniform dispersion of titanium dioxide, resulting in lower test results and poor reproducibility; if the temperature is too high (>290℃), the PC resin is prone to thermal degradation under high-temperature shear, which leads to a decrease in the intrinsic impact strength of the material and interferes with the accuracy of the test results. This invention controls the extrusion temperature at 250℃-290℃, which ensures both sufficient melting of PC resin and good dispersion of titanium dioxide, while avoiding the impact of high-temperature degradation on the test results.
[0036] (2) Regarding the water cooling method: The water cooling method is used to quickly cool the extruded strip, which can quickly "freeze" the molecular chain conformation of the molten PC, prevent the titanium dioxide particles from agglomerating again during the slow cooling process, effectively maintain the dispersion state of titanium dioxide in the color particles, and ensure the consistency of titanium dioxide dispersion in the subsequent injection molding sample.
[0037] (3) Synergistic effect of processing temperature and water cooling method: The appropriate extrusion temperature ensures the full dispersion of titanium dioxide in the melt extrusion stage, while rapid water cooling "locks" this good dispersion state in the color particles. Both are indispensable and together ensure the batch stability of color particle quality.
[0038] In the above embodiments, in step S2, the drying temperature of the color particles is 120℃±2℃, and the drying time is 1-4 hours. Preferably, the drying time is 2 hours, 3 hours, or 4 hours.
[0039] In this embodiment, PC resin has strong hygroscopicity. When the moisture content is too high, it will cause hydrolysis and degradation of the PC molecular chain during high-temperature injection molding, resulting in a significant reduction in impact strength. This will mask the true impact of titanium dioxide on impact performance and cause the test results to be distorted.
[0040] This invention sets the drying temperature to 120℃±2℃, which efficiently removes adsorbed moisture from the color particles without causing the volatilization loss of low-molecular-weight additives such as PETS (the decomposition temperature of PETS is much higher than 120℃). The drying time is set to 1-4 hours, providing a flexible time window: if the drying time is too short (<1 hour), the moisture in the center of the color particles will not be sufficiently removed; if the drying time is too long (>4 hours), energy consumption will increase and the detection cycle will be prolonged.
[0041] The drying conditions set by this invention can provide users with a flexible selection space of 1-4 hours while ensuring sufficient dehumidification. Among them, a good detection effect of about 59kJ / m² can be achieved after drying for 2 hours, realizing the best balance between detection efficiency and dehumidification effect.
[0042] In the above embodiment, in step S2, the color particles are laid flat in an enamel or stainless steel tray with a thickness of ≤1cm.
[0043] In this embodiment, the thickness of the pigment particle stack directly affects the contact efficiency between hot air and the surface of the pigment particles during the drying process, as well as the path length for moisture to diffuse from the inside of the pigment particles to the outside. This invention controls the thickness of the pigment particles to ≤1cm, ensuring that hot air can penetrate the entire pigment particle layer, resulting in uniform heating of the upper and lower layers and simultaneous moisture removal. This avoids uneven heating of the surface pigment particles due to insufficient drying in the central area caused by excessive stacking.
[0044] Enameled or stainless steel trays have a smooth surface, good thermal conductivity, and high temperature resistance, which is conducive to uniform heating of color particles and easy cleaning, avoiding cross-contamination between different samples.
[0045] This embodiment can work synergistically with the above-mentioned drying temperature (120℃±2℃) and drying time (1-4 hours): under the premise that the flat layer thickness is ≤1cm, the hot air at 120℃ can fully penetrate the color particle layer, and the drying time of 1-4 hours is sufficient to make all the color particles reach moisture balance. The three factors together ensure the batch consistency of the drying effect and the reproducibility of the test results.
[0046] In the above embodiments, in step S2, the maximum processing temperature for injection molding is 250℃-290℃. Preferably, it is 260℃±2℃ or 270℃±2℃.
[0047] In this embodiment, the injection molding temperature directly affects the flowability of the PC melt and the molding quality of the sample. If the temperature is too low (<250℃), the melt flow front temperature is insufficient, and defects such as weld lines or incomplete filling may exist inside the sample, resulting in more stress concentration points during impact testing, lower test results, and large data dispersion. If the temperature is too high (>290℃), the high-temperature residence time of PC in the injection molding machine barrel is longer, increasing the risk of thermo-oxidative degradation of the molecular chains, resulting in a decrease in the intrinsic impact strength of the sample, which cannot truly reflect the application performance of titanium dioxide.
[0048] This invention controls the injection molding temperature between 250℃ and 290℃, matching the extrusion temperature during the granule preparation stage. This ensures the consistency of the PC resin's thermal history throughout the entire process from granule preparation to sample injection molding, avoiding material performance fluctuations caused by excessive temperature differences. This temperature range also fully considers the low shear heat of small laboratory injection molding machines, ensuring that even on small equipment, qualified samples with full filling and uniform internal structure can be obtained.
[0049] In the above embodiment, in step S3, the temperature of the constant temperature and humidity environment is 23℃±2℃, the relative humidity is 50%±5%, and the conditioning time is at least 16 hours. Preferably, the conditioning time is 16 hours.
[0050] In this embodiment, the impact properties of the polymer material are highly sensitive to temperature and humidity: as temperature increases, the mobility of the PC molecular chains increases, leading to higher impact strength; as humidity increases, the adsorbed moisture acts as a plasticizer, also altering the impact strength. Without standardized temperature and humidity conditioning, test results from different batches of samples will be incomparable due to variations in environmental conditions.
[0051] This invention sets the conditioning temperature to 23℃±2℃ and the relative humidity to 50%±5%, which are internationally accepted standard environmental conditions (ISO 291 standard environment) in the field of plastic impact strength testing, and are completely consistent with the GB / T1843 standard referenced in this method. The conditioning time is at least 16 hours to ensure that the internal temperature and adsorbed water content of the sample reach sufficient equilibrium with the environment, allowing different samples to be tested under the same benchmark conditions and eliminating the interference of environmental factors on the test results.
[0052] In the above embodiment, in step S3, the number of splines is 5 parallel splines.
[0053] In this embodiment, the use of 5 parallel splines for testing is based on the effective sample size considered in statistics. The test results of 5 splines can be used to calculate the average value and range, which can effectively identify and eliminate outliers caused by sample preparation defects or test operation errors, and avoid the drawback of high randomness in the test results of single or a small number of splines.
[0054] According to the experimental data, the impact strength range of multiple specimens prepared using the method of this invention is all <10 kJ / m², indicating that the sample preparation method of this invention itself has good uniformity. Based on this good performance, using five parallel specimens is sufficient to obtain statistically valid test results, ensuring the reliability of the test data while controlling the workload.
[0055] Five parallel splines were tested one by one under the test conditions specified in GB / T 1843 / 8.2 standard, and the average value was taken as the final result, which further improved the reliability and persuasiveness of the test results.
[0056] In the above embodiments, in step S3, the injection molding is performed according to GB / T 1843 / A standard; in step S4, the impact strength test is performed according to GB / T 1843 / 8.2 standard.
[0057] Injection molding is performed according to GB / T 1843 / A standard. GB / T 1843 / A standard clearly specifies the dimensions of the specimen (including length 80mm±2mm, width 10mm±0.2mm, thickness 4mm±0.2mm, and standard dimensions of the A-type notch), the range of injection molding process parameters, and the quality requirements of the specimen. This invention directly adopts this standard for injection molding, ensuring that the geometric dimensions and notch shape of the prepared specimen meet the fixture requirements and testing specifications of the impact strength testing equipment, thus ensuring the validity of the test results.
[0058] Impact strength testing was conducted according to GB / T 1843 / 8.2 standard. GB / T 1843 / 8.2 standard specifies in detail the clamping method of the specimen, impact direction, pendulum selection (selecting a suitable pendulum based on the specimen's breaking energy so that the impact absorption energy is within 10%-80% of the pendulum's range), impact velocity (3.5 m / s), and other specific test operation procedures. Directly referencing this standard ensures the standardization of the testing operation and the objectivity of the test results.
[0059] The two standardized operational features of this invention are interconnected and mutually reinforcing: in the initial stage, qualified sample strips conforming to GB / T1843 / A standard are injection molded, and in the later stage, standardized testing is carried out according to GB / T 1843 / 8.2 standard. This makes the testing method of this invention fully compliant with the requirements of the national standard system, with good standardization and universality, facilitating the comparison and reproduction of test results between different laboratories, and promoting the widespread application of this testing method.
[0060] The technical solutions of the present invention will be described in detail below through specific embodiments.
[0061] Example 1 (Scheme 1, mainstream detection method) This embodiment provides a method for testing the impact strength of titanium dioxide in PC resin, including the following steps: a. Preparation of colored particles: Titanium dioxide is added at 6% of the mass of PC resin; pentaerythritol stearate (PETS) is added at 0.3% of the mass of PC resin; melt extrusion is carried out at the maximum processing temperature of 260℃±2℃, and the extruded strip is granulated after being cooled by water to obtain colored particles.
[0062] b. Sample preparation: The color particles are spread evenly in an enamel tray with a thickness of ≤1cm and dried at an ambient temperature of 120℃±2℃ for 4 hours; under the condition of the highest processing temperature of 260℃±2℃, they are injection molded according to GB / T 1843 / A standard to obtain the sample.
[0063] c. Conditioning of the sample strips: Take 5 parallel sample strips for each sample and condition them for 16 hours under the conditions of ambient temperature 23℃±2℃ and relative humidity 50%±5%.
[0064] d. Impact strength test: The impact strength of the condition-adjusted specimens shall be tested in accordance with GB / T 1843 / 8.2 standard.
[0065] Example 2 (Scheme 2, Pure Low-Powder Detection Method) This embodiment provides a method for testing the impact strength of titanium dioxide in PC resin, including the following steps: a. Preparation of colored particles: The amount of titanium dioxide added is 6% of the mass of PC resin; no processing aids are added (the amount of PETS added is 0%); melt extrusion is carried out at the maximum processing temperature of 260℃±2℃, and the extruded strip is granulated after being cooled by water to obtain colored particles.
[0066] b. Sample preparation: The color particles are spread evenly in an enamel tray with a thickness of ≤1cm and dried at an ambient temperature of 120℃±2℃ for 4 hours; under the condition of the highest processing temperature of 260℃±2℃, they are injection molded according to GB / T 1843 / A standard to obtain the sample.
[0067] c. Conditioning of the sample strips: Take 5 parallel sample strips for each sample and condition them for 16 hours under the conditions of ambient temperature 23℃±2℃ and relative humidity 50%±5%.
[0068] d. Impact strength test: The impact strength of the condition-adjusted specimens shall be tested in accordance with GB / T 1843 / 8.2 standard.
[0069] Example 3 (Scheme 3, low powder + 0.4% PETS detection method) This embodiment provides a method for testing the impact strength of titanium dioxide in PC resin, including the following steps: a. Preparation of colored particles: Titanium dioxide is added at 6% of the mass of PC resin; pentaerythritol stearate (PETS) is added at 0.4% of the mass of PC resin; melt extrusion is carried out at the maximum processing temperature of 260℃±2℃, and the extruded strip is granulated after being cooled by water to obtain colored particles.
[0070] b. Sample preparation: The color particles are spread evenly in an enamel tray with a thickness of ≤1cm and dried at an ambient temperature of 120℃±2℃ for 4 hours; under the condition of the highest processing temperature of 260℃±2℃, they are injection molded according to GB / T 1843 / A standard to obtain the sample.
[0071] c. Conditioning of the sample strips: Take 5 parallel sample strips for each sample and condition them for 16 hours under the conditions of ambient temperature 23℃±2℃ and relative humidity 50%±5%.
[0072] d. Impact strength test: The impact strength of the condition-adjusted specimens shall be tested in accordance with GB / T 1843 / 8.2 standard.
[0073] Example 4 (Scheme 4, medium powder + 0.4% PETS detection method) This embodiment provides a method for testing the impact strength of titanium dioxide in PC resin, including the following steps: a. Preparation of colored particles: Titanium dioxide is added at 10% of the mass of PC resin; pentaerythritol stearate (PETS) is added at 0.4% of the mass of PC resin; melt extrusion is carried out at the maximum processing temperature of 260℃±2℃, and the extruded strip is granulated after being cooled by water to obtain colored particles.
[0074] b. Sample preparation: The color particles are spread evenly in an enamel tray with a thickness of ≤1cm and dried at an ambient temperature of 120℃±2℃ for 4 hours; under the condition of the highest processing temperature of 260℃±2℃, they are injection molded according to GB / T 1843 / A standard to obtain the sample.
[0075] c. Conditioning of the sample strips: Take 5 parallel sample strips for each sample and condition them for 16 hours under the conditions of ambient temperature 23℃±2℃ and relative humidity 50%±5%.
[0076] d. Impact strength test: The impact strength of the condition-adjusted specimens shall be tested in accordance with GB / T 1843 / 8.2 standard.
[0077] Example 5 (Scheme 5, high-gluten powder + 0.4% PETS detection method) This embodiment provides a method for testing the impact strength of titanium dioxide in PC resin, including the following steps: a. Preparation of colored particles: Titanium dioxide is added at 15% of the mass of PC resin; pentaerythritol stearate (PETS) is added at 0.4% of the mass of PC resin; melt extrusion is carried out at the maximum processing temperature of 260℃±2℃, and the extruded strip is granulated after being cooled by water to obtain colored particles.
[0078] b. Sample preparation: The color particles are spread evenly in an enamel tray with a thickness of ≤1cm and dried at an ambient temperature of 120℃±2℃ for 4 hours; under the condition of the highest processing temperature of 260℃±2℃, they are injection molded according to GB / T 1843 / A standard to obtain the sample.
[0079] c. Conditioning of the sample strips: Take 5 parallel sample strips for each sample and condition them for 16 hours under the conditions of ambient temperature 23℃±2℃ and relative humidity 50%±5%.
[0080] d. Impact strength test: The impact strength of the condition-adjusted specimens shall be tested in accordance with GB / T 1843 / 8.2 standard.
[0081] Example 6 (Scheme 6, High Temperature Low Powder + 0.4% PETS Detection Method) This embodiment provides a method for testing the impact strength of titanium dioxide in PC resin, including the following steps: a. Preparation of colored particles: Titanium dioxide is added at 6% of the mass of PC resin; pentaerythritol stearate (PETS) is added at 0.4% of the mass of PC resin; melt extrusion is carried out at the maximum processing temperature of 270℃±2℃, and the extruded strip is granulated after being cooled by water to obtain colored particles.
[0082] b. Sample preparation: The color particles are spread evenly in an enamel tray with a thickness of ≤1cm and dried at an ambient temperature of 120℃±2℃ for 4 hours; under the condition of the highest processing temperature of 270℃±2℃, they are injection molded according to GB / T 1843 / A standard to obtain the sample.
[0083] c. Conditioning of the sample strips: Take 5 parallel sample strips for each sample and condition them for 16 hours under the conditions of ambient temperature 23℃±2℃ and relative humidity 50%±5%.
[0084] d. Impact strength test: The impact strength of the condition-adjusted specimens shall be tested in accordance with GB / T 1843 / 8.2 standard.
[0085] Example 7 (Scheme 7, High Temperature Low Powder + 0.4% PETS Dry Detection Method) This embodiment provides a method for testing the impact strength of titanium dioxide in PC resin, including the following steps: a. Preparation of colored particles: Titanium dioxide is added at 6% of the mass of PC resin; pentaerythritol stearate (PETS) is added at 0.4% of the mass of PC resin; melt extrusion is carried out at the maximum processing temperature of 270℃±2℃, and the extruded strip is granulated after being cooled by water to obtain colored particles.
[0086] b. Sample preparation: The color particles are spread evenly in an enamel tray with a thickness of ≤1cm and dried at an ambient temperature of 120℃±2℃ for 3 hours; under the condition of the highest processing temperature of 270℃±2℃, they are injection molded according to GB / T 1843 / A standard to obtain the sample.
[0087] c. Conditioning of the sample strips: Take 5 parallel sample strips for each sample and condition them for 16 hours under the conditions of ambient temperature 23℃±2℃ and relative humidity 50%±5%.
[0088] d. Impact strength test: The impact strength of the condition-adjusted specimens shall be tested in accordance with GB / T 1843 / 8.2 standard.
[0089] Example 8 (Scheme 8, High Temperature Low Powder + 0.4% PETS Fast Drying Detection Method) This embodiment provides a method for testing the impact strength of titanium dioxide in PC resin, including the following steps: a. Preparation of colored particles: Titanium dioxide is added at 6% of the mass of PC resin; pentaerythritol stearate (PETS) is added at 0.4% of the mass of PC resin; melt extrusion is carried out at the maximum processing temperature of 270℃±2℃, and the extruded strip is granulated after being cooled by water to obtain colored particles.
[0090] b. Sample preparation: Spread the color particles evenly in an enamel tray with a thickness of ≤1cm, and dry them at an ambient temperature of 120℃±2℃ for 2 hours; then, under the condition of a maximum processing temperature of 270℃±2℃, injection mold them according to GB / T 1843 / A standard to obtain the sample.
[0091] c. Conditioning of the sample strips: Take 5 parallel sample strips for each sample and condition them for 16 hours under the conditions of ambient temperature 23℃±2℃ and relative humidity 50%±5%.
[0092] d. Impact strength test: The impact strength of the condition-adjusted specimens shall be tested in accordance with GB / T 1843 / 8.2 standard.
[0093] Test case Comparison of test results Using the same titanium dioxide sample and the same batch of PC resin, impact strength tests were conducted according to the methods described in Examples 1-8 above. The results are as follows (refer to...). Figure 2 As shown: Using the methods of Examples 1, 2, 4, and 5 (i.e., granulation and injection molding of the specimens using a small-scale twin-screw extruder in the laboratory), the impact strength of the obtained specimens was generally low, only about 20 kJ / m², which is significantly different from the known actual impact strength of the titanium dioxide sample in PC (testing environment temperature: 23℃±2℃) of about 50 kJ / m².
[0094] Using the method in Example 3, the impact strength reached 57.93 kJ / m² in the first verification, but it dropped to about 17 kJ / m² in subsequent verifications, indicating poor reproducibility.
[0095] Using the methods of Examples 6 to 8, the impact strength (testing ambient temperature: 23℃±2℃) can all reach approximately 59kJ / m², and the test reproducibility is good (the range of impact strength between the 5 parallel samples is all <10kJ / m²). Among them, Example 8 has the shortest testing cycle and the lowest testing cost.
[0096] The above results show that by optimizing key parameters such as processing temperature (270℃±2℃), drying time (2-4 hours), and PETS addition amount (0.3%-0.4%), the present invention can effectively overcome the shortcomings of poor dispersion conditions in laboratory small twin-screw extruders and obtain impact strength test results that are in good agreement with the true values and have excellent reproducibility.
[0097] Therefore, this invention has successfully established a rapid detection method for the impact strength of titanium dioxide samples in PC resin at the kilogram level by systematically optimizing key process parameters such as titanium dioxide addition amount (5%-15%, preferably 6%), processing temperature (250℃-290℃, preferably 270℃±2℃), drying time (1-4 hours, preferably 2-4 hours), and selective addition of PETS (0-0.5%, preferably 0.3%-0.4%). This method not only requires less sample, has a shorter detection cycle (saving 2-3 hours compared to existing large-scale production line methods), and is low-cost, but also effectively overcomes the shortcomings of poor dispersion conditions in small-scale laboratory twin-screw extruders and injection molding machines. The detection results highly match the true values (impact strength can reach approximately 59 kJ / m²), and the range between parallel samples is <10 kJ / m², demonstrating excellent reproducibility. This invention provides an accurate, reliable, and efficient detection method for rapid batch screening in the small-scale research and development stage of titanium dioxide, and has broad prospects for widespread application.
[0098] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of the present invention. Any modifications or equivalent substitutions made to the present invention without departing from the spirit and scope thereof should be covered within the protection scope of the claims of the present invention.
Claims
1. A method for testing the impact strength of titanium dioxide in PC resin, characterized in that, Includes the following steps: Color particle preparation: Titanium dioxide and PC resin are mixed, melt extruded, cooled, and granulated to obtain color particles; Sample preparation: The color particles are dried and then injection molded to obtain the sample. Spline conditioning: The spline is conditioned in a constant temperature and humidity environment; Impact strength test: The impact strength of the spline after condition adjustment is tested.
2. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the step of preparing the colored particles, the amount of titanium dioxide added is 5%-15% of the mass of PC resin.
3. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the step of preparing colored particles, pentaerythritol stearate is added, wherein the amount of pentaerythritol stearate added is not higher than 0.5% of the mass of PC resin.
4. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the step of color particle preparation, the maximum processing temperature of the melt extrusion is 250℃-290℃; the cooling method is water cooling.
5. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the sample preparation step, the drying temperature of the color particles is 120℃±2℃, and the drying time is 1-4 hours.
6. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the sample preparation step, the color particles are laid flat in an enamel or stainless steel tray with a thickness of ≤1cm.
7. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the sample preparation step, the maximum processing temperature of the injection molding is 250℃-290℃.
8. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the spline conditioning step, the temperature of the constant temperature and humidity environment is 23℃±2℃, the relative humidity is 50%±5%, and the conditioning time is at least 16 hours.
9. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the spline state adjustment step, the number of splines is 5 parallel splines.
10. The method for testing the impact strength of titanium dioxide in PC resin according to claim 1, characterized in that, In the sample preparation step, the injection molding is carried out in accordance with GB / T 1843 / A standard; in the impact strength testing step, the impact strength testing is carried out in accordance with GB / T 1843 / 8.2 standard.