A macrostructure display method for low-carbon gear steel continuous casting billet solidification structure

By combining online high-temperature sampling and forced air cooling with sawing, grinding, and constant-temperature acid etching, the problem of uneven solidification structure in low-carbon gear steel continuous casting billets was solved, achieving stable and reliable evaluation of the solidification structure. This method is applicable to various low-carbon gear steel grades and is suitable for online sampling in continuous casting production lines.

CN123155294APending Publication Date: 2026-11-24BAOSTEEL SPECIAL STEEL SHAOGUAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611389382.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing methods for displaying the solidification structure of low-carbon gear steel continuous casting billets have significant uniformity problems. This results in insufficient clarity in the display of solidification structures in different batches of samples and different areas of the same sample, making it difficult to accurately distinguish the boundary between pearlite and bainite, which affects the quantitative evaluation of solidification structure and process traceability analysis.

Method used

Online high-temperature sampling and forced air cooling were adopted to control the sampling temperature to no less than 730℃. After sawing and grinding, the sample was subjected to constant-temperature acid etching in hydrochloric acid aqueous solution until the low-magnification solidified structure morphology of the sample was clearly distinguishable. The clear structure display was obtained by adjusting the acid etching time.

Benefits of technology

It achieves stable and reliable display of the solidification structure of low-carbon gear steel continuous casting billets, ensuring clear boundaries of the structure between different batches of samples and different regions of the same sample, providing accurate solidification structure morphology data support, applicable to various low-carbon gear steel grades, and is simple to operate and low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123155294A_ABST
    Figure CN123155294A_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal smelting technology and discloses a method for low-magnification display of the solidification structure of a continuous casting billet of low-carbon gear steel. The method includes: S1, cutting a continuous casting billet sample from the continuous casting production line; S2, immediately subjecting the cut sample to forced air cooling to continuously cool it to room temperature; S3, sawing to obtain the test sample, and then processing the test surface of the test sample until it is smooth, clean, and free of machining marks and oxide layers; S4, immersing the test surface of the sample in a hydrochloric acid aqueous solution, then rinsing with clean water, and finally drying; S5, observing the low-magnification solidification structure morphology of the sample and taking photographs; if the structure is not clearly displayed, repeating step S4 and observing again until the structure meets the evaluation requirements. This invention solves the problem of uneven cooling leading to a multiphase mixed structure in the low-magnification display of the solidification structure of a continuous casting billet of low-carbon gear steel, resulting in large differences in display effects and insufficient clarity in different samples and different areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal smelting technology, and more specifically, to a method for low-magnification display of the solidification structure of a continuous casting billet of low-carbon gear steel. Background Technology

[0002] The solidification structure of continuously cast steel billets is the core foundation determining the final properties of the steel. A typical solidification structure of a continuously cast billet consists of three parts: fine equiaxed grain zones on the surface, columnar grain zones in the middle, and equiaxed grain zones at the center. Accurately displaying and quantitatively evaluating the morphology, proportion, and distribution of the solidification structure is the core technical basis for optimizing continuous casting process parameters and improving billet quality.

[0003] The current national standard GB / T 24178, "Low-Magnification Evaluation Method for Solidification Structure of Continuously Cast Steel Billets," specifies the rules for low-magnification evaluation of the solidification structure of continuously cast steel billets. The microstructure display method adopts the acid etching process from GB / T 226, "Acid Etching Test Method for Low-Magnification Microstructure and Defects in Steel." However, in industrial testing practice of low-carbon gear steels (such as SAE8620H and 20CrMnTiH), the low-magnification microstructure obtained using the above standard method exhibits significant uniformity issues: the clarity and morphology of the solidification structure vary greatly between different batches of samples, and even between different areas of the same sample. The boundaries between columnar and equiaxed crystals are difficult to distinguish accurately, severely interfering with the quantitative evaluation of the solidification structure and process traceability analysis.

[0004] The root cause of these problems lies in the lack of structural control over the cooling process after billet sampling: under normal natural cooling conditions, different locations on the low-carbon gear steel billet experience inconsistent cooling rates due to varying heat dissipation conditions, resulting in a mixed structure of pearlite and bainite. Because pearlite and bainite exhibit significantly different corrosion rates in the hydrochloric acid etching system, this ultimately leads to obvious regional differences in the low-magnification microstructure, failing to accurately reflect the intrinsic morphology of the billet's solidification structure. Currently, there is no dedicated low-magnification detection method for low-carbon gear steel that can stably and clearly display the solidification structure.

[0005] In summary, it is necessary to propose a low-magnification method for displaying the solidification structure of low-carbon gear steel continuous casting billets in order to solve the above problems. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the present invention aims to provide a method for low-magnification display of the solidification structure of low-carbon gear steel continuous casting billets, thereby solving the problem that uneven cooling leads to the formation of multiphase mixed structures, resulting in significant differences in display effects and insufficient clarity for different samples and regions in low-magnification display of the solidification structure of low-carbon gear steel continuous casting billets.

[0007] The above-mentioned technical objective of the present invention is achieved through the following technical solution: A method for low-magnification visualization of the solidification structure of a continuous casting billet of low-carbon gear steel includes the following steps: S1. Online high-temperature sampling: Samples of continuously cast billets are taken from the continuous casting production line; S2, Forced air cooling control: The cut sample is immediately subjected to forced air cooling to continuously cool the sample to room temperature; S3. Sample processing and preparation: The sample to be tested is obtained by sawing, and then the test surface of the sample is processed to be flat and smooth without processing marks and oxide layer; S4. Constant temperature acid etching treatment: Immerse the test surface of the sample in hydrochloric acid aqueous solution, then rinse with clean water to remove the corrosion products on the test surface, and finally blow dry. S5. Observation and etching: Observe the morphology of the solidified structure of the sample at low magnification. If the boundaries of the fine equiaxed crystal zones, columnar crystal zones, and central equiaxed crystal zones are clearly distinguishable, take a picture and record it. If the structure is not clearly displayed, repeat step S4 and observe again until the structure meets the evaluation requirements.

[0008] In one embodiment, in step S1, the temperature of the continuous casting billet is ≥730°C during sampling, and the thickness of the sample obtained is ≥60mm.

[0009] In one embodiment, in step S1, the continuous casting billet sample is cut by flame cutting.

[0010] In one embodiment, in step S3, the test sample is obtained by sawing along the thickness direction of the continuously cast billet at a position ≥25mm away from the heat-affected surface of the flame cutting.

[0011] In one embodiment, in step S3, the sample to be tested is obtained by sawing with a saw or a high-speed saw.

[0012] In one embodiment, in step S3, the test surface of the sample to be tested is milled by a milling machine or ground by a grinding machine until it is smooth and free of machining marks and oxide layer.

[0013] In one embodiment, in step S4, the acid etching temperature is 70-80°C and the acid etching soaking time is 15-30 min.

[0014] In one embodiment, in step S4, the volume ratio of hydrochloric acid to water in the hydrochloric acid aqueous solution is 1:1.

[0015] In summary, the present invention has the following beneficial effects: This invention eliminates unevenness at its source: By controlling the sampling temperature to be no less than 730℃ and using forced air cooling, this invention suppresses the pearlite phase transformation, enabling the entire sample to obtain a uniform bainite + intercrystalline ferrite structure, thus completely eliminating the problem of uneven regional display caused by the difference in corrosion rate of multiphase structures.

[0016] The test results of this invention are stable and reliable: the solidification structure of different batches of samples and different areas of the same sample shows good consistency, and the structure boundary is clearly distinguishable. It can truly reflect the actual morphology of the solidification structure of the billet and provide accurate test data support for the optimization of continuous casting process.

[0017] The present invention has strong process adaptability: it can be directly connected to the continuous casting production line for online sampling, without the need for additional heat treatment equipment and processes, the operation process is simple, the testing cost is low, and it is easy to promote and apply on a large scale in industrial sites.

[0018] This invention has a wide range of applications: it can be adapted to various low-carbon gear steel grades, and good display effects can be obtained by finely adjusting the acid etching time. Attached Figure Description

[0019] Figure 1 This is a low-magnification tissue image of Example 1.

[0020] Figure 2 This is a low-magnification tissue image of Example 2.

[0021] Figure 3 This is a low-magnification tissue diagram of Comparative Example 1.

[0022] Figure 4 This is a low-magnification tissue diagram of Comparative Example 2.

[0023] Figure 5 This is the microstructure morphology of the air-cooled to room temperature microstructure in Example 1.

[0024] Figure 6 The microstructure of Comparative Example 1 is shown after air cooling to room temperature. Detailed Implementation

[0025] The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0026] It is worth noting that the directional terms such as "up" and "down" used in this article are all relative to the perspective of the attached figures and are only for the purpose of description. They should not be interpreted as limitations on the technical solutions.

[0027] This invention proposes a method for low-magnification visualization of the solidification structure of a continuously cast low-carbon gear steel billet, comprising the following steps: S1. Online high-temperature sampling: Samples of continuously cast billets are taken by flame cutting on the continuous casting production line; S2. Forced air cooling structure control: The cut sample is immediately subjected to forced air cooling, such as using an industrial fan for forced air cooling, so that the sample is continuously cooled to room temperature, so that the sample as a whole obtains bainite + intergranular ferrite structure. S3. Sample processing and preparation: The sample to be tested is obtained by sawing, for example by sawing with a saw or high-speed saw. Then the test surface of the sample is milled by a milling machine or ground by a grinding machine until it is flat and smooth without machining marks and oxide layer. S4. Constant temperature acid etching treatment: Immerse the test surface of the sample in hydrochloric acid aqueous solution, then rinse with clean water to remove the corrosion products on the test surface, and finally blow dry. S5. Observation and etching: Observe the morphology of the solidified structure of the sample at low magnification. If the boundaries of the fine equiaxed crystal zones, columnar crystal zones, and central equiaxed crystal zones are clearly distinguishable, take a picture and record it. If the structure is not clearly displayed, repeat step S4 and observe again until the structure meets the evaluation requirements.

[0028] Preferably, in step S1, the continuous casting billet temperature is ≥730℃ during sampling, and the thickness of the sample obtained is ≥60mm.

[0029] Preferably, in step S3, the test sample is obtained by sawing along the thickness direction of the continuously cast billet at a position ≥25 mm away from the heat-affected surface of the flame cutting.

[0030] Preferably, in step S4, the acid etching temperature is 70-80℃ and the acid etching soaking time is 15-30 min.

[0031] Preferably, in step S4, the volume ratio of hydrochloric acid to water in the hydrochloric acid aqueous solution is 1:1.

[0032] The technical solution of the present invention will be described below with reference to specific embodiments.

[0033] Example 1

[0034] This embodiment deals with SAE8620H low-carbon gear steel continuous casting billets, and the specific steps are as follows: S1. Online high-temperature sampling: During the continuous casting process, the billet sample is cut by flame cutting. The billet temperature is 750℃ and the sample thickness is 70mm. S2. Forced air cooling: After cutting, the sample is immediately subjected to continuous forced air cooling by an industrial fan until it reaches room temperature. The sample as a whole obtains bainitic structure + intergranular ferrite structure. S3. Sample processing: Cut the sample to be tested along the thickness direction of the billet using a saw at a distance of 30mm from the flame cutting surface, and mill the test surface with a milling machine until it is flat and smooth, without any machining marks. S4. Acid etching treatment: Immerse the test surface of the sample in a 75℃, 1:1 volume ratio hydrochloric acid aqueous solution for 30 minutes, then remove it, rinse it with clean water, and dry it with compressed air. S5. Observation of structure: The solidified structure of the sample is clearly distinguishable at low magnification. The boundaries of the fine equiaxed crystal zones on the surface, columnar crystal zones, and central equiaxed crystal zones are distinct. The display effect of different areas of the same sample is highly consistent. It can be directly photographed and recorded for solidification structure evaluation.

[0035] In this embodiment, the low-magnification tissue image is as follows: Figure 1 As shown, the microstructure morphology from air cooling to room temperature is as follows: Figure 5 As shown.

[0036] Example 2

[0037] This embodiment deals with 20CrMnTiH low-carbon gear steel continuous casting billets, and the specific steps are as follows: S1. Online high-temperature sampling: During the continuous casting process, the billet sample is cut by flame cutting. The billet temperature is 740℃ and the sample thickness is 65mm. S2. Forced air cooling: After cutting, the sample is immediately subjected to continuous forced air cooling by an industrial fan until it reaches room temperature. The sample as a whole obtains a bainite + intergranular ferrite structure. S3. Sample processing: Cut the sample to be tested along the thickness direction of the billet using a high-speed saw at a distance of 28mm from the flame cutting surface, and grind the test surface to a smooth and clean surface using a grinding machine. S4. Acid etching treatment: Immerse the test surface of the sample in a 72℃, 1:1 volume ratio hydrochloric acid aqueous solution for 15 minutes, then remove it, rinse with clean water and blow dry. S5. Tissue observation: Initial observation revealed insufficient tissue clarity. The tissue was then immersed in hydrochloric acid solution under the same conditions for an additional 15 minutes. After being removed, cleaned, and dried, the coagulated tissue showed clear and uniform morphology in each region, and the boundaries between columnar and equiaxed crystal regions could be accurately distinguished, meeting the evaluation requirements.

[0038] In this embodiment, the low-magnification tissue image is as follows: Figure 2 As shown.

[0039] Example 3

[0040] This embodiment deals with 20CrMoH low-carbon gear steel continuous casting billets, and the specific steps are as follows: S1. Online high-temperature sampling: During the continuous casting process, the billet sample is cut by flame cutting. The billet temperature is 790℃ and the sample thickness is 65mm. S2. Forced air cooling: After cutting, the sample is immediately subjected to continuous forced air cooling by an industrial fan until it reaches room temperature. The sample as a whole obtains a bainite + intergranular ferrite structure. S3. Sample processing: Cut the sample to be tested along the thickness direction of the billet using a high-speed saw at a distance of 30mm from the flame cutting surface, and grind the test surface with a grinding machine until it is flat and smooth. S4. Acid etching treatment: Immerse the test surface of the sample in a 78°C, 1:1 volume ratio hydrochloric acid aqueous solution for 20 minutes, then remove it, rinse with clean water and blow dry. S5. Observation of structure: The solidified structure of the sample is clearly distinguishable at low magnification. The boundaries of the fine equiaxed crystal zones on the surface, columnar crystal zones, and central equiaxed crystal zones are distinct. The display effect of different areas of the same sample is highly consistent. It can be directly photographed and recorded for solidification structure evaluation.

[0041] Comparative Example 1 This comparative example uses a SAE8620H low-carbon gear steel continuous casting billet. The conventional natural cooling method is employed, and all other parameters are consistent with Example 1. Online sampling: Flame cutting sampling during continuous casting production, sampling temperature 750℃, sample thickness 70mm; Cooling method: The sample was placed in air and allowed to cool naturally to room temperature; The sample processing and acid etching process were the same as in Example 1; In this comparative example, the low-magnification tissue images are as follows: Figure 3 As shown, the microstructure morphology from air cooling to room temperature is as follows: Figure 6 As shown. Observation results: The columnar crystal regions in different parts of the sample showed significant differences, and the grain boundaries in some areas were blurred and mottled, making it impossible to accurately determine the width of the columnar crystals and the ratio of the central equiaxed crystals, which did not meet the requirements for solidification structure evaluation.

[0042] Comparative Example 2 The subject of this comparative example is a 20CrMnTiH low-carbon gear steel continuous casting billet. The sampling temperature of this comparative example is below 730℃, and the other parameters are the same as those in Example 2. Online sampling: The billet temperature was 650℃ and the sample thickness was 65mm during sampling; Cooling method: Forced air cooling with industrial fans to room temperature; The sample processing and acid etching process were the same as in Example 2; In this comparative example, the low-magnification tissue images are as follows: Figure 4 As shown. Observation results: The overall morphology of each crystal zone in the columnar crystal region is blurred, the boundaries are difficult to distinguish, and the solidification structure is poorly displayed, making it unsuitable for accurate evaluation.

[0043] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.

Claims

1. A method for low-magnification visualization of the solidification structure of a continuously cast low-carbon gear steel billet, characterized in that, Includes the following steps: S1. Online high-temperature sampling: Samples of continuously cast billets are taken from the continuous casting production line; S2, Forced air cooling control: The cut sample is immediately subjected to forced air cooling to continuously cool the sample to room temperature; S3. Sample processing and preparation: The sample to be tested is obtained by sawing, and then the test surface of the sample is processed to be flat and smooth without processing marks and oxide layer; S4. Constant temperature acid etching treatment: Immerse the test surface of the sample in hydrochloric acid aqueous solution, then rinse with clean water to remove the corrosion products on the test surface, and finally blow dry. S5. Observation and etching: Observe the morphology of the solidified structure of the sample at low magnification. If the boundaries of the fine equiaxed crystal zones, columnar crystal zones, and central equiaxed crystal zones are clearly distinguishable, take a picture and record it. If the structure is not clearly displayed, repeat step S4 and observe again until the structure meets the evaluation requirements.

2. The method for low-magnification display of the solidification structure of a low-carbon gear steel continuously cast billet as described in claim 1, characterized in that, In step S1, the temperature of the continuous casting billet is ≥730℃ during sampling, and the thickness of the sample obtained is ≥60 mm.

3. The method for low-magnification display of the solidification structure of a low-carbon gear steel continuously cast billet as described in claim 1, characterized in that, In step S1, the continuous casting billet sample is cut using a flame cutting method.

4. The method for low-magnification display of the solidification structure of a continuously cast low-carbon gear steel billet as described in claim 1, characterized in that, In step S3, the test sample is obtained by sawing along the thickness direction of the continuously cast billet at a position ≥25 mm away from the heat-affected surface of the flame cutting.

5. The method for low-magnification display of the solidification structure of a low-carbon gear steel continuously cast billet as described in claim 1, characterized in that, In step S3, the sample to be tested is obtained by sawing with a saw or a high-speed saw.

6. The method for low-magnification display of the solidification structure of a low-carbon gear steel continuously cast billet as described in claim 1, characterized in that, In step S3, the test surface of the sample to be tested is milled by a milling machine or ground by a grinding machine until it is flat and smooth without machining marks or oxide layer.

7. The method for low-magnification display of the solidification structure of a low-carbon gear steel continuously cast billet as described in claim 1, characterized in that, In step S4, the acid etching temperature is 70-80℃ and the acid etching soaking time is 15-30min.

8. The method for low-magnification display of the solidification structure of a continuously cast low-carbon gear steel billet as described in claim 1, characterized in that, In step S4, the volume ratio of hydrochloric acid to water in the hydrochloric acid aqueous solution is 1:1.