Method for predicting stress corrosion life of in-service pipeline and test device thereof
By conducting constant load stress corrosion tests simultaneously in the laboratory and on-site, and combining them with a nonlinear regression model, a correlation model between the laboratory and the field was established. This solved the quantitative problem of predicting pipeline stress corrosion life in existing technologies, and enabled accurate assessment and management optimization of pipeline life.
Patent Information
- Application Number
- CN202611366565.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-24
Smart Images

Figure CN123155304A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of pipeline service safety technology, and relates to a method for predicting the stress corrosion life of pipelines in service and its testing device. Background Technology
[0002] Oil and gas pipelines are buried in complex and variable soil environments for extended periods, and stress corrosion cracking is one of the main failure modes threatening their safe operation. Currently, the prediction of pipeline life under stress corrosion mainly relies on laboratory testing methods. Among these, the slow strain rate tensile test is widely used due to its short cycle and high efficiency. The slow strain rate tensile test is a laboratory testing method that rapidly assesses whether a material is prone to stress corrosion cracking by applying extremely slow tensile deformation to a specimen in a corrosive environment. However, this method uses a dynamic loading approach, which is fundamentally different from the near-static stress state experienced by pipelines during actual service. This makes it difficult for the assessment results to accurately reflect the stress corrosion behavior of the pipe material during long-term operation, and thus difficult to predict the actual life.
[0003] To simulate actual working conditions, the stress ring constant load test has been proposed, which can provide constant stress loading conditions that are closer to those in the field. However, the application of this method in soil environments is extremely limited, mainly because the test cycle is too long, often requiring months or even years to obtain effective data.
[0004] However, neither slow strain rate tensile tests nor stress ring tests have established an effective, quantitative model linking laboratory and field conditions. The lack of a reliable bridge between laboratory data and actual service life in the field makes it difficult to quantitatively guide engineering practice, leaving pipeline integrity management largely reliant on qualitative or semi-quantitative experience-based judgments. Summary of the Invention
[0005] The purpose of this invention is to provide a method and test device for predicting the stress corrosion life of pipelines in service in the field, so as to solve the technical problems that existing solutions are difficult to quantitatively guide engineering practice and difficult to accurately predict pipeline life.
[0006] To achieve the above objectives, the present invention provides a specific technical solution for predicting the stress corrosion life of pipelines in service in the field, as follows: A method for predicting the stress corrosion life of pipelines in service in the field includes the following steps: Obtain the load-strain calibration relationship of the pipeline under test under target stress, and determine the corresponding target strain value; The samples from the same batch were divided into two groups. The first group of pipes was subjected to constant load stress corrosion test in a standard corrosion environment in the laboratory. The second group of pipes was buried at the service site of the target pipe and subjected to constant load stress corrosion test. In the field test, the load was applied to the sample according to the target strain value. The duration of crack initiation in the pipeline under test in a laboratory environment was obtained based on the first set of experiments. The duration of crack initiation in the pipeline under test in a field environment was obtained based on the second set of experiments. The environmental parameters include chloride ion concentration, temperature, and pH value. The laboratory crack initiation duration, field crack initiation duration, and corresponding environmental parameters of each set of experiments were used as sample data. The laboratory crack initiation duration, chloride ion concentration, temperature, and pH value were used as input variables, and the field crack initiation duration was used as the target variable. A correlation model was established through nonlinear regression fitting. The correlation model was used to characterize the quantitative relationship between the field crack initiation duration, the laboratory crack initiation duration, and the environmental parameters. For the target pipe section to be predicted, the crack initiation time of the pipe material under laboratory conditions is obtained, and the chloride ion concentration, temperature and pH value of the target pipe section at the service site are collected. The above data are substituted into the correlation model to calculate the predicted value of the crack initiation time of the pipe section under the field service conditions, which serves as the basis for evaluating the stress corrosion life of the pipe section.
[0007] Furthermore, the association model is as follows: ; In the formula, The crack initiation time of the pipeline under test in the field environment. The crack initiation time of the pipeline under test in a laboratory environment. The chloride ion concentration in the on-site environment. The absolute temperature of the site environment. For the on-site environment value, As a comprehensive scale factor, This represents the relationship coefficient between the laboratory environment and the field environment over a time scale. This represents the promoting factor of chloride ion concentration on crack initiation. This represents the coefficient of influence of temperature on crack initiation. For the on-site environment The value is the influence coefficient on crack initiation.
[0008] Furthermore, the on-site chloride ion concentration and on-site pH value are calculated using a time-weighted average.
[0009] Furthermore, the data fitting employs the Levenberg-Marquardt algorithm, aiming to minimize the sum of squared residuals between predicted and measured values, to determine the coefficients to be fitted in the correlation model; the specific values of the coefficients to be fitted are determined by fitting the sample data, and the values of the coefficients vary for different pipe materials and different corrosive environments.
[0010] Furthermore, it also includes the step of establishing the load-strain calibration relationship of the pipe material before the test: in the laboratory, the specimen is subjected to incremental loads step by step, and the load values and corresponding strain values under each load are recorded simultaneously, and a load-strain calibration curve is plotted. The target strain value corresponding to the target stress is determined according to the calibration curve. In the field test, the specimen is loaded until the strain value reaches the target strain value, so that the stress level of the field specimen is consistent with the target stress in the laboratory.
[0011] Furthermore, after loading the specimen to the target stress, the load is continuously monitored in the initial stage. When the load relaxes due to thread engagement or initial deformation of the specimen, the load is restored to the target value by adjusting the loading device. This process is repeated until the load fluctuation is less than ±1% of the target load within 72 consecutive hours, at which point it is recorded as the start time of the test. The target stress is 95% of the specified minimum yield strength of the pipe to be tested.
[0012] Furthermore, in the field embedding test of the second group of samples, the data obtained by monitoring were used to verify the accuracy of the initial loading during embedding and to record the load stability during the test period; after the test, the sample data with a deviation of less than ±5% from the target strain value were considered valid, and the sample data with a deviation of more than ±10% were discarded.
[0013] The method for predicting the stress corrosion life of pipelines in service in the field, as proposed in this invention, has the following advantages: This invention divides the same batch of samples into two groups, simultaneously conducting laboratory constant load tests and field-installed constant load tests. Using laboratory crack initiation time and field environmental parameters (chloride ion concentration, temperature, pH) as input variables, and field crack initiation time as the target variable, a quantitative correlation model is established through nonlinear regression fitting. This model serves as a transformation bridge, enabling subsequent predictions of crack initiation time for the target pipe section under field service conditions to be obtained only through short-term laboratory tests combined with field environmental parameters. This invention places accelerated laboratory testing and real-world field service environments within a unified quantitative framework, achieving a leap from qualitative classification to quantitative prediction, and providing reliable data support for optimizing inspection cycles, prioritizing maintenance, and controlling risks in pipeline integrity management. Attached Figure Description
[0014] Figure 1 This is a flowchart of the life prediction method for pipelines in service under stress corrosion according to the present invention. Figure 2 This is a schematic diagram of the constant load stress device of the present invention; Figure 3 This is a schematic diagram of the constant load stress device for removing solution from the tank according to the present invention.
[0015] Figure label: 1. Stress ring; 2. Loading nut; 3. Loading bolt; 4. Bearing bolt; 5. Solution tank; 6. Stress measurement unit; 7. Strain measurement unit; 8. Pipe to be tested. Detailed Implementation
[0016] The technical solutions of this application will now be described clearly and in detail with reference to the accompanying drawings. In the description of the embodiments of this application, unless otherwise stated, "multiple" refers to two or more. The terms "first" and "second" are used for descriptive purposes only and should not be construed as implying or suggesting relative importance or implicitly indicating the number of indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature.
[0017] like Figure 1 As shown, this invention provides a method for predicting the stress corrosion life of pipelines in service in the field, comprising the following steps: S1. Obtain the load-strain calibration relationship of the pipeline under test under target stress, and determine the corresponding target strain value.
[0018] S2. The samples from the same batch were divided into two groups. The first group of pipes was subjected to constant load stress corrosion test in a standard corrosion environment in the laboratory. The second group of pipes was buried at the service site of the target pipe and subjected to constant load stress corrosion test. In the field test, the load was applied to the samples according to the target strain value.
[0019] S3. Based on the first set of experiments, the time for crack initiation in the pipeline under test in a laboratory environment is obtained. Based on the second set of experiments, the field environmental parameters and the time for crack initiation in the pipeline under test in a field environment are obtained. The environmental parameters include chloride ion concentration, temperature, and pH value. The laboratory crack initiation time, field crack initiation time, and corresponding environmental parameters of each set of experiments are used as sample data. The laboratory crack initiation time, chloride ion concentration, temperature, and pH value are used as input variables, and the field crack initiation time is used as the target variable. A correlation model is established through nonlinear regression fitting. The correlation model is used to characterize the quantitative relationship between the field crack initiation time, the laboratory crack initiation time, and the environmental parameters.
[0020] S4. For the target pipe section to be predicted, obtain the crack initiation time of the pipe material under laboratory conditions, and collect the chloride ion concentration, temperature, and pH value of the pipe section at the service site. Substitute the above data into the correlation model to calculate the predicted crack initiation time of the pipe section under the service conditions, which serves as the basis for evaluating the stress corrosion life of the pipe section.
[0021] In step S1, the test specimen is a standard round bar tensile test piece cut circumferentially from a reserved pipe section of the same batch and model as the target in-service pipe. In the laboratory, one specimen from the first group is placed in a solution bath (without solution flow) and mounted on a portable stress ring device, connected in series with a high-precision stress sensor. Strain gauges are attached to the surface of the specimen's gauge length and connected to a strain acquisition device. The load is slowly applied by tightening the loading nut, simultaneously recording the stress sensor reading (F) and the strain acquisition device reading (ε) until the target stress level (e.g., 80% SMYS) is reached. The F-ε calibration curve of the specimen is plotted, and the target strain value εtarget corresponding to the target stress is calculated.
[0022] In step S2, the pipelines prepared in the same batch are randomly divided into two groups. The first group of pipelines is tested in a laboratory, and the second group is tested in a field environment. The first group of pipelines is loaded with the target load and a simulated solution prepared according to the field soil analysis (pH adjusted to match the field conditions) is applied. A N2 / CO2 mixed gas is continuously introduced to simulate the oxygen-deficient environment, initiating the laboratory accelerated corrosion test. The second group of pipelines is subjected to the target strain value through the load-strain calibration relationship described above to achieve the same target stress as in the laboratory. The second group of pipelines is then buried in a pit in the field environment and backfilled and compacted with the original soil. In this step, "field loading is based on strain" rather than relying on stress sensors. This minimizes the power demand of the entire field monitoring system. This design fundamentally solves the two core bottlenecks faced by traditional stress ring tests in field applications: "difficulty in obtaining a stable power supply for a long period" and "easy failure of electronic sensors in soil," making the field deployment of this invention highly feasible and reliable. The second group of field deployments includes:
[0023] Site selection for field tests and deployment of environmental monitoring points. Along the target in-service pipeline, select a representative location (such as a known high-risk corrosion area or a region with varying soil resistivity) that is also convenient for safe operation as the field test site. Bury soil corrosion monitoring probes near this site to continuously or periodically monitor key soil parameters: soil resistivity, moisture content, pH value, redox potential, chloride / sulfate ion concentration, temperature, etc.
[0024] Field Specimen Load Stabilization and Installation. Trench Excavation: At the selected point, excavate a trench with a depth consistent with the pipeline burial depth and sufficient dimensions to accommodate the stress ring device and specimens, ensuring the specimen installation environment is consistent with the soil conditions of the adjacent pipeline. Device Installation: Install the second set of specimens onto another identical portable stress ring device. Connect the stress sensor in series and load until the stress sensor displays Ftarget. Then perform the same one-week load stabilization adjustment until the load remains continuously stable under field conditions. Load Application: According to the obtained calibration relationship, tighten the loading nut and directly load the specimen until the strain value reaches εtarget (i.e., the strain value corresponding to the target load calibrated in the laboratory). Sealing and Protection: Seal all metal connection parts and strain gauge locations of the loaded device with PTFE tape to prevent corrosion.
[0025] Installation and backfilling: The entire device is placed in the pit, with a temperature and humidity recorder placed next to it. The device is then backfilled in layers with undisturbed soil and lightly compacted to simulate real installation conditions. Strain acquisition lines are led out to a weatherproof data acquisition box on the ground.
[0026] Long-term on-site monitoring and data acquisition. The data acquisition box is powered by solar panels or long-life batteries, automatically collecting and storing strain data of the samples (for indirect monitoring of load stability) and environmental parameters of the installation points on a weekly basis. Regular (e.g., quarterly) manual inspections are conducted to check the condition of the device.
[0027] In step S3, two sets of test pipelines are periodically removed, and the crack initiation status is observed using a scanning electron microscope. "Crack initiation" is defined as the first observation of a crack with a length ≥ 0.1 mm. Multiple sets of data on crack initiation time in field and laboratory environments, along with field environmental parameters, are collected. Through data fitting, a correlation model is obtained between the time for crack initiation in the field environment and the time for crack initiation in the laboratory environment, and the field environmental parameters. The laboratory environment is not completely identical to the field environment, but follows the principle of "chemical parameter benchmarking and mechanical parameter acceleration": key chemical parameters such as pH, [Cl⁻], and oxygen content are kept consistent with the field environment to ensure the transferability of the corrosion mechanism; simultaneously, crack initiation is accelerated by significantly increasing the stress level (e.g., 95% SMYS vs. 50%-80% SMYS in the field (typical range of actual pipeline operating stress)) and using a solution system (faster mass transfer than soil). Therefore, the laboratory time is much shorter than the field time, which is also a prerequisite for establishing the correlation model.
[0028] Data correlation analysis and model building include: Comparison of failure data between laboratory and field samples. After a certain number of days (e.g., one year) of testing, samples from both the laboratory (Group 1) and the field (Group 2) can be removed and the crack growth (number, length, etc.) observed using light microscopy or electron microscopy. Alternatively, if field non-destructive testing confirms that a sample in either the laboratory (Group 1) or the field (Group 2) has reached a predetermined crack length, the test for that sample can be terminated. The number of cracks or the time it takes for cracks to propagate to the critical size is obtained for both groups of samples. Simultaneously, the crack length or crack morphology is compared and analyzed to determine the failure mechanism.
[0029] A correlation model of corrosion behavior between the laboratory and the field was established. This involves not simply comparing failure times, but conducting in-depth correlation analysis. For example, the ratio of crack initiation time (K = T_crack-field / T_crack-lab) in the laboratory environment to the field environment under the same stress level was calculated using the time conversion factor method. This ratio K can be considered as a "deceleration factor" of the field environmental severity relative to the accelerated laboratory environment. The model also incorporates field-monitored soil parameters (such as average Cl) into the model. - Using concentration, pH value, temperature, soil resistivity, and material strength grade as input variables, and the material stress corrosion threshold value K_ISCC or crack propagation rate da / dt measured in the laboratory as a benchmark, an empirical or semi-empirical model for predicting crack initiation or propagation under field conditions is established through data fitting.
[0030] After the model is established, it needs to be validated and modified. A new pipe segment not involved in the model construction is selected, its pipe material is obtained, and accelerated testing is conducted in the laboratory, while its soil environmental parameters are measured. The obtained data is input into the parameterized model to calculate the predicted crack initiation time Tpred for the pipe segment. The actual crack initiation time Tactual is obtained by conducting short-term field embedded segment tests on the pipe segment or analyzing its historical detection data. If the relative error between Tpred and Tactual is within ±25%, the model is considered validated and can be used for the safety assessment of the pipeline system.
[0031] In step S4, a rapid laboratory test is conducted on the pipeline under test and its field environmental parameters are measured. The crack initiation time of the pipeline under test in the laboratory environment and the field environmental parameters are input into the correlation model to obtain the crack initiation time of the pipeline under test, which can be used as the life of the pipeline under test.
[0032] Specifically, correlation models are used to guide on-site pipeline safety assessments. For the pipe sections requiring assessment, soil samples are taken and their key corrosion parameters are analyzed. Pipe samples are then subjected to standard stress ring accelerated testing in the laboratory to obtain basic corrosion data. This data, along with soil parameters, is input into a validated correlation model, which outputs the predicted stress corrosion crack initiation time or remaining safe life of the pipe section under the current operating stress.
[0033] Develop pipeline integrity management recommendations. Based on the forecast results, propose targeted maintenance, inspection, or depressurization operation recommendations. For example, if the predicted lifespan is less than the next planned inspection cycle, it is recommended to shorten the ultrasonic guided wave or internal inspection cycle for that pipe section; if the predicted threshold is very low, it is recommended to evaluate the effectiveness of the cathodic protection system or consider coating repair.
[0034] In the life prediction method for pipelines in service under stress corrosion according to this invention, the load-strain relationship of the pipeline under test is first calibrated. Then, constant load tests are simultaneously conducted in the laboratory and in the field. Next, a laboratory-in-field correlation model is established. Finally, this correlation model is used to obtain the crack initiation time of the pipeline under test, i.e., the life of the pipeline. This invention establishes a mathematical bridge between accelerated laboratory testing and the actual service environment in the field by quantifying environmental factors. Using this model, subsequent rapid laboratory tests on the pipeline under test and measurement of its field environmental parameters are sufficient to accurately predict its life.
[0035] In some embodiments of the present invention, the association model is as follows: .
[0036] In the formula, The crack initiation time of the pipeline under test in the field environment. The crack initiation time of the pipeline under test in a laboratory environment. The chloride ion concentration in the on-site environment. The absolute temperature of the site environment. For the on-site environment value, As a comprehensive scale factor, This represents the relationship coefficient between the laboratory environment and the field environment over a time scale. This represents the promoting factor of chloride ion concentration on crack initiation. This represents the coefficient of influence of temperature on crack initiation. For the on-site environment The values are the influence coefficients on crack initiation, where A, B, C, D, and E are all coefficients greater than 0 (see Table 1 for details).
[0037] Table 1 shows the meanings of A, B, C, D, and E, which are related to... Impact coefficient symbol Physical meaning right Impact just Comprehensive scale factor Overall scaling of prediction time, The larger the value, the longer the prediction time. just Laboratory and field time nonlinearity index Field time is increasing faster than laboratory time; Field time increases more slowly than laboratory time; Linear relationship just Chloride ion sensitivity coefficient The higher the chloride ion concentration, The smaller the value, the shorter the prediction time (acceleration effect). just Temperature sensitivity coefficient The higher the temperature, The smaller the value, the shorter the prediction time (acceleration effect); if the actual data is the opposite, it can be adjusted to... just pH sensitivity index The higher the pH, the better. The smaller the value, the shorter the prediction time (in this example, pH increase inhibits SCC); if the actual result is the opposite, it can be adjusted. In this embodiment, a parametric empirical model incorporating multiple environmental parameters such as chloride ion concentration ([Cl⁻]), temperature (T), and pH value is introduced to achieve a more realistic simulation and quantitative characterization of the complex soil environment on site. By incorporating multiple key environmental parameters into a unified framework in a product form, the parameters are independent yet synergistic, which can more realistically reflect the comprehensive corrosion situation of the on-site environment.
[0038] Specifically, chloride ions are the key ion in the model, responsible for damaging the metal passivation film, inducing pitting corrosion, and promoting crack initiation. The model employs an exponential term. To describe its effects, C is typically negative, indicating that higher chloride ion concentrations accelerate pitting corrosion and crack initiation. Different pH ranges correspond to different SCC mechanisms. For example, SCC in high pH (>9) environments is mainly controlled by intergranular crack propagation, while SCC in near-neutral pH (6.5-7.5) environments is related to the synergistic effect of hydrogen embrittlement and anodic dissolution. The model uses a power function (pH)^E to describe this effect, where the sign and magnitude of E reflect the promoting or inhibiting effect of pH on the SCC mechanism of a specific pipe material. Temperature affects the electrochemical reaction rate according to the Arrhenius relation. The exp(D / T) term in the model is derived from classical electrochemical theory, D=Ea / R (Ea is the apparent activation energy, and R is the gas constant). By continuously measuring temperature on-site and substituting this exponential term, the model can accurately reflect the cumulative contribution of diurnal temperature differences and seasonal variations to the corrosion rate.
[0039] In some embodiments of the present invention, the on-site environment The value and chloride ion concentration are determined based on the following formula: ; in, For the first i The representative value of this parameter within a time period. For the first i The duration of each time period The total duration of the entire experiment. n The total number of time periods divided into the entire experiment.
[0040] In this embodiment, chloride ion concentration is used for illustration. Assuming the field test lasted 18 months, monitoring data showed that the average chloride ion concentration was 120 mg / L for days 1-90, 80 mg / L for days 91-180, 110 mg / L for days 181-270, 90 mg / L for days 271-360, 115 mg / L for days 361-450, and 85 mg / L for days 451-540. A time-weighted average was used.
[0041] (120×90+80×90+110×90+90×90+115×90+85×90) / 540=100 mg / L.
[0042] The same method is used for pH value.
[0043] This embodiment calculates environmental parameters using a time-weighted average, which more scientifically reflects the true impact of these parameters. Because corrosion is a cumulative process, the longer a parameter value persists, the greater its contribution to the corrosion process throughout the entire test cycle. Using a time-weighted average avoids excessive interference from short-term, drastic fluctuations in the overall evaluation results, making the environmental parameters input into the model more representative of the long-term, steady-state corrosion environment, thereby significantly improving the prediction accuracy and robustness of the correlation model.
[0044] In some embodiments of the present invention, the data fitting employs the Levenberg-Marquardt algorithm.
[0045] In this embodiment, the specific calculation process is as follows: (1) Data preparation: Collect at least 5 sets of “laboratory-field” paired data, each set of data containing an input vector. x i = (T lab , i ,[Cl−] i ,T i pH i ) and the corresponding measured crack initiation time in the field y i =T field,i .
[0046] (2) Define the objective function: The objective is to minimize the sum of squared residuals (SSE), that is: ; The goal of fitting is to find a set of coefficients (A, B, C, D, E) that minimizes SSE.
[0047] (3) Setting initial values and iteration: Set initial values for the coefficients based on experience or literature (e.g., .
[0048] The algorithm begins to iterate, and each iteration combines the fast convergence of the Gauss-Newton method with the stability of the gradient descent method to dynamically adjust the direction and step size of the coefficient increment.
[0049] (4) Convergence and output: When the change of SSE is less than the preset threshold or the maximum number of iterations is reached, the algorithm terminates and outputs the optimal coefficient set (A,B,C,D,E) that minimizes SSE.
[0050] In this embodiment, the Levonburg-Marquardt algorithm is used for data fitting. The goal is to minimize the sum of squared residuals between predicted and measured values to determine the coefficients to be fitted in the correlation model. The specific values of these coefficients are determined by fitting the sample data; the values vary depending on the pipe material and the corrosive environment. The Levonburg-Marquardt algorithm is a classic algorithm commonly used in nonlinear regression, offering advantages such as fast convergence and insensitivity to initial values. Using this algorithm ensures the standardization of the model fitting process and the reproducibility of the results. Those skilled in the art can directly implement this algorithm using MATLAB's `lsqcurvefit` function or Python's `curve_fit` function (which is based on this algorithm), eliminating the need to reinvent the algorithm and reducing the technical implementation difficulty. This algorithm can quickly find the globally optimal or near-optimal solution, ensuring that the established correlation model has the best predictive accuracy.
[0051] In some embodiments of the present invention, before the test, both the first group of pipes to be tested and the second group of pipes to be tested are loaded to the load corresponding to the target stress, the load is continuously monitored, and the load relaxation of the pipes to be tested is adjusted until the load fluctuation is less than the preset value.
[0052] In this embodiment, a load stabilization step is performed on both laboratory and field samples before the formal corrosion test begins. This specifically includes the following steps:
[0053] (1) Initial loading: Load the specimen to the target load using the loading nut (confirmed in the laboratory by stress sensor, and on site by strain value).
[0054] (2) Relaxation monitoring and compensation: In the initial stage after loading (e.g., for 5-7 days), monitor the load daily. Due to thread engagement, initial creep of the sample, etc., the load may relax. Once the load drop exceeds the preset threshold (e.g., 1% of the initial load), fine-tune the loading nut again to restore the load to the target value.
[0055] (3) Stability Criterion: Repeat the above process until the load fluctuation is less than the preset value (e.g., ±1% of the target load) within 72 consecutive hours. At this point, the system is considered to have reached a stable state, and the test time is officially recorded as zero (T=0), and the corrosion test begins.
[0056] If deviations are detected, handle them according to the following principles: 1. Deviation in the initial stage of the test (first 1-2 weeks): After stabilization adjustment in step 6, the load can be buried only after it is confirmed that the fluctuation is less than ±1% within 72 hours.
[0057] 2. Deviation during long-term burial: No excavation or adjustment is performed; deviation data is recorded solely through a strain gauge. After the test, if the deviation is within ±5% of the target strain value, the sample data is considered valid; if the deviation exceeds ±10%, the sample data is discarded and not used as the basis for model establishment.
[0058] 3. Under the same conditions, most samples deviate significantly: The reasons should be analyzed (such as failure of the loading device, abnormal interference from the field environment, etc.), and the test plan should be improved before re-burying the samples and carrying out the test. It is not recommended to introduce empirical correction factors to avoid increasing the uncertainty of the model.
[0059] In this embodiment, the load stabilization process is crucial because stress corrosion cracking is extremely sensitive to load. If the initial load relaxation is not compensated, the actual stress acting on the specimen will be lower than the target stress, leading to inconsistent test conditions and ultimately affecting T. lab and T field The accuracy and comparability of the data. This step ensures that the specimen is subjected to precise and constant target stress throughout the entire testing period, which can last for months or even years. This is a prerequisite for establishing a high-precision correlation model.
[0060] In some embodiments of the present invention, the target stress is 95% of the specified minimum yield strength of the pipe to be tested.
[0061] In this embodiment, in actual engineering, the operating stress of pipelines is typically 80% or lower of SMYS. Under this stress, the crack initiation time at near-neutral pH may be as long as 10 years or more. If field tests were conducted at this stress, the cycle would be too long and unacceptable. This invention uses a high stress of 95% SMYS for testing, the principle of which is "acceleration without altering the mechanism." According to the theory of creep and crack initiation in metallic materials, while maintaining the crack initiation mechanism unchanged, increasing the stress level will significantly shorten the crack initiation incubation period by increasing the local plastic deformation rate at the crack tip.
[0062] For example, this embodiment takes stress corrosion cracking (SCC) of an X65 grade oil and gas pipeline in a near-neutral pH soil environment as the research object, and specifically illustrates the complete process from data acquisition, model establishment, verification to engineering application. To ensure the feasibility of field testing, the field test also uses a stress level of 95% SMYS for acceleration, so as to obtain observable crack data within a reasonable period.
[0063] Basic data acquisition: as shown in Table 2 Table 2 Basic Data Table The field test employed the same 95% SMYS high-stress method as the laboratory test, aiming to simulate actual working conditions at pipe coating defects or stress concentration points and to accelerate the testing process. Based on engineering experience, near-neutral pH-SCC crack initiation can take more than 10 years under 80% SMYS; however, under 95% SMYS, this process is accelerated to approximately 2 years, making the field comparative test technically and economically feasible.
[0064] The data comes from corrosion monitoring probes buried near the target pipe section, which have been continuously monitored for 18 months.
[0065] pH and Cl- concentration exhibit seasonal fluctuations, and the model was established using their time-weighted average values.
[0066] Establishment of a parametric empirical model. The following parametric empirical model is used to correlate crack initiation time between the laboratory and field:
[0067] Data fitting process. Five sets of data were collected for the same pipe material, all obtained under 95% SMYS conditions. , ,[Cl - A paired dataset (T, pH) was used. The Levenburg-Marquardt algorithm was employed for nonlinear multiple regression.
[0068] Example of fitting results. Based on the above data fitting, a set of exemplary coefficients is obtained:
[0069] A = 2.25 × 10 -3 Given B=0.89, C=0.07, D=4300, E=0.04, substitute these values into the following formula. Important Note: The coefficients A, B, C, D, and E above are merely example values derived from the example data and are used to illustrate the model building process. In actual evaluation, it is necessary to refit the model using synchronous test data corresponding to the target pipeline to obtain targeted model parameters.
[0070] To verify the predictive reliability of the model, a section of similar X65 pipeline that was not involved in the modeling was selected for independent validation. (See Table 3)
[0071] Table 3 Validation Data Table Verification conclusion: The model prediction error is much less than ±25%, indicating that the correlation model has good prediction accuracy and engineering applicability for pipelines in such near-neutral pH environments.
[0072] The validated model (based on 95% SMYS data) was used to predict the crack initiation time of the pipeline under actual operating stress (80% SMYS). This requires introducing a stress correction factor R. stress .
[0073] The stress correction factor R stress This can be obtained through additional laboratory comparative tests. The specific method is as follows: Take pipe samples from the same batch and conduct constant load stress corrosion tests at two stress levels (80% SMYS and 95% SMYS) under the same standard corrosion environment (e.g., NS4 solution, 25°C, pH=6.5), and record the crack initiation time. 80 and 95. Then the stress correction factor R stress It can be defined as the ratio of the two:
[0074] R stress = 80 / 95 The R determined by this method stress It has a clear physical meaning (the accelerating effect of stress level on crack initiation time), and is transferable to the same type of pipe under similar corrosion mechanisms, providing a general and reliable technical path for extrapolating the model from accelerating stress to service stress.
[0075] This ratio reflects the factor by which crack initiation time is prolonged when the stress level decreases from 95% SMYS to 80% SMYS under the same corrosive environment. The R obtained by this method... stress This can serve as a bridge, reliably extrapolating the correlation model established based on high-stress (95% SMYS) accelerated testing to life prediction under actual operating stress (80% SMYS) conditions. To simplify this example, it is assumed that the stress correction factor R for the X65 pipe under the current environment has been determined using the aforementioned testing methods. stress ≈2.5. That is, under the same corrosive environment, when the stress decreases from 95%SMYS to 80%SMYS, the crack initiation time is extended by about 2.5 times.
[0076] Input data: Laboratory accelerated data (NS4, 95% SMYS): =5000 hours Stress correction factor: R stress =2.5 Laboratory reference time converted to 80% SMYS: =5000 × 2.5 = 12500 hours Average parameters from field monitoring: Cl- =2.0 g / L, pH=7.4, T=13°C (286 K), model prediction: #imgpt61# Converted to operating years: 55000 / (24×365)≈6.3 years Risk assessment: The predicted crack initiation time is approximately 6.3 years, which is longer than the accelerated testing cycle but still shorter than the generally accepted safety window of more than 10 years, indicating that this pipe section has a medium to high risk.
[0077] Inspection strategy: It is recommended to shorten the internal inspection cycle (such as ultrasonic guided wave) of this pipe section from the usual 5-8 years to 3-4 years, and to focus on it.
[0078] Maintenance measures: Immediately assess whether the cathodic protection potential of the area meets the standard, and plan to conduct coating inspection and repair.
[0079] Dynamic monitoring: An online corrosion monitoring system was added to this pipe section to track environmental and stress changes in real time, enabling dynamic updates and early warnings of the prediction model.
[0080] Choosing 95% SMYS is a theoretically and experimentally verified approach. It ensures both the feasibility of the experiment and the consistency of the crack initiation mechanism with that under low stress, representing the best balance between "accelerated testing" and "mechanism fidelity".
[0081] In some embodiments of the present invention, such as Figure 1 and Figure 3 As shown, the constant load stress corrosion test of the pipeline under test 8 is achieved through a constant load stress device. The constant load stress device includes a stress ring 1, a loading nut 2, a loading bolt 3, a bearing bolt 4, a solution tank 5, a stress measurement unit 6, and a strain measurement unit 7. The loading bolt 3 passes through the top of the stress ring 1 and extends into the stress ring 1; the loading nut 2 mates with the loading bolt 3. The bearing bolt 4 is located inside the stress ring 1 and below the loading bolt 3; the loading bolt 3 and the bearing bolt 4 are used to connect the pipeline under test 8. The solution tank 5 is located outside the pipeline under test 8 and is sealed to the loading bolt 3 and the bearing bolt 4; the solution tank 5 is used to hold the test solution and to introduce the test gas. The stress measurement unit 6 is used to detect the load applied to the pipeline under test 8, and the strain measurement unit 7 is used to detect the strain of the pipeline under test 8.
[0082] In this embodiment, a laboratory test is used as an example. The two ends of the pipe to be tested 8 are connected to the loading bolt 3 and the bearing bolt 4 respectively. The prepared corrosive solution is injected into the solution pool 5. The loading nut 2 and the loading bolt 3 are used to load the pipe to be tested 8. The stress and strain of the pipe to be tested 8 are measured by the stress measurement unit 6 and the strain measurement unit 7 respectively.
[0083] The device in this embodiment is compact, robust, and reliable. The stress ring 1 itself has a self-locking characteristic; once a load is applied via the nut, it can maintain a substantially constant force value over a long period, providing a physical basis for long-term on-site installation. The sealed design of the solution tank 5 ensures precise control of the laboratory environment, while during on-site installation, the solution tank 5 is removed, allowing the sample to directly contact the soil. This device successfully combines the precise loading capabilities of the laboratory with easy on-site operation.
[0084] In some embodiments of the present invention, the constant load stress device further includes a power supply unit for supplying power to the strain measurement unit 7. The power supply unit is a solar panel or a battery.
[0085] In this embodiment, when the pipe under test 8 is initially loaded to the target strain value, a portable strain acquisition device is used to read the strain data, a process with extremely low power consumption. During long-term monitoring: To achieve long-term, automated strain data acquisition (e.g., automatically acquiring data weekly to monitor load stability), power is required for the data acquisition module and the remote transmission module. In outdoor environments with sufficient sunlight, small solar panels can be configured to power the acquisition device and the battery via float charging, enabling long-term unattended operation. In areas without sunlight or where the pipe is buried deeply, high-capacity industrial-grade lithium batteries with low self-discharge rates can be used, sufficient to support several years of intermittent data acquisition. In extreme cases, manual inspection can also be used, with handheld devices periodically connecting to read data, completely independent of on-site power supply.
[0086] It is understood that the present invention has been described through some embodiments, and those skilled in the art will recognize that various changes or equivalent substitutions can be made to these features and embodiments without departing from the spirit and scope of the invention. Furthermore, under the teachings of the present invention, these features and embodiments can be modified to adapt to specific situations and materials without departing from the spirit and scope of the invention. Therefore, the present invention is not limited to the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application are within the protection scope of the present invention.
Claims
1. A method for predicting the stress corrosion life of pipelines in service in the field, characterized in that, Includes the following steps: Obtain the load-strain calibration relationship of the pipeline under test under target stress, and determine the corresponding target strain value; The samples from the same batch were divided into two groups. The first group of pipes was subjected to constant load stress corrosion test in a standard corrosion environment in the laboratory. The second group of pipes was buried at the service site of the target pipe and subjected to constant load stress corrosion test. In the field test, the load was applied to the sample according to the target strain value. The duration of crack initiation in the pipeline under test in a laboratory environment was obtained based on the first set of experiments. The duration of crack initiation in the pipeline under test in a field environment was obtained based on the second set of experiments. The environmental parameters include chloride ion concentration, temperature, and pH value. The laboratory crack initiation duration, field crack initiation duration, and corresponding environmental parameters of each set of experiments were used as sample data. The laboratory crack initiation duration, chloride ion concentration, temperature, and pH value were used as input variables, and the field crack initiation duration was used as the target variable. A correlation model was established through nonlinear regression fitting. The correlation model was used to characterize the quantitative relationship between the field crack initiation duration, the laboratory crack initiation duration, and the environmental parameters. For the target pipe section to be predicted, the crack initiation time of the pipe material under laboratory conditions is obtained, and the chloride ion concentration, temperature and pH value of the target pipe section at the service site are collected. The above data are substituted into the correlation model to calculate the predicted value of the crack initiation time of the pipe section under the field service conditions, which serves as the basis for evaluating the stress corrosion life of the pipe section.
2. The life prediction method for pipelines in service under stress corrosion according to claim 1, characterized in that, The association model is as follows: ; In the formula, The crack initiation time of the pipeline under test in the field environment. The crack initiation time of the pipeline under test in a laboratory environment. The chloride ion concentration in the on-site environment. The absolute temperature of the site environment. For the on-site environment value, As a comprehensive scale factor, This represents the relationship coefficient between the laboratory environment and the field environment over a time scale. This represents the promoting factor of chloride ion concentration on crack initiation. This represents the coefficient of influence of temperature on crack initiation. For the on-site environment The value is the influence coefficient on crack initiation.
3. The life prediction method for pipelines in service under stress corrosion according to claim 2, characterized in that, The on-site chloride ion concentration and on-site pH value are calculated using a time-weighted average.
4. The method for predicting the service life of pipelines in field operation under stress corrosion according to claim 1, characterized in that, The data fitting uses the Levenberg-Marquardt algorithm, aiming to minimize the sum of squared residuals between predicted and measured values, to determine the coefficients to be fitted in the correlation model; the specific values of the coefficients to be fitted are determined by fitting the sample data, and the values of the coefficients are different for different pipe materials and different corrosion environments.
5. The method for predicting the service life of pipelines in field operation under stress corrosion according to claim 1, characterized in that, It also includes the step of establishing the load-strain calibration relationship of the pipe before the test: in the laboratory, the specimen is subjected to incremental loads step by step, and the load value and corresponding strain value under each load are recorded simultaneously. The load-strain calibration curve is plotted, and the target strain value corresponding to the target stress is determined according to the calibration curve. In the field test, the specimen is loaded until the strain value reaches the target strain value, so that the stress level of the field specimen is consistent with the target stress in the laboratory.
6. The method for predicting the service life of pipelines in field operation under stress corrosion according to claim 5, characterized in that, After the specimen is loaded to the target stress, the load is continuously monitored in the initial stage. When the load relaxes due to thread engagement or initial deformation of the specimen, the load is restored to the target value by adjusting the loading device. This process is repeated until the load fluctuation is less than ±1% of the target load within 72 consecutive hours. This is recorded as the start time of the test. The target stress is 95% of the specified minimum yield strength of the pipe to be tested.
7. The method for predicting the service life of pipelines in field operation under stress corrosion according to claim 1, characterized in that, In the second group of on-site burial tests, the data obtained by monitoring were used to verify the accuracy of the initial loading during burial and to record the load stability during the test period. After the test, the data of the samples that deviated from the target strain value within ±5% were considered valid, and the data of the samples that deviated from the target strain value by more than ±10% were discarded.