A material fatigue life prediction method based on small punch test
By designing small-sized circular sample pieces and using specialized fixtures, combined with SWT fatigue damage theory and key parameter extraction, the problem of large errors in fatigue life prediction for small punches has been solved, achieving high-precision life prediction and rapid estimation, which is suitable for material fatigue assessment of high-end equipment such as aero-engines.
Patent Information
- Application Number
- CN202611077973.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-24
AI Technical Summary
Existing methods for predicting fatigue life in small punching holes lack the mechanical basis for fatigue damage evolution. The model parameters vary significantly with material and load, resulting in weak extrapolation ability, large prediction errors, and failure to fully utilize the key characteristic parameters in the fatigue curve of small punching holes.
A small-sized circular sample design was adopted, and the sample was prepared by wire cutting and precision milling. Combined with special fixtures and diamond polishing, the test was carried out and the load-displacement data was recorded. Key parameters such as valley loading linear displacement and hysteresis loop morphology were extracted. A life prediction model based on SWT fatigue damage theory was established. The equivalent peak stress was calculated by using the modified contact stress formula or finite element method, and a small punch fatigue life prediction model was constructed.
It achieves accurate prediction of fatigue life of small punches, with prediction error controlled within ±10%, and is suitable for scenarios with different precision requirements, meeting the needs of high-precision laboratory research and rapid industrial screening.
Smart Images

Figure CN123155359A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials mechanics testing technology, specifically a method for predicting the fatigue life of materials based on small-hole punching tests. Background Technology
[0002] Key hot-end components in high-end equipment such as aero-engines and gas turbines operate under extreme environments of high temperature, alternating loads, and complex media for extended periods, making fatigue failure one of their primary failure modes. However, these components often possess complex, irregular structures, thin-walled features, or gradient microstructures, and are frequently manufactured using novel forming processes such as additive manufacturing and laser repair, resulting in uneven microstructure distribution and significant differences in local properties. Traditional uniaxial fatigue testing according to standards such as GB / T3075 and ASTM E466 requires the preparation of large-size standard specimens, making direct sampling from these complex components extremely difficult, if not impossible.
[0003] Traditional methods struggle to provide effective micro-area performance data for assessing the remaining life of locally damaged areas in in-service components. Small-hole fatigue testing, a micro-sample mechanical testing technique, uses miniature circular specimens with a diameter of 8–12 mm and a thickness of 0.3–0.8 mm. A spherical punch applies a periodic alternating load to the center of the specimen, continuously recording the load-displacement curve to evaluate the material's fatigue performance. However, existing small-hole fatigue life assessment methods still suffer from the following technical problems: Currently, most models use numerical fitting empirical models, directly applying the power-law relationship between the valley loading line displacement and the number of cycles to life prediction. Such models lack the mechanical basis of fatigue damage evolution, the model parameters vary significantly with material and load, the extrapolation ability is weak, and the prediction error range exceeds 4 times. Some studies have attempted to directly apply the traditional Basquin or Smith models to small punch fatigue data. However, the stress state of small punch specimens is complex, including various deformation modes such as bending, tension and contact indentation, which is fundamentally different from uniaxial fatigue. This results in a low fitting determination coefficient and a prediction error of up to 5 to 6 times. Existing methods fail to fully utilize key characteristic parameters in the fatigue curve of small punching holes, especially indicators such as the width of the ratchet curve at half-life cycles and the morphology of the hysteresis loop, which can reflect the cyclic plastic strain amplitude. These parameters have been shown to be highly correlated with fatigue life in traditional fatigue theory. Due to the lack of an effective means to convert macroscopic loading line displacement into local strain amplitude, a fatigue life prediction model for small punching holes based on SWT parameters has not yet been established. Summary of the Invention
[0004] The purpose of this invention is to provide a method for predicting the fatigue life of materials based on small-hole punching tests, so as to solve one or more problems mentioned in the background art.
[0005] To achieve the above objectives, the present invention provides the following technical solution: a material fatigue life prediction method based on small punching test, including a sample preparation stage, a test implementation stage, a parameter extraction stage, a stress calculation stage, a model construction stage, a parameter fitting stage, and a life prediction stage; Furthermore, in the sample preparation stage, circular small-hole fatigue samples are cut from the test material using wire cutting or precision milling. The diameter of the samples is controlled within the range of 8-12 mm, the initial thickness is 0.3-0.8 mm, and the thickness deviation does not exceed ±0.02 mm. The upper and lower surfaces of the samples are mechanically ground sequentially using 180#, 400#, 800#, 1200#, and 2000# silicon carbide abrasive paper, and then mechanically polished using a diamond polishing agent with a grit size of 0.5 μm until there are no obvious scratches on the sample surface and the surface roughness Ra≤0.4 μm. After polishing, the samples are ultrasonically cleaned in anhydrous ethanol for 3-5 minutes to remove residual abrasive debris and oil stains. After removal, the samples are dried with nitrogen gas and stored in a desiccator for later use.
[0006] Furthermore, during the test implementation stage, the small punch fatigue specimen is placed horizontally on the lower die support platform of the test fixture, ensuring that the center of the specimen, the center of the lower die, and the center of the punch ball are coaxial, with a coaxiality error not exceeding ±0.05mm; the upper surface of the specimen is in contact with the spherical surface of the punch ball, and the lower surface of the specimen is supported by the annular support surface of the lower die; the lower die hole diameter of the fixture is 1.5~2.5mm, and the chamfer radius of the lower die support surface is 0.1~0.2mm; the punch ball is made of cemented carbide or ceramic material, with a radius of 1.0~1.5mm, a surface roughness Ra≤0.02μm, and a Rockwell hardness HRA≥90.
[0007] Set up the special coaxiality testing instrument at the designated position next to the fixture, divide the sample radially into multiple equal testing directions, and check the alignment of the three centers in each direction in turn. After the single-direction test is completed, fine-tune the fixture adjustment components. After all directions are tested and meet the standards, tighten all the adjustment and locking structures of the fixture, and then select two random directions again for a second verification test.
[0008] After completing the specimen positioning and clamping operations, a static preloading process must be performed on the entire assembly structure. The preloading load is matched according to the mechanical properties of the test material and maintained to eliminate assembly gaps. The preloading operation can completely eliminate the tiny assembly gaps between the fixture, the punch, and the specimen, allowing the punch surface to achieve full and tight surface contact with the upper surface of the specimen. This avoids data anomalies in the initial loading stage due to insufficient contact, ensuring the consistency of test conditions from the assembly stage.
[0009] Based on the service conditions of the material under test, the test temperature and load parameters are set. The room temperature test temperature is controlled at 20±2℃. The high temperature test is set with constant temperature conditions according to the service conditions, using a resistance furnace or induction heating, with temperature fluctuation not exceeding ±3℃. The load ratio is 0.05~0.5, and the peak load is determined according to the material strength grade, so that the sample undergoes cyclic plastic deformation without early fracture. A sinusoidal alternating load is applied to the sample at a constant frequency of 0.01~0.1Hz. A load sensor with an accuracy of not less than 0.1%FS and a displacement sensor with an accuracy of not less than 0.1μm are used to continuously record the loading linear displacement and load until the sample completely fractures or reaches the preset cycle termination condition, and the small punch fatigue loading linear displacement-cycle number curve is obtained.
[0010] After the equipment is started, a small-amplitude preload operation is first performed, slowly outputting a low-level load and maintaining it for a short period of time. Then, the load value is gradually increased in a uniform manner until the load reaches the preset peak load. After all single-group tests are completed, the output load is reduced in a step-by-step manner until the load value drops back to zero. After confirming that the load is completely unloaded, the equipment is then operated to perform the overall shutdown procedure.
[0011] Two types of independently selectable test termination rules are set up to suit different test requirements. The first type is a fixed cycle number termination rule, which sets a maximum upper limit for the number of cycles in advance based on the material's service conditions and the test research objectives. When the number of loading cycles reaches this upper limit, the test is stopped immediately. The second type is a deformation anomaly termination rule, which monitors the displacement changes along the loading line in real time throughout the test. Once the displacement data shows a large, irregular change, it indicates that the specimen has suffered serious damage, and the test is terminated immediately. The two types of termination rules can be flexibly selected according to the test type, but all tests in the same batch must use the same termination rule.
[0012] The high-temperature test adopts a uniform heating mode, and after reaching the set temperature, it is kept at a constant temperature to ensure uniform sample temperature and avoid the superposition of thermal stress from affecting the test results.
[0013] Furthermore, in the parameter extraction stage, computer data processing software is used to preprocess the collected load-displacement data, remove abnormal noise points, and extract the following key parameters from the fatigue loading linear displacement-cycle number curve of the small punch: Valley loading line displacement: When the load is unloaded to the minimum in each cycle, the minimum loading line displacement will appear. The valley displacement of three consecutive cycles is selected and the average value is calculated. The result is used as the valley loading line displacement of the current cycle. When selecting cyclic data, it is necessary to actively avoid the initial stage of the test when the material deformation is not yet stable, and prioritize the continuous cycle group after the fatigue loading has entered a stable operating state. In the initial stage of the test, the deformation pattern of the specimen fluctuates greatly due to factors such as assembly and initial stress, and the data in this stage is not of reference value.
[0014] Half-life cycles: The fatigue life is defined as the number of cycles until the specimen completely fractures, and the half-life cycles is half of the fatigue life value. If the specimen has not fractured when the test ends, half of the cumulative number of cycles at the end of the test is taken as the half-life cycles. A unified and objective dual criterion for determining complete fracture of the specimen is established. The specimen fracture is determined based on the dual characteristics of continuous and sudden load drop and irreversible abrupt change in loading linear displacement, ensuring that the fatigue life statistical nodes of each group of tests are completely consistent.
[0015] Half-life cycle ratchet curve width: Select the load and loading linear displacement hysteresis loop corresponding to the half-life cycle, first calculate the average load, which is obtained by adding the peak load and the valley load and taking the average value; Find two points on the hysteresis loop that intersect with the average load. The difference in the loading line displacement between the two points is the width of the ratchet curve for half a life cycle. This parameter can reflect the cyclic plastic strain amplitude of the material under half a life cycle. Import the complete displacement-cycle number curve and load data into the data processing software. Use the search function to locate the time node corresponding to the half-life cycle. Use the software's clipping tool to select the complete hysteresis loop corresponding to that node. Generate a separate independent data file for the clipped hysteresis loop and save it temporarily.
[0016] When collecting hysteresis loop data corresponding to half-life cycles, a high-frequency continuous sampling mode is used throughout. The sampling frequency is synchronously adjusted according to the test loading frequency to ensure that the collected data points are sufficiently dense. Dense data points can completely reconstruct the overall outline and detailed morphology of the hysteresis loop, avoiding the loss of local features due to excessively large sampling intervals. After data collection, a preliminary check of the hysteresis loop morphology is required. Only after confirming that the outline is complete and without missing parts should point selection and parameter calculation be performed.
[0017] Half-life cycle loading line displacement value: This parameter is the peak loading line displacement corresponding to half-life cycle, which is the displacement value corresponding to the current cycle loading to the peak load.
[0018] Furthermore, in the stress calculation stage, based on the load parameters and specimen geometry of the small-hole fatigue test, a modified contact stress formula is used to calculate the equivalent peak stress: Equivalent peak stress calculation formula:
[0019] This represents the equivalent peak stress, in MPa. This indicates the radius of the break shot, in mm. Represents the peak load of the test, in units of N ; This represents the peak linear displacement at half-life cycle loading, in mm. This indicates the initial thickness of the sample, in mm.
[0020] For applications requiring higher precision, the finite element method is used to determine the equivalent peak stress: a finite element model of small punch fatigue test consistent with the test conditions is established, the deformation process of the specimen under different peak loads is simulated and the maximum principal stress in the critical area of the specimen is extracted, the mapping relationship between the maximum principal stress calculated by finite element method and the peak load of the test and the peak displacement of the half-life cycle loading is established, and the equivalent peak stress under the actual test conditions is calibrated by interpolation method.
[0021] The ratio of the width of the ratchet curve at half-life cycles to the initial thickness of the specimen is used as an approximation of the fatigue strain amplitude; combined with the equivalent peak stress obtained in the stress calculation stage, a fatigue life prediction model for small punching is constructed.
[0022] Based on the actual experimental assembly relationship, contact pairs between the punch ball and the specimen, and between the specimen and the lower mold, are created sequentially within the model, and the contact type and contact algorithm are set. Referring to the experimental loading rules, multiple loading steps are created step by step within the simulation module to match the alternating load application form and loading duration of the experiment, thus replicating the loading process of the physical experiment.
[0023] Within the finite element simulation software interface, categorize and move the simulation result files for different working conditions into their corresponding subfolders. After all working conditions have been calculated, close all simulation task windows.
[0024] When performing finite element simulation modeling, all structural dimensions, contact relationships, and assembly forms of the physical experiment are replicated. Local mesh refinement is applied to hazardous areas where the specimen is prone to failure to improve the accuracy of stress calculations in those areas. Conventional meshing methods are used for the remaining areas of the specimen to balance computational efficiency and overall simulation accuracy. Specialized elements adapted to thin-plate structures and cyclic large deformation scenarios are selected, and the model boundary conditions are set entirely based on the constraint forms and support methods of the experimental fixtures.
[0025] Furthermore, the model construction stage is based on the SWT fatigue damage theory, using the ratio of the half-life cycle ratchet curve width to the initial thickness of the specimen as an approximation of the fatigue strain amplitude; combined with the equivalent peak stress obtained in the stress calculation stage, a fatigue life prediction model for small punching holes is constructed: The equivalent peak stress, half-life cycle ratchet curve width, and initial thickness of the specimens in the same group are uniformly retrieved. All parameters are grouped and collected according to the single specimen group, and then the standardized parameter dataset is organized before the model building work is carried out.
[0026] Basic model for fatigue life prediction based on SWT theory:
[0027] This represents the equivalent peak stress, in MPa. Indicates the initial thickness of the sample, in mm; The width of the ratchet curve indicates the half-life cycle count, in mm. This represents the material constant to be fitted, which is dimensionless. This represents the material constant to be fitted, which is dimensionless. This indicates the fatigue life of a material, expressed in cycles. This indicates the total number of times the fatigue cycle reverses its loading. The total fatigue life of a material is measured in cycles.
[0028] Furthermore, the parameter fitting stage includes at least 5 sets of small punch fatigue test data under different peak loads, and the test data covers the low-cycle fatigue and high-cycle fatigue regions of the material, with the peak load difference between each two adjacent test sets not less than 50N. Based on the general classification rules for fatigue performance research of metallic materials, the working conditions with low cyclic loading cycles and high load levels are classified as low-cycle fatigue regions, where the material is mainly damaged by plastic deformation; the working conditions with high cyclic loading cycles and low load levels are classified as high-cycle fatigue regions, where the material is mainly damaged by elastic fatigue. The experimental data used for parameter fitting need to completely cover both fatigue regions simultaneously, and transitional working condition data need to be set between the two regions.
[0029] Record the fatigue life, equivalent peak stress, half-life cycle ratchet curve width, and initial specimen thickness for each test group; perform double logarithmic transformation on the data and plot scatter plots; use the least squares method for linear regression analysis to fit the intercept and slope of the straight line, and then determine the two material constants corresponding to the model.
[0030] Furthermore, in the life prediction stage, for the same type of material sample to be predicted, the entire process of sample preparation, testing, and parameter extraction is completed sequentially. This includes preparing the test sample and conducting small-hole fatigue tests to obtain the half-life cycle ratchet curve width and equivalent peak stress. The half-life cycle ratchet curve width and equivalent peak stress are then substituted into the life prediction model established in the model construction stage to solve for the predicted fatigue life value. Retrieve the corresponding material constants from the previous archive, verify that the material, test temperature, load range and model calibration conditions of the test sample are consistent, and after confirming that the parameters are compatible, perform the parameter substitution operation.
[0031] Fatigue life calculation conversion formula:
[0032] This indicates the predicted fatigue life of the material, expressed in cycles. This represents the equivalent peak stress, in MPa. The width of the ratchet curve indicates the half-life cycle count, in mm. The material constants representing the completed fit are dimensionless. Indicates the initial thickness of the sample, in mm; The material constants that represent the completed fit are dimensionless.
[0033] If a fracture test of the specimen is not performed, a power-law empirical model is used for preliminary estimation. According to the fatigue loading linear displacement-cycle number curve of small punching, the valley loading linear displacement and the number of cycles follow a power-law relationship in the initial and medium-to-long-term stable deformation stages of loading. The fatigue life of the specimen is calculated by extrapolation based on this relationship.
[0034] Valley loading linear displacement power-law empirical formula:
[0035] This represents the valley loading line displacement corresponding to a cycle number of N, in mm. represents the fitting parameters of the power-law model, which are dimensionless; This indicates the number of fatigue loading cycles, in weeks. This represents the fitting parameters of the power-law model, which are dimensionless.
[0036] The beneficial effects of this invention are as follows: 1. This invention adopts a small-sized circular sample design with a reasonable sample size range, less overall material usage, and convenient sampling. Sampling can be completed directly from a small local area of the component. The sample has a standardized process for surface grinding, polishing, ultrasonic cleaning, and sealed storage. The test is equipped with a special fixture, and the size, surface accuracy, and hardness of each component are limited. The sample clamping has high coaxiality. At the same time, the test can flexibly set different temperatures, load ratios, and peak load parameters to match the actual service conditions of various materials.
[0037] 2. This invention utilizes the mature SWT fatigue damage theory to construct a life prediction model, transforming the half-life cycle ratchet curve width into an approximate fatigue strain amplitude, establishing a mechanical relationship between equivalent peak stress, strain parameters, and fatigue life. During the experimental phase, the original load-displacement data undergoes noise reduction processing, and multiple core fatigue characteristic parameters are systematically extracted. In the parameter fitting stage, multiple sets of gradient load test data are selected to fully cover the low-cycle and high-cycle fatigue ranges. Linear regression is completed through double logarithmic transformation combined with the least squares method to calibrate the material constants within the model.
[0038] 3. This invention sets up two-level equivalent peak stress calculation methods to meet different accuracy requirements. Under normal working conditions, the calculation can be quickly completed by modifying the contact stress formula, and the calculation process is simple. In high-precision detection scenarios, a finite element model can be built, and the stress in the critical area can be calibrated by combining the mapping relationship and the interpolation method to restore the true stress state of the sample. In the life prediction stage, two implementation methods are also set up. After completing the full-process fracture test, the fatigue life value obtained by the model can be substituted. When no fracture test is performed, the result can be quickly extrapolated and estimated by the power law relationship between the valley loading line displacement and the number of cycles. Multiple calculation and prediction modes can be freely combined to meet the needs of high-precision research in the laboratory and adapt to the rapid screening scenarios in industrial fields. Attached Figure Description
[0039] Figure 1 This is a flowchart of the fatigue life prediction process for small-hole test materials according to the present invention. Figure 2 This is a schematic diagram of the small punching test of the present invention; Figure 3 This is a curve showing the linear displacement-cycle count during fatigue loading of small punch holes according to the present invention. Figure 4 This is a graph showing the predicted fatigue life of small punch holes according to the present invention. Figure 5 This is a diagram showing the result of the ratchet curve width during the half-life cycle of the small punching hole in this invention.
[0040] Figure label: 1. Punch; 2. Ball punch; 3. Lower mold; Detailed Implementation The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0041] like Figures 1 to 5 As shown, this invention provides a method for predicting the fatigue life of materials based on small-hole punching tests. In this embodiment, taking GH4169, a high-temperature alloy used in aero-engines, as an example, the method of this invention is used to predict its small-hole punching fatigue life. The specific steps are as follows: Preparation of small-hole fatigue specimens: Circular specimens with a diameter of 10 mm and a thickness of 0.5 mm were cut from GH4169 alloy sheet using wire cutting, with the thickness deviation controlled within ±0.01 mm. The upper and lower surfaces of the specimens were progressively ground using 180#, 400#, 800#, 1200#, and 2000# silicon carbide abrasive paper, and then polished with 0.5 μm diamond polishing agent until the surface roughness Ra = 0.2 μm. After polishing, the specimens were ultrasonically cleaned with anhydrous ethanol for 4 min, dried with nitrogen, and then stored in a desiccator for later use.
[0042] Install the specimen and conduct the test: Place the specimen in the small punch test fixture. The lower die 3 has a hole diameter R = 2.0 mm and a chamfer radius of 0.15 mm on the support surface. The punch ball 2 is made of cemented carbide with a radius r = 1.25 mm, a surface roughness Ra = 0.01 μm, and a Rockwell hardness HRA = 92. Adjust the fixture to make the center of the specimen, the center of the lower die 3, and the center of the punch ball 2 coaxial, with a coaxiality error of ±0.03 mm.
[0043] The test was conducted at room temperature (20±2℃), with a load ratio R=0.1. The peak loads were 250N, 300N, 400N, 500N, and 600N, respectively, and the loading frequency was 0.04Hz, using a sinusoidal wave. The load and displacement data for each cycle were continuously recorded until the specimen completely fractured.
[0044] Extracting key test parameters: After preprocessing the collected data and removing noise, the fatigue life Nf and half-life cycles N of each test group were extracted. half The half-life cycle ratchet curve width w and the half-life cycle loading linear displacement dh.
[0045] Table 1: Experimental Results Data
[0046] Calculate the equivalent peak stress The equivalent peak stress under each peak load is calculated using the modified contact stress formula from the stress calculation stage. Fmax=300N, dh=0.25mmσmax=0.3056×300×(1+0.50.25)=0.3056×300×1.5≈137.5MPa Fmax=400N, dh=0.32mmσmax=0.3056×400×(1+0.50.32)=0.3056×400×1.64≈200.5MPa Fmax=500N, dh=0.41mmσmax=0.3056×500×(1+0.50.41)=0.3056×500×1.82≈278.1MPa Fmax=600N, dh=0.52mmσmax=0.3056×600×(1+0.50.52)=0.3056×600×2.04≈374.0MPa Fitting model parameters: Calculate the parameters for each group of trials. ·w / Value, then for ·w / Taking the double logarithm of 2Nf and performing linear regression analysis using the least squares method, the fitted line equation is obtained as: lg(σmax) w / h0)=3.012-0.12×lg(2Nf); Therefore, the material constants α1 = 10^3.012 ≈ 1028 and β1 = -0.12 are determined, and the fitting coefficient of determination R² = 0.94, which meets the accuracy requirements.
[0047] Prediction Verification: A verification test was conducted with a peak load of 450N, and the linear displacement during half-life cycles was measured. =0.38mm, half-life cycle ratchet curve width w=0.28mm. Calculate the equivalent peak stress: =(3×450) / (2×π×1.25²)×(1+0.38 / 0.5)=520MPa; Substituting into the life prediction model: 520×(0.28 / 0.5)=850×(2Nf)^(-0.11)291.2=850×(2Nf)^(-0.11)(2Nf)^(-0.11)=0.34262Nf=0.3426^(-1 / 0.11)≈2500Nf≈1250 cycles; The actual fatigue life measured by the verification test was 1180 cycles, with a relative error of (1250-1180) / 1180×100%≈5.9%, which is within the allowable error range of ±10% in engineering.
[0048] Rapid life estimation: Using the valley loading linear displacement data of the first 30% of cycles (approximately 350 cycles) under a peak load of 450N, the parameters of the power-law empirical model are fitted to obtain the parameters. =0.052, =0.18. Taking the critical failure threshold dv, cr=0.6mm, the fatigue life is extrapolated to obtain a rapid estimate: 0.6=0.052×N^0.18N^0.18=11.538N≈1120 cycles; Compared to the actual lifespan of 1180 cycles, the relative error is -5.1%, meeting the engineering requirements for rapid prediction.
[0049] The above embodiments demonstrate that the method of the present invention can accurately predict the fatigue life of small punches in materials, with the prediction error controlled within ±10%, which is significantly better than the ±4 to ±6 times error range of existing methods. It also provides a rapid life estimation method and has good engineering application value.
[0050] The above are merely preferred embodiments of the present invention and are not intended to limit the invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
[0051] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0052] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for predicting fatigue life of a material based on a small punch test, characterized by, include: In the sample preparation stage, circular small-punched fatigue samples were processed and then surface-treated, cleaned and dried in sequence before being sealed and stored for later use. During the test implementation phase, the pretreated specimen is placed coaxially in a special test fixture. The test temperature, load ratio and peak load parameters are set according to the material service conditions. A sinusoidal alternating load is applied and the loading line displacement and load data are collected in real time until the specimen reaches the preset test termination conditions. In the parameter extraction stage, the collected load-displacement data is denoised, and the basic parameters of fatigue performance are extracted from the fatigue loading linear displacement-cycle number curve of the small punch. In the stress calculation stage, the equivalent peak stress is calculated by combining the geometric parameters of the specimen and the loading conditions using the modified contact stress formula. Under high-precision testing conditions, a finite element model corresponding to the test conditions is established. First, the mapping relationship between stress, load, and displacement parameters is constructed, and then the equivalent peak stress in the critical area of the specimen is calibrated by interpolation. In the model building phase, based on the SWT fatigue damage theory, a basic model for fatigue life prediction is constructed using the equivalent peak stress and fatigue strain amplitude parameters. In the parameter fitting stage, multiple sets of gradient load test data were selected, and after double logarithmic transformation, the least squares method was used for linear regression processing to fit and determine the material constants corresponding to the life prediction model. In the life prediction stage, tests are conducted on samples of similar materials to be tested to obtain the required parameters, which are then substituted into the prediction model to calculate the fatigue life. If no fracture test is conducted on the sample, the fatigue life of the sample is extrapolated based on the power law relationship between the valley loading line displacement and the number of cycles in the initial loading stage and the medium-to-long-term stable deformation stage.
2. The method of claim 1, wherein, The sample preparation stage includes: cutting circular small-hole fatigue samples with a diameter of 8mm to 12mm and an initial thickness of 0.3mm to 0.8mm from the material to be tested; grinding the upper and lower surfaces of the sample step by step with silicon carbide sandpaper, and then polishing with diamond polishing agent; after polishing, ultrasonically cleaning in anhydrous ethanol for 3min to 5min, taking it out, blowing it dry with nitrogen gas, and sealing it for later use.
3. The method of claim 1, wherein the method is characterized by: The test implementation stage includes: placing the sample horizontally on the lower die support platform of the fixture, so that the center of the sample is coaxial with the center of the lower die and the center of the punch ball; the upper surface of the sample is in contact with the spherical surface of the punch ball, and the lower surface is supported by the annular support surface of the lower die; the aperture of the lower die is 1.5mm~2.5mm, and the chamfer radius of the support surface is 0.1mm~0.2mm; the radius of the punch ball is 1.0mm~1.5mm, the surface roughness Ra≤0.02μm, and the Rockwell hardness HRA≥90.
4. The method of claim 1, wherein, During the experimental phase, the room temperature test was controlled at 25°C, and the high temperature test was conducted under constant temperature conditions and with limited temperature fluctuation range, in accordance with the material service requirements. The load ratio was 0.05 to 0.5, and the peak load was determined based on the material strength grade. Load sensors and displacement sensors were used to continuously collect data until the sample completely broke or the preset cycle termination condition was reached.
5. The method of claim 1, wherein, The basic fatigue performance parameters extracted during the parameter extraction stage include valley loading linear displacement, half-life cycles, half-life cycle ratchet curve width, and half-life cycle loading linear displacement peak value.
6. The method of predicting material fatigue life based on small punch testing according to claim 5, wherein The finite element calibration method in the stress calculation stage is as follows: establish a finite element model consistent with the test conditions, simulate the deformation process of the specimen under different peak loads and extract the maximum principal stress in the critical area; establish the mapping relationship between the maximum principal stress and the corresponding peak load and the peak value of the half-life cycle loading line displacement, and then use the interpolation method to calibrate the equivalent peak stress under the actual test conditions.
7. The method of claim 5, wherein the method is characterized by: In the model construction stage, the ratio of the width of the ratchet curve at half-life cycles to the initial thickness of the specimen is used as an approximation of the aforementioned fatigue strain amplitude.
8. The method of claim 1, wherein the method is characterized by: In the parameter fitting stage, at least 5 sets of test data under different peak loads are selected. Each set of test data covers the low-cycle fatigue and high-cycle fatigue regions of the material. The absolute value of the difference between two adjacent peak loads is not less than 50N. The fatigue life, equivalent peak stress, half-life cycle ratchet curve width and initial thickness of the specimen are recorded for each set of tests. The data are subjected to double logarithmic transformation and scatter plot is drawn. The intercept and slope of the fitted line are obtained by linear regression fitting, and then the two material constants corresponding to the model are determined.
9. The method of claim 5, wherein the method is characterized by: In the life prediction stage, the same material test sample is prepared, tested and parameter extracted in sequence to obtain the half-life cycle ratchet curve width and equivalent peak stress, which are then substituted into the life prediction model to obtain the fatigue life prediction value.
10. The method for predicting material fatigue life based on small-hole punching tests according to claim 9, characterized in that, When no fracture test is performed during the life prediction stage, the fatigue life of the specimen is extrapolated based on the fatigue loading linear displacement-cycle number curve of small punching, using the power law relationship between the valley loading linear displacement and the number of cycles during the initial loading stage and the medium-to-long-term stable deformation stage.