A method for testing the incubation period damage of a cementitious material to cavitation
By employing nanoindentation technology with specific depth interception and multiphase statistical deconvolution, combined with single-bubble impact and flow field energy input, the problem of quantitative identification and engineering risk assessment of cavitation erosion incubation damage in cement-based materials has been solved, achieving more accurate assessment of cavitation erosion resistance and risk warning.
Patent Information
- Application Number
- CN202611259888.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies are insufficient to effectively identify microscopic damage during the cavitation incubation period of cement-based materials, and there is a lack of effective connection between laboratory microscopic detection results and engineering cavitation risk assessment.
By employing methods such as specific depth interception, abnormally high modulus screening, and multiphase statistical deconvolution, nanoindentation technology is used to obtain quantifiable changes in the volume fraction of microphases. Combined with single-bubble impact and flow field energy input, quantitative identification and risk assessment of cavitation erosion incubation damage are achieved.
It improves the quantification and relevance of cavitation erosion evaluation for cement-based materials, accurately reflects the cavitation erosion resistance of materials, provides a unified critical damage threshold for engineering risk assessment, and achieves effective integration of laboratory results and engineering applications.
Smart Images

Figure CN123155369A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cavitation damage testing technology, and specifically to a method for testing cavitation damage during the incubation period of cement-based materials. Background Technology
[0002] Mortar is a typical multiphase heterogeneous brittle material, its microstructure consisting of a porous phase, hydrated calcium silicate gel (CSH), calcium hydroxide (CH), unhydrated particles, and interfacial transition zones. Under conditions of high-speed flow, insufficient aeration, or significant local pressure drop, cavitation erosion easily occurs on the surface of hydraulic structures. When cavitation bubbles grow and collapse near the wall, they generate localized high-pressure shock waves and microjets, initially causing structural loosening, mortar skeleton degradation, and microcrack initiation and propagation on the material surface. This stage is typically characterized by the cavitation erosion incubation period, where microscopic damage has occurred internally, but no obvious erosion pits, mass loss, or significant strength reduction have yet appeared on the surface.
[0003] Existing methods for evaluating cavitation erosion in cement-based materials mainly include mass loss methods, surface morphology methods, macroscopic mechanical property comparison methods, and microscopic observation methods. These methods are relatively easy to identify cavitation damage after visible spalling, volume loss, or obvious cracks appear. However, for early-stage damage during the incubation period, which is dominated by microcracks and microstructural loosening, they suffer from insufficient sensitivity, poor quantification, and delayed early warning, making it difficult to meet the needs of service safety assessment of hydraulic structures and early identification of the cavitation resistance of materials.
[0004] Nanoindentation technology can obtain local mechanical parameters such as modulus and hardness of materials at the micrometer / nanometer scale. Existing research has applied it to characterize the intrinsic properties of hydration products in cement-based materials, interfacial transition zones, and the micromechanical evolution under durability effects such as carbonation, calcium dissolution, and freeze-thaw cycles. Most of these applications target processes accompanied by changes in chemical composition, with relatively clear degradation boundaries, or easily identifiable mechanical gradients. In such cases, the mechanical differences between degraded and undegraded regions are relatively easy to identify through variations in average modulus, average hardness, or depth distribution.
[0005] However, for cavitation erosion, a purely mechanical and physical damage process primarily caused by localized high-frequency impacts, characterized by microcracks and structural loosening, and not necessarily accompanied by significant chemical phase transitions in its early stages, nanoindentation data often exhibits greater dispersion. On one hand, cement-based materials themselves possess significant heterogeneity, with overlapping distributions of mechanical parameters across different microphases. On the other hand, cavitation-induced localized cracks and structural loosening further amplify the dispersion of the indentation response, making traditional methods based on single-point values, mean comparisons, or simple partitioned statistics ineffective in distinguishing between "material background heterogeneity" and "mechanical degradation caused by impact damage." Therefore, current technology lacks a method capable of effectively removing background influences from highly discrete nanoindentation data and quantitatively identifying microphysical damage during the cavitation erosion incubation period.
[0006] Furthermore, at the engineering application level, existing cavitation risk assessments typically focus on empirical evaluations based on flow field parameters such as flow velocity, cavitation number, and duration. The cavitation resistance of materials is often replaced by empirical coefficients, macroscopic test results, or literature recommendations. There is a lack of a method that can establish a critical damage threshold based on the measured results of material micro-damage and further correlate and compare it with the flow field energy input. As a result, a complete chain has not yet been formed between laboratory micro-testing and engineering risk prediction. Summary of the Invention
[0007] The purpose of this invention is to provide a testing method for cavitation damage during the incubation period of cement-based materials. By using specific depth interception, abnormally high modulus screening, and multiphase statistical deconvolution, the indentation response, which is traditionally regarded as "discrete noise," is transformed into a quantifiable microscopic phase volume fraction change or phase deflection index. This enables the quantitative identification of purely mechanical microphysical damage, thereby solving the problems of cavitation evaluation methods being insensitive to damage during the cavitation incubation period, having difficulty identifying damage effects, and insufficient connection between microscopic detection results and engineering cavitation risk assessment.
[0008] The technical solution of this invention to solve the above-mentioned technical problems is as follows: A method for testing damage during the cavitation incubation period of cement-based materials is provided, comprising the following steps: S1. Sample preparation and determination of single-bubble impact region; S2, Mesh-based nanoindentation test; S3, Fixed indentation depth data extraction; S4. High modulus data screening; S5. Statistical deconvolution and quantization of cavitation micro-damage; S6. Critical cumulative cavitation energy threshold calibration; S7. Flow field energy input comparison and risk mapping.
[0009] Furthermore, S1 includes the following sub-steps: S11. The cement-based material to be tested is sequentially cut, terminated hydration, vacuum dried, cold inlaid, ground step by step and fine polished to obtain a flat test surface suitable for nanoindentation testing. S12. Single bubble impacts are generated on the flat test surface of the cement-based material to be tested by laser-induced cavitation or electric spark-induced cavitation. The maximum radius of the cavitation bubble, the collapse dynamic process, and the projection position of the bubble core on the surface of the cement-based material to be tested are obtained by high-speed photography. The single bubble impact area is determined according to the projection position of the bubble core and the impact influence range.
[0010] Furthermore, in S11, the cement-based material to be tested is cut and immersed in a high-concentration alcohol solution to terminate hydration, vacuum dried, then resin cold-mounted, and the test surface bubbles are reduced by vacuum treatment. After the resin is cured, it is sanded and polished step by step with sandpaper and polishing liquid, and then ultrasonically cleaned.
[0011] Furthermore, in S12, a test sample with a side length of 1 mm is cut off with the projection point of the bubble core as the center; for samples that need to be analyzed for the range of damage influence, samples can also be taken simultaneously within the secondary collapse coverage area at a certain distance from the bubble core as a control.
[0012] In S1, the complex random multi-bubble cavitation flow field is replaced by single-bubble impact, making the impact location, impact energy and action area traceable and locatable, providing a basis for establishing a correspondence between the micromechanical test results and specific impact events.
[0013] Furthermore, in S2, a nanoindenter equipped with a Berkovich indenter is used to randomly perform gridded point testing on the slurry region of the cement-based material under test in the single bubble impact zone under continuous stiffness measurement mode, so as to obtain the continuous indentation curve.
[0014] Furthermore, during the gridded test, the load is linearly applied from the initial contact between the indenter and the sample, increasing at a rate of 12 mN / min to 2 mN, and then unloaded after 5 s. At least one test area is selected on each sample surface for gridded testing, and each test area can be arranged as a 10×10 dot matrix with an indentation spacing of 5 μm.
[0015] In S2, the continuous response curves of the same pressure point at different depths are obtained through the continuous stiffness measurement mode, avoiding the randomness of single pressure depth results; and a statistically significant sample set is obtained through gridded point layout, overcoming the interference of the microscopic heterogeneity of cement-based materials on single-point results.
[0016] Furthermore, in S3, the indentation modulus and hardness data at a fixed indentation depth are extracted from the continuous indentation curve as the basis for statistical analysis. The fixed indentation depth is determined by the micro-phase scale of the cement-based material to be tested, the stable range of the indenter response, and the stability analysis of the deconvolution results at different depths.
[0017] In S3, by optimizing the truncation depth rather than simply fixing a single depth, consistent and stable data input can be provided for statistical deconvolution, reducing phase resolution errors caused by material differences and improper depth selection, and improving the comparability and reliability of results under different materials and impact conditions.
[0018] Furthermore, in S4, outlier screening is performed on the basic statistical analysis data based on the abnormal high modulus screening threshold to remove abnormal high modulus points caused by the pressure head touching unhydrated clinker particles, aggregate edges, or other abnormal hard inclusions. The abnormally high modulus screening threshold is determined by the frequency distribution characteristics of the indentation modulus at a fixed depth in unimpacted samples or control samples. Specifically, it is determined based on the constituent materials of the mortar. Generally, the number n of phases in the mortar can be calculated from the constituent materials. The main dataset of nanoindentations before deconvolution is a weighted superposition of n normal distributions, and the mechanical properties of each phase follow a normal distribution. Therefore, when searching for high modulus, it is necessary to repeatedly calculate the screening threshold for abnormal high modulus. First, observe the frequency distribution of the main dataset, perform multi-peak fitting, and observe the standard deviation of the data at the high modulus peak. If the standard deviation is much larger than the other peaks, then use the high modulus peak as threshold 1, and add ±10 MPa to form a new threshold 2 / 3, for a total of 3 thresholds. Use different thresholds to select three sets of data for deconvolution analysis, and compare the impact of the three sets of data on the low modulus peak after deconvolution. Use the maximum threshold that does not change the results of other low modulus peaks as the screening threshold for abnormal high modulus, so that the subsequent deconvolution results more realistically reflect the slurry and its damage evolution characteristics, rather than being masked by unhydrated particles, aggregate edges, or other high modulus interference terms to obscure the changes in the micromechanics of hydration products.
[0019] In S4, by adapting the screening threshold for abnormal high modulus, the contamination of statistical distribution by non-target phases or local abnormal contacts can be effectively eliminated, so that the subsequent deconvolution results can more realistically reflect the slurry and its damage evolution characteristics, rather than being masked by unhydrated particles, aggregate edges or other high modulus interference terms to obscure the micromechanical changes of hydration products.
[0020] Furthermore, in S5, frequency distribution statistics are performed on the screened data, and a Gaussian mixture model is used to perform four-phase deconvolution on the frequency distribution of indentation modulus. Then, the deconvolution results of the impacted area and the unimpacted control area are compared, and the combined damage criterion is determined. The four phases are a porous / loose phase, a low-density CSH phase, a high-density CSH phase, and a high-modulus phase; The combined damage criterion is the increase in the porosity / loose phase ratio and the decrease in the elastic properties of the low-density CSH phase. Both the increase and decrease mentioned above are the differences between two consecutive results.
[0021] Porous / loose phase refers to porous or loose phase.
[0022] In S5, quantifiable and comparable damage indicators are extracted from highly discrete indentation data for the first time, transforming traditionally difficult-to-use dispersion information into damage identification information, thereby improving the detection sensitivity of micro-damage during the cavitation incubation period.
[0023] Furthermore, S6 includes the following sub-steps: S61. Measure the pressure wave generated by the collapse of a single bubble using a pressure sensor, and calculate the characteristic output energy of a single bubble in a single event by combining the bubble radius and the liquid pressure difference. S62. Repeated single-bubble impact tests under fixed conditions are conducted using spark-induced cavitation or laser-induced cavitation. When the impacted area of the cement-based material under test shows an increase in the proportion of pores / loose phases and a decrease in the elastic properties of the low-density CSH phase compared to the unimpacted control area, and the change ratio of the combined damage criterion exceeds a preset threshold, it is determined that the cement-based material under test has undergone identifiable micro-damage. The corresponding number of impacts is multiplied by the single-bubble characteristic output energy or the total action energy calculated by the cumulative formula is used as the critical cumulative cavitation energy threshold of the cement-based material under test.
[0024] Furthermore, in S62, the preset threshold is set based on the results of repeatability tests, the fluctuation range of control samples, and engineering needs. Specifically, when the combination of an increase in the porosity / loose phase ratio and a decrease in the elastic properties of the low-density CSH phase (i.e., the combined damage criterion) changes by more than 20%, the material is considered to have suffered micro-damage.
[0025] In S6, the threshold is not obtained by changing the single bubble energy level, but by establishing the relationship between cumulative action and micro-damage evolution through repeated impacts under fixed single bubble action conditions. This transforms the material cavitation resistance, which could only be qualitatively described, into a critical cumulative energy parameter with physical meaning, providing a unified scale for cross-sectional comparison between different materials and subsequent engineering risk assessment.
[0026] Furthermore, in S7, based on numerical fluid analysis, engineering experience relationships, or existing flow field results, the flow velocity, pressure, cavitation number, and duration data at different locations on the flow surface are obtained, and the distribution of input energy or equivalent impact parameters is constructed. The input energy is compared with the critical cumulative cavitation energy threshold to obtain the relative risk level at different locations on the flow surface, and risk zoning maps, cloud maps, or early warning results are generated.
[0027] S7 enables the connection between identifying microscopic damage in materials and assessing macroscopic risks on structural surfaces, allowing laboratory calibration results to serve engineering applications.
[0028] This invention addresses the following problems: Existing cavitation erosion evaluation methods are not sensitive to damage during the cavitation erosion incubation period, making it difficult to identify early microscopic degradation before significant mass loss and surface erosion occur; nanoindentation data under cavitation erosion are highly discrete due to the superposition of microcracks, porosity, and material heterogeneity, making it difficult to identify damage effects using traditional mean value methods, single-point methods, or simple peak observation methods; and there is insufficient connection between existing laboratory microscopic detection results and engineering cavitation erosion risk assessment, lacking a complete method that can establish the material's critical damage threshold using experimental calibration results and further compare and analyze it with the cavitation energy input of the flow field. This paper presents a testing method for cavitation erosion damage in cement-based materials. By using specific depth interception, abnormally high modulus screening, and multiphase statistical deconvolution, the indentation response, traditionally considered "discrete noise," is transformed into a quantifiable micro-phase volume fraction change or phase deflection index, thereby achieving quantitative identification of purely mechanical microphysical damage. It also provides a calibration approach for the critical cavitation erosion energy threshold of materials. By combining single-bubble impacts at different energy levels with nano-indentation damage criteria, the critical impact energy corresponding to the occurrence of identifiable micro-damage in the material is determined. Furthermore, it provides a method for bridging laboratory material micro-calibration with risk mapping of engineering flow surfaces, comparing the critical cavitation erosion energy threshold with the cavitation erosion energy input of the target structural surface flow field for cavitation risk zoning and early warning.
[0029] The present invention has the following beneficial effects: 1. This invention expands the application boundaries of nanoindentation in the evaluation of cavitation erosion in cement-based materials: The cavitation resistance of cement-based materials depends not only on the material's composition and microstructure but also on the form, location, and fluid load input characteristics of cavitation impact. While existing methods such as ultrasonic vibration, Venturi tube testing, and water tunneling can be used for cavitation research, the localized energy of ultrasonic vibration is difficult to accurately correspond to specific damaged areas. Furthermore, the generation, migration, and collapse locations of cavitation bubbles in Venturi tube or water tunneling methods exhibit strong randomness, hindering accurate sampling and quantitative analysis of damaged areas using subsequent micro-area testing such as nanoindentation. This invention, however, combines repeated single-bubble impact with high-speed photography to enable the tracking and localization of the near-wall impact location and process of cavitation bubbles. Combined with nanoindentation meshing testing and statistical deconvolution analysis of the surface slurry region, a direct correspondence is achieved between fluid impact events, sampling areas, and microscopic damage responses. Since cavitation damage exhibits a significant surface-to-interior development characteristic, nanoindentation is more suitable than traditional bulk mechanical property testing for characterizing the evolution of localized surface micro-damage. Therefore, this invention can more realistically and sensitively reflect the cavitation resistance of cement-based materials, improving the pertinence and quantification of cavitation resistance evaluation. By optimizing the cut-off depth and screening for abnormally high modulus thresholds, the stability, adaptability, and reliability of the test results are improved.
[0030] Furthermore, this invention goes beyond general nanoindentation data acquisition; it establishes a parameter optimization analysis process applicable to multiphase cement-based materials. By comparing the stability of deconvolution results at different cutting depths, the optimal indentation depth for the target material system is determined. Through modulus frequency distribution and threshold sensitivity analysis of unimpacted or control samples, the abnormally high modulus screening threshold for the target material system is determined. This method effectively controls shallow indentation depth errors, cross-phase interference, and contamination of the statistical distribution by local abnormally high values, significantly improving the stability of multiphase deconvolution results and the comparability between different samples and materials.
[0031] 2. This invention can calibrate the critical cumulative cavitation energy threshold of materials, providing a unified index for comparing the cavitation erosion resistance of materials: This invention establishes a correlation between cumulative effect and micro-damage criteria through repeated impact tests under fixed single-bubble impact conditions. When the impacted area shows an increase in the porosity / loose phase ratio and a decrease in the elastic properties of the low-density CSH phase exceeding a preset range compared to the unimpacted control area, identifiable micro-damage is identified in the material. The total cumulative energy corresponding to this point is determined as the material's critical cumulative cavitation erosion energy threshold. This threshold transforms the previously difficult-to-quantify cavitation erosion resistance into a cumulative energy parameter with clear physical meaning, which can be used for a unified comparison of the cavitation erosion resistance performance of materials with different formulations, service ages, or service conditions.
[0032] 3. It has application value that can be extended to engineering risk assessment: The critical threshold established in this invention at the laboratory level can be further compared with the intensity of the flow field on the engineering flow surface, thereby enabling a zonal assessment of structural cavitation risk. This approach is compatible with existing numerical flow field analysis systems and has good engineering applicability and promotional value. Attached Figure Description
[0033] Figure 1 This is a flowchart of a test method for cavitation damage during the incubation period of cement-based materials. Detailed Implementation
[0034] The present invention will be further illustrated below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods, and equipment used in the present invention are conventional reagents, methods, and equipment in this technical field.
[0035] Example 1:
[0036] This invention provides a method for testing cavitation erosion damage during the incubation period of cement-based materials, such as... Figure 1 As shown, it includes the following steps: S1. Sample preparation and determination of single-bubble impact region; The above S1 includes the following sub-steps: S11. The cement-based material to be tested is sequentially cut, terminated hydration, vacuum dried, cold inlaid, ground step by step and fine polished to obtain a flat test surface suitable for nanoindentation testing. Specifically, the cement-based material to be tested is cut and immersed in a high-concentration alcohol solution to stop hydration, vacuum dried, then resin cold-mounted, and vacuum treatment is used to reduce air bubbles on the test surface. After the resin has cured, it is sanded and polished step by step with sandpaper and polishing liquid, and then ultrasonically cleaned. S12. Single bubble impacts are generated on the flat test surface of the cement-based material to be tested by laser-induced cavitation or electric spark-induced cavitation. The maximum radius of the cavitation bubble, the collapse dynamic process, and the projection position of the bubble core on the surface of the cement-based material to be tested are obtained by high-speed photography. The single bubble impact area is determined according to the projection position of the bubble core and the impact influence range.
[0037] Specifically, a test sample with a side length of 1 mm is cut off with the projection point of the bubble core as the center; for samples that need to be analyzed for the extent of damage, samples can also be taken simultaneously as a control within the secondary collapse coverage area at a certain distance from the bubble core.
[0038] S2, Mesh-based nanoindentation test; In S2 above, a nanoindenter equipped with a Berkovich indenter is used to randomly perform gridded point tests on the slurry region of the cementitious material under test in the single-bubble impact zone under continuous stiffness measurement mode, obtaining a continuous indentation curve. During the gridded point test, the load is linearly applied from the initial contact between the indenter and the sample, increasing at a rate of 12 mN / min to 2 mN, and then unloaded after 5 s. At least one test area is selected on each sample surface for gridded point placement, and each test area can be arranged as a 10×10 lattice with an indentation point spacing of 5 μm.
[0039] S3, Fixed indentation depth data extraction; In S3 above, the indentation modulus and hardness data at a fixed indentation depth are extracted from the continuous indentation curve as the basis for statistical analysis; the fixed indentation depth is determined by the micro-phase scale of the cement-based material to be tested, the stable range of the indenter response, and the stability analysis of the deconvolution results at different depths.
[0040] Specifically, multiple candidate indentation depths can be selected for comparative analysis. The changes in the mean modulus, volume fraction, and fitting residuals of each phase obtained by deconvolution at each depth can be compared. The depth that balances shallow indentation depth error control, phase resolution, and fitting stability can be selected as the subsequent unified analysis depth.
[0041] In a specific embodiment of the present invention, the indentation modulus data at an indentation depth of 200 nm ± 10 nm is selected as the input for subsequent analysis of the mortar material.
[0042] The reason for optimizing the indentation depth is that when the indentation depth is too shallow, the passivation effect of the indenter tip and the area function calibration error have a significant impact on the measurement results; when the indentation depth is too large, the stress influence zone below the indenter increases, making it easier to cross phase boundaries and reducing the ability to resolve individual hydrated phases. By comparing and analyzing different indentation depths, data extraction conditions more suitable for the target material can be obtained.
[0043] S4. High modulus data screening; In S4 above, outlier screening is performed on the basic statistical analysis data based on the abnormal high modulus screening threshold to remove abnormal high modulus points caused by the indenter touching unhydrated clinker particles, aggregate edges, or other abnormal hard inclusions; the abnormal high modulus screening threshold is determined by the indentation modulus frequency distribution characteristics of the non-impacted sample or control sample at a fixed depth.
[0044] Specifically, frequency distribution statistics can be performed on the indentation modulus data of unimpacted samples or control samples to identify the main peak distribution range and high value scatter intervals. Then, combined with sensitivity analysis of the mean modulus, volume fraction and fitting stability of each phase under different screening thresholds, the abnormal high modulus screening threshold applicable to the target material system can be determined.
[0045] In a specific embodiment of the present invention, when 50 GPa is used as the screening threshold for the mortar material, the changes in the mean modulus and volume fraction of each phase are small, and the deconvolution results are relatively robust. Therefore, 50 GPa is preferred.
[0046] S5. Statistical deconvolution and quantification of cavitation micro-damage; In S5 above, frequency distribution statistics are performed on the screened data, and a Gaussian mixture model is used to deconvolve the frequency distribution of indentation modulus in four phases. The deconvolution results of the impacted area and the unimpacted control area are compared, and the combined damage criterion is determined. The four phases are porosity / loose phase, low-density CSH phase, high-density CSH phase and high-modulus phase. The combined damage criterion is the increase in the proportion of porosity / loose phase and the decrease in the elastic properties of low-density CSH phase.
[0047] S6. Critical cumulative cavitation energy threshold calibration; The above S6 includes the following sub-steps: S61. Measure the pressure wave generated by the collapse of a single bubble using a pressure sensor, and calculate the characteristic output energy of a single bubble in a single event by combining the bubble radius and the liquid pressure difference. S62. Repeated single-bubble impact tests under fixed conditions are conducted using spark-induced cavitation or laser-induced cavitation. When the impacted area of the cement-based material under test shows an increase in the proportion of pores / loose phases and a decrease in the elastic properties of the low-density CSH phase compared to the unimpacted control area, and the change ratio of the combined damage criterion exceeds a preset threshold, it is determined that the cement-based material under test has undergone identifiable micro-damage. The corresponding number of impacts is multiplied by the single-bubble characteristic output energy or the total action energy calculated by the cumulative formula is used as the critical cumulative cavitation energy threshold of the cement-based material under test.
[0048] Specifically, the preset threshold is set based on the results of repeatability tests, the fluctuation range of control samples, and engineering needs.
[0049] In one specific embodiment of the present invention, when the change in the combination of increased porosity / loose phase ratio and decreased elastic properties of low-density CSH phase (i.e., combined damage criterion) exceeds 20%, the material is considered to have suffered micro-damage.
[0050] S7. Flow field energy input comparison and risk mapping.
[0051] In S7 above, based on numerical fluid analysis, engineering experience relationships, or existing flow field results, the flow velocity, pressure, cavitation number, and duration data at different locations on the flow surface are obtained, and the distribution of input energy or equivalent impact parameters is constructed. The input energy is compared with the critical cumulative cavitation energy threshold to obtain the relative risk level at different locations on the flow surface, and risk zoning maps, cloud maps, or early warning results are generated.
[0052] Example 2:
[0053] The above test method was applied to a specific mortar test, and the details are as follows: 1. Preparation of test materials and specimens This embodiment selects mortar as the research object. Mortar retains the basic characteristics of cementitious phase, pore structure, and fine aggregate skeleton in cement-based materials, while avoiding the significant interference of coarse aggregate scale effect on near-wall cavitation collapse morphology and local damage path. Before coarse aggregate is exposed on the concrete surface, the surface mortar phase and its cementitious matrix are usually the main areas of direct impact from cavitation and early damage accumulation. Therefore, using mortar as the research object for single-bubble cavitation micro-damage can more clearly reveal the early damage evolution law of materials.
[0054] This embodiment designed five groups of mortar specimens to analyze the effects of water-cement ratio, mineral admixtures, and fine aggregate composition on the evolution of single-bubble cavitation damage. The mortar mix proportions for each group are shown in Table 1. The total amount of cementitious materials was set at a mass ratio of 1.0, and PO 42.5 ordinary Portland cement was used. Standard sand was used as the fine aggregate in the STS group, and 70-110 mesh quartz sand was used in the QTZ group. Tap water was used for mixing. The mineral admixtures included silica fume and fly ash.
[0055] Table 1 Mortar Mix Proportion
[0056] The mortar was mixed according to GB / T 17671-2021: first, the cement, fine aggregate, and mineral admixtures were dry-mixed for 30 seconds to ensure uniform dispersion of the powder; then, mixing water was added in batches and mixing continued for a total mixing time of 180 seconds; the freshly mixed mortar was then poured into a 100 mm cube mold and compacted on a vibrating table to remove obvious air bubbles. After molding, the mortar was covered with a thin film, allowed to stand at room temperature for 24 hours, then demolded, and then cured in a standard curing environment of 20±2 ℃ and relative humidity greater than 95% for 28 days.
[0057] To conduct single-bubble impact tests, specimens cured for 28 days were cut into 100 mm × 100 mm × 10 mm sheet samples. After cutting, the sample surface was observed to avoid selecting areas with obvious macroscopic cracks, edge damage, and large pores as the impact loading surface. Two repeated tests were performed for each impact cycle to reduce the influence of random errors.
[0058] In addition, three standard compressive strength specimens were prepared for each mix proportion according to GB / T 17671-2021, and their compressive strength was tested at 28 days. The results are shown in Table 2. These results are used to characterize the macroscopic mechanical properties of different mix proportions and provide a reference for subsequent analysis of the differences in microdamage thresholds of different materials.
[0059] Table 2. Results of compressive strength test at 28 days.
[0060] While maintaining the typical cementitious structure and fine aggregate skeleton of cement-based materials, the interference of coarse aggregate scale effect on the near-wall collapse behavior of single bubbles and local damage paths is reduced, thereby improving the representativeness and comparability of micro-damage identification results.
[0061] 2. Repeated spark-induced single-bubble impact test To capture the cumulative damage process caused by repeated impacts during the cavitation incubation period, this embodiment employs an electrical spark-induced repeated single-bubble impact test. This method can control the relative position of the cavitation bubble to the sample surface and the number of impacts, thereby obtaining resolvable and repeatable local impact loads.
[0062] The apparatus includes a transparent water tank, a high-voltage pulsed power supply, discharge electrodes, a three-dimensional displacement platform, a sample fixing device, and a high-speed imaging system. The specimen is fixed in a fixture within the water tank, ensuring the impact surface remains vertical and is completely submerged in deionized water. The vertical distance between the cavitation bubble center and the specimen surface is defined as L, and the maximum radius of a single bubble is defined as R. max And using the dimensionless parameter γ=L / R max Characterizes the position of the cavitation bubble relative to the wall.
[0063] In this embodiment, by adjusting the electrode position and discharge parameters, γ is controlled at approximately 1.3, R max The cavitation depth was controlled at approximately 20.5 mm, and the measured salinity of the test liquid was approximately 0.65% to ensure comparison of different specimens under similar single-bubble impact conditions. After each discharge, high-speed photography was used to confirm whether the cavitation formation location, maximum radius, and collapse process met the test requirements. If a cavitation significantly deviated from the predetermined position or multiple bubbles interfered, the result of that test was not included in the statistics, and a supplementary test was conducted.
[0064] Each sample was subjected to repeated single-bubble impacts within the same bubble core projection area. The number of impacts N was set to 0, 2, 5, 7, 10, 12, 15, 17, 20, 22, and 25; the maximum number of impacts for the 0.45STS group was 20. By repeatedly loading the same area, the cumulative process of multiple cavitation impacts experienced by a local micro-region during the cavitation incubation period can be simulated.
[0065] 3. Single bubble dynamics and collapse energy quantification To quantitatively characterize the collapse intensity of a single bubble, this embodiment utilizes a custom-designed pressure sensor to measure the pressure wave released during cavitation collapse. The pressure sensor has an overload capacity of 130%, a zero-point output of 0.20 mA, a full-scale net output of 96.80 mV, and a zero-point temperature coefficient of 0.3 × 10⁻⁶. -4 / ℃·FS, sensitivity temperature coefficient is 0.3×10 -4 / ℃·FS. Each condition should be repeated at least 5 times to improve the reliability of the pressure wave measurement results. For each valid cavitation event, the energy released by single-bubble collapse (single-bubble single-cycle characteristic output energy) is calculated as follows: ; Where E is the energy released by the collapse of a single bubble, R is the maximum radius of the expanded bubble, r is the bubble radius, and ΔP is the vapor pressure difference inside the bubble; In this embodiment, the vapor pressure Pv inside the bubble is taken as 0 kPa. In this step, the purpose of pressure wave measurement is not to directly replace the actual local impact pressure on the wall, but to provide a unified and comparable impact intensity or energy index for different single bubble events, thereby providing a quantitative basis for subsequent critical damage threshold calibration.
[0066] 4. Surface damage observation and selection of nano-indentation areas To ensure that the nanoindentation test area represents the actual damage area generated by a single bubble impact, the impact area was marked on the specimen surface before the test, and the surface morphology of the specimen was observed and recorded before and after the test to ensure that the bubble core projection position was within a pre-set circular area with a radius of 1 mm. The projection position of the bubble core on the specimen surface was determined by real-time high-speed photography. Subsequently, a diamond cutter was used to locally sample the area centered on the bubble core projection area to obtain micro-test samples with a side length of approximately 1 mm.
[0067] 5. Nanoindentation Sample Processing and Mesh Testing The cut micro-test samples were immersed in a high-concentration alcohol solution for 24 hours to stop hydration, and then dried in a vacuum environment. The dried samples were cold-mounted and air bubbles near the test surface were removed by vacuum treatment. After the resin was completely cured, the samples were taken out and then polished, ultrasonically cleaned and mirror polished in sequence to obtain a high-quality test surface suitable for nanoindentation testing.
[0068] Nanoindentation testing was performed using the KLA iNano nanoindenter with a Berkovich indenter. The Poisson's ratio was set to 0.2 according to the literature. Continuous Stiffness Measurement (CSM) mode was used during testing. The load was increased linearly from the initial contact between the indenter and the sample, at a rate of 12 mN / min to 2 mN. After reaching the peak value, the load was held for 5 s to eliminate the creep effect before unloading. Three points were selected for each specimen, with a 7×7 lattice at each point, and the spacing between adjacent indentation points was 5 μm. This testing method can simultaneously obtain the curves of continuous variation of indentation modulus and hardness with indentation depth, and the stability of the results is improved through multi-point statistical analysis.
[0069] 6. Optimization of specific indentation depth and unified data extraction Since the indentation results are significantly affected by the indentation depth, this embodiment compares and analyzes the indentation modulus and hardness data at three depths: 150 nm, 200 nm, and 250 nm. Four-phase Gaussian mixture deconvolution was performed on the same group of specimens subjected to the same number of impacts, and the results are shown in Table 3.
[0070] Table 3. Comparison of phase modulus and volume fraction at different cutting depths
[0071] As shown in Table 3, the deconvolution results at 200 nm and 250 nm are quite similar, with the mean modulus difference of the LD CSH phase being only 0.05% and the mean modulus difference of the HD CSH phase being 3.6%. However, the results at 150 nm are significantly different from those at 200 nm, with the mean modulus of the porous phase being lower and the volume fraction of the HD CSH phase being significantly higher, and the fitting residual being larger. This indicates that the results at 150 nm are still significantly affected by the shallow indentation effect, the blunting of the indenter tip, and the area function error.
[0072] Taking all factors into consideration, this embodiment uniformly selects 200 nm ± 10 nm as the data cutoff depth for all subsequent samples. This depth avoids the significant shallow pressure depth effect range while maintaining effective resolution of the various microphases of the cement paste in the stress-affected zone of approximately 600-1000 nm below the indenter.
[0073] 7. Screening of High Modulus Outliers and Robustness Analysis In nanoindentation testing, when the indenter touches unhydrated clinker particles, the edges of fine aggregates, or localized hard inclusions, the obtained modulus values are often significantly higher than the normal range of slurry hydration products. If such abnormally high values are directly included in the statistical deconvolution, it will interfere with the distribution fitting of the porous / loose phase, LD CSH phase, HD CSH phase, and CH phase, leading to deviations in the calculation of phase volume fraction and mean modulus.
[0074] To determine a reasonable high modulus screening threshold, this embodiment statistically analyzed the indentation modulus frequency distribution at 200 nm for all non-impact samples. The results showed that the main distribution peaks were in the 0-30 GPa range, corresponding to the porous / loose phase, LD CSH phase, and HD CSH phase; a small distribution was present in the 35-50 GPa range, which could correspond to the CH phase and some unhydrated particles; only a very few discrete points appeared above 50 GPa, with obvious frequency intervals between them and the main distribution, presumably due to the indenter touching the aggregate edge or abnormal contact.
[0075] Accordingly, this embodiment sets the abnormally high modulus screening threshold M to 50 GPa, retaining only data with a modulus no greater than 50 GPa for subsequent deconvolution. Sensitivity analysis was further performed on three thresholds: 40 GPa, 50 GPa, and 60 GPa, and the results are shown in Table 4.
[0076] Table 4. Results of Sensitivity Analysis of High Modulus Screening Threshold
[0077] As shown in Table 4, when screening using 40 GPa, 50 GPa and 60 GPa, the maximum relative difference in the mean modulus and volume fraction of each phase is less than 10%, indicating that the deconvolution result is not overly sensitive to the screening threshold. 50 GPa can effectively eliminate abnormally high value interference without mistakenly deleting normal slurry phase data, so it is the better choice.
[0078] 8. Statistical deconvolution and micro-damage recognition Statistical analysis was performed on indentation data uniformly cut to a depth of 200 nm and filtered using a 50 GPa threshold. A Gaussian mixture model (GMM) was used for four-phase deconvolution. The four phases were defined as: porous / loose phase, low-density CSH phase, high-density CSH phase, and high-modulus phase (CH or unhydrated particles). The corresponding hardness (H), modulus (E), standard deviation (SD), and relative content were obtained through fitting.
[0079] Taking some representative results as an example, in a group of unimpacted samples, the volume fractions of porous / defective phase, LD CSH phase, HD CSH phase, and CH / unhydrated particulate phase were approximately 13.93%, 63.38%, 18.04%, and 4.65%, respectively. However, after repeated single-bubble impacts, with the increase of the number of impacts, the proportions of porous / defective phase and low-density phase increased to varying degrees, while the proportion of high-resolution load-bearing phase decreased or redistributed. This change indicates that the microcrack initiation, structural loosening, and load-bearing skeleton degradation caused by single-bubble impacts can be statistically represented as the transformation of high-density load-bearing phase to low-density phase and porous / defective phase.
[0080] This embodiment does not simply regard the discrete indentation data generated by cavitation as invalid noise, but regards the discretization itself as one of the manifestations of damage evolution, and transforms it into the offset of each micro-phase ratio and mechanical parameter through multi-peak distribution fitting, thereby realizing the quantitative identification of micro-damage during the cavitation incubation period.
[0081] 9. Critical damage evolution and engineering application ideas Based on the above-described statistical deconvolution process of repeated single-bubble impact-nanoplasty, a correlation can be established between the number of impacts / impact intensity, microphase volume fraction deflection, and damage degree. For specimens with different mix proportions, the variation ranges of porous / defective phases, LD CSH phases, and HD CSH phases under the same single-bubble impact conditions can be compared, thereby distinguishing their resistance to cavitation micro-damage.
[0082] For example, in this embodiment, the 0.40QTZ+SF group exhibits a high 28-day compressive strength (62.30 MPa) and demonstrates a relatively stable load-bearing phase ratio under certain impact conditions. However, different water-cement ratios, different fine aggregate systems, and different mineral admixture incorporation methods lead to variations in the evolution path of cavitation erosion micro-damage. Therefore, the condition under which a certain mix proportion begins to show significant phase shift at a given single-bubble impact energy level can be used as the experimental calibration basis for its critical cavitation erosion damage threshold.
[0083] In engineering applications, this critical damage threshold can be further compared with the flow field intensity, cavitation conditions, or equivalent input energy on the surface of the flowing structure to achieve a zonal evaluation of cavitation erosion risk in different regions. While the input parameters for this part can be obtained through numerical fluid analysis or empirical models, this does not affect the validity of the core method for identifying material micro-damage based on statistical deconvolution of nanoindentation in this embodiment.
[0084] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for testing cavitation erosion damage during the incubation period of cement-based materials, characterized in that, Includes the following steps: S1. Sample preparation and determination of single-bubble impact region; S2, Mesh-based nanoindentation test; S3, Fixed indentation depth data extraction; S4. High modulus data screening; S5. Statistical deconvolution and quantification of cavitation micro-damage; S6. Critical cumulative cavitation energy threshold calibration; S7. Flow field energy input comparison and risk mapping.
2. The method for testing cavitation erosion damage during the incubation period of cement-based materials according to claim 1, characterized in that, S1 includes the following steps: S11. The cement-based material to be tested is sequentially cut, terminated hydration, vacuum dried, cold inlaid, ground step by step and fine polished to obtain a flat test surface suitable for nanoindentation testing. S12. A single bubble impact is generated on the flat test surface of the cement-based material to be tested. The maximum radius of the cavitation bubble, the collapse dynamic process, and the projection position of the bubble core on the surface of the cement-based material to be tested are obtained. The single bubble impact area is determined based on the projection position of the bubble core and the impact influence range.
3. The method for testing cavitation erosion incubation damage of cement-based materials according to claim 1, characterized in that, In step S2, the cement-based material to be tested is randomly subjected to gridded point testing in the slurry region of the single-bubble impact zone to obtain a continuous indentation curve.
4. The method for testing cavitation erosion damage during the incubation period of cement-based materials according to claim 1, characterized in that, In step S3, the indentation modulus and hardness data at a fixed indentation depth are extracted from the continuous indentation curve as the basis for statistical analysis.
5. The method for testing cavitation erosion incubation damage of cement-based materials according to claim 4, characterized in that, The fixed indentation depth is determined by the micro-phase scale of the cement-based material to be tested, the stable range of the indenter response, and the stability analysis of the deconvolution results at different depths.
6. The method for testing cavitation erosion incubation damage of cement-based materials according to claim 1, characterized in that, In step S4, outlier points are filtered out from the basic statistical analysis data based on the outlier high modulus screening threshold. The abnormally high modulus screening threshold is determined by the frequency distribution characteristics of the indentation modulus at a fixed depth of the unimpacted sample or control sample.
7. The method for testing cavitation erosion incubation damage of cement-based materials according to claim 1, characterized in that, In step S5, frequency distribution statistics are performed on the screened data, and a Gaussian mixture model is used to perform four-phase deconvolution on the frequency distribution of indentation modulus. The deconvolution results of the impacted area and the unimpacted control area are compared, and the combined damage criterion is determined. The four phases are a porous / loose phase, a low-density CSH phase, a high-density CSH phase, and a high-modulus phase. The combined damage criterion is the increase in the porosity / loose phase ratio and the decrease in the elastic properties of the low-density CSH phase.
8. The method for testing cavitation erosion incubation damage of cement-based materials according to claim 1, characterized in that, S6 includes the following sub-steps: S61. Measure the pressure wave generated by the collapse of a single bubble, and calculate the characteristic output energy of a single bubble in a single event by combining the bubble radius and the liquid pressure difference. S62. Under fixed conditions, repeated single-bubble impact tests are conducted. When the impacted area of the cement-based material under test shows an increase in the proportion of pores / loose phases and a decrease in the elastic properties of the low-density CSH phase compared to the unimpacted control area, and the change ratio of the combined damage criterion exceeds the preset threshold, it is determined that the cement-based material under test has undergone identifiable micro-damage. The corresponding number of impacts is multiplied by the single-bubble characteristic output energy or the total action energy calculated by the cumulative formula is used as the critical cumulative cavitation energy threshold of the cement-based material under test.
9. The method for testing cavitation erosion incubation damage of cement-based materials according to claim 8, characterized in that, In step S62, the preset threshold is set based on the results of repeatability tests, the fluctuation range of control samples, and engineering requirements.
10. The method for testing cavitation erosion incubation damage of cement-based materials according to claim 1, characterized in that, In S7, based on numerical fluid analysis, engineering experience relationships, or existing flow field results, the flow velocity, pressure, cavitation number, and duration data at different locations on the flow surface are obtained, and the distribution of input energy or equivalent impact parameters is constructed. The input energy is compared with the critical cumulative cavitation energy threshold to obtain the relative risk level at different locations on the flow surface, and a risk zoning map, cloud map, or early warning result is generated.