Method for determining the oxidation rate of molybdenum ores

By performing single-particle mineralogical analysis and liberation correction on molybdenum ore, the problem of deviation in oxidation rate measurement results in existing technologies has been solved, and the accurate measurement of oxidation rate of molybdenum ore has been achieved, providing a scientific basis for mineral processing.

CN123155407APending Publication Date: 2026-11-24CHANGCHUN GOLD RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611680345.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies struggle to accurately distinguish the amount of molybdenum that appears as molybdenum sulfide in automated mineralogical analysis due to gangue encapsulation but is actually difficult to recover by flotation. The lack of discrimination against molybdenum sulfide-molybdenum oxide composite particles leads to discrepancies between oxidation rate measurement results and actual flotation performance.

Method used

By grinding and screening molybdenum ore and performing single-particle mineralogical analysis, combining morphology and elemental distribution, molybdenum sulfide and molybdenum oxide particles were distinguished, and the degree of liberation correction coefficient was calculated to establish an oxidation rate correction model based on particle degree of liberation.

Benefits of technology

It significantly improves the accuracy of oxidation rate determination results, enhances the guidance value for flotation processes, reduces misjudgment of phases caused by impurities in the internal structure of particles, and ensures accurate determination of oxidation rate parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123155407A_ABST
    Figure CN123155407A_ABST
Patent Text Reader

Abstract

This application provides a method for determining the oxidation rate of molybdenum ore, belonging to the field of mineral processing and process mineralogy. The method includes grinding and sieving the sample to be tested to prepare automated mineralogical analysis samples of different particle sizes; determining and obtaining mineral composition data of various molybdenum mineral particles; initially classifying the analysis samples and determining the mass fraction of each type of particle; then performing morphological and elemental distribution analysis on aggregate particles containing molybdenum oxide and molybdenum sulfide, performing secondary classification, calculating the molybdenum content and total molybdenum in the actual molybdenum oxide, and obtaining the oxidation rate of the whole molybdenum ore sample; calculating a correction coefficient based on the ore liberation degree deviation, and obtaining the actual molybdenum ore oxidation rate after correction. This application achieves accurate quantification of the oxidation rate of molybdenum ore by determining the liberation degree parameters and various molybdenum contents of samples of different particle sizes, combined with structural discrimination of mixed particles and coarse-grained liberation correction, providing support for the efficient development and utilization of molybdenum resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of mineral processing and process mineralogy, specifically to a method for determining the oxidation rate of molybdenum ore. Background Technology

[0002] Molybdenum, as an important strategic resource, is widely used in steel metallurgy, aerospace, defense, and chemical catalysis. Molybdenite (MoS2) is the primary carrier of molybdenum, and among the various molybdenum-bearing minerals discovered, it is the preferred target for beneficiation and recovery due to its excellent floatability. However, molybdenum ores in nature often contain associated molybdenum oxide minerals such as molybdenite oxide (MoO3), iron-molybdenite oxide [Fe2(MoO4)3·8H2O], molybdenite (CaMoO4), and pyrite (PbMoO4). These latter minerals are naturally hydrophilic, have very low hydrophobicity, poorly crystallized, and are often fine-grained disseminated, making direct flotation recovery difficult. For flotation processes, the degree of oxidation of molybdenum ore is a key indicator determining the beneficiation process route and recovery rate. The industry typically classifies ores into sulfide ores, mixed ores, and oxide ores based on their oxidation rate (the ratio of molybdenum content in oxide to total molybdenum content). The higher the oxidation rate, the greater the difficulty of flotation recovery and the higher the recovery cost. Current methods for determining oxidation rate mainly rely on chemical phase analysis, which involves selectively leaching molybdenum oxide with a specific solvent and then determining the molybdenum content in the oxidized and sulfide phases using ICP-AES or thiocyanate spectrophotometry to calculate the oxidation rate. However, this method relies on the chemical difference that molybdenum oxide is soluble in acid while molybdenum sulfide is insoluble, and cross-contamination can lead to uncontrollable errors.

[0003] Existing research indicates that during the oxidation process, the polar and non-polar faces of molybdenite exhibit different oxidation-dissolution characteristics. Sulfur is more easily oxidized than molybdenum, and the dissolution behavior of the oxidation products varies depending on the crystal face. Some particles exhibit a core-shell structure of "outer layer molybdenum sulfide, inner layer molybdenum oxide or gangue," while others show the opposite, exhibiting a reverse distribution of "outer layer oxidation, inner core sulfide." Simultaneously, molybdenite is often encased in fine-grained disseminated form within gangue minerals (such as garnet, diopside, quartz, etc.), or forms intergrowths with molybdenum-free minerals. This physical occurrence is typically counted as molybdenum sulfide in traditional chemical analysis, but it cannot actually come into contact with flotation reagents and should be defined as molybdenum oxide. With the mature application of automated quantitative mineral analysis systems (such as MLA and QEMSCAN), process mineralogy research has evolved from traditional qualitative observation using polarized light microscopy to particle-by-particle quantitative characterization, aiming to effectively address the aforementioned issues based on image recognition technology. However, existing technologies struggle to distinguish molybdenum that appears as molybdenum sulfide in automated mineralogical analysis due to gangue encapsulation but is actually difficult to recover by flotation; they lack the ability to distinguish molybdenum sulfide-molybdenum oxide composite particles; and they have not established an oxidation rate correction model based on particle dissociation, resulting in discrepancies between oxidation rate measurement results and actual flotation performance.

[0004] Therefore, this invention establishes a precise method for determining the oxidation rate of molybdenum ore based on single-particle mineralogical analysis, which can simultaneously identify the occurrence state and internal structural characteristics of particles and obtain the degree of liberation correction coefficient. This method fills the gap in existing technology, ensures the accurate determination of oxidation rate parameters, and provides a scientific basis for the selection and optimization of mineral processing technology. Summary of the Invention

[0005] In view of the technical problems existing in the background art, this application provides a method for determining the oxidation rate of molybdenum ore. By classifying and determining the dissociation characteristics of samples of different particle sizes, and combining the structural discrimination of mixed particles and coarse particle dissociation correction, the oxidation rate of molybdenum ore can be accurately quantified, providing support for the efficient development and utilization of molybdenum resources.

[0006] To achieve the above objectives, in a first aspect, embodiments of this application provide a method for determining the oxidation rate of molybdenum ore, comprising: S1, the sample to be tested is ground and sieved to obtain samples A of various particle sizes. i The yield is a i ; S2, sample A of each particle size i Analytical sample B for automated mineralogical analysis was prepared by drying, mixing, and reducing the sample size. i ; S3, for analyzing sample B i Automated mineralogical analysis was performed on a particle-by-particle basis to obtain analytical sample B. i Mineral composition data of molybdenum mineral grains; Based on mineral composition data, sample B was analyzed. i The molybdenum content in molybdenum minerals was determined, and the molybdenum content of molybdenum sulfide minerals in the molybdenum mineral particles was y. h.e The molybdenum content of molybdenum oxide minerals in molybdenum mineral particles is y. n.f ; Based on mineral composition data, sample B was analyzed. i The molybdenum mineral particles were initially classified, including molybdenum sulfide particles B. i.h.e and molybdenum oxide particles B i.n.f ;in, Molybdenum sulfide particles B i.h.e Including Liansheng Granules B i 1 .h.e Encapsulated particle B i 2 .h.e and monomer particles B i 3 .h.e ; Determination of molybdenum sulfide particles B i.h.eand molybdenum oxide particles B i.n.f The mass fractions of molybdenum mineral particles are b i.h.e and b i.n.f Continuous growth particles B i 1 .h.e and encapsulated particles B i 2 .h.e In sample B i The mass fractions in are b i 1 .h.e b i 2 .h.e Monomer particles B i 3 .h.e In molybdenum sulfide particles B i.h.e The mass fraction in is b i 3 .h.e ; S4, initially classified as B i 1 .h.e Or B i 2 .h.e The molybdenum mineral grains in the analyzed samples underwent morphological and elemental distribution analysis and secondary classification, including sulfide-type grains and oxide-type grains; among them, The mass fraction of molybdenum contained in the molybdenum oxide minerals in the sulfide-type particles is c, which is the proportion of molybdenum in all molybdenum oxide minerals. n.f ; The mass fraction of molybdenum in the oxidized molybdenum sulfide minerals relative to the total molybdenum sulfide minerals is d. h.e ; S5, calculate the total oxidation rate α = Σ(Mcontinuous + Mencapsulation + Moxidation) / Mtotal × 100%; where... M continuum = Σa i ×b i 1 .h.e ×y h.e ×(1+d h.e ); M package = Σa i ×b i 2 .h.e ×y h.e ; M oxidation = Σa i ×b i.n.f ×y n.f ×(1-c n.f ); M_total = Σa i×b i.n.f ×y n.f +Σa i ×b i.h.e ×y h.e ; Where i represents the sample type to be screened, i=1 or 2, where i=1 represents the sample that passes through the sieve, and i=2 represents the sample that passes through the sieve; h represents the molybdenum sulfide mineral, e is the mineral category number among the molybdenum sulfide minerals, e can take values ​​from 1 to m, where m is a positive integer greater than 1; n represents the molybdenum oxide mineral, f is the mineral category number among the molybdenum oxide minerals, f can take values ​​from 1 to p, where p is a positive integer greater than 1; S6, based on sample A of each particle size i The dissociation degree difference is used to obtain the dissociation degree correction coefficient λ, and the corrected oxidation rate α' = α × λ is calculated.

[0007] Furthermore, based on sample A of each particle size... i The dissociation degree difference is used to obtain the dissociation degree correction coefficient λ. The steps for calculating the corrected oxidation rate include: According to b i 3 .h.e Calculate the degree of dissociation deviation coefficient DI=Σ(a1×b1) 3 .h.e ×y h.e ) / Σ(a2×b2 3 .h.e ×y h.e ); Based on the dissociation degree deviation coefficient DI, the dissociation degree correction coefficient λ is obtained, and the corrected oxidation rate α' = α × λ is calculated; where... When DI<85%, λ=1+(85%-DI); When DI≥85%, λ=1.

[0008] Further grinding processes include: The sample to be tested was ground until it all passed through a 1.0 mm sieve to obtain a coarse sample; The coarse sample was sieved using a sieve with a mesh size of 0.074 mm to obtain coarse particles A1 on the sieve and fine particles A2 on the sieve.

[0009] Furthermore, samples A of each particle size were... i Analytical sample B for automated mineralogical analysis was prepared by drying, mixing, and reducing the sample size. i The steps include: For each particle size sample A i The samples were dried, mixed, and reduced in size to obtain the reduced sample. The reduced sample was subjected to resin injection curing, demolding, polishing, and carbon spraying to obtain analytical sample B for automated mineralogical analysis. i.

[0010] Furthermore, B i 1 .h.e Including B1 1 .h.e and B2 1 .h.e At least one of them; B1 1 .h.e The area of ​​molybdenum sulfide minerals is ≤75%, and they are associated with other molybdenum-free gangue minerals; B2 1 .h.e The area of ​​molybdenum sulfide minerals is ≤85%, and they are associated with other molybdenum-free gangue minerals.

[0011] Furthermore, B i 2 .h.e Including B1 2 .h.e and B2 2 .h.e At least one of them; B1 2 .h.e The molybdenum sulfide minerals are completely enclosed by gangue minerals or molybdenum oxide minerals, with no exposed boundaries; B2 2 .h.e The molybdenum sulfide mineral is partially enclosed by gangue minerals or molybdenum oxide minerals, and the enclosed side length accounts for ≥65% of the perimeter of the molybdenum sulfide mineral.

[0012] Furthermore, B i.n.f Including B 1.n.f and B 2.n.f At least one of them; B 1.n.f The area of ​​medium-oxidized molybdenum minerals accounts for ≥70%; B 2.n.f The area ratio of medium-oxidized molybdenum minerals is ≥80%.

[0013] Furthermore, the outer layer of the sulfide particles is molybdenum sulfide mineral, and the inner layer is metal oxide or gangue. On the outer contour of the sulfide particles, the perimeter of molybdenum sulfide mineral accounts for ≥50%. The outer layer of the oxidized particles is molybdenum oxide mineral, and the inner layer is molybdenum sulfide mineral. On the outer contour of the oxidized particles, the perimeter of molybdenum oxide mineral accounts for ≥50%.

[0014] Further steps in automated mineralogical analysis include: Set the instrument parameters and select the particle measurement mode to measure the gold standard sample; Adjust the instrument's working distance to 10mm-14mm and the accelerating voltage to 20kV-25kV so that the full-view energy spectrum count rate of the gold sample reaches 60kcps-100kcps, the gray value of the gold sample is 230-250, and the gray value of the epoxy resin is 8-12. Under the same parameter conditions, the analysis sample B was subjected to... i Particle-by-particle measurements are performed, and the measured mineral energy spectrum lines are matched with theoretical mineral energy spectrum databases or user-defined mineral spectral line libraries to identify and analyze sample B. i The types of minerals.

[0015] Furthermore, setting the instrument parameters includes: Adjust the magnification factor to make the actual pixel size of the image 0.3μm-0.5μm; Set the background subtraction grayscale threshold to 120-160; The number of image frames was used as the measurement termination condition.

[0016] The beneficial technical effects of this application are as follows: In the technical solution of this application, molybdenum ore is divided into two independent classification systems based on particle size: coarse and fine. Furthermore, based on the statistical classification of molybdenum oxide and molybdenum sulfide particles, molybdenum sulfide particles are further subdivided into intergrowth molybdenum sulfide particles, encapsulated molybdenum sulfide particles, and single molybdenum sulfide particles. This overcomes the problem of oxidation rate deviation caused by differences in the dissociation behavior of coarse and fine particles in traditional mixed analysis. For the structural discrimination of molybdenum sulfide-molybdenum oxide composite particles, secondary classification is performed based on the spatial distribution of molybdenum sulfide and molybdenum oxide minerals in morphology and elemental distribution analysis. This effectively distinguishes between primary and oxidized superposition phenomena, reducing misclassification of phases caused by the mixing of internal particle structures. The phase calculation results are coupled with the molybdenum sulfide dissociation degree parameter to obtain a correction coefficient λ, which corrects the final oxidation rate. This allows the measurement results to simultaneously reflect the influence of the mineral dissociation degree on the apparent value of the oxidation rate, significantly improving the guiding value of the oxidation rate measurement results for the flotation process.

[0017] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0018] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.

[0019] Figure 1 This is a measurement chart of the sulfurized particles in Example 1 of this application; Figure 2 for Figure 1 Energy dispersive spectral analysis diagrams at various measurement points in the particle; Figure 3 This is a measurement diagram of oxidized particles in Example 1 of this application. Detailed Implementation

[0020] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.

[0022] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0023] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0024] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0025] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0026] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0027] Unless otherwise specified, the terms "comprising" and "including" as used in this application are open-ended. For example, "comprising" and "including" may mean that other components not listed may also be included or contained.

[0028] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.

[0029] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.

[0030] Molybdenum, as an important strategic resource, is widely used in steel metallurgy, aerospace, defense, and chemical catalysis. Molybdenite (MoS2) is the primary carrier of molybdenum, and among the various molybdenum-bearing minerals discovered, it is the preferred target for beneficiation and recovery due to its excellent floatability. However, molybdenum ores in nature often contain associated molybdenum oxide minerals such as molybdenite oxide (MoO3), iron-molybdenite oxide [Fe2(MoO4)3·8H2O], molybdenite (CaMoO4), and pyrite (PbMoO4). These latter minerals are naturally hydrophilic, have very low hydrophobicity, poorly crystallized, and are often fine-grained disseminated, making direct flotation recovery difficult. For flotation processes, the degree of oxidation of molybdenum ore is a key indicator determining the beneficiation process route and recovery rate. The industry typically classifies ores into sulfide ores, mixed ores, and oxide ores based on their oxidation rate (the ratio of molybdenum content in oxide to total molybdenum content). The higher the oxidation rate, the greater the difficulty of flotation recovery and the higher the recovery cost. Current methods for determining oxidation rate mainly rely on chemical phase analysis, which involves selectively leaching molybdenum oxide with a specific solvent and then determining the molybdenum content in the oxidized and sulfide phases using ICP-AES or thiocyanate spectrophotometry to calculate the oxidation rate. However, this method relies on the chemical difference that molybdenum oxide is soluble in acid while molybdenum sulfide is insoluble, and cross-contamination can lead to uncontrollable errors.

[0031] Existing research indicates that during the oxidation process, the polar and non-polar faces of molybdenite exhibit different oxidation-dissolution characteristics. Sulfur is more easily oxidized than molybdenum, and the dissolution behavior of the oxidation products varies depending on the crystal face. Some particles exhibit a core-shell structure of "outer layer molybdenum sulfide, inner layer molybdenum oxide or gangue," while others show the opposite, exhibiting a reverse distribution of "outer layer oxidation, inner core sulfide." Simultaneously, molybdenite is often encased in fine-grained disseminated form within gangue minerals (such as garnet, diopside, quartz, etc.), or forms intergrowths with molybdenum-free minerals. This physical occurrence is typically counted as molybdenum sulfide in traditional chemical analysis, but it cannot actually come into contact with flotation reagents and should be defined as molybdenum oxide. With the mature application of automated quantitative mineral analysis systems (such as MLA and QEMSCAN), process mineralogy research has evolved from traditional qualitative observation using polarized light microscopy to particle-by-particle quantitative characterization, aiming to effectively address the aforementioned issues based on image recognition technology. However, existing technologies struggle to distinguish molybdenum that appears as molybdenum sulfide in automated mineralogical analysis due to gangue encapsulation but is actually difficult to recover by flotation; they lack the ability to distinguish molybdenum sulfide-molybdenum oxide composite particles; and they have not established an oxidation rate correction model based on particle dissociation, resulting in discrepancies between oxidation rate measurement results and actual flotation performance.

[0032] Therefore, this invention establishes a precise method for determining the oxidation rate of molybdenum ore based on single-particle mineralogical analysis, which can simultaneously identify the occurrence state and internal structural characteristics of particles and obtain the degree of liberation correction factor, in order to fill the gap in the existing technology, ensure the accurate determination of oxidation rate parameters, and provide a scientific basis for the selection and optimization of mineral processing technology.

[0033] To address the aforementioned technical problems, this application provides a method for determining the oxidation rate of molybdenum ore, comprising: S1, the sample to be tested is ground and sieved to obtain samples A of various particle sizes. i The yield is a i ; S2, sample A of each particle size i Analytical sample B for automated mineralogical analysis was prepared by drying, mixing, and reducing the sample size. i ; S3, for analyzing sample B i Automated mineralogical analysis was performed on a particle-by-particle basis to obtain analytical sample B. i Mineral composition data of molybdenum mineral grains; Based on mineral composition data, sample B was analyzed. i The molybdenum content in molybdenum minerals was determined, and the molybdenum content of molybdenum sulfide minerals in the molybdenum mineral particles was y. h.e The molybdenum content of molybdenum oxide minerals in molybdenum mineral particles is y. n.f ; Based on mineral composition data, sample B was analyzed. iThe molybdenum mineral particles were initially classified, including molybdenum sulfide particles B. i.h.e and molybdenum oxide particles B i.n.f ;in, Molybdenum sulfide particles B i.h.e Including Liansheng Granules B i 1 .h.e Encapsulated particle B i 2 .h.e and monomer particles B i 3 .h.e ; Determination of molybdenum sulfide particles B i.h.e and molybdenum oxide particles B i.n.f The mass fractions of molybdenum mineral particles are b i.h.e and b i.n.f Continuous growth particles B i 1 .h.e and encapsulated particles B i 2 .h.e In sample B i The mass fractions in are b i 1 .h.e b i 2 .h.e Monomer particles B i 3 .h.e In molybdenum sulfide particles B i.h.e The mass fraction in is b i 3 .h.e ; S4, initially classified as B i 1 .h.e Or B i 2 .h.e The molybdenum mineral grains in the analyzed samples underwent morphological and elemental distribution analysis and secondary classification, including sulfide-type grains and oxide-type grains; among them, The mass fraction of molybdenum contained in the molybdenum oxide minerals in the sulfide-type particles is c, which is the proportion of molybdenum in all molybdenum oxide minerals. n.f ; The mass fraction of molybdenum in the oxidized molybdenum sulfide minerals relative to the total molybdenum sulfide minerals is d. h.e ; S5, calculate the total oxidation rate α = Σ(Mcontinuous + Mencapsulation + Moxidation) / Mtotal × 100%; where... M continuum = Σa i ×bi 1 .h.e ×y h.e ×(1+d h.e ) M package = Σa i ×b i 2 .h.e ×y h.e M oxidation = Σa i ×b i.n.f ×y n.f ×(1-c n.f ); M_total = Σa i ×b i.n.f ×y n.f +Σa i ×b i.h.e ×y h.e ; Where i represents the sample type to be screened, i=1 or 2, where i=1 represents the sample that passes through the sieve, and i=2 represents the sample that passes through the sieve; h represents the molybdenum sulfide mineral, e is the mineral category number among the molybdenum sulfide minerals, e can take values ​​from 1 to m, where m is a positive integer greater than 1; n represents the molybdenum oxide mineral, f is the mineral category number among the molybdenum oxide minerals, f can take values ​​from 1 to p, where p is a positive integer greater than 1; S6, based on sample A of each particle size i The dissociation degree difference is used to obtain the dissociation degree correction coefficient λ, and the corrected oxidation rate α' = α × λ is calculated.

[0034] In the technical solution of this application, the particle size difference resulting from the grinding process of molybdenum ore leads to different degrees of liberation of the ore. Coarse-grained mineral particles A1, with a yield of a1, typically contain more intergrowths; molybdenite, molybdenum oxide minerals are intergrowthed with gangue or other minerals and are encapsulated, resulting in insufficient liberation. Fine-grained mineral particles A2, with a yield of a2, have a higher degree of individual liberation and more fully exposed mineral surfaces. Two independent classification systems are established for coarse and fine grains, respectively. Modeling and correction are performed based on the liberation behavior and oxidation rate response of each particle size, making the classification boundaries more closely match the true oxidation degree and selectivity of that particle size, which is beneficial for more accurate characterization of the true oxidation rate of each particle size. Using anionic groups and molybdenum valence state as the core, and combined with a scanning electron microscope equipped with an automated mineralogical analysis system, molybdenum minerals are divided into molybdenum sulfide minerals and molybdenum oxide minerals, denoted as h and n, respectively. Among them, molybdenum sulfide minerals h include molybdenite and / or molybdenite sulfide, and their types are represented by e; molybdenum oxide minerals n include molybdenite ore, molybdenite-calcium molybdenite, ferromolybdenite ore, lead molybdenite, and / or copper molybdenite, and their types are represented by f. Particle-by-particle analysis is performed on the analytical samples to obtain the mineral composition data of molybdenum mineral particles in each sample, so as to establish respective molybdenum mineral phase classification and molybdenum content calculation models, and obtain the molybdenum content y of molybdenum sulfide minerals in the molybdenum minerals. h.e The molybdenum content y of molybdenum oxide minerals in molybdenum minerals n.f Based on data obtained from automated particle-by-particle mineralogical analysis, the analyzed sample was divided into molybdenum sulfide particles, B. i.h.e and molybdenum oxide particles B i.n.f Among them, molybdenum sulfide particles B i.h.e Including Liansheng Granules B i 1 .h.e Encapsulated particle B i 2 .h.e and monomer particles B i 3 .h.e Molybdenum oxide particles B i.n.f This indicates that all the molybdenum minerals in the particles are molybdenum oxide minerals; molybdenum sulfide particles B i.h.e This means removing B. i.n.f All molybdenum sulfide particles other than granules. Continuous particle B i 1 .h.e This indicates that the molybdenum-containing metal sulfides are intergrowths with gangue and metal oxides; encapsulated particles B i 2 .h.e This indicates that the molybdenum-containing metal sulfides are encapsulated by gangue or metal oxides, and the surface of the molybdenum-containing minerals is not sufficiently exposed; monomeric particle B i 3 .h.eThis indicates that the molybdenum minerals in the particles exist as molybdenum sulfide monomeric particles, and the molybdenum minerals are largely liberated from the gangue and other minerals. The molybdenum sulfide particles are initially classified as B. i 1 .h.e and B i 2 .h.e The molybdenum-containing particles exhibit a complex mixture with other gangue or metal oxides. Morphological and elemental distribution analyses were performed, and based on the results, they were reclassified into sulfide-type and oxide-type particles. The proportion of molybdenum contained in the sulfide-type particles (B0) of molybdenum oxide minerals was determined to be that of all the molybdenum oxide particles. i.n.f mass fraction c n.f And the proportion of molybdenum contained in molybdenum sulfide minerals in oxidized particles to the total molybdenum sulfide particles B i.h.e mass fraction d h.e In this context, sulfide particles represent ore particles dominated by sulfide states, while oxide particles represent ore particles dominated by oxide states. Sulfide particles, due to their dominant molybdenum sulfide minerals, can directly interact with flotation reagents and dominate particle surface wettability and floatability; therefore, the total molybdenum mass of these particles is entirely included in the molybdenum sulfide portion, while the mass of inner metal oxides or gangue is excluded from the molybdenum oxide portion. Oxidation particles, due to the dominant molybdenum oxide minerals' hydrophilic surface and poor floatability, are difficult to effectively interact with conventional sulfide ore flotation reagents and inhibit the floatability of molybdenum sulfide minerals; therefore, the total molybdenum mass of these particles is entirely included in the molybdenum oxide portion, while the mass of their molybdenum sulfide is also included in the molybdenum oxide portion. The total oxidation rate α is calculated as α = Σ(Mintercalation + Mencapsulation + Moxidation) / Mtotal × 100%; where, M continuum = Σa i ×b i 1 .h.e ×y h.e ×(1+d h.e ) M package = Σa i ×b i 2 .h.e ×y h.e M oxidation = Σa i ×b i.n.f ×y n.f ×(1-c n.f ); M_total = Σa i ×b i.n.f ×y n.f +Σa i ×b i.h.e ×y h.e ; Where i represents the sample type being sieved, i=1 or 2, where i=1 represents the oversize sample and i=2 represents the undersize sample. During calculation, the analytical sample data for both the oversize and undersize particle sizes are substituted into the corresponding formulas. Finally, based on sample A of each particle size... i The degree of liberation difference is used to obtain the degree of liberation correction coefficient λ, which is used to correct the final oxidation rate. This allows the measurement results to simultaneously reflect the influence of the degree of mineral liberation on the apparent value of the oxidation rate, thereby improving the guiding value of the oxidation rate measurement results for the flotation process.

[0035] It can be explained that automated mineralogical analysis uses automated quantitative mineral analysis systems (such as MLA and QEMSCAN) to perform particle-by-particle scanning analysis of the sample, obtaining mineral composition data for each molybdenum mineral particle, including molybdenum mineral type, molybdenum mineral content, elemental composition, S / Mo / O atomic ratio, molybdenum sulfide / molybdenum oxide phase assignment, dissociation state such as monomers, intergrowth relationships, inclusion relationships, surface exposure degree, molybdenum content and mass percentage, etc. Morphology and elemental distribution analysis uses high-resolution backscattered electron (BSE) image analysis and elemental surface scanning analysis to characterize the sample, and performs secondary discrimination based on the internal morphology, phase distribution, and specific elemental distribution of the sample.

[0036] It can be explained that Mintergrowth is the sum of the molybdenum mass fractions in the molybdenum sulfide fractions initially identified as intergrowth particles in automated mineralogical analysis and those subsequently identified as oxide particles in morphology and elemental distribution analysis; Mencapsulation is the mass fraction of molybdenum in the initially identified encapsulated particles. All encapsulated molybdenum sulfide is equivalent to molybdenum oxide and thus included in the oxidation rate calculation to correct for the bias of an overestimation of apparent molybdenum sulfide content and an underestimation of oxidation rate caused by the physical encapsulation of molybdenum sulfide minerals by gangue or molybdenum oxide, which fails to dissolve during selective leaching of chemical phases; Moxidation is the sum of the molybdenum mass fractions in the initially identified molybdenum oxide particles and the molybdenum oxide fraction excluding those subsequently identified as sulfide particles; Mtotal is the total mass fraction of molybdenum in all molybdenum-containing particles in the whole sample.

[0037] In some embodiments, based on each particle size sample A i The dissociation degree difference is used to obtain the dissociation degree correction coefficient λ. The steps for calculating the corrected oxidation rate include: According to b i 3 .h.e Calculate the degree of dissociation deviation coefficient DI=Σ(a1×b1) 3 .h.e ×y h.e ) / Σ(a2×b2 3 .h.e ×y h.e ); Based on the dissociation degree deviation coefficient DI, the dissociation degree correction coefficient λ is obtained, and the corrected oxidation rate α' = α × λ is calculated; where... When DI<85%, λ=1+(85%-DI); When DI≥85%, λ=1.

[0038] In this embodiment, the degree of dissociation deviation coefficient DI and the degree of dissociation correction coefficient λ are calculated using the molybdenum content of molybdenum sulfide monomer particles in the coarse particles on the sieve and the fine particles on the sieve. The threshold of DI is set to 85%. When DI < 85%, it indicates that the degree of dissociation of the coarse particles on the sieve and the fine particles on the sieve is large, and the oxidation rate calculation result needs to be corrected. The degree of dissociation correction coefficient λ is defined as 1 + (85% - DI). When DI ≥ 85%, the degree of dissociation of the coarse particles on the sieve and the fine particles on the sieve is consistent, and λ = 1 can be taken.

[0039] In some embodiments, the grinding process includes: The sample to be tested was ground until it all passed through a 1.0 mm sieve to obtain a coarse sample; The coarse sample was sieved using a sieve with a mesh size of 0.074 mm to obtain coarse particles A1 on the sieve and fine particles A2 on the sieve.

[0040] In this embodiment, the sample to be tested is ground to achieve a particle size of -1.0 mm. The coarse sample that has passed through a 1.0 mm sieve is then subjected to wet or dry sieving using a 0.074 mm standard sieve to obtain coarse particles (A1) and fine particles (A2) that pass through the sieve. Generally, coarse-grained ore particles contain more intergrowths and have a lower degree of liberation; fine-grained ore particles contain more monomers and have a higher degree of liberation. Using sieves of two different particle sizes sequentially reduces the interference of particle size differences on the degree of liberation, thereby improving the accuracy of molybdenum ore oxidation rate determination.

[0041] In some embodiments, each particle size sample A i Analytical sample B for automated mineralogical analysis was prepared by drying, mixing, and reducing the sample size. i The steps include: For each particle size sample A i The samples were dried, mixed, and reduced in size to obtain the reduced sample. The reduced sample was subjected to resin injection curing, demolding, polishing, and carbon spraying to obtain analytical sample B for automated mineralogical analysis. i .

[0042] In this embodiment, the test samples of each particle size are dried to make them loose and dry, facilitating accurate weighing. The test samples are then mixed to improve the uniformity of composition and mineral structure across particle size fractions, ensuring representativeness. Reduction of the sample size reduces the sample quantity while maintaining representativeness, obtaining a reduced sample that meets the requirements for dissociation degree determination. Epoxy resin and curing agent are mixed at a volume ratio of 1:(0.2-0.5) to obtain an epoxy resin mixture solution. The reduced sample is then injected and cured, with the volume ratio of the reduced sample to the epoxy resin mixture solution controlled at 1:(2-5), and the liquid level controlled at 1cm-1.3cm. Ultrasonic vibration is applied for 6-12 minutes, and curing is accelerated at 40℃-65℃. After curing, the sample is demolded and subjected to coarse grinding to expose 90% or more of the ore particle cross-section. Subsequently, fine grinding, precision grinding, and polishing are performed sequentially to eliminate scratches and obtain a smooth, polished surface for subsequent mineral analysis. Finally, carbon spraying is performed using a multi-functional coating instrument to spray carbon with a thickness of 10nm-30nm, which improves the surface conductivity of the analytical sample and ensures the stability and accuracy of subsequent mineral analysis.

[0043] In some embodiments, B i 1 .h.e Including B1 1 .h.e and B2 1 .h.e At least one of them; B1 1 .h.e The area of ​​molybdenum sulfide minerals is ≤75%, and they are associated with other molybdenum-free gangue minerals; B2 1 .h.e The area of ​​molybdenum sulfide minerals is ≤85%, and they are associated with other molybdenum-free gangue minerals.

[0044] In this embodiment, B i 1 .h.e Including B1 in the coarse particles on the sieve 1 .h.e B2 in the sieved fine particles 1 .h.e At least one of the following; for coarse particles on the sieve, if the cross-sectional area of ​​the molybdenum sulfide mineral accounts for ≤75% of the total cross-sectional area of ​​the mineral particle and is associated with other molybdenum-free gangue minerals, it is classified as B1. 1 .h.e For undersized fine particles, if the cross-sectional area of ​​the molybdenum sulfide mineral accounts for ≤85% of the total cross-sectional area of ​​the mineral particle and is associated with other molybdenum-free gangue minerals, it is classified as B2. 1 .h.eBecause the target mineral, molybdenum sulfide, has a low proportion and is difficult to dissociate due to its intergrowth state, resulting in a small leakage range and a small contact area with flotation reagents, it is not suitable for flotation. Its properties are consistent with those of molybdenum oxide, so it is included in the calculation scope of molybdenum oxide.

[0045] In some embodiments, B i 2 .h.e Including B1 2 .h.e and B2 2 .h.e At least one of; B1 2 .h.e The molybdenum sulfide minerals are completely enclosed by gangue minerals or molybdenum oxide minerals, with no exposed boundaries; B2 2 .h.e The molybdenum sulfide mineral is partially enclosed by gangue minerals or molybdenum oxide minerals, and the enclosed side length accounts for ≥65% of the perimeter of the molybdenum sulfide mineral.

[0046] In this embodiment, B i 2 .h.e Including B1 in the coarse particles on the sieve 2 .h.e B2 in the sieved fine particles 2 .h.e At least one of the following; for coarse particles on the sieve, when the molybdenum sulfide minerals are completely encapsulated by gangue minerals or molybdenum oxide minerals without exposed boundaries, it is classified as B1. 2 .h.e For undersized fine particles, if the molybdenum sulfide minerals are partially encapsulated by gangue minerals or molybdenum oxide minerals, and the encapsulated side length of the molybdenum sulfide minerals accounts for ≥65% of the perimeter of the molybdenum sulfide minerals, it is classified as B2. 2 .h.e Because the surface of molybdenum sulfide minerals is covered, molybdenum sulfide is difficult to expose and cannot effectively contact molybdenum sulfide collectors, thus exhibiting a non-molybdenum sulfide phase, and is therefore included in the calculation of molybdenum oxide.

[0047] In some embodiments, B i.n.f Including B 1.n.f and B 2.n.f At least one of them; B 1.n.f The area of ​​medium-oxidized molybdenum minerals accounts for ≥70%; B 2.n.f The area ratio of medium-oxidized molybdenum minerals is ≥80%.

[0048] In this embodiment, B i.n.f Including B in the coarse particles on the sieve 1.n.f and B in the sieved fine particles 2.n.fAt least one of the following; for coarse particles on the sieve, if the area ratio of molybdenum oxide minerals is ≥70%, it is judged as B. 1.n.f For undersized fine particles, if the area ratio of molybdenum oxide minerals is ≥80%, it is classified as B. 2.n.f Since molybdenum oxide minerals dominate in this mineral grain, and the small amount of molybdenum sulfide cannot be fully exposed to react with flotation reagents, it is included in the molybdenum oxide calculation.

[0049] In some embodiments, the outer layer of the sulfide particles is molybdenum sulfide mineral, and the inner layer is metal oxide or gangue. On the outer contour of the sulfide particles, the perimeter of molybdenum sulfide mineral accounts for ≥50%. The outer layer of the oxidized particles is molybdenum oxide mineral, and the inner layer is molybdenum sulfide mineral. On the outer contour of the oxidized particles, the perimeter of molybdenum oxide mineral accounts for ≥50%.

[0050] In this embodiment, the morphology and elemental distribution of particles with intergrowth of molybdenum sulfide and molybdenum oxide minerals, as well as particles with mutual encapsulation of molybdenum sulfide and molybdenum oxide minerals, are analyzed, and secondary determination is made based on their internal structural characteristics. Combined with elemental composition analysis, when the BSE image of the particles shows a bright edge and a dark core, it indicates that the outer layer of the particle is mainly molybdenum sulfide mineral, and the inner layer is mainly metal oxide or gangue. Because the outer layer of molybdenum sulfide mineral can directly interact with flotation reagents and dominates the wettability and floatability of the particle surface, such particles are classified as sulfide-type particles. Combined with elemental composition analysis, when the BSE image of the particles shows a dark edge and a bright core, it indicates that the outer layer of the particle is mainly molybdenum oxide mineral, and the inner layer is mainly molybdenum sulfide mineral. Because the outer layer of molybdenum oxide mineral has a hydrophilic surface and poor floatability, it is difficult to effectively interact with conventional sulfide mineral flotation reagents and inhibits the floatability of the inner layer of molybdenum sulfide mineral, such particles are classified as oxide-type particles.

[0051] In some embodiments, the steps of automated mineralogical analysis include: Set the instrument parameters and select the particle measurement mode to measure the gold standard sample; Adjust the instrument's working distance to 10mm-14mm and the accelerating voltage to 20kV-25kV, so that the full-view energy spectrum count rate of the gold sample reaches 60kcps-100kcps, the gray value of the gold sample is 230-250, and the gray value of the epoxy resin is 8-12. Under the same parameter conditions, the analysis sample B was subjected to... i Particle-by-particle measurements are performed, and the measured mineral energy spectrum lines are matched with theoretical mineral energy spectrum databases or user-defined mineral spectral line libraries to identify and analyze sample B. i Parameters such as mineral types, liberation states, and content.

[0052] In this embodiment, instrument parameters are set, and a particle measurement mode is used to measure the gold-labeled sample. This establishes a unified grayscale reference and energy spectrum acquisition conditions, ensuring clear backscattered electron images, distinct particle boundaries, and a high signal-to-noise ratio in the energy spectrum. Subsequently, sample B is analyzed under the same parameter conditions. i Particle-by-particle measurements are performed, and the measured mineral energy spectrum lines are matched with theoretical mineral energy spectrum databases or user-defined mineral spectral line libraries to automatically identify and analyze sample B. i The parameters, such as mineral types, are included. This improves the accuracy and automation of mineral identification, reduces human error, ensures the comparability and repeatability of analytical results between different samples, and provides a reliable basis for the liberation degree, intergrowth relationship, and beneficiation process optimization of molybdenum-bearing minerals.

[0053] In some embodiments, setting instrument parameters includes: Adjust the magnification factor to make the actual pixel size of the image 0.3μm-0.5μm; Set the background subtraction grayscale threshold to 120-160; The number of image frames was used as the measurement termination condition.

[0054] In this embodiment, by limiting the actual pixel size of the image to 0.3μm-0.5μm, measurement efficiency can be balanced while ensuring the identification of mineral particles. By setting the background subtraction grayscale threshold to 120-160, interference from epoxy resin, pores, and the background can be effectively eliminated, improving the accuracy of particle segmentation and mineral identification. Using the number of image frames acquired as the measurement termination condition ensures that the BSE image has sufficient signal-to-noise ratio and statistical stability, avoiding under- or over-acquisition. This improves the accuracy, repeatability, and comparability of automatic mineral identification, particle size statistics, dissociation degree, and stratigraphic relationship analysis.

[0055] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0056] Example 1 S1. A 5.0 kg sample of raw molybdenum ore was taken, crushed to <3 mm using a jaw crusher, and then wet-milled using a conical ball mill at a grinding concentration of 65% for 8 minutes. The ground product passed through a 1.0 mm standard sieve, yielding the undersize product. After mixing, 100.00 g of the undersize product was further wet-sieved using a 0.074 mm standard sieve to obtain coarse particles A1 (+0.074 mm) and fine particles A2 (-0.074 mm), with yields of a1 = 41.26% and a2 = 58.74%, respectively. S2. Dry, mix, and reduce the concentrations of A1 and A2 separately. Take 5.0g of each representative sample and mix them with an epoxy resin mixture (epoxy resin:curing agent = 1:0.3) at a volume ratio of 1:3. Pour the mixture into a mold to a height of 1.2cm, ultrasonically vibrate for 8 minutes, and then cure in a 55℃ oven for 6 hours. After curing, demold and perform coarse grinding, fine grinding, and polishing in sequence to ensure that the exposed particle area is ≥90% and the surface is free of scratches. Subsequently, a 15nm thick carbon layer is sprayed using a multi-functional coating machine to obtain analytical samples B1 and B2. S3 uses an MLA system for automated mineralogical analysis, with a working distance of 12 mm and an accelerating voltage of 25 kV. Grayscale calibration is as follows: gold sample grayscale 240, epoxy resin grayscale 10, background threshold grayscale 140, pixel size 0.4 μm, and image frame rate set to 500 frames as the termination condition. Particle-by-particle scanning acquires the energy dispersive spectral data of molybdenum mineral particles in B1 and B2, which is then matched against a mineral database to identify the mineral species.

[0057] The sulfides were identified as molybdenite, and the molybdenum oxides as molybdenite and molybdenum-bearing serpentine. h represents the molybdenum sulfide mineral, e is the mineral category number among the molybdenum sulfide minerals, and e is 1 when it represents molybdenite. n represents the molybdenum oxide mineral, f is the mineral category number among the molybdenum oxide minerals, and f is 1 when it represents molybdenite, and f is 2 when it represents molybdenum-bearing serpentine. Among them, the molybdenum content y in molybdenite h.1 =58.25%, molybdenum content y in molybdenum-calcium ore n.1 =41.33%, molybdenum content y in molybdenum-bearing serpentine n.2 =24.27%; Based on mineral composition data, sample B was analyzed. i Initial classification includes molybdenum sulfide particles B. i.h.e and molybdenum oxide particles B i.n.f Among them, molybdenum sulfide particles B i.h.e Including Liansheng Granules B i 1 .h.e Encapsulated particle B i 2 .h.eand monomer particles B i 3 .h.e The mass fraction of each type of particle was determined to be b. i.h.e b i.n.f b i 1 .h.e b i 2 .h.e and b i 3 .h.e Where i represents the type of sample to be screened, i=1 or 2, i=1 represents the sample that passes through the sieve, and i=2 represents the sample that passes through the sieve. Table 1 shows the results of the automated mineralogical analysis in Example 1 (%). S4, initially classified as B i 1 .h.e Or B i 2 .h.e The samples were analyzed for morphology and elemental distribution and then classified into sulfide particles and oxidized particles. like Figure 1 The sulfide-type particles shown have molybdenite on the periphery and molybdenum-bearing serpentine in the middle. The mass fraction of molybdenum contained in the molybdenum oxide minerals is c. n.1 =5.74%; Figure 2 for Figure 1 Energy dispersive spectroscopy (EDS) plots at five measurement points in the sulfurized particles. The horizontal axis (KeV) represents energy, and the vertical axis (cps / eV) represents the count rate per unit energy interval. Point 1 is scheelite (the contents of each element are W: 51.42%, O: 32.16%, Ca: 14.52%, S: 1.90%). Point 2 is molybdenite (the contents of each element are Mo: 57.67% and S: 42.33%). Point 3 is molybdenite (the contents of each element are Mo: 57.64% and S: 42.36%). Measurement point 4 is serpentine (gangue mineral); Measurement point 5 is fluorite (gangue mineral).

[0058] like Figure 3 In the oxidized particles shown, the outer layer is molybdenite (zone b), and the middle layer is molybdenite (zone a). The mass fraction of molybdenum contained in the molybdenum sulfide minerals is d. h.1 =8.26%; S5, Calculate the overall oxidation rate of the sample. Table 2 is a breakdown of the calculations for Example 1 (%). Table 3 shows the total M calculation (%) for Example 1. M continuum = Σa i ×b i 1 .h.e ×y h.e ×(1+d h.e = 1.9711% × (1 + 8.26%) = 2.1339%; M package = Σa i ×b i 2 .h.e ×y h.e =0.3884%; M oxidation = Σa i ×b i.n.f ×y n.f ×(1-c n.f = (0.2625% + 0.4093%) × (1 - 5.74%) = 0.6332%; M_total = Σa i ×b i.n.f ×y n.f +Σa i ×b i.h.e ×y h.e =0.2625% + 0.4093% + 5.0241% = 5.6959%; The overall oxidation rate α = Σ(M_continuous growth + M_encapsulation + M_oxidation) / M_total × 100% = (2.1339% + 0.3884% + 0.6332%) ÷ 5.6959% × 100% = 55.40%.

[0059] S6, based on sample A of each particle size i The degree of dissociation difference DI is used to obtain the degree of dissociation correction coefficient λ, and the corrected oxidation rate is calculated.

[0060] DI=Σ(a1×b1 3 .h.e ×y h.e ) / Σ(a2×b2 3 .h.e ×y h.e = (41.26% × 29.34% × 58.25%) ÷ (58.74% × 58.51% × 58.25%) = 35.23%; Since DI < 85.00%, then λ = 1 + (85% - 35.21%) = 1.10; The corrected oxidation rate α' = α × λ = 55.40% × 1.10 = 60.94%.

[0061] Verification test: The same ore sample as in Example 1 was ground to a particle size distribution of -0.074 mm (75%) and added to a flotation cell. The pulp concentration was adjusted to 35%. Sodium silicate 1500 g / t, kerosene 160 g / t, butanol black reagent 20 g / t, and MIBC 20 g / t were added sequentially. All reagent dosages were based on the dry ore feed rate. A flotation process consisting of one roughing, two cleaning, and three scavenging stages was employed. The middlings produced were returned to the previous operation stage according to the process flow. After flotation, the concentrate and tailings were collected separately, filtered, dried, weighed, and their grade and recovery rate were analyzed. The molybdenum grade of the flotation concentrate was 26.29%, the molybdenum concentrate yield was 8.67%, and the molybdenum flotation recovery rate was 26.29% × 8.62% ÷ 5.6959% = 39.79%. The theoretical recovery rate calculated using the method of this application was 100.00% - 60.94% = 39.06%, indicating that the oxidation rate calculated by the method of this application is in good agreement with the measured results and can accurately reflect the molybdenum flotation recovery, thus verifying the accuracy and reliability of the method.

[0062] Example 2 Another molybdenum oxide ore sample was selected, and the remaining determination steps were the same as in Example 1.

[0063] S1. Take 5.0 kg of another molybdenum ore sample. After crushing to <3 mm using a jaw crusher, perform wet grinding using a conical ball mill. The grinding concentration is 65%, and the grinding time is 8 min. The ground product passes through a 1.0 mm standard sieve completely, obtaining the undersize product. After mixing, take 100.00 g of this product, and then perform wet sieving using a 0.074 mm standard sieve to obtain the coarse oversize product A1 (+0.074 mm) and the fine undersize product A2 (-0.074 mm), with yields of a1=53.77% and a2=46.23%, respectively. Steps S2 and S3 are the same as in Example 1; Table 4 shows the results of the automated mineralogical analysis in Example 2 (%). S4, initially classified as B i 1 .h.e Or B i 2 .h.e The samples were analyzed for morphology and elemental distribution, and then classified into sulfide particles and oxidized particles. In sulfide-type particles, the mass fraction of molybdenum contained in molybdenum oxide minerals is c. n.1=3.11%; In oxidized particles, the mass fraction of molybdenum contained in molybdenum sulfide minerals is d. h.1 =6.40%; S5, Calculate the overall oxidation rate of the sample. Table 5 shows the breakdown of calculations (%) for Example 2. Table 6 shows the total M calculation (%) for Example 2. M continuum = Σa i ×b i 1 .h.e ×y h.e ×(1+d h.e = 0.4563% × (1 + 6.40%) = 0.4855%; M package = Σa i ×b i 2 .h.e ×y h.e =0.2764%; M oxidation = Σa i ×b i.n.f ×y n.f ×(1-c n.f = 0.2699% × (1 - 3.11%) = 0.2615%; M_total = Σa i ×b i.n.f ×y n.f +Σa i ×b i.h.e ×y h.e =0.2699% + 1.4615% = 1.7314%; The overall oxidation rate α = Σ(M_continuous growth + M_encapsulation + M_oxidation) / M_total × 100% = (0.4855% + 0.2764% + 0.2615%) ÷ 1.7314% = 59.11%.

[0064] S6, based on sample A of each particle size i The degree of dissociation difference DI is used to obtain the degree of dissociation correction coefficient λ, and the corrected oxidation rate is calculated.

[0065] DI=Σ(a1×b1 3 .h.e ×y h.e ) / Σ(a2×b2 3 .h.e ×y h.e= (53.77% × 45.80% × 58.25%) ÷ (46.23% × 55.05% × 58.25%) = 96.77%; Since DI ≥ 85.00%, then λ = 1; The corrected oxidation rate α' = α × λ = 59.11% × 1 = 59.11%.

[0066] Verification test: The same ore sample as in Example 2 was ground to a particle size distribution of -0.074 mm (80%) and added to a flotation cell. The pulp concentration was adjusted to 35%. Sodium silicate 1350 g / t, kerosene 150 g / t, butanol black reagent 25 g / t, and MIBC 20 g / t were added sequentially. All reagent dosages were based on the dry ore feed rate. A flotation process consisting of one roughing, two cleaning, and two scavenging stages was employed. The middlings produced were returned to the previous operation stage according to the process flow. After flotation, the concentrate and tailings were collected separately, filtered, dried, weighed, and their grade and recovery rate were analyzed. The molybdenum grade of the flotation concentrate was 27.90%, the molybdenum concentrate yield was 2.53%, and the molybdenum flotation recovery rate was 40.77%. The theoretical recovery rate calculated using the method of this application was 100.00% - 59.11% = 40.89%, indicating that the oxidation rate calculated by the method of this application is in good agreement with the measured results and can accurately reflect the molybdenum flotation recovery, thus verifying the accuracy and reliability of the method.

[0067] Comparative Example 1 Unlike Example 1, the oxidation rate of molybdenum ore from the same source was determined by the method described in "Research on Separation Method of Molybdenum Phase in Ore" published by Su Kai et al. ("Gold", 2009, 30(10): 55-58). The content of molybdenum oxide was 56.33% and the content of molybdenum sulfide was 43.67%.

[0068] Comparative Example 2 Unlike Example 2, the oxidation rate of molybdenum ore from the same source was determined by the method described in "Research on Separation Method of Molybdenum Phase in Ore" published by Su Kai et al. ("Gold", 2009, 30(10): 55-58). The content of molybdenum oxide was 57.90% and the content of molybdenum sulfide was 42.10%.

[0069] Results Analysis: Comparative Examples 1 and 2 used conventional chemical leaching to determine the oxidation rate of molybdenum ore. On the one hand, some molybdenum oxide was encapsulated by gangue minerals, making it difficult for the leaching agent to fully contact it, resulting in incomplete dissolution of molybdenum oxide and a lower oxidation rate value. On the other hand, for particles of oxide minerals encapsulated by sulfide minerals, the internal molybdenum oxide was difficult to be effectively leached and included in the oxidation phase, also leading to a lower oxidation rate result. These factors caused a certain deviation between the oxidation rate determination results and the flotation recovery rate data. At the same time, incomplete phase separation during conventional leaching also posed a risk of cross-contamination between molybdenum sulfide and molybdenum oxide, further affecting the accuracy of the determination results. Therefore, Comparative Examples 1 and 2 could not accurately characterize the true content of molybdenum oxide in molybdenum ore. The method of this application, however, divides molybdenum ore into two independent classification systems based on particle size: coarse and fine. Based on the statistical classification of molybdenum oxide and molybdenum sulfide particles, it further subdivides molybdenum sulfide particles into intercalated molybdenum sulfide particles, encapsulated molybdenum sulfide particles, and single molybdenum sulfide particles, overcoming the problem of oxidation rate deviation caused by the difference in the dissociation behavior of coarse and fine particles in traditional mixed analysis.

[0070] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing embodiments by combining some of the constituent elements, are also included in the scope of this application without departing from the spirit of this application.

[0071] Furthermore, although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for determining the oxidation rate of molybdenum ore, characterized in that, include: S1, the sample to be tested is ground and sieved to obtain samples A of various particle sizes. i The yield is a i ; S2, the particle size samples A i Analytical sample B for automated mineralogical analysis was prepared by drying, mixing, and reducing the sample size. i ; S3, for the analytical sample B i Automated mineralogical analysis was performed on a particle-by-particle basis to obtain the analytical sample B. i Mineral composition data of molybdenum mineral grains; Based on the mineral composition data, the analytical sample B was analyzed. i The molybdenum content in the molybdenum mineral was determined, and the molybdenum content of the molybdenum sulfide minerals in the molybdenum mineral particles was y. h.e The molybdenum content of the molybdenum oxide mineral in the molybdenum mineral particles is y. n.f ; Based on the mineral composition data, the analytical sample B was analyzed. i The molybdenum mineral particles were initially classified, including molybdenum sulfide particles B. i.h.e and molybdenum oxide particles B i.n.f ;in, The molybdenum sulfide particles B i.h.e Including Liansheng Granules B i 1 .h.e Encapsulated particle B i 2 .h.e and monomer particles B i 3 .h.e ; Determination of molybdenum sulfide particles B i.h.e and the molybdenum oxide particles B i.n.f The mass fractions of the molybdenum mineral particles are b i.h.e and b i.n.f The intercalated particles B i 1 .h.e and the encapsulated particle B i 2 .h.e In sample B i The mass fractions in are b i 1 .h.e b i 2 .h.e The monomer particles B i 3 .h.e The molybdenum sulfide particles B i.h.e The mass fraction in is b i 3 .h.e ; S4, initially classified as B i 1 .h.e Or B i 2 .h.e The molybdenum mineral grains in the analyzed samples underwent morphological and elemental distribution analysis and secondary classification, including sulfide-type grains and oxide-type grains; among them, The molybdenum content of the molybdenum oxide mineral in the sulfide particles accounts for c% of the total molybdenum oxide mineral mass. n.f ; The molybdenum content of the molybdenum sulfide mineral in the oxidized particles accounts for d% of the total molybdenum sulfide mineral content. h.e ; S5, calculate the total oxidation rate α = Σ(Mcontinuous + Mencapsulation + Moxidation) / Mtotal × 100%; where... M_consecutive = Σa i ×b i 1 .h.e ×y h.e ×(1+d h.e ); M package = Σa i ×b i 2 .h.e ×y h.e ; M oxidation = Σa i ×b i.n.f ×y n.f ×(1-c n.f ); M_total=Σa i ×b i.n.f ×y n.f +Σa i ×b i.h.e ×y h.e ; Wherein, i represents the type of sample to be screened, i=1 or 2, where i=1 represents the sample that passes through the sieve, and i=2 represents the sample that passes through the sieve; h represents the molybdenum sulfide mineral, e is the mineral category number among the molybdenum sulfide minerals, e can take values ​​from 1 to m, where m is a positive integer greater than 1; n represents the molybdenum oxide mineral, f is the mineral category number among the molybdenum oxide minerals, f can take values ​​from 1 to p, where p is a positive integer greater than 1; S6, based on the particle size sample A i The dissociation degree difference is used to obtain the dissociation degree correction coefficient λ, and the corrected oxidation rate α' = α × λ is calculated.

2. The method for determining the oxidation rate of molybdenum ore according to claim 1, characterized in that, According to the particle size sample A i The dissociation degree difference is used to obtain the dissociation degree correction coefficient λ. The steps for calculating the corrected oxidation rate include: According to b i 3 .h.e Calculate the degree of dissociation deviation coefficient DI=Σ(a1×b1) 3 .h.e ×y h.e ) / Σ(a2×b2 3 .h.e ×y h.e ); Based on the dissociation deviation coefficient DI, the dissociation correction coefficient λ is obtained, and the corrected oxidation rate α' = α × λ is calculated; where... When DI<85%, λ=1+(85%-DI); When DI≥85%, λ=1.

3. The method for determining the oxidation rate of molybdenum ore according to claim 1, characterized in that, The grinding process includes: The sample to be tested was ground until it all passed through a 1.0 mm sieve to obtain a coarse sample; The coarse sample was sieved using a sieve with a mesh size of 0.074 mm to obtain coarse particles A1 on the sieve and fine particles A2 on the sieve.

4. The method for determining the oxidation rate of molybdenum ore according to claim 1, characterized in that, The particle size samples A are then... i Analytical sample B for automated mineralogical analysis was prepared by drying, mixing, and reducing the sample size. i The steps include: For each particle size sample A i The samples were dried, mixed, and reduced in size to obtain the reduced sample. The reduced sample was subjected to adhesive injection curing, demolding, polishing, and carbon spraying to obtain analytical sample B for automated mineralogical analysis. i .

5. The method for determining the oxidation rate of molybdenum ore according to claim 1, characterized in that, The B i 1 .h.e Including B1 1 .h.e and B2 1 .h.e At least one of them; The B1 1 .h.e The area of ​​the molybdenum sulfide minerals described herein is ≤75%, and they are associated with other molybdenum-free gangue minerals; The B2 1 .h.e The area of ​​the molybdenum sulfide minerals described herein is ≤85%, and they are associated with other molybdenum-free gangue minerals.

6. The method for determining the oxidation rate of molybdenum ore according to claim 1, characterized in that, The B i 2 .h.e Including B1 2 .h.e and B2 2 .h.e At least one of them; The B1 2 .h.e The molybdenum sulfide minerals described herein are completely encapsulated by gangue minerals or molybdenum oxide minerals, with no exposed boundaries; The B2 2 .h.e The molybdenum sulfide mineral described herein is partially enclosed by gangue minerals or molybdenum oxide minerals, and the enclosed side length accounts for ≥65% of the perimeter of the molybdenum sulfide mineral.

7. The method for determining the oxidation rate of molybdenum ore according to claim 1, characterized in that, The B i.n.f Including B 1.n.f and B 2.n.f At least one of them; The B 1.n.f The area ratio of the molybdenum oxide minerals mentioned above is ≥70%; The B 2.n.f The area ratio of the molybdenum oxide minerals mentioned above is ≥80%.

8. The method for determining the oxidation rate of molybdenum ore according to claim 1, characterized in that, The outer layer of the sulfide particles is the molybdenum sulfide mineral, and the inner layer is a metal oxide or gangue. On the outer contour of the sulfide particles, the perimeter of the molybdenum sulfide mineral accounts for ≥50%. The outer layer of the oxidized particle is the molybdenum oxide mineral, and the inner layer is the molybdenum sulfide mineral. On the outer contour of the oxidized particle, the perimeter of the molybdenum oxide mineral accounts for ≥50%.

9. The method for determining the oxidation rate of molybdenum ore according to claim 1, characterized in that, The steps of the automated mineralogical analysis include: Set the instrument parameters and select the particle measurement mode to measure the gold standard sample; Adjust the working distance of the instrument to 10mm-14mm and the accelerating voltage to 20kV-25kV so that the full-view energy spectrum count rate of the gold sample reaches 60kcps-100kcps, the gray value of the gold sample is 230-250, and the gray value of the epoxy resin is 8-12. Under the same parameter conditions, the analytical sample B was subjected to... i Particle-by-particle measurements are performed, and the measured mineral energy spectrum lines are matched with theoretical mineral energy spectrum databases or user-defined mineral spectral line libraries to identify the analytical sample B. i The types of minerals.

10. The method for determining the oxidation rate of molybdenum ore according to claim 9, characterized in that, The instrument parameters to be set include: Adjust the magnification factor to make the actual pixel size of the image 0.3μm-0.5μm; Set the background subtraction grayscale threshold to 120-160; The number of image frames was used as the measurement termination condition.