Test and evaluation method for self-repairing performance of self-repairing coating for car film
By using standardized scratch tools and microscopic monitoring, combined with multi-time point recording, the self-healing index is calculated, which solves the problems of standardization and quantification in automotive coating testing, realizes a reliable evaluation method, and is suitable for differentiated testing of room temperature and heat-healing coatings.
Patent Information
- Application Number
- CN202611420297.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-24
AI Technical Summary
The existing testing and evaluation methods for self-healing coatings for car wraps lack standardization and quantification, resulting in inconsistent scratch fabrication, unclear repair conditions, single evaluation indicators, failure to distinguish between room temperature and heat repair types, and failure to consider the influence of coating thickness, leading to unreliable and incomparable test results.
Scratches were prepared using standardized scratch tools and a controllable load scratch instrument. Combined with optical microscopy monitoring, the repair process was recorded at multiple time points. The scratch repair rate, gloss recovery rate, and repair speed factor were calculated to establish a comprehensive self-healing index that is suitable for different environmental conditions of room temperature and heat-healing coatings.
It achieves standardization and quantification of scratch fabrication, precise control of repair conditions, and multidimensional quantification of evaluation indicators, improving the repeatability and comparability of test results, providing objective evaluation standards, and offering technical support for coating formulation optimization and product quality evaluation.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention discloses a method for testing and evaluating the self-healing performance of self-healing coatings for car wraps, belonging to the field of coating performance testing technology. Background Technology
[0002] Paint Protection Film (PPF), commonly known as "invisible car wrap," is a transparent functional film applied to the surface of a car's paint to provide protection. It typically consists of a topcoat (self-healing coating), a substrate layer (mostly thermoplastic polyurethane (TPU), and a pressure-sensitive adhesive layer. The topcoat, as the functional layer directly exposed to the external environment, has self-healing properties that are one of the most crucial functional indicators of the film. When subjected to minor scratches, the self-healing coating can automatically fill the scratches and restore a smooth surface by being triggered by heat (such as sunlight, hot water, or hot air) or by the rearrangement and flow of the coating's molecular chains at room temperature. Currently, the mainstream self-healing coatings for car wraps are mainly divided into two categories: room temperature repair type (repairs at 20-35℃) and heat repair type (requires heating to approximately 60℃ to trigger repair). Self-healing performance has become a key factor in evaluating the quality of car wrap products, determining their market competitiveness, and user satisfaction.
[0003] However, current testing and evaluation methods for the self-healing performance of self-healing coatings for car wraps still have several prominent technical problems: First, the methods for creating scratches are inconsistent and unquantifiable. The industry commonly uses tools such as steel brushes, steel wool, keys, and pen tips to randomly create scratches. Different testers use different types of tools, apply varying degrees of force, and scratch the same material multiple times and at different angles, resulting in significant differences in scratch depth, width, and density, making subsequent comparisons of repair effects unobjective. Second, the repair conditions lack standardized regulations. Triggering self-healing methods include hot water pouring, hot air gun baking, hand rubbing, and sunlight exposure, but the water temperature, hot air gun temperature and distance, and exposure time and intensity are not clearly defined, leading to significant differences in the repair effect of the same product depending on the triggering conditions. Third, the evaluation indicators are singular and rely on subjective judgment; existing methods often use the "scratch disappearance / non-disappearance" criterion. The binary judgment or vague description of "fast / slow repair" lacks quantitative evaluation indicators. The evaluation results rely on the visual observation of testers, which varies from person to person and lacks objective and repeatable quantitative standards. Fourth, there is a lack of systematic evaluation of repair dynamics. Existing methods usually only observe the two states before and after repair, without recording the dynamic changes during the repair process, and cannot evaluate the repair speed, a key dimension that distinguishes different qualities of self-healing coatings. Fifth, there is no distinction between different evaluation systems for room temperature repair and thermal repair. The repair mechanisms and triggering conditions of the two types of coatings are different, but existing testing and evaluation methods often confuse them or make the evaluation confusing. Sixth, the influence of coating thickness on the repair effect is not considered. The repairable scratch depth of a self-healing coating is closely related to its thickness. Existing testing and evaluation methods do not take coating thickness as a consideration factor, which makes it impossible to compare test results of the same coating at different coating thicknesses.
[0004] Therefore, there is an urgent need for a new testing and evaluation method for the self-healing performance of self-healing coatings for car wraps, in order to achieve standardization and quantification of scratch production, precise control of repair conditions, multi-dimensional quantification of evaluation indicators, and classification evaluation of room temperature repair type and heat repair type, thereby improving the repeatability and comparability of test results and providing technical support for standardizing product quality evaluation in the industry and guiding the optimization of coating formulations. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a method for testing and evaluating the self-healing performance of self-healing coatings for car wraps, comprising the following steps: S1. Sample preparation: Cut the car wrap film made of self-healing coating, measure the thickness, place it in a standard environment to allow the coating to fully balance, clean the surface, and let it stand for 30 minutes. S2. Reference performance measurement: including initial gloss measurement, initial haze measurement and coating hardness measurement; S3. Scratch fabrication: Scratch treatment is performed using standardized scratch tools. Scratch treatment includes light scratches, medium scratches, or heavy scratches. After the scratch treatment is completed, the initial width and depth of the scratches are observed and recorded using an optical microscope. S4. Repair Trigger and Repair Process Monitoring: Determine whether the self-healing coating is a room temperature repair type or a heat repair type; If the self-healing coating is a room temperature repair type, place the scratched sample in a standard environment for static repair. Observe and record the width of the scratch using an optical microscope at repair times of 0 min, 1 min, 5 min, 10 min, 30 min, 60 min, 120 min, and 240 min. If the scratch completely disappears within 240 min, record the time required for complete repair. If it is not completely repaired within 240 min, continue observation until 720 min and record the final repair status. If the self-healing coating is heat-healing type, place the scratched sample in an environment of 60±2℃ for heating and repair. At repair times of 0 min, 30 s, 1 min, 2 min, 5 min, 10 min, 20 min, and 30 min, remove the sample and observe and record the width of the scratch using an optical microscope within 5 min. If the scratch completely disappears within 30 min, record the time required for complete repair. If it is not completely repaired within 30 min, record the final repair status at 30 min. S5. Evaluation and Grading: After the repair is completed, test the gloss of the sample surface, calculate the gloss recovery rate G, and calculate the gloss recovery factor C based on G. Calculate the scratch repair rate R, and then calculate the repair rate factor A based on R; Calculate the complete repair time T, and calculate the repair rate factor B based on T; Based on the repair rate factor A, the repair speed factor B, and the gloss recovery factor C, calculate the comprehensive self-healing index S of the room temperature repair coating or the heat repair coating, S = 0.5×A + 0.3×B + 0.2×C.
[0006] This invention unifies the basic state of samples through sample cutting, coating thickness measurement, standard environmental balancing, and surface cleaning and settling, avoiding interference from sample differences, surface impurities, and environmental fluctuations. Benchmark performance determination uses corresponding national standards to obtain original baselines for gloss, haze, and hardness, used to compare performance changes before and after repair. Scratch fabrication employs standardized tools to prepare scratches of different grades, and the initial scratch size is recorded using a microscope, achieving controllable and quantifiable scratch damage and establishing a unified damage benchmark. Repair triggering and monitoring differentiate between room-temperature and heat-repair coatings, matching corresponding repair environments and setting multiple time points to collect scratch width data, considering both the repair endpoint and the repair kinetics process, while limiting observation time to reduce test errors caused by environmental shifts. The evaluation and grading steps convert scratch repair rate, complete repair time, and gloss recovery rate into repair rate factors, repair speed factors, and gloss recovery factors, and then calculate a comprehensive self-repair index using a fixed weighted formula, transforming subjective qualitative evaluation by the naked eye into an objective and calculable quantitative evaluation system. The weighting prioritizes the degree of repair while also considering repair speed and appearance.
[0007] The testing and evaluation method provided by this invention can eliminate the result bias caused by arbitrary operation and uncontrollable conditions in traditional testing, ensure good repeatability of the test, and achieve fair horizontal comparison of different self-healing coating products for car wraps. By using classification testing to adapt the repair mechanism and actual use conditions of the two types of coatings, it avoids evaluation misjudgment. At the same time, it can reflect the performance differences in repair degree and repair speed, get rid of the subjective limitations of simple visual observation, and provide objective and standardized testing basis for coating formulation development, product quality control, and third-party performance testing.
[0008] As an feasible example, the standard environment temperature in step S1 is 23±2℃, the relative humidity is 50±5%, and the placement time under the standard environment is ≥24h.
[0009] As an feasible example, the method for determining the initial gloss is as follows: according to the GB / T 9754-2025 standard, the initial gloss of the sample surface is measured using a gloss meter at an incident angle of 60°. At least 5 different locations are measured for each sample, and the average value is taken.
[0010] As an feasible example, the initial haze determination method is as follows: the initial haze value of the sample is measured using a haze meter in accordance with the GB / T 2410-2008 standard.
[0011] As an feasible example, the coating hardness determination method is as follows: the pencil hardness of the coating is determined by the pencil hardness method according to GB / T 6739-2022 standard.
[0012] As an implementable example, the standardized scratching tools include type A, type B, or type C scratching tools; type A scratching tools are used for light scratches, type B scratching tools are used for medium scratches, and type C scratching tools are used for heavy scratches.
[0013] Furthermore, the Type A scratching tool is a tungsten carbide steel needle with a diameter of 0.5 mm and a tip curvature radius of 0.1 mm; the Type B scratching tool is a tungsten carbide steel needle with a diameter of 1.0 mm and a tip curvature radius of 0.2 mm; and the Type C scratching tool is a standard copper brush (a copper brush conforming to ASTM D3359, with a bristle diameter of 0.3 mm).
[0014] Furthermore, for light scratches, the scratching tool is mounted on a controllable load scratching instrument, with the applied load set to 1.0~2.0N, the scratching speed to 50±5mm / s, the scratch length to be no less than 30mm, and the interval between each scratch to be no less than 5mm; for medium scratches, the applied load is set to 2.0~4.0N (excluding 2.0N), the scratching speed to 50±5mm / s, the scratch length to be no less than 30mm, and the interval between each scratch to be no less than 5mm; for heavy scratches, the applied load is set to 4.5~5.5N, and the scratching speed to be 30±2mm / s. This invention uses dedicated A, B, and C type scratching tools for light, medium, and heavy scratches respectively, specifying the material and size specifications of each tool. It also defines the process parameters such as instrumentation, applied load, scratching speed, scratch length, and scratch spacing for different levels of scratches. By precisely defining the physical parameters of the scratching tool, instrument load, and motion parameters, the uncertainties caused by human scratching with non-standard tools such as keys and steel wool are avoided, enabling stable reproduction of scratches of light, medium, and heavy damage levels. Constraints on load, speed, and scratch spacing ensure controllable scratch damage while preventing interference between scratches and edge effects from affecting test results, providing a unified and reproducible damage benchmark for subsequent self-healing tests. Furthermore, different testers and different test batches can prepare light, medium, and heavy gradient scratches with consistent parameters, exhibiting good reproducibility in scratch width and depth. This simulates different degrees of scratching encountered during actual use of automotive coatings, allowing for the evaluation of the coating's repair capabilities for scratches of varying degrees of damage. It eliminates the shortcomings of traditional scratch fabrication methods, which suffer from high randomness and incomparable damage levels, providing a reliable experimental basis for subsequent horizontal comparisons and quantitative evaluations of self-healing performance.
[0015] As an feasible example, the scratch repair rate R = (W0 - W) t ) / W0 × 100%, where W0 is the initial width of the scratch (μm), W t The remaining width of the scratch (μm) after repair time t.
[0016] As an implementable example, the gloss recovery rate G = G t / G0 × 100%, where G0 is the initial gloss, G t is the gloss after repair.
[0017] As an implementable example, the complete repair time T is the time required for the scratch width to recover to 0 μm (i.e., the scratch is not visible to the naked eye or under a microscope) (unit: seconds or minutes).
[0018] Further, the method for defining the repair rate factor A of the room-temperature repair coating is as follows: A=5 when the scratch repair rate R≥95%, A=4 when 80%≤R<95%, A=3 when 60%≤R<80%, A=2 when 40%≤R<60%, and A=1 when R<40%.
[0019] Further, the method for defining the repair rate factor A of the thermal repair coating is as follows: A=5 when the scratch repair rate R≥95%, A=4 when 80%≤R<95%, A=3 when 60%≤R<80%, A=2 when 40%≤R<60%, and A=1 when R<40%.
[0020] Further, the method for defining the repair speed factor B of the room-temperature repair coating is as follows: B=5 when the complete repair time T≤5min, B=4 when 5min<T≤30min, B=3 when 30min<T≤120min, B=2 when 120min<T≤480min, and B=1 when T>480min or the coating is not completely repaired.
[0021] Further, the method for defining the repair speed factor B of the thermal repair coating is as follows: B=5 when the complete repair time T≤30s, B=4 when 30s<T≤2min, B=3 when 2min<T≤5min, B=2 when 5min<T≤15min, and B=1 when T>15min or the coating is not completely repaired.
[0022] Further, the method for defining the gloss recovery factor C of the room-temperature repair coating is as follows: C=5 when the gloss recovery rate G≥98%, C=4 when 95%≤G<98%, C=3 when 90%≤G<95%, C=2 when 80%≤G<90%, and C=1 when G<80%.
[0023] Furthermore, the gloss recovery factor C of the heat-repairing coating is defined as follows: C=5 when gloss recovery rate G≥98%, C=4 when 95%≤G<98%, C=3 when 90%≤G<95%, C=2 when 80%≤G<90%, and C=1 when G<80%. This invention converts scratch repair rate, complete repair time, and gloss recovery rate into repair rate factor A, repair speed factor B, and gloss recovery factor C, respectively. Repair rate factor A and gloss recovery factor C use the same grading system for both room-temperature and heat-repairing coatings to ensure a unified evaluation standard for repair degree and surface appearance restoration effect. Repair speed factor B sets differentiated time thresholds for the two types of coatings, combining their different repair triggering mechanisms. Room-temperature repair coatings use a long-time evaluation level, while heat-repairing coatings use a short-time evaluation level, adapting to their respective actual repair response characteristics. By clearly defining the grading levels, quantitative experimental data such as scratch width measured under a microscope, repair time, and gloss measured by instruments are transformed into scores that can be used in calculations. This eliminates the ambiguity of subjective judgment by the naked eye and provides standardized score input for the calculation of the comprehensive self-healing index. On the one hand, the repair rate factor A and gloss recovery factor C adopt unified evaluation standards, which can fairly compare the performance differences between the two types of coatings in terms of scratch repair degree and surface gloss restoration ability. On the other hand, the repair speed factor B sets differentiated time thresholds to avoid using the fast response standard of heat repair to criticize room temperature repair products, or using the time scale of room temperature repair to underestimate heat repair products, thus achieving a scientific evaluation by classification. The entire set of factor grading rules transforms qualitative descriptions into quantifiable scores, making the self-healing performance between different samples comparable, and ensuring that the test results are objective and traceable, providing a reliable basis for subsequent calculation of the comprehensive self-healing index and product grade determination.
[0024] This invention classifies self-healing levels based on the comprehensive self-healing index S. When S ≥ 4.5, it is designated as Grade A (Excellent), corresponding to high paint repair rate, fast repair speed, and good gloss recovery; when S ≤ 3.5 < 4.5, it is designated as Grade B (Good), corresponding to relatively high paint repair rate, relatively fast repair speed, and relatively good gloss recovery; when S ≤ 2.5 < 3.5, it is designated as Grade C (Average), corresponding to moderate paint repair rate, average repair speed, and average gloss recovery; when S < 2.5, it is designated as Grade D (Poor), corresponding to low paint repair rate, slow repair speed, or inability to completely repair.
[0025] In this invention, before scratching, a scratch area needs to be marked on the sample surface to ensure that the distance between each scratch and between the scratch and the sample edge is not less than 5mm, thus avoiding the interference of edge effects on the test results. The same scratching tool and the same load are used to scratch the same sample to ensure consistent scratch conditions. During optical microscope observation, the lighting conditions, magnification, and observation angle are kept consistent to reduce systematic errors introduced by the observation. The heat-repairing coating can adjust the heat-repairing temperature according to the product instructions, but the actual repair temperature must be recorded in the output test report. At the same time, a differentiated repair speed factor judgment standard is adopted for the two types of self-healing coatings, namely room temperature repair and heat repair, so as to truly reflect the self-healing performance of the coating in the actual use scenario.
[0026] The testing method provided by this invention can provide a test report as needed after the test results are tested. The test report should fully record the basic information of the sample, including the coating name, room temperature or heat repair type, batch, coating process, coating thickness, etc. It should also record the standard environmental conditions of the test, the benchmark performance data such as initial gloss, initial haze, and pencil hardness, the type of tool used to create the scratch, the load, the speed, and the initial average width and average depth of the scratch, the room temperature or heating temperature conditions used for repair, the repair process monitoring data of the scratch width at each time point, the scratch repair rate, the complete repair time, the gloss recovery rate, the comprehensive self-healing index and the final self-healing level, and should also specify the test date, test personnel and test institution.
[0027] Beneficial effects (1) Standardized scratching tools such as tungsten carbide steel needles and standard copper brushes are used in conjunction with a controllable load scratching instrument to precisely limit the material size, applied load and scratching speed of the tools. This eliminates the operation of randomly scratching with keys and wire brushes, removes uncontrollable variables caused by human operation, and improves the reproducibility and comparability of results from different laboratories and different test batches.
[0028] (2) Clear environmental conditions were set for both room temperature repair coatings and heat repair coatings. Room temperature repair coatings were repaired under a standard environment (23±2℃ / 50±5%RH), while heat repair coatings were repaired under a constant temperature of (60±2)℃. Non-standard triggering methods such as hot water pouring, hot air gun baking, and sun exposure were abandoned to avoid errors caused by unstable repair conditions and ensure that the test results are scientific and reliable.
[0029] (3) The detection method sets multiple time nodes to track the scratch width, not limited to the repair endpoint result, and can obtain key information on repair speed, effectively distinguish the performance differences of different products in repair speed, and completely restore the self-repair process over time.
[0030] (4) This invention combines scratch repair rate, complete repair time and gloss recovery rate to establish a comprehensive self-repair index calculation method, which gets rid of the defects of subjective judgment by the naked eye; at the same time, it adopts differentiated evaluation standards for room temperature and heat repair coatings to avoid one-size-fits-all evaluation errors; the test records the coating thickness, and the test results can be correlated with the coating thickness for analysis, which is convenient for analyzing the intrinsic repair ability of the coating.
[0031] (5) All the instruments used in the test are conventional laboratory instruments, and no expensive special equipment is required. The whole operation process is clear and standardized, and can be widely used by coating companies, testing institutions and scientific research units to carry out research and development screening, quality inspection and third-party performance evaluation. Detailed Implementation
[0032] Example The main instruments used in implementing the testing method of this invention include: Type A scratch tool (0.5mm diameter tungsten carbide needle, tip curvature radius 0.1mm); Type B scratch tool (1.0mm diameter tungsten carbide needle, tip curvature radius 0.2mm); Type C scratch tool (standard copper brush, bristle diameter 0.3mm conforming to ASTM D3359 requirements); controllable load scratch tester (load accuracy ±0.1N, speed accuracy ±1mm / s); automatic reciprocating friction tester (speed accuracy ±1 time / minute); optical microscope (equipped with charge-coupled device CCD image acquisition system, magnification 100~500x, measurement accuracy ±0.5μm); constant temperature drying oven (temperature control accuracy ±1℃); gloss meter (60°, accuracy ±0.5GU); haze meter (accuracy ±0.1%); coating thickness gauge (accuracy ±0.5μm); and pencil hardness tester.
[0033] Example 1 (Commercially available room temperature repair polyurethane coating, coating thickness 20μm) This example provides a method for testing and evaluating the self-healing performance of self-healing coatings for car wraps, including the following steps: S1. Sample preparation: Cut the car wrap film made of self-healing coating into 4 samples of 120mm (length) × 120mm (width), measure the thickness, and then place it in a standard environment (25℃, 50%RH) for 24h to allow the coating to fully balance. Gently wipe the surface clean with a lint-free cloth dipped in anhydrous ethanol, and then let it stand for 30min. S2. Reference Performance Measurement: This includes initial 60° gloss (measured according to GB / T 9754 standard, using a gloss meter at a 60° incident angle to measure the initial gloss of the sample surface, with at least 5 different locations measured for each sample and the average value taken), initial haze (measured according to GB / T 2410 standard, using a haze meter to measure the initial haze value of the sample), and coating hardness (measured according to GB / T 6739 standard, using the pencil hardness method to determine the pencil hardness of the coating); the actual measured initial 60° gloss was 92.5 GU, the initial haze was 0.8%, and the coating (pencil) hardness was HB; S3. Scratch Preparation: Use a Type A scratch tool (standardized scratch tool) to create 5 parallel scratches (30 mm in length, 5 mm apart) on each sample surface; the scratches are light scratches, with a load of 1.5 N and a speed of 50 mm / s; within 5 minutes after the scratch treatment, observe and record the initial width and depth of the scratches using a 200x optical microscope (average width of 5 scratches W0 = 8.2 μm). S4. Repair Triggering and Repair Process Monitoring: It is known that the self-healing coating is a room temperature repair type. The scratched sample was placed in a standard environment (25℃, 50%RH) for static repair. The width of the scratch was observed and recorded using an optical microscope at repair times of 0 min, 1 min, 5 min, 10 min, 30 min, 60 min, 120 min, and 240 min. The test results are detailed in Table 1. Table 1
[0034] S5. Evaluation and Grading: After the repair is completed, the 60° gloss of the test sample surface is 91.8 GU, the gloss recovery rate is calculated to be G=99.2%, and the gloss recovery factor C=5 is calculated based on G (G=99.2%≥98%). Calculate the scratch repair rate R=100%, and calculate the repair rate factor A=5 based on R (R=100%≥95%). The complete healing time is calculated to be T = 60 min. Based on T, the healing rate factor B = 3 (30 min). <T≤120min); Based on the repair rate factor A, repair speed factor B, and gloss recovery factor C, the comprehensive self-healing index S of the room temperature repair coating or the heat repair coating is calculated as follows: S = 0.5×A + 0.3×B + 0.2×C = 4.4. In this example, the self-healing level of the coating is recorded as Grade B (excellent repair rate and excellent gloss recovery, but moderate repair speed).
[0035] Example 2 (Commercially available heat-repairing polyurethane coating system, coating thickness 18μm) The specific implementation method in this example is the same as in Example 1, except that: 1. Initial 60° gloss is 94.0 GU, initial haze is 0.6%, initial (pencil) hardness is F; initial average scratch width W0 = 9.5 μm; 2. After the repair is completed, the 60° gloss level is measured. The test results are detailed in Table 2. Table 2
[0036] After the repair was completed, the 60° gloss of the test sample surface was 93.5 GU, the gloss recovery rate was calculated to be G=99.5%, and the gloss recovery factor C=5 was calculated based on G (G=99.5%≥98%). Calculate the scratch repair rate R=100%, and calculate the repair rate factor A=5 based on R (R=100%≥95%). Calculate the complete repair time T=5min, and based on T, calculate the repair rate factor B=3 (2min). <T≤5min); Based on the repair rate factor A, repair speed factor B, and gloss recovery factor C, the comprehensive self-healing index S of the room temperature repair coating or the heat repair coating is calculated as follows: S = 0.5×A + 0.3×B + 0.2×C = 4.4. In this example, the self-healing level of the coating is recorded as Grade B (excellent repair rate and excellent gloss recovery, but moderate repair speed).
[0037] Example 3 (Commercially available heat-repairing silicone-modified polyurethane coating, coating thickness 25 μm) The specific implementation method in this example is the same as in Example 2, except that: 1. Using three types of scratching tools—Type A (applied load of 1.5N), Type B (applied load of 3.0N), and Type C (applied load of 5.0N)—scratches were made in different areas of the same sample. The remaining test steps were the same as in Example 2. The test results are detailed in Table 3.
[0038] Table 3
[0039] In this example, the coating exhibits excellent self-healing performance for minor scratches (Type A) (S=4.7, Grade A), and good self-healing performance for medium scratches (Type B) and copper brush scratches (Type C) (S=4.1 and 3.9, Grade B, respectively). This indicates that the coating's self-healing ability decreases with increasing scratch severity, but it can completely repair Type A minor scratches within 2 minutes, demonstrating excellent shallow scratch repair capability. This invention, through comparative testing with various scratching tools, can comprehensively evaluate the coating's repair capability for different degrees of damage.
[0040] Example 4 (Commercially available room temperature repair polyurethane coatings, with coating thicknesses of 12, 20, and 30 μm) The specific implementation method in this example is the same as in Example 1, except that the coating is divided into 3 groups, which are 12, 20 and 30 μm respectively; the test results are detailed in Table 4.
[0041] Table 4
[0042] Under the same formulation, thicker coatings result in shorter complete repair time and higher overall self-healing index. The sample with a thickness of 12 μm had an S=3.9 (Grade B), the sample with a thickness of 20 μm had an S=4.4 (Grade B), and the sample with a thickness of 30 μm had an S=4.7 (Grade A). This indicates that coating thickness has a significant impact on self-healing performance. Thicker coatings provide more "repair material" reserves, enabling faster scratch filling. This invention, by recording coating thickness and analyzing its correlation with self-healing performance, provides important background information for understanding the test results.
[0043] Comparative Example 1 (Traditional steel brush random scrubbing method) Test evaluation method: The industry-standard simple steel brush test method is adopted: Take an ordinary steel wire brush, hold it in your hand and rub it back and forth on the surface of the car wrap film about 10 times (the force, speed and number of times are not controlled). After visually observing obvious scratches, use a heat gun (temperature, distance and time are not controlled) to heat the scratched area and observe whether the scratches disappear.
[0044] Test results: For the same brand A car wrap film sample (same as Example 1), three different testers conducted tests and obtained three different conclusions for the same product.
[0045] Personnel 1: After lightly scratching the surface 5 times with a steel brush, the scratches were shallow. After heating with a hot air gun, the scratches "basically disappeared", indicating "good self-healing performance". Personnel 2: After scratching 15 times with a steel brush, the scratches were deep. Even after heating with a hot air gun, there were still obvious scratches, which was judged as "average self-healing performance". Personnel 3: Scratched the sample 10 times with a steel brush, heated it for a long time with a hot air gun very close to the sample (about 5cm), the scratches disappeared but the surface showed an "orange peel" phenomenon, which was judged as "good self-healing performance but the coating was burned".
[0046] Results Analysis: The traditional random rubbing method with a steel brush has the following serious defects. (1) The scratching force, number of times, and angle are arbitrary, and the depth and density of scratches created by different testers vary greatly; (2) The temperature, distance and heating time of the hot air gun were not controlled. Excessive temperature may damage the coating (resulting in orange peel), while excessively low temperature cannot effectively trigger the repair. (3) The evaluation criteria are vague (descriptions such as "basically disappeared" and "still have obvious scratches" are highly subjective). These factors make the test results completely incomparable and unreproducible.
[0047] Comparative Example 2 (using only hot water pouring method) Test evaluation method: Referring to the test evaluation method commonly used by some merchants and users: After scratching the surface of the car wrap with a car key, pour hot water of about 80~90℃ onto the scratched area and observe whether the scratch disappears. The test environment is a normal indoor environment, and the water temperature is estimated by "feeling hot to the touch".
[0048] Test results: After hot water was poured onto the brand B heat-repair type car wrap sample (same as in Example 2), the scratches became noticeably lighter but did not completely disappear, and were judged to have "medium self-repair effect". However, when the sample was tested using the method of Example 2 of this invention (heating at 60°C for 5 minutes), the scratches completely disappeared, and the comprehensive self-repair index S=4.4 (Grade B), and the self-repair performance was actually "good".
[0049] Results Analysis: The hot water pouring method has the following problems. (1) Hot water temperature is uncontrollable: "80~90℃" is only an estimate. The actual water temperature drops significantly from the time it is poured out to the time it is poured onto the film surface. (2) Uneven heating: Hot water flows on the membrane surface, and the heating time and temperature of different areas are inconsistent; (3) Hot water may cause thermal shock or water stains to the coating, interfering with the evaluation; (4) The pouring time is short (a few seconds), and the repair is insufficient, which leads to an underestimation of the actual self-healing ability of the coating.
[0050] This invention uses a constant temperature drying oven to precisely control the heating temperature and time, ensuring the controllability and repeatability of the repair conditions.
[0051] Comparative Example 3 (based solely on visual observation, without quantitative measurement) Test evaluation method: After creating scratches on the surface of the car wrap and triggering repair, the qualitative judgment of "scratches disappeared / not disappeared" is given only by visual observation, without using optical microscopes or any measuring equipment.
[0052] Test results: Two car wrap samples, brand A (Example 1) and brand C (Example 4, 30μm thickness), were tested. Both evaluators agreed that "the scratches have disappeared" and judged that the self-healing performance of both products was "good".
[0053] However, using the quantitative testing and evaluation methods of Examples 1 and 4 of this invention, it was found that: the complete repair time for brand A was 60 minutes (S=4.4, Grade B), while the complete repair time for brand C (30μm thickness) was 30 minutes (S=4.7, Grade A). Both were "invisible to the naked eye," but brand C's repair speed was twice that of brand A, indicating a significant performance difference between the two.
[0054] Results analysis: The human eye has the following limitations in perceiving scratches: (1) When the width of the scratch is less than about 50 μm, it is difficult to distinguish with the naked eye, but it is still clearly visible under a microscope. At this time, "not visible to the naked eye" does not mean "the scratch has been completely repaired"; (2) The difference in repair speed cannot be perceived by the human eye: Both products may have scratches that are "invisible to the naked eye" after 10 minutes, but one has already repaired 80% in 1 minute, while the other has only repaired 20% in 1 minute. The naked eye cannot distinguish this difference. (3) The human eye cannot quantify and record data, which is not conducive to product quality traceability and continuous improvement.
[0055] This invention introduces an optical microscope to accurately measure the width of scratches and sets multiple time points for dynamic monitoring, elevating the evaluation from qualitative to quantitative levels, thus significantly improving the objectivity and accuracy of the evaluation.
[0056] Comparative Example 4 (Single time point evaluation, ignoring repair dynamics) Test evaluation method: After creating a scratch and triggering repair, observe the scratch status only once at a single time point (such as "after 30 minutes of placement" or "after 2 minutes of heating"), and make a judgment based on whether the scratch is "not visible".
[0057] Test Results: After heating for 2 minutes, the scratches on the car wrap sample (same as in Example 2) were "no longer visible," indicating "excellent self-healing performance." However, using the multi-time-point dynamic monitoring method of Example 2 of this invention, it was found that the repair rate of this sample was only about 70% after 2 minutes (the scratch width decreased from 10.2 μm to 3.1 μm). The scratches were "no longer visible" because they became shallower to the point of being invisible to the naked eye, but residual scratch grooves were still visible under a microscope. The scratches did not completely disappear under a microscope until 8 minutes later (the width returned to 0 μm). The actual complete repair time of this sample was 8 minutes, and the comprehensive self-healing index S=3.8 (Grade B), which is not "excellent."
[0058] Results Analysis: Single-point-of-time evaluation has the following problems. (1) “Scratches are not visible” does not mean “scratches have been completely repaired”. The depth of the scratches may still remain, but the width has been narrowed to below the resolution of the naked eye. (2) The repair speed cannot be evaluated: the scratches may be "invisible" at the same time, but one is completely repaired as early as 2 minutes, while the other is not completely repaired until 30 minutes, showing a significant performance difference; (3) A single time point cannot depict the decay or recovery curve of self-healing performance over time.
[0059] This invention, by setting up dynamic monitoring at multiple time points, can accurately capture the entire repair process and truly reflect the repair kinetics of the coating.
[0060] Comparative Example 5 (Evaluation of mixed room temperature repair and thermal repair) Testing and evaluation methods: No distinction is made between the repair types of the coatings. The testing process of "creating scratches → heating → observation" is uniformly adopted, and the same heating conditions and evaluation standards are used for all samples.
[0061] Test Results: A sample of a room-temperature self-healing car wrap performed excellently under heating conditions (scratches disappeared quickly) and was rated as having "excellent self-healing performance." However, the repair speed of this sample at room temperature (without heating) was extremely slow; according to the room-temperature test evaluation method of Example 1 of this invention, the complete repair time exceeded 240 minutes, and the comprehensive self-healing index S=2.8 (Grade C, average). In actual use (car owners usually do not actively heat the car wrap), the self-healing experience of this product is far less than what was shown in the test.
[0062] Results Analysis: The self-healing mechanisms of room-temperature repair and thermal repair are different. Room-temperature repair relies on the chain segment movement of coating molecules at room temperature to achieve repair, while thermal repair requires thermal energy input to break intermolecular forces and promote molecular flow. Equating the two in evaluation presents the following problems: (1) Applying heat to room temperature repair products is equivalent to "cheating". Heating will accelerate the molecular movement of all types of coatings, but it cannot truly reflect their performance in room temperature use scenarios. (2) If insufficient heat energy is provided to heat-repair products, their actual performance will be underestimated; heat-repair products may hardly repair at room temperature, but repair rapidly when heated to 60°C; (3) A uniform evaluation standard cannot fairly reflect the real performance differences of different types of coatings.
[0063] This invention tests and evaluates room temperature repair type and heat repair type separately, making the test results more scientific and fair.
[0064] The test results of the corresponding test evaluation methods for Examples 1-4 and Comparative Examples 1-5 are summarized in Table 5.
[0065] Table 5
[0066] In Comparative Example 1, three testers used the same steel brush but with different pressures and number of strokes, arriving at three different conclusions about the same product. This clearly demonstrates that standardization of scratch fabrication methods is the cornerstone of self-healing performance testing—the depth and width of the scratch directly determine the difficulty and time required for repair. This invention, through standardized scratching tools (tungsten carbide needles / standard copper brushes) and a controllable load scratcher, minimizes the variables in scratch fabrication, ensuring the accuracy of the test. Example 3, through a systematic comparison of three different scratching tools, demonstrates the differences in self-healing performance under different degrees of damage, providing data support for a comprehensive evaluation.
[0067] In Comparative Example 2, the hot water pouring method resulted in a misjudgment of "average" performance for the Brand B heat-repair coating due to uncontrollable water temperature, uneven heating, and short heating time. However, the correct test result from the present invention, heating at a constant temperature of 60℃ for 5 minutes, showed its performance to be "good" (S=4.4). This clearly demonstrates that precise control of repair conditions is crucial for accurately evaluating self-healing performance; excessively high temperatures may damage the coating (resulting in orange peel texture in Comparative Example 1), while excessively low temperatures will fail to effectively trigger repair (Comparative Example 2), both of which lead to distorted evaluations.
[0068] In Comparative Example 3, visual observation led to the misjudgment of two products with significantly different performance—Brand A (complete repair time 60 min) and Brand C (complete repair time 30 min)—as "both good." This reveals the limitations of visual observation—the human eye has limited resolution (approximately 50 μm) and cannot perceive differences in repair speed. This invention uses an optical microscope to precisely measure the scratch width (accuracy ±0.5 μm) and calculates the repair rate over time by monitoring at multiple time points, transforming "invisible" microscopic differences into quantifiable data and completely eliminating the bias of subjective judgment.
[0069] In Comparative Example 4, a single time-point evaluation misjudged a state where "residues are not visible to the naked eye but still exist under a microscope" as "complete repair." This invention, through monitoring multiple time points set in Examples 1-4, clearly demonstrates the change curve of the repair rate over time. In Example 1, Brand A achieved a repair rate of 90.2% after 30 minutes, but complete repair requires 60 minutes; if observation is only conducted at 30 minutes, it might be misjudged as "near complete repair," ignoring the time required for the final 10% of repair. This dynamic information is crucial for a comprehensive evaluation of the coating's repair performance.
[0070] In Comparative Example 5, the room-temperature repair coating was overestimated under heating conditions, while the heat-repair coating was underestimated under non-heating conditions. This invention sets different repair conditions and evaluation criteria (especially the threshold for the repair rate factor) for the two types, making the evaluation more scientific and reasonable. Although Example 1 (room-temperature repair type, complete repair in 60 minutes, S=4.4) and Example 2 (heat-repair type, complete repair in 5 minutes, S=4.4) have the same comprehensive index, the classification evaluation accurately reflects the true performance of the two coatings under different triggering conditions.
[0071] Therefore, the testing and evaluation method for the self-healing performance of self-healing coatings for car wraps provided by this invention has good industrial applicability. It can be applied to the coating research and development stage, using quantitative data on repair rate and repair speed to screen and optimize different formulation systems, and guide formulation design. It can be used for product quality control by car wrap manufacturers, realizing incoming material inspection and outgoing inspection of self-healing coating raw materials and finished car wraps. It can also verify the authenticity of product claims such as "instant repair" and "rapid repair" by enterprises, preventing false advertising. At the same time, it can provide third-party testing institutions with objective and fair performance evaluation and comparison of car wrap products on the market, and can also provide a technical basis for the formulation of relevant industry standards and national standards for testing self-healing coatings for car wraps. Moreover, the equipment and materials used in this method are all standard laboratory configurations, the operation process is standardized and clear, no expensive special equipment is required, and it has good prospects for promotion and application.
Claims
1. A method for testing and evaluating the self-healing performance of a self-healing coating for car wraps, characterized in that, Includes the following steps: S1. Cut the car wrap film made of self-healing coating, place it in a standard environment to allow the coating to fully balance, clean the surface, and let it stand for 30 minutes. S2. Perform initial gloss measurement, initial haze measurement and coating hardness measurement; S3. Use standardized scratching tools to scratch the car wrap film. The scratches include light scratches, medium scratches, or heavy scratches. After the scratching is completed, use an optical microscope to observe and record the initial width and depth of the scratches. S4. Determine whether the self-healing coating is a room temperature repair type or a heat repair type; If the self-healing coating is a room temperature repair type, place the scratched sample in a standard environment for static repair. Observe and record the width of the scratch using an optical microscope at repair times of 0 min, 1 min, 5 min, 10 min, 30 min, 60 min, 120 min, and 240 min. If the scratch completely disappears within 240 min, record the time required for complete repair. If it is not completely repaired within 240 min, continue observation until 720 min and record the final repair status. If the self-healing coating is heat-healing type, place the scratched sample in an environment of 60±2℃ for heating and repair. At repair times of 0 min, 30 s, 1 min, 2 min, 5 min, 10 min, 20 min, and 30 min, remove the sample and observe and record the width of the scratch using an optical microscope within 5 min. If the scratch completely disappears within 30 min, record the time required for complete repair. If it is not completely repaired within 30 min, record the final repair status at 30 min. S5. After the repair is completed, test the gloss of the sample surface, calculate the gloss recovery rate G, and calculate the gloss recovery factor C based on G. Calculate the scratch repair rate R, and then calculate the repair rate factor A based on R; Calculate the complete repair time T, and calculate the repair rate factor B based on T; Based on the repair rate factor A, the repair speed factor B, and the gloss recovery factor C, calculate the comprehensive self-healing index S of the room temperature repair coating or the heat repair coating, S = 0.5×A + 0.3×B + 0.2×C; evaluate the self-healing performance of the coating based on the comprehensive self-healing index S.
2. The testing and evaluation method according to claim 1, characterized in that, The method for determining the initial gloss is as follows: according to the GB / T 9754-2025 standard, the initial gloss of the sample surface is measured using a gloss meter at an incident angle of 60°. At least 5 different positions are measured for each sample, and the average value is taken.
3. The testing and evaluation method according to claim 1, characterized in that, The method for determining the initial haze is as follows: the initial haze value of the sample is measured using a haze meter in accordance with the GB / T 2410-2008 standard.
4. The testing and evaluation method according to claim 1, characterized in that, The coating hardness test method is as follows: the pencil hardness of the coating is determined by the pencil hardness method according to GB / T 6739-2022 standard.
5. The testing and evaluation method according to claim 1, characterized in that, The standardized scratching tools include type A scratching tools, type B scratching tools, or type C scratching tools; When the scratch is a minor scratch, use a type A scratching tool; When the scratch is a medium scratch, use a type B scratching tool; When the scratch is a heavy scratch, use a C-type scratch tool.
6. The testing and evaluation method according to claim 5, characterized in that, The Type A scratch tool is a tungsten carbide steel needle with a diameter of 0.5 mm and a tip curvature radius of 0.1 mm; The Type B scratch tool is a tungsten carbide steel needle with a diameter of 1.0 mm and a tip curvature radius of 0.2 mm; The Type C scratch tool is a standard copper brush with a filament diameter of 0.3 mm.
7. The testing and evaluation method according to claim 5, characterized in that, When the scratch is a light scratch, the applied load is set to 1.0-2.0 N, the scratch speed is 50±5 mm / s, the scratch length is no less than 30 mm, and the interval between each scratch is no less than 5 mm; When the scratch is a medium scratch, the applied load is set to 2.0-4.0 N, the scratch speed is 50±5 mm / s, the scratch length is no less than 30 mm, and the interval between each scratch is no less than 5 mm; When the scratch is a heavy scratch, the applied load is set to 4.5-5.5 N, and the scratch speed is 30±2 mm / s.
8. The testing and evaluation method according to claim 1, characterized in that, It includes the following steps: The scratch repair rate R = (W0 - W) t ) / W0 × 100%, where W0 is the initial width of the scratch, W t The remaining width of the scratch after repair time t; The gloss recovery rate G = G t / G0 × 100%, where G0 is the initial gloss level, G t The gloss level after repair; The complete repair time T is the repair time required for the scratch width to recover to 0 μm.
9. The testing and evaluation method according to claim 1, characterized in that, The method for defining the repair rate factor A of the room-temperature repair coating is as follows: A=5 when the scratch repair rate R≥95%, A=4 when 80%≤R<95%, A=3 when 60%≤R<80%, A=2 when 40%≤R<60%, and A=1 when R<40%; The method for defining the repair speed factor B of the room-temperature repair coating is as follows: B=5 when the complete repair time T≤5 min, B=4 when 5 min<T≤30 min, B=3 when 30 min<T≤120 min, B=2 when 120 min<T≤480 min, and B=1 when T>480 min or the scratch is not completely repaired; The method for defining the gloss recovery factor C of the room-temperature repair coating is as follows: C=5 when the gloss recovery rate G≥98%, C=4 when 95%≤G<98%, C=3 when 90%≤G<95%, C=2 when 80%≤G<90%, and C=1 when G<80%.
10. The testing and evaluation method according to claim 1, characterized in that, The method for defining the repair rate factor A of the thermal repair coating is as follows: A=5 when the scratch repair rate R≥95%, A=4 when 80%≤R<95%, A=3 when 60%≤R<80%, A=2 when 40%≤R<60%, and A=1 when R<40%; The method for defining the repair speed factor B of the thermal repair coating is as follows: B=5 when the complete repair time T≤30 s, B=4 when 30 s<T≤2 min, B=3 when 2 min<T≤5 min, B=2 when 5 min<T≤15 min, and B=1 when T>15 min or the scratch is not completely repaired; The method for defining the gloss recovery factor C of the thermal repair coating is as follows: C=5 when the gloss recovery rate G≥98%, C=4 when 95%≤G<98%, C=3 when 90%≤G<95%, C=2 when 80%≤G<90%, and C=1 when G<80%.