A TiO2 nanoribbon-MoS2 nanosheet composite dual-semiconductor heterojunction SERS substrate material and its preparation method

By employing a phase transformation-in-situ growth coupled construction method based on a self-templating potassium titanate ball, the problem of preparing TiO₂ nanoribbons and MoS₂ nanosheets composite heterojunctions was solved, realizing a simple and efficient TiO₂@MoS₂ dual semiconductor heterojunction SERS substrate material for organic dye detection, exhibiting excellent SERS performance and good reproducibility.

CN123155502APending Publication Date: 2026-11-24WEIHAI JINYU ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611155726.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-31
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The difficulty in preparing existing TiO₂ nanoribbon and MoS₂ nanosheet composite heterojunctions lies in the synergistic regulation of the precursor transformation process and the in-situ growth of MoS₂, which leads to poor substrate reproducibility, complex preparation methods, and low sensitivity.

Method used

A phase transformation-in-situ growth coupled construction method using bobbed potassium titanate as a self-template was adopted to prepare a dual semiconductor heterojunction SERS substrate material with close contact between TiO₂ nanoribbons and MoS₂ nanosheets by controlling the hydrothermal reaction conditions and the amount of precursor.

Benefits of technology

A high-performance TiO₂@MoS₂ dual semiconductor heterojunction SERS substrate was easily prepared for the detection of organic dyes. It exhibits excellent SERS performance and good repeatability, with a detection limit of 1×10⁻⁸M.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123155502A_ABST
    Figure CN123155502A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of surface-enhanced Raman scattering (SERS) substrate material preparation technology, specifically relating to a simplified preparation method for a TiO2@MoS2 nanoribbon and MoS2 nanosheet composite dual-semiconductor heterojunction SERS substrate material. It solves the problems of poor repeatability, complex preparation methods, and low sensitivity of existing non-metallic SERS substrates for detecting organic dyes. This invention prepares a TiO2@MoS2 dual-semiconductor heterojunction SERS substrate material using a simple hydrothermal method for organic dye detection, avoiding complex composite steps, reducing cost, and achieving good repeatability of the resulting heterojunction SERS substrate. It solves the problems of complex preparation and low sensitivity of traditional substrates, achieving a detection limit of 10 for crystal violet. ‑8 M exhibits excellent repeatability and signal uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of surface-enhanced Raman scattering (SERS) substrate material preparation technology, specifically relating to a dual-semiconductor heterojunction (SERS) substrate material composed of TiO2 nanoribbons and MoS2 nanosheets and its preparation method. Background Technology

[0002] Surface-enhanced Raman spectroscopy (SERS) has attracted much attention in environmental monitoring, biomedicine, and other fields due to its ultra-high sensitivity and rapid, non-destructive characteristics. The substrate material, as the core material of SERS technology, directly affects the detection accuracy and sensitivity. While traditional precious metal substrates such as gold and silver can significantly enhance Raman signals through surface plasmon resonance, they are prone to aggregation and deactivation in complex food matrices, are costly, and have weak anti-interference capabilities. Single-semiconductor SERS substrates, although exhibiting good stability, have significantly lower detection sensitivity compared to precious metal SERS substrates. In contrast, dual-semiconductor heterojunction substrates, with their unique band matching and interfacial charge separation mechanisms, not only extend carrier lifetime and improve electron-hole pair separation efficiency but also enhance the adsorption efficiency of analytes through synergistic effects, further increasing signal intensity.

[0003] Currently, there are few reports on TiO2 nanoribbons and MoS2 nanosheets composite heterojunctions. The preparation of TiO2 nanoribbons and MoS2 nanosheets composite heterojunctions is not a simple mixing of the two semiconductor materials; the main challenge lies in the synergistic control of the precursor conversion process and the in-situ growth process of MoS2. On the one hand, it is necessary to make the yarn-like K2Ti8O... 17 The precursor must be fully converted to TiO2, and its nanoribbon framework and hierarchical porous structure should be maintained as much as possible during the conversion process to avoid nanoribbon breakage, agglomeration, and a decrease in specific surface area due to dissolution, recrystallization, or overgrowth. On the other hand, it is necessary to control the amount of molybdenum and sulfur sources added, as well as the hydrothermal reaction temperature and time, so that MoS2 preferentially nucleates heterogeneously on the TiO2 nanoribbon surface and forms uniformly dispersed nanosheets. When the amount of MoS2 generated is insufficient, it is difficult to form a continuous and effective heterogeneous interface; when the amount generated is too large, MoS2 is prone to free nucleation, stacking, and agglomeration, and may excessively cover the adsorption sites on the TiO2 surface. In addition, the distribution density, size, and interfacial contact degree of MoS2 nanosheets with TiO2 nanoribbons will directly affect the adsorption capacity of the substrate for the target molecules, the interfacial charge transfer efficiency, and the uniformity and batch repeatability of the SERS signal. Therefore, how to simultaneously achieve uniform in-situ growth of MoS2 nanosheets while maintaining the multi-level structure of TiO2 nanoribbons, and construct a tight, stable and uniformly distributed TiO2 / MoS2 heterostructure interface, is a key technical problem that needs to be solved in the preparation of this type of dual semiconductor heterostructure SERS substrate. Summary of the Invention

[0004] The purpose of this invention is to address the problems of poor repeatability, complex preparation methods, and low sensitivity of existing non-metallic SERS substrates, and to provide a dual-semiconductor heterojunction SERS substrate material composed of TiO2 nanoribbons and MoS2 nanosheets, as well as its preparation method. The preparation method is a phase transformation-in-situ growth coupled construction method based on a self-templating potassium titanate ball, which can also be defined as a phase transformation-in-situ growth coupled construction method based on a self-templating potassium titanate ball. The prepared substrate exhibits excellent SERS performance when used for crystal violet detection.

[0005] The characteristics of the TiO2 nanoribbon-MoS2 nanosheet composite dual-semiconductor heterojunction SERS substrate material prepared in this application are as follows: 1. Micrometer scale: A large number of TiO2 nanoribbons intertwine to form a yarn-like network; 2. Nanoscale: MoS2 nanosheets are distributed on the surface of TiO2 nanoribbons; 3. Interface scale: TiO2 and MoS2 form a tight contact region. This structure provides a spatial basis for the entry, adsorption, and interfacial charge transfer of analyte molecules.

[0006] The preparation method is as follows: Step 1: Add Ti2AlN to KOH aqueous solution, stir magnetically, and then transfer to a reaction vessel. React at 120~160 ℃ for 12~36 h. After the reaction, wash and dry the product to obtain yarn-like K2Ti8O. 17 ; Step 2: Take the above-mentioned ball of yarn-like K2Ti8O 17 The TiO2@MoS2 heterojunction substrate material was added to an aqueous solution of CH4N2S and (NH4)2MoO4, magnetically stirred, and then transferred to a reaction vessel. The mixture was reacted at 180–200 °C for 18–24 h. After the reaction, the product was washed and dried to obtain the TiO2@MoS2 heterojunction substrate material. This is a composite SERS substrate for organic dye detection, thus completing the simplified preparation method described above.

[0007] Due to K2Ti8O 17 The conversion to TiO2 may involve ion exchange, dissolution, and recrystallization. Insufficient reaction may leave potassium titanate residue; excessive reaction may lead to: 1. collapse of the tufted structure; 2. breakage or significant coarsening of nanoribbons; 3. material agglomeration; 4. separate growth of MoS2 and TiO2. Therefore, the conditions of 180–200 °C and 18–24 h should not be regarded merely as general parameter ranges, but should be linked to the technical effect of "completing the phase transformation while maintaining the three-dimensional nanoribbon framework and forming a heterogeneous interface".

[0008] In the second hydrothermal reaction, MoS2 exhibits two competing growth mechanisms: 1. heterogeneous nucleation on the surface of TiO2 nanoribbons; 2. free nucleation in solution, forming MoS2 aggregates. Insufficient addition of molybdenum and sulfur sources results in inadequate heterostructures; excessive addition leads to the formation of free MoS2 or an excessively thick capping layer, reducing the accessibility of the TiO2 surface. Therefore, this application controls the amount of precursors, reaction temperature, and reaction time to preferentially attach MoS2 to the nanoribbon surface.

[0009] Step 3: Disperse the above TiO2@MoS2 heterojunction substrate in crystal violet ethanol solutions of different concentrations, soak for 4-8 h, then remove the substrate and drop it onto a silicon wafer to dry at room temperature until the solution is completely evaporated.

[0010] Furthermore, in step one, the mass-to-volume ratio of Ti2AlN to KOH aqueous solution is (0.5~2 g):(50~100 mL); wherein the molar concentration of KOH aqueous solution is 10 M; and the particle size of Ti2AlN is 200~500 mesh.

[0011] Furthermore, the magnetic stirring described in step one: the magnetic stirring speed is 500~2000 rpm, and the stirring time is 5~20 min.

[0012] Furthermore, the washing and drying process described in step one involves washing with deionized water 2-5 times and then drying at 50-80°C for 8-16 hours.

[0013] Furthermore, the preparation method of the mixed solution in step two is as follows: weigh 10~50 mg of (NH4)2MoO4 and 20~100 mg of CH4N2S respectively, dissolve them in water and stir for 10~40 min until completely dissolved, the mass ratio of (NH4)2MoO4 to CH4N2S is 1:2.

[0014] Furthermore, in step three, the amount of crystal violet ethanol solution is 3-5 mL.

[0015] Furthermore, the amount of solution aspirated in step three is 50~300 μL.

[0016] Furthermore, the drying time of the solution in step three is 10~40 min.

[0017] Furthermore, in step three, the amount of substrate added to the crystal violet ethanol solution is 2-10 mg.

[0018] The beneficial technical effects of the present invention are as follows: 1. This invention prepares a TiO2@MoS2 dual-semiconductor heterojunction SERS substrate material using a simple hydrothermal method, avoiding complex composite steps; this invention employs a hydrothermal alkaline etching method, using highly alkaline KOH to etch the Al atomic layer in Ti2AlN to obtain a ball-shaped K2Ti8O 17 Materials. Then take the ball of yarn-like K2Ti8O. 17 K2Ti8O was dispersed in an aqueous solution of CH4N2S and (NH4)2MoO4, and then subjected to hydrothermal treatment. 17 The process involves converting the material into TiO2 and simultaneously generating MoS2 nanosheets on the surface of the TiO2 nanoribbons, thus obtaining a TiO2@MoS2 dual semiconductor heterojunction substrate material. The TiO2 nanoribbons have a diameter of 100~500 nm and a line length of <20 μm, while the MoS2 nanosheets grown on the TiO2 nanoribbons have a diameter of 10~30 nm.

[0019] 2. The TiO2@MoS2 dual-semiconductor heterojunction SERS substrate material prepared by this invention can be used as an inorganic nanomaterial for the detection of organic dyes. The preparation method of this invention is simple, low-cost, and produces products with excellent performance. It solves the problems of poor repeatability and high cost of traditional substrates while maintaining excellent SERS performance, achieving a detection limit of 1×10⁻⁶ for crystal violet. -8 M exhibits excellent repeatability and signal uniformity.

[0020] 3. This invention is applicable to the simple preparation of TiO2@MoS2 dual semiconductor heterojunction SERS substrate materials. Attached Figure Description

[0021] Figure 1 The image shows the XRD pattern of the TiO2@MoS2 dual semiconductor heterojunction SERS substrate material obtained in the examples. Figure 2 The image shows a SEM image of the TiO2@MoS2 dual semiconductor heterojunction SERS substrate material obtained in the examples. Figure 3 The image shows a SEM image of the TiO2@MoS2 dual semiconductor heterojunction SERS substrate material obtained in the examples. Figure 4 The image shows a TEM image of the TiO2@MoS2 dual semiconductor heterojunction SERS substrate material obtained in the examples. Figure 5 The image shows the lowest detection limit of crystal violet for the TiO2@MoS2 dual semiconductor heterojunction SERS substrate material obtained in the examples. Figure 6 The images show the Raman spectra of the TiO2@MoS2 dual semiconductor heterojunction SERS substrate material obtained in the examples at 15 different points on the same sample. Figure 7 The dual-semiconductor heterojunction SERS substrate material obtained in the examples was at 1178 cm⁻¹. -1 Raman peak intensity at the location Spectrum; Figure 8 The dual-semiconductor heterojunction SERS substrate material obtained in the examples was at 1178 cm⁻¹. -1 The graph shows the variation of Raman peak intensity at a given location with concentration. Detailed Implementation

[0022] The technical solution of the present invention is not limited to the specific embodiments listed below, but also includes any combination of the specific embodiments.

[0023] Specific Implementation Method 1: In this implementation method, Ti₂AlN is added to a KOH aqueous solution, magnetically stirred, and then transferred to a reaction vessel. The mixture is reacted at 120-160 °C for 12-36 h. After the reaction, the product is washed and dried to obtain a yarn-like K₂Ti₈O₃. 17 ; II. The above-mentioned yarn-like K2Ti8O 17 The TiO2@MoS2 heterojunction substrate material was added to an aqueous solution of CH4N2S and (NH4)2MoO4, magnetically stirred, and then transferred to a reaction vessel. The mixture was reacted at 180–200 °C for 18–24 h. After the reaction, the product was washed and dried to obtain the TiO2@MoS2 heterojunction substrate material. This is a composite SERS substrate for organic dye detection, thus completing the simplified preparation method described above.

[0024] 3. The above TiO2@MoS2 heterojunction substrate was dispersed in crystal violet ethanol solutions of different concentrations, soaked for 4-8 h, and then the substrate was removed and dropped onto a silicon wafer and dried at room temperature until the solution was completely evaporated.

[0025] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the mass-to-volume ratio of Ti₂AlN to KOH aqueous solution in step one is (0.5~2 g):(50~100 mL); the molar concentration of the KOH aqueous solution is 10 M; and the particle size of the Ti₂AlN is 200~500 mesh. Other steps and parameters are the same as in Specific Implementation Method One.

[0026] Specific Implementation Method Three: This implementation method differs from Specific Implementation Method One in that the magnetic stirring in step one is performed at a speed of 500-2000 rpm for a duration of 5-20 minutes. All other steps and parameters are the same as in Specific Implementation Method One.

[0027] Specific Implementation Method Four: This implementation method differs from Specific Implementation Method One in that the washing and drying in step one involves washing with deionized water 2-5 times and then drying at 50-80°C for 8-16 hours. Other steps and parameters are the same as in Specific Implementation Method One.

[0028] Specific Implementation Method Five: This implementation method differs from Specific Implementation Method One in that the preparation method of the mixed solution in step two is as follows: Weigh 10-50 mg of (NH4)2MoO4 and 20-100 mg of CH4N2S respectively, dissolve them in water, and stir for 10-40 min until completely dissolved. The mass ratio of (NH4)2MoO4 to CH4N2S is 1:2. Other steps and parameters are the same as in Specific Implementation Method One.

[0029] Specific Implementation Method Six: This implementation method differs from Specific Implementation Method One in that the amount of crystal violet ethanol solution in step three is 3-5 mL. Other steps and parameters are the same as in Specific Implementation Method One.

[0030] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Method One in that the solution aspirated in step three... The amount is 50~300 μL. Other steps and parameters are the same as in Specific Implementation Method 1.

[0031] Specific Implementation Method Eight: This implementation method differs from Specific Implementation Method One in that the drying time of the solution in step three is 10-40 minutes. Other steps and parameters are the same as in Specific Implementation Method One.

[0032] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Method One in that the amount of substrate added to the crystal violet ethanol solution in step three is 2~10 mg.

[0033] The beneficial effects of the present invention are verified through the following embodiments:

[0034] A simplified method for preparing a TiO2 nanoribbon-MoS2 nanosheet composite dual-semiconductor heterojunction (SERS) substrate material is disclosed, which is achieved through the following steps: 1. Ti₂AlN was added to a KOH aqueous solution, magnetically stirred, and then transferred to a reaction vessel. The reaction was carried out at 150 °C for 16 h. After the reaction was completed, the product was washed and dried to obtain a ball-shaped K₂Ti₈O. 17 ; II. The above-mentioned yarn-like K2Ti8O 17The mixture was added to an aqueous solution of CH4N2S and (NH4)2MoO4, magnetically stirred, and then transferred to a reaction vessel. The reaction was carried out at 200 °C for 24 h. After the reaction, the product was washed and dried to obtain the TiO2@MoS2 heterojunction substrate material. This is a dual-semiconductor heterojunction SERS substrate for organic dye detection, thus completing the simplified preparation method described above.

[0035] 3. The above TiO2@MoS2 heterojunction substrate was dispersed in crystal violet ethanol solutions of different concentrations, soaked for 8 h, and then the substrate was removed and dropped onto a silicon wafer and dried at room temperature until the solution was completely evaporated.

[0036] In step one, the mass-to-volume ratio of Ti2AlN to KOH aqueous solution is 1 g:70 mL; the molar concentration of KOH aqueous solution is 10 M; and the particle size of Ti2AlN is 200 mesh.

[0037] The magnetic stirring described in step one: the magnetic stirring speed is 500 rpm and the stirring time is 10 min; The washing and drying process described in step one involves washing three times with deionized water and then drying at 60 ℃ for 8 hours. The mixed solution described in step two contains 30 mg (NH4)2MoO4 and 60 mg CH4N2S, and is stirred for 30 min until completely dissolved; The volume of crystal violet ethanol solution in step three is 4 mL; The amount of solution aspirated in step three is 300 μL; The drying time for the solution described in step three is 20 minutes; In step three, 5 mg of the substrate was added to the crystal violet ethanol solution.

[0038] The TiO2@MoS2 dual-semiconductor heterojunction SERS substrate material prepared in this embodiment can be used for organic dye detection. Laser Raman spectroscopy testing of this material is performed as follows: TiO2@MoS2 dual semiconductor heterojunction SERS substrate material was dispersed in 4 mL of crystal violet ethanol solution for 8 h. The substrate was then removed from the solution using a pipette, and 200 μL of crystal violet ethanol solution was added dropwise. The substrate was dried at room temperature for 20 min, and then laser Raman spectroscopy was performed under the conditions of laser wavelength of 532 nm, exposure time of 10 s, and laser power of 10%.

[0039] The TiO2@MoS2 dual-semiconductor heterojunction SERS substrate material prepared in this embodiment was subjected to X-ray diffraction phase analysis (XRD) (as shown in the figure). Figure 1As shown in the figure, the XRD pattern shows characteristic peaks of TiO2 and MoS2, which correspond to the TiO2 crystal plane of PDF#21-1272 and the MoS2 crystal plane of PDF#37-1492, respectively, proving the existence of pure TiO2 and MoS2 phases in the substrate material.

[0040] The TiO2@MoS2 dual-semiconductor heterojunction SERS substrate material prepared in this embodiment is in powder form and was characterized by scanning electron microscopy (SEM) and transmission electron microscopy (TEM). Figure 2 , Figure 3 ( Figure 3 for Figure 2 (A local magnification) shows that the prepared TiO2 is formed by numerous interlaced fine ribbon-like structures, with a line diameter of approximately 200 nm and a single line length of approximately 10 μm. From Figure 4 As can be seen, MoS2 nanosheets are bonded to the surface of TiO2 nanoribbons, and the two materials are tightly bonded to form a TiO2@MoS2 dual semiconductor heterojunction.

[0041] The TiO2@MoS2 dual-semiconductor heterojunction SERS substrate material prepared in this embodiment exhibits excellent SERS performance, with a minimum detection limit for crystal violet reaching 10. -8 M (see) Figure 5 Raman spectra at 15 different points on the same sample (see) Figure 6 ) and at 1178 cm -1 Raman peak intensity map at (see) Figure 7 As shown in the figure, the obtained TiO2@MoS2 dual semiconductor heterojunction exhibits good signal uniformity and repeatability as a SERS substrate for detecting crystal violet, with a peak value of 1178 cm⁻¹. -1 The relative standard deviation (RSD) of the Raman peak intensity repeated tests at the concentration was 9.19%. Its signal intensity decreased linearly with increasing negative logarithm of concentration (see...). Figure 8 ).

[0042] This embodiment uses a simple hydrothermal method to prepare a dual-semiconductor heterojunction SERS substrate material composed of TiO2 nanoribbons and MoS2 nanosheets. By combining two semiconductors, TiO2 and MoS2, as the substrate, the problem of poor repeatability, complex preparation method and low sensitivity of existing non-metallic SERS substrates is solved.

[0043] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A dual-semiconductor heterojunction SERS substrate material composed of TiO2 nanoribbons and MoS2 nanosheets, characterized in that: The substrate material is an inorganic dual-semiconductor composite powder without noble metal doping, consisting of a tightly packed heterogeneous interface formed by a three-dimensionally interwoven TiO2 nanoribbon framework in the shape of a ball of yarn and MoS2 nanosheets uniformly grown in situ on its surface. The TiO2 nanoribbons have a diameter of 100–500 nm and a line length of less than 20 μm. The MoS2 nanosheets have a single-sheet diameter of 10–30 nm and are free of free aggregated particles. The substrate phase contains pure TiO2 and pure MoS2, and the XRD patterns match the standard cards PDF#21-1272 and PDF#37-1492, respectively, with no impurity peaks. The substrate improves the separation efficiency of photogenerated electron-hole pairs by relying on the band matching effect between TiO2 and MoS2. When the substrate material is used for crystal violet SERS detection, the lowest detection limit reaches 1 × 10⁻⁻⁻⁶. 8 mol / L; with 1178 cm⁻¹ as the quantitative characteristic peak, the relative standard deviation (RSD) of multiple tests on the same sample was 9.19%, and the negative logarithmic linear correlation coefficient (R²) between Raman peak intensity and crystal violet concentration was 0.9743.

2. The dual-semiconductor heterojunction SERS substrate material composed of TiO2 nanoribbons and MoS2 nanosheets according to claim 1, characterized in that: The substrate material has a microstructure consisting of a large number of TiO2 nanoribbons interwoven to form a porous network structure resembling a tuft of yarn, with MoS2 nanosheets completely coated and attached to the surface of the nanoribbons, and the two phases are tightly bonded at the interface.

3. A method for preparing a dual-semiconductor heterojunction SERS substrate material composed of TiO2 nanoribbons and MoS2 nanosheets as described in any one of claims 1 to 2, characterized in that, Includes the following steps: Step 1: Alkali etching to prepare a yarn-like potassium titanate precursor: Ti₂AlN powder was added to a KOH aqueous solution, magnetically stirred until homogeneous, and then sealed in a hydrothermal reactor. The reaction was carried out at 120–160 °C for 12–36 h. The reaction product was washed with deionized water and dried to obtain a ball-shaped K₂Ti₈O₃. 17 ; Step 2: In-situ hydrothermal vulcanization composite preparation TiO2@MoS2 heterojunction substrate: Prepare a mixed aqueous solution containing ammonium molybdate and thiourea, wherein the mass ratio of (NH4)2MoO4 to CH4N2S is fixed at 1:2; The K2Ti8O obtained in step one... 17 The powder is dispersed into the mixed solution and stirred until the solid is completely dissolved. Then it is transferred to a hydrothermal reactor and hydrothermally reacted at 180–200 °C for 18–24 h. After washing and drying, the product yielded a TiO2@MoS2 dual semiconductor heterojunction SERS substrate. Step 3: SERS Sample Pretreatment: TiO2@MoS2 substrates were dispersed in crystal violet ethanol solutions of different concentrations and soaked at room temperature for 4–8 h. The substrate dispersion was then drop-coated onto a silicon wafer and allowed to stand at room temperature until the solvent completely evaporated to obtain the sample to be tested.

4. The preparation method according to claim 1, characterized in that, In step one, the mass-volume ratio of Ti2AlN powder to KOH is (0.5-2 g):(50-100 mL); the magnetic stirring speed is 500-2000 rpm, and the stirring time is 5-20 min.

5. The preparation method according to claim 5, characterized in that, In step one, the molar concentration of the KOH aqueous solution is 10 M; the particle size of Ti2AlN is 200 mesh.

6. The preparation method according to claim 1, characterized in that, In step two, the raw material ratio of the mixed aqueous solution is as follows: (NH4)2MoO4 is added at 10-50 mg, CH4N2S is added at 20-100 mg, and the mixture is stirred at room temperature for 10-40 min until the solid is completely dissolved.

7. The application of a dual-semiconductor heterojunction SERS substrate material composed of TiO2 nanoribbons and MoS2 nanosheets as described in any one of claims 1 to 2, characterized in that, The substrate is used for rapid, non-destructive qualitative and quantitative detection of trace amounts of the organic dye crystal violet in environmental and food systems using surface-enhanced Raman spectroscopy.

8. The application according to claim 6, characterized in that, During the test, the sample to be tested was subjected to laser Raman spectroscopy under the conditions of a laser wavelength of 532 nm, an exposure time of 10 s, and a laser power of 10%.