A SERS substrate based on noble metal nanoparticles and a to-be-detected molecule cooperative assembly and a preparation method and application thereof
By simultaneously assembling noble metal nanoparticles and target molecules at the liquid-liquid interface to form a dense monolayer structure, the problem of low probability of target molecules entering hotspot regions is solved, achieving highly sensitive and reliable SERS detection, which is suitable for rapid drug screening.
Patent Information
- Application Number
- CN202611364933.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-24
AI Technical Summary
Existing SERS detection technologies, while constructing hotspot structures, have a low probability of target molecules entering the hotspot region. Especially in complex samples, they are easily affected by molecular diffusion restriction, competitive adsorption, and signal interference, leading to a decrease in detection limit and repeatability, making it difficult to meet the needs of rapid drug screening.
By simultaneously assembling noble metal nanoparticles and analyte molecules at the liquid-liquid interface to form a dense monolayer structure, the analyte molecules are confined to the hot spot region of the nano-gap. Combined with multidimensional spectral matching identification methods, the sensitivity and reliability of detection are improved.
This method increases the contact probability between the target molecule and the plasmon enhancement region, enhances the SERS signal response, and reduces the influence of peak overlap and background interference through multidimensional spectral matching identification, thereby improving the sensitivity and reliability of drug detection in complex systems.
Smart Images

Figure CN123155504A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of analytical detection technology, specifically to a SERS substrate based on the co-assembly of noble metal nanoparticles and analyte molecules, its preparation method, and its application. Background Technology
[0002] Surface-enhanced Raman scattering (SERS) is a spectroscopic analysis technique that combines high sensitivity, rapid response, and molecular fingerprinting capabilities. Its enhancement effect primarily originates from localized surface plasmon resonances on the surfaces of noble metal nanostructures. When the analyte molecule is located in the electromagnetic enhancement region formed by nanostructures such as gold or silver, its Raman scattering signal can be significantly amplified, thus achieving highly sensitive detection of trace molecules. Compared with analytical methods such as fluorescence, mass spectrometry, and chromatography, SERS offers advantages such as fast detection speed, small sample volume, relatively simple pretreatment process, and the ability to provide molecular structure information. Therefore, it has received widespread attention in fields such as environmental pollutant monitoring, food safety analysis, biomedical diagnostics, drug quality control, and screening. Especially in rapid drug screening, target molecules are often characterized by low content, diverse types, similar structures, and urgent need for on-site detection. While traditional laboratory analytical methods offer high accuracy, they often rely on complex instruments and lengthy analytical procedures, making it difficult to meet the requirements of rapid, portable, and initial screening applications. SERS technology can directly reflect the vibrational structure information of molecules through characteristic Raman peaks, and provides high molecular recognition ability while achieving low concentration response. Therefore, it is considered one of the important candidate technologies for rapid on-site drug detection.
[0003] SERS detection performance primarily depends on the construction of isotropic "hot spots" on the substrate and the spatial matching degree between the analyte and the hot spot regions. Typically, the nano-interstic spaces formed between noble metal nanoparticles generate strong local electromagnetic field enhancement, which is a key region for obtaining high SERS signals. Therefore, constructing nanoparticle assembly structures with high-density hot spots, good uniformity, and stability has always been a core issue in SERS substrate research. Compared to monodisperse nanoparticles, nanoparticle-assembled films can form numerous hot spots in the interparticle spaces, and the enhancement effect can be optimized by controlling particle size, morphology, spacing, and assembly method. Currently, common assembled SERS substrates often employ a method of first assembling noble metal nanoparticles on the surface of a solid substrate to form a thin film, and then immersing it in a solution of the analyte molecules for detection, i.e., the Soak detection mode. This method is simple to operate, has a wide range of applications, and facilitates the preparation of relatively stable solid SERS substrates. However, in this mode, the analyte molecules mainly rely on subsequent diffusion and adsorption to enter the nanoparticle spaces, and their efficiency in entering the hot spot region is easily affected by factors such as molecular charge, adsorption capacity, steric hindrance, solution environment, and substrate surface state. For molecules with weak adsorption capacity, limited diffusion, or insufficient interaction with the substrate surface, their effective enrichment is limited, often leading to problems such as insufficient signal intensity, limited detection limit, and decreased repeatability in practical detection. Therefore, how to increase the probability of target molecules entering the hotspot region while constructing hotspot structures is the key to further improving the detection performance of assembled SERS substrates.
[0004] For complex samples, the above problems are even more pronounced. Real-world samples often contain multiple drug components, excipients, diluents, metabolic byproducts, or other interfering substances. The adsorption capacity and Raman scattering cross-section of different components on the surface of metal nanostructures vary significantly, easily leading to competitive adsorption and selective signal enhancement. Certain strongly adsorbed or strongly Raman-responsive molecules may preferentially occupy hotspot regions, weakening or even masking the signal of low-concentration target drugs. Simultaneously, the Raman spectrum in a mixed system typically exhibits the superposition of characteristic peaks from multiple components. The characteristic peaks of different molecules may overlap, exhibit slight peak position shifts, change peak intensity ratios, or local peak shape variations, making traditional identification methods relying on single peak positions or manual comparisons difficult to accurately determine the presence of target molecules. For low-dose, high-risk drugs such as sufentanil and midazolam, their concentration in mixed samples may be low, and once coexisting with other drugs or additives, the target peak is more susceptible to interference from strong background and adjacent peaks.
[0005] Therefore, the detection of drug mixtures not only requires highly sensitive SERS-enhanced substrates, but also multidimensional identification methods that can adapt to complex spectral changes in order to improve the reliability and interpretability of detection results. Summary of the Invention
[0006] To address the aforementioned shortcomings in existing technologies, the present invention aims to provide a SERS substrate based on the co-assembly of noble metal nanoparticles and target molecules, along with its preparation method and applications. The SERS substrate enables the simultaneous assembly of target molecules and nanoparticles at the liquid-liquid interface, confining the molecules in situ within dynamically shrinking nano-interstitial hotspots. This solves the problem of detecting low-abundance component signals due to limited molecular diffusion and competitive adsorption in traditional immersion methods.
[0007] To achieve the above-mentioned objectives, the technical solution adopted by this invention is as follows: A SERS substrate based on the co-assembly of noble metal nanoparticles and analyte molecules is provided, comprising a substrate carrier and a noble metal nanoparticle film loaded on the surface of the substrate carrier. The noble metal nanoparticle film is a dense monolayer structure assembled from noble metal nanoparticles, and the analyte molecules are confined within the hot spot region of the nano gaps between the noble metal nanoparticles; the SERS substrate is prepared by co-assembling noble metal nanoparticles and analyte molecules at the liquid-liquid interface.
[0008] Preferably, the noble metal nanoparticles are Au@Ag core-shell nanocubes, comprising a gold nanosphere core and a silver shell; the particle size of the gold nanosphere core is 10-50 nm, and the thickness of the silver shell is 5-30 nm.
[0009] Preferably, the surface of the noble metal nanoparticles is coated with polyvinylpyrrolidone (PVP) ligand; the substrate carrier is any one of silicon wafer, glass plate, or quartz plate.
[0010] A method for preparing a SERS substrate is also provided, comprising the following steps: (1) Preparation of a dispersion of noble metal nanoparticles coated with PVP; (2) The noble metal nanoparticle dispersion, organic solvent and aqueous solution containing the analyte molecules are mixed to form a mixed system; (3) Add an inducer to the mixed system to drive noble metal nanoparticles to migrate to the water-oil interface and undergo interfacial self-assembly. During this process, the molecule to be tested is simultaneously confined in the gaps between nanoparticles to form an interfacial nanoparticle film. (4) The interfacial nanoparticle film is transferred to the surface of the substrate carrier and dried to obtain the SERS substrate.
[0011] Preferably, in step (2), the organic solvent is dichloromethane; in step (3), the inducing agent is n-hexane.
[0012] Preferably, the volume ratio of the noble metal nanoparticle dispersion, organic solvent, aqueous solution and inducer is 1:0.5-1:1-2:0.3-0.6.
[0013] The invention also provides an application of a SERS substrate in the detection of drug mixtures, the application including the use of the SERS substrate for SERS spectral acquisition and multidimensional spectral matching identification.
[0014] Preferably, the detection method includes the following steps: S1: Provide the SERS substrate, wherein the drug mixture molecules to be tested are confined in the SERS substrate; S2: Acquire SERS spectral signals using a Raman spectrometer; S3: Construct a multidimensional spectral matching algorithm model to intelligently identify and analyze the collected SERS spectra and determine whether the mixture contains the target drug component.
[0015] Preferably, the analysis process of the multidimensional spectral matching algorithm model in step S3 includes the following sub-steps: S3-1: Preprocessing of standard SERS spectra and mixture SERS spectra of single-target drugs; S3-2: Calculate the matching score from three dimensions: peak position matching, peak intensity ratio matching, and local waveform similarity matching; S3-3: The scores of the three dimensions are weighted and fused to obtain the overall confidence level. If the overall confidence level is higher than the set threshold, the target drug molecule is determined to exist.
[0016] Preferably, the drug includes one or more of sufentanil and midazolam.
[0017] The beneficial effects of this invention are as follows: This invention introduces the analyte molecule into the assembly process of Au@Ag core-shell nanocubes, allowing the target molecule to accumulate in the interparticle spaces and hotspot regions while forming a dense monolayer structure within the nanoparticles. This increases the contact probability between the molecule and the plasmon enhancement region, effectively enhancing the SERS signal response. Furthermore, addressing issues such as peak overlap, peak intensity variations, and background interference in mixture spectra, this invention establishes a multidimensional spectral matching and identification method by combining peak position matching, peak intensity ratio matching, and local spectral similarity analysis. This method can evaluate the retention of target molecule characteristic peaks in mixtures from multiple perspectives and determine the presence of the target drug through comprehensive confidence. Compared to single-peak interpretation methods, this strategy exhibits better stability and anti-interference capabilities, improving the sensitivity and reliability of drug detection in complex systems. Attached Figure Description
[0018] Figure 1The following are the characterization and assembly of Au@Ag core-shell nanocubes in the embodiments of the present invention; wherein, (A) the assembly process of gold and silver core-shell nanocubes; (B) the characterization of gold and silver core-shell nanocubes; (C) the absorption spectrum of gold and silver core-shell nanocubes; (D) the characterization of gold and silver core-shell cubic monolayer films, and the inserted figure is elemental imaging. Figure 2 This invention illustrates the effect of particle spacing variation on local electric field distribution during the interface assembly process of Au@Ag NCs in this embodiment; where (A) is a large gap; (B) is a medium gap; and (C) is a small gap; the left side is a schematic diagram of the assembly structure; and the right side is an electric field distribution cloud map of the XY plane and XZ plane obtained from FDTD simulation. E max Represents the maximum amplitude of the local electric field. E 0 represents the polarization direction of the incident photoelectric field. k The wave vector of the incident light; reducing the gap between particles enhances the near-field coupling of the plasma, which significantly improves the electromagnetic hotspot signal within the nanogap. Figure 3 This invention provides a comparison of the detection performance of probe molecules using different detection methods in various embodiments; wherein, (A) the molecular structure and SERS spectrum of the cationic probe molecule R6G; (B) the molecular structure and SERS spectrum of the anionic probe molecule Scarlet; and (C) the molecular structure and SERS spectrum of the drug molecule benzimidazole. Figure 4 The following are SERS spectra of the mixtures in the embodiments of the present invention (comparing the differences between the conventional immersion mode and the co-assembly mode in the detection of cation probe mixtures); wherein, immersion mode: (A) crystal violet and rhodamine 6G (CV and R6G); (B) malachite green and rhodamine 6G (MG and R6G); (C) malachite green and crystal violet (MG and CV); co-assembly mode: (D) crystal violet and rhodamine 6G (CV and R6G); (E) malachite green and rhodamine 6G (MG and R6G); (F) malachite green and crystal violet (MG and CV); Figure 5 illustrates the co-assembled SERS strategy used for trace detection and mixture identification of drug molecules in this embodiment of the invention; wherein, (A) SERS spectra of midazolam and sufentanil; (B, C) SERS spectra of midazolam and sufentanil at different concentrations; (D) SERS spectra of sufentanil / midazolam mixture; (E) Flowchart of multidimensional spectral matching algorithm; (F) Comparison of standard spectrum of midazolam and mixture spectrum and selection of characteristic peaks; (G) Multidimensional matching score and comprehensive confidence in midazolam mixture identification; Figure 6 These are scanning electron microscope (SEM) images of Au@Ag gold-silver core-shell nanocrystal monolayers prepared with probe molecule solutions of different concentrations in this embodiment of the invention; wherein, (A) 10 -6 M; (B) 10-5 M; (C) 10 -4 M; Figure 7 The SERS spectra and molecular models of different substances in the embodiments of the present invention are shown; wherein, (A) crystal violet (CV); (B) malachite green (MG); Figure 8 The SERS spectra and molecular models of different substances in the embodiments of the present invention are shown; wherein, (A) Sunset Yellow; (B) Prussian Blue; Figure 9 The SERS spectra and molecular models of different substances in the embodiments of the present invention are shown; wherein, (A) ampicillin; (B) avanafil; Figure 10 The SERS spectrum of 4-mercaptobenzoic acid in the embodiments of the present invention; Figure 11 For the soaking time in embodiment of the present invention, (A) 4 mercaptobenzoic acid (4) (MBA), (B) Effects of Rhodamine 6G (R6G) on SERS signal; Figure 12 In this embodiment of the invention, a co-assembled SERS strategy is used for trace detection of drug molecules and identification of mixtures; wherein, (A) comparison of the standard spectrum of sufentanil and the spectrum of the mixed system, and selection of characteristic peaks; (B) multidimensional matching score and overall confidence level for identification of mixed samples; Figure 13 In this embodiment of the invention, a co-assembled SERS strategy is used for trace detection of drug molecules and identification of mixtures; wherein, (A) the comparison between the standard crystal violet spectrum and the spectrum of the mixed system, and the selection of characteristic peaks; (B) the multidimensional matching score and overall confidence level of mixed sample identification. Detailed Implementation
[0019] The specific embodiments of the present invention are described below to enable those skilled in the art to understand the present invention. However, it should be understood that the present invention is not limited to the scope of the specific embodiments. For those skilled in the art, various changes are obvious as long as they are within the spirit and scope of the present invention as defined and determined by the appended claims. All inventions utilizing the concept of the present invention are protected.
[0020] Example 1. Materials and Methods 1.1 Preparation of 10 nm gold spheres 10 nm gold nanospheres were prepared using a seed-mediated growth method. First, 0.6 mL of NaBH4 solution (10 mM) was rapidly injected into 10 mL of a mixed solution containing HAuCl4 (0.25 mM) and CTAB (0.1 M), and thoroughly mixed at room temperature to allow Au³⁺ to grow. + The seeds were rapidly reduced to form a gold seed solution. The resulting seed solution was then allowed to stand at room temperature for 3 hours to age, in order to improve seed stability and ensure the controllability of the subsequent growth process.
[0021] Subsequently, 150 μL of the aged gold seed solution was added to a 30 mL scintillation bottle, followed by the addition of 6 mL of CTAC solution (0.2 M) and 4.5 mL of ascorbic acid (AA) solution (0.1 M). After thorough mixing, 6 mL of HAuCl4 solution (0.5 mM) was rapidly injected. Under the combined action of CTAC as a surfactant and AA as a mild reducing agent, gold ions continued to be reduced and deposited on the seed surface, thus growing into gold nanospheres of approximately 10 nm. After the reaction was completed, the resulting gold nanosphere solution was centrifuged at 14500 rpm for 30 min, and the centrifugation and washing were repeated twice to remove excess surfactant and unreacted precursors. Finally, the precipitate was redispersed in 3 mL of deionized water to obtain a 10 nm gold nanosphere stock solution, which was used for the subsequent preparation of Au@Ag core-shell nanocubes.
[0022] 1.2 Preparation of gold and silver core-shell nanocubes 10 nm gold nanospheres were used as seeds and obtained through silver shell epitaxial growth. Specifically, 100 μL of the prepared 10 nm gold nanosphere solution and 0.25 mL of AgNO3 solution (10 mM) were added to 10 mL of CTAC solution (20 mM). The mixture was stirred at 65 °C for 15 min to ensure thorough mixing of the silver precursor, gold seeds, and surfactant. Subsequently, 0.25 mL of ascorbic acid solution (0.1 mM) was added as a reducing agent, and the reaction temperature was adjusted to 60 °C. The mixture was stirred continuously for 4 h to promote Ag... + Controlled reduction and anisotropic epitaxial growth occur on the surface of gold nanospheres.
[0023] In this process, CTAC not only stabilizes the nanoparticles but also regulates the growth rate of the silver shell on different crystal faces, thereby inducing the formation of Au@Ag core-shell nanostructures with a cubic morphology. After the reaction is complete, the resulting product is collected by centrifugation to remove unreacted AgNO3, free surfactants, and other small molecule impurities. Finally, the precipitate is redispersed in 1 mL of CTAC solution (20 mM) to obtain an Au@Ag NCs dispersion, which is then stored for later use.
[0024] 1.3 Assembly of Nanoparticles The assembly of Au@Ag NCs was achieved using a liquid-liquid interface-induced assembly method. First, the original surfactant on the nanoparticle surface was converted into a polyvinylpyrrolidone (PVP) coating layer via centrifugation displacement, resulting in PVP-modified Au@Ag NCs. Specifically, the nanoparticles were transferred to centrifuge tubes and centrifuged at 5000-10000 rpm for 10 minutes. After centrifugation, the supernatant was removed. A PVP solution in ethanol (0.01%-10% by mass) was added to the centrifuge tubes and sonicated for 1-10 minutes. The mixture was then centrifuged again to remove excess PVP solution from the supernatant. Finally, the precipitate was dispersed in 1-10 mL of ethanol solution to obtain the PVP-modified Au@Ag NCs. The introduction of PVP helps improve the colloidal stability of the nanoparticles in the organic / aqueous system and promotes their ordered arrangement at the liquid-liquid interface.
[0025] Subsequently, the PVP-coated nanoparticle dispersion was mixed with 0.7 mL of dichloromethane in a centrifuge tube. 2 mL of deionized water was added to the system, followed by the detection molecule. After vigorous shaking for 10 s, the nanoparticles redistributed between the aqueous and organic phases. Then, 0.5 mL of n-hexane was added, and by adjusting the interfacial energy, the nanoparticles were driven to the water-n-hexane interface. As the nanoparticles gradually accumulated and aligned at the interface, a densely packed monolayer nanoparticle film was formed.
[0026] Finally, the nanoparticle monolayer film formed at the water-n-hexane interface was transferred to the silicon wafer surface using a peel-over transfer method. After the transfer was completed, the substrate was left to air dry naturally, allowing the nanoparticle monolayer film to stably adhere to the silicon wafer, resulting in an Au@Ag NCs substrate for SERS detection.
[0027] 1.4 Introduction to the Algorithm Model 1.4.1 Complete and fixed parameters for spectral preprocessing All spectra in this study underwent a standardized preprocessing procedure, with all parameters fixed as follows: Baseline correction: Iterative adaptive polynomial fitting, polynomial order = 5, number of iterations = 30; Smoothing and noise reduction: Seven-point moving average filter, sampling window width = 7 Raman sampling points; Intensity normalization: Based on the maximum signal intensity of a single spectrum, the full spectrum signal is mapped to the [0, 1] interval; Feature peak selection threshold: Only signal peaks with a signal-to-noise ratio (SNR) ≥ 3 are retained; those below this threshold are considered baseline noise and are directly removed.
[0028] 1.4.2 Calculation Formulas and Variable Definitions for Three-Dimensional Matching Peak position matching score S p Calculation formula: S p = N match / N total Variable description: N total The total number of characteristic peaks pre-extracted from the standard reference spectrum; the standard spectra of midazolam and sufentanil each contain 10 characteristic peaks; N match The number of characteristic peaks that successfully match the test spectrum of the mixture with the standard spectrum; Matching criteria: The difference in Raman shift between the target peak and the standard characteristic peak is ≤ 8 cm. - ¹, is considered a successful match; Score range: 0 ≤ S p ≤ 1.
[0029] Peak intensity ratio matching score S i Calculation formula: S i = Variable description: I mix,k : The signal intensity of the k-th matching characteristic peak in the mixture spectrum; I mix,max : Maximum signal intensity across the full spectrum of the mixture; I ref,k : The signal intensity corresponding to the k-th characteristic peak in the standard reference spectrum; I ref,max : Maximum signal intensity across the entire standard reference spectrum; Score range: 0 ≤ S i ≤ 1, the closer the value is to 1, the higher the consistency of the relative intensity distribution of the peak.
[0030] Local waveform similarity score S w (Cosine similarity) Calculation formula: S w = Variable description: f mix,k(x) The k-th matching peak is 15 cm to the left and right.- ¹The local spectral vector of the mixture within the window; f ref,k(x) The k-th matching peak is 15 cm to the left and right. - ¹The local spectral vector of the standard reference spectrum within the window; x: Raman displacement corresponding to each sampling point within the local window; Score range: 0 ≤ S w ≤ 1, the closer the value is to 1, the higher the local peak shape matching degree.
[0031] Total confidence fusion calculation formula: Conf = w p ×S p + w i ×S i + w w ×S w w p + w i + w w = 1 Variable description: Conf: Overall confidence score after multidimensional matching fusion; w p Peak position matching score weight; w i Peak intensity ratio matching score weight; w w Local waveform similarity score weights; The optimal weight combination in this study is: w p = 0.4, w i = 0.3, w w = 0.3; Positive detection threshold: Conf ≥ 0.6. If the value is greater than or equal to the threshold, the sample is determined to contain the target drug.
[0032] To achieve intelligent identification of target components in drug mixtures, this study constructs an algorithm model based on SERS spectral multidimensional feature matching. This model uses the standard SERS spectrum of a single-component drug as a reference spectrum and the SERS spectrum of the mixture sample as the spectrum to be detected. Through unified data preprocessing, feature peak extraction, multidimensional matching scoring, and comprehensive confidence assessment, it determines the presence of target molecules in the mixture.
[0033] First, the input reference spectrum and mixture spectrum undergo consistency preprocessing, including spectral reading, baseline correction, smoothing and noise reduction, and intensity normalization, to reduce the impact of background drift, noise fluctuations, and overall signal strength differences on the matching results. Based on this preprocessing, characteristic peaks are extracted from the reference spectrum, and representative Raman peaks are selected as the spectral fingerprints of the target molecule. The selection of characteristic peaks primarily considers peak intensity, peak prominence, and peak position distribution to avoid interference from weak noise peaks or non-characteristic background peaks in the identification results.
[0034] Subsequently, the algorithm performs matching analysis between the mixture spectrum and the reference spectrum from three dimensions. First, peak position matching is performed, determining whether a corresponding peak in the reference spectrum can be found within a similar wavenumber range in the mixture spectrum. A certain wavenumber tolerance is set during the matching process to accommodate slight peak position shifts that may occur in the experiment. Second, peak intensity ratio matching is performed, comparing the relative intensity relationship between characteristic peaks in the reference spectrum with the relative intensity relationship of the corresponding peaks in the mixture. This indicator can reduce the impact of overall signal strength variations and reflect whether the characteristic peak combinations of the target molecule remain similar. Third, local spectral similarity matching is performed, selecting a local spectral window near the target characteristic peak and calculating the waveform similarity between the reference spectrum and the mixture spectrum within the local region, thereby further determining whether the mixture retains the local fingerprint characteristics of the target molecule.
[0035] After obtaining peak position matching scores, peak intensity ratio matching scores, and local spectral similarity scores, the algorithm uses weighted fusion to obtain a comprehensive confidence score. If the comprehensive confidence score is higher than a set threshold, the target molecule is determined to be present in the mixture; if it is lower than the threshold, it is determined not to be detected. The model output includes information such as the target molecule name, whether it was detected, the comprehensive confidence score, matching scores for each dimension, the number of matching peaks, peak position deviation, and spectral similarity. Compared with traditional methods that rely on manual interpretation of a single feature peak, this algorithm can simultaneously consider peak position, relative intensity, and local spectral shape information, improving the reliability and accuracy of identification in mixture spectra with peak overlap, peak intensity variations, or background interference.
[0036] 2. Results and Discussion Figure 1 The structural characterization, optical properties, and interfacial assembly process of Au@Ag nanocubes (Au@Ag NCs) are presented. To construct a SERS-active substrate with high-density hotspots, CTAC-stabilized Au@Ag NCs were first converted to a PVP-coated state to improve their dispersibility in dichloromethane and promote their ordered assembly at the water / oil interface. Figure 1As shown in Figure A, PVP-coated Au@Ag NCs are first dispersed in dichloromethane, followed by the addition of an aqueous phase to form a water / dichloromethane interface. Then, the detection molecules are added to the aqueous phase, allowing them to contact the nanoparticles before assembly. After vigorous shaking and the addition of n-hexane, the nanoparticles rapidly migrate to the liquid / liquid interface and assemble to form a monolayer film. After removing the n-hexane, the interfacial monolayer film can be transferred to the silicon wafer surface using a dip-coating method for subsequent SERS testing. Unlike traditional post-film formation immersion adsorption methods, this method allows the detection molecules to participate in the interfacial migration and stacking process of the nanoparticles, thereby being simultaneously confined within the nanopores between the particles during monolayer film formation. This dynamic trapping process helps increase the probability of weakly adsorbed molecules entering the SERS hotspot region and provides a basis for reducing the competitive adsorption effects in mixture detection.
[0037] After clarifying the assembly strategy, the structure of Au@Ag NCs was further characterized. TEM images showed that the obtained nanoparticles had a relatively uniform cubic morphology, clear edges and corners, and a narrow size distribution. Figure 1 (Image B). High-resolution TEM images further revealed the presence of an Au core within the particle, surrounded by a well-crystalline Ag shell with clearly visible lattice fringes, indicating the successful construction of an Au@Ag core-shell nanocube. Since the sharp corners and edges of the Ag shell can induce strong localized electromagnetic fields, this structure provides effective plasmon units for subsequent SERS enhancement. Subsequently, the optical properties of the nanoparticles before and after ligand conversion were investigated using UV-Vis absorption spectroscopy. Figure 1 As shown in Figure C, both CTAC-coated and PVP-coated Au@Ag NCs exhibit characteristic plasmon absorption peaks at approximately 346, 394, and 485 nm, indicating that the main optical response of the nanocubes is preserved after ligand exchange. The absorption in the long-wavelength region changes slightly after PVP coating, possibly due to alterations in the dielectric environment of the particle surface and differences in interparticle interactions. Overall, the ligand exchange process does not significantly disrupt the morphology and plasmon properties of Au@Ag NCs, suggesting their suitability for further interfacial assembly.
[0038] Finally, the Au@Ag NCs film transferred to the silicon wafer surface was characterized by SEM. Figure 1 As shown in Figure D, the nanocubes form a continuous and dense two-dimensional monolayer film on the substrate surface, with closely packed particles generating numerous nano-interstic gaps. These gaps can serve as effective SERS hotspots, providing a structural basis for molecular signal enhancement. Elemental imaging results in the inset show that Au and Ag signals coexist within a single nanocube and exhibit corresponding spatial distributions, further confirming the formation of the Au@Ag core-shell structure. These results demonstrate that the prepared Au@Ag NCs possess regular morphology, stable optical response, and good interfacial assembly capabilities, making them suitable as an active substrate for subsequent molecularly confined SERS detection.
[0039] Figure 2 Further FDTD simulations were used to analyze the effect of interparticle spacing changes on the local electric field distribution of Au@Ag NCs during interfacial assembly, to verify the feasibility of molecular confinement in hotspot regions during interfacial film formation. In the model, Au@Ag NCs are located near the water / oil interface, and yellow symbols represent probe molecules in the solution. It should be noted that... Figure 2 The arrangement of nanoparticles was established based on a combination of theoretical structure and experimental observation: theoretically, nanocubes with square projections tend to arrange themselves side-by-side at the interface in a face-to-face adjacent manner; simultaneously, Figure 1 The local area marked by the red dashed box in D also shows the side-by-side assembly characteristics of adjacent nanocubes, providing experimental evidence for this simulation model. As interface assembly proceeds, the nanocubes gradually accumulate at the interface from a relatively dispersed state and form a dense arrangement, thereby reducing the gaps between particles and inducing stronger plasmon coupling.
[0040] like Figure 2 As shown in Figure A, when the distance between adjacent Au@Ag NCs is large, the electric field is mainly distributed in the edge and corner regions of individual nanocubes, the interparticle coupling is weak, and the electric field enhancement in the gap region is limited. At this time, although the probe molecules are already present in the aqueous phase and close to the nanoparticle surface, the SERS enhancement that can be obtained is relatively weak because the hot spots have not yet fully formed. As the assembly process continues, the nanocubes move closer together at the interface and undergo ordered stacking, and the interparticle spacing decreases significantly. Figure 2 As shown in Figure B, significant electromagnetic coupling begins to occur between adjacent nanocubes, and the local electric field gradually concentrates in the interparticle gap region. Compared with the dispersed state, the hot spot intensity is significantly increased in this stage, indicating that the interfacial compression and particle stacking processes can effectively promote the formation of nano-gap hot spots. For probe molecules in the aqueous phase, this dynamic process helps them to be introduced into or confined near the hot spot during gap formation.
[0041] When Au@Ag NCs are further assembled into a dense monolayer, the interparticle spacing reaches its minimum, and the electric field enhancement is most significant. Figure 2 (C). Simulation results show that the strong electric field is mainly localized in the narrow gaps between adjacent nanocubes, indicating that densely packed Au@Ag NCs can generate high-density, high-intensity SERS hotspots. More importantly, in the actual assembly process, the probe molecules are pre-dispersed in the aqueous phase and participate in the interfacial assembly together with the nanoparticles during migration and approach. Therefore, as the nanogap gradually shrinks, the probe molecules can be synchronously held within the hotspot region, rather than relying entirely on their adsorption affinity to the metal surface.
[0042] The simulation results provide theoretical support for the molecular trapping mechanism in this work. In traditional post-film formation immersion methods, molecules need to diffuse into the narrow nano-gap formed by the film, a process easily limited by steric hindrance, surface adsorption capacity, and competitive adsorption. In contrast, this strategy utilizes the dynamic gap shrinkage during the interfacial assembly process to introduce probe molecules into the vicinity of nanoparticles before hotspot formation, achieving in-situ confinement during film formation. Therefore, the simulation results not only demonstrate the excellent electromagnetic enhancement capability of the dense monolayer Au@Ag NCs, but also indicate that the interfacial assembly process can provide higher hotspot accessibility for weakly adsorbed molecules and low-abundance components in complex mixtures.
[0043] Using the cationic probe molecule R6G as a model, the effect of its concentration on the interface assembly morphology of Au@Ag NCs was investigated. Figure 6 As shown, when the R6G concentration is 10... -6 At M, Au@Ag NCs can still form a continuous and dense two-dimensional monolayer film, indicating that low concentrations of R6G have virtually no effect on the interfacial assembly process. However, when the concentration increases to 10... -5 At M, local voids began to appear in the assembled film, indicating that higher concentrations of R6G could interfere with the tight packing of nanoparticles at the interface to some extent. Further increasing to 10... -4 After M, the intramembrane porosity significantly increased, and the assembly continuity decreased, indicating that high concentrations of R6G have a more significant impact on monolayer membrane formation. Therefore, at 10 -5 Within the R6G concentration range below M, the interfacial assembly morphology of Au@Ag NCs remains basically stable, which can meet the requirements of subsequent SERS detection.
[0044] To verify the SERS detection performance of the co-assembly strategy for different types of molecules, the cation probe R6G, the anion probe scarlet, and the drug molecule benzimidazole were selected as representative molecules for testing, and compared with the traditional immersion method. The immersion method involves first assembling Au@Ag NCs into a film and transferring it to a silicon wafer surface, then immersing the substrate in a solution of the analyte for adsorption and detection. The co-assembly method, on the other hand, involves simultaneously introducing the analyte during the Au@Ag NCs interface assembly process, allowing the molecule to be confined in situ within the interparticle spaces as the nanoparticles approach and hotspots form.
[0045] like Figure 3 As shown in Figure A, for the cationic molecule R6G, the SERS signal obtained by the co-assembly method is significantly stronger than that obtained by the immersion method, and at 611 cm⁻¹... - ¹ It exhibits a good concentration response at characteristic peaks. Similarly, the anionic molecule scarlet also shows a stronger characteristic peak signal under co-assembly conditions, especially at 1361 cm⁻¹. -The Raman peak at position ¹ is significantly enhanced ( Figure 3 (B) This demonstrates that this method is not only applicable to positively charged molecules but can also effectively capture negatively charged molecules. Further, taking the drug molecule benzimidazole as an example, the co-assembly method also significantly improved its SERS detection signal, and a clear 778 cm⁻¹ could be observed even at low concentrations. - ¹Characteristic peaks ( Figure 3 (C) In contrast, the signals obtained by the immersion method are generally weaker, indicating that molecules have difficulty fully diffusing into the narrow hotspot region after film formation. The enhanced advantage of the co-assembly method mainly comes from the dynamic molecular trapping mechanism during the interfacial assembly process. As nanoparticles gradually approach each other from a dispersed state to form a dense monolayer film, the analyte molecules are pre-existing in the aqueous phase and can be synchronously confined to the hotspot region as the interparticle gaps shrink. Therefore, this method reduces the dependence of detection performance on the adsorption capacity of molecular surfaces and the ability to diffuse into the nano-gap, thus exhibiting higher detection efficiency for molecules with different charge types and structures.
[0046] Furthermore, to further verify the universality of this strategy, CV and MG of other cationic molecules were tested respectively. Figure 7 Sunset Yellow and Bruce Blue (anionic molecules) Figure 8 ), and the drug molecules ampicillin and avanafil ( Figure 9 The same comparison was performed. The results showed that, compared to the immersion method, the co-assembly method consistently yielded stronger SERS characteristic signals, further demonstrating that this method is suitable for the efficient detection of various types of molecules. Furthermore, the same results were obtained for chemically bonded 4-MBA molecules. Figure 10 It should be noted that at higher concentrations, the number of molecules that can accommodate or effectively contribute to the SERS signal within the hotspot region tends to saturate. Further increasing the analyte concentration does not further enhance the characteristic peak intensity in the co-assembly mode, indicating that the detection signal is mainly controlled by the hotspot confinement capacity and the degree of effective hotspot occupancy. Furthermore, for the immersion mode, the immersion time also affects the test results. Figure 11 As time progressed, the detection signal of the substrate for molecules first increased and then decreased, which may be due to the nanoparticles detaching from the silicon wafer carrier caused by prolonged immersion.
[0047] Figure 4 The differences between the traditional immersion mode and the co-assembly mode in the detection of cation probe mixtures were compared. Figure 4 In the middle, A and C represent the SERS spectra of the R6G+CV, R6G+MG, and CV+MG mixed systems under immersion mode, respectively. It can be seen that the mixture spectra are not a simple superposition of the individual component spectra, but exhibit obvious molecular dependence. Figure 4The A, R6G+CV hybrid system mainly exhibits the characteristic signal of CV, while R6G has a 611 cm⁻¹ characteristic signal. - ¹The characteristic peaks are significantly suppressed; Figure 4 The 1615 cm of the MG in the B, R6G+MG hybrid system. - ¹The characteristic peaks dominate, and the R6G signal is also severely masked; Figure 4 The spectrum of the C, CV+MG mixed system also showed uneven signal contribution, indicating that there are obvious competitive adsorption and hot spot occupancy differences among different molecules under immersion mode.
[0048] In comparison, Figure 4 The results for the same mixture in the co-assembly mode are shown in Figure 4 (DF). In Figure 4, the R6G+CV mixture simultaneously retains 611 cm⁻¹ of R6G. - ¹Characteristic peak and CV at 1385 cm⁻¹ - ¹Characteristic peak; Figure 4 In the E, R6G+MG mixture, a 611 cm⁻¹ of R6G can be observed simultaneously. - ¹ and MG's 1615 cm - ¹Characteristic peak; Figure 4 The F, MG+CV mixture also exhibits the main characteristic peaks of both MG and CV. More importantly, the intensity distribution of the characteristic peaks in the mixture spectrum under co-assembly mode is closer to the superposition of the Raman signals of each individual component, indicating that the contributions of different molecules in the hot spot region are more balanced.
[0049] The above results indicate that in the traditional immersion mode, molecules need to diffuse and compete for adsorption on the surface of the formed Au@Ag NCs monolayer and within the nano-interstitial spaces. This easily leads to molecules with strong adsorption capacity dominating hot spots and masking signals from other components. In contrast, the co-assembly mode introduces the analyte molecules simultaneously during the nanoparticle interface assembly process. These molecules can be co-confined within the interparticle spaces during hot spot formation, effectively mitigating signal bias caused by competitive adsorption. These results demonstrate that the co-assembly strategy can more completely preserve multi-component Raman information in mixture detection and is suitable for the simultaneous identification and analysis of complex systems.
[0050] After demonstrating that co-assembly can improve the sensitivity of single-molecule detection and effectively alleviate signal masking caused by competitive adsorption in mixed systems, this strategy was further extended to the SERS detection of actual drug molecules. Drug molecules are typically characterized by complex structures, dense characteristic peaks, and severe peak overlap in mixed systems. Therefore, not only is a high signal enhancement capability required from the substrate, but accurate identification against complex spectral backgrounds is also necessary. Based on this, two representative controlled drugs, sufentanil and midazolam, were selected as detection targets to systematically evaluate the application potential of the co-assembly SERS strategy in single-drug identification, trace detection, and mixture analysis. Figure 5 As shown in Figure A, the single-component SERS spectra of sufentanil and midazolam were first acquired, and their main Raman characteristic peaks were assigned. Midazolam showed peaks at 689, 827, and 1036 cm⁻¹. - ¹Symptoms show distinct characteristic peaks at positions such as 1004, 1079, and 1172 cm⁻¹. - ¹Distinguished fingerprint signals were observed at various locations; the corresponding vibrational modes are summarized in Table 1. These results demonstrate that co-assembled SERS substrates can effectively obtain characteristic fingerprint information of two types of drug molecules, providing a spectroscopic basis for subsequent concentration-dependent detection and mixture identification.
[0051] Table 1. Assignment of characteristic SERS peaks for midazolam and sufentanil Figure 5 China B and Figure 5 Table C shows the SERS spectra of midazolam and sufentanil at different concentrations to evaluate the trace detection capability of this method. For midazolam, as the concentration gradually decreased from 100 ppm to 0.5 ppm, the SERS spectra at 689, 827, and 1036 cm⁻¹ were observed. - The intensity of characteristic peaks ¹ generally shows a decreasing trend, but clear characteristic peak signals can still be observed at the lowest test concentration. Figure 5 (Middle B). For sufentanil, as the concentration decreased from 100 ppm to 5 ppm, its 1004, 1079, and 1172 cm⁻¹ values decreased. - ¹The characteristic peaks also gradually weaken, but still maintain good identifiability. Figure 5 (C). The above results demonstrate that the co-assembly SERS method has high detection sensitivity for both drugs and can achieve rapid screening of low concentrations of drug molecules.
[0052] Further investigation is needed into the strategy's ability to identify drug mixtures. For example... Figure 5As shown in Figure D, representative characteristic peaks of both drugs can be observed simultaneously in the SERS spectrum of the sufentanil / midazolam mixture. Orange marks correspond to the sufentanil characteristic peak, green marks to the midazolam characteristic peak, and blue areas indicate locations where characteristic peaks overlap or contribute jointly in the mixture. This result demonstrates that the co-assembly mode can simultaneously capture the Raman fingerprint information of different drug molecules in mixed samples, possessing the capability for mixture detection. However, compared with… Figure 5 Compared to the standard spectrum of component A, the peak positions, relative intensities, and local peak shapes in the mixture spectrum show significant changes, with some characteristic peaks overlapping or shifting. Therefore, relying solely on manual peak position comparison is insufficient for accurate identification of complex mixtures, necessitating the introduction of algorithms to assist in identification.
[0053] To address the issues of overlapping characteristic peaks, varying peak intensities, and the inherent subjectivity of manual interpretation in mixture spectra, a machine learning-assisted multidimensional spectral matching algorithm was constructed. Figure 5 The algorithm outlines the overall process: First, input the standard SERS spectrum of a single drug and the SERS spectrum of a mixture, and extract spectral features; then, analyze from three dimensions: peak position matching, peak intensity ratio matching, and local waveform similarity matching; finally, obtain the comprehensive matching score through confidence fusion, and output the judgment result of "detected" or "not detected" according to the set threshold.
[0054] Figure 5 The algorithm further demonstrates the specific process of feature peak selection and matching. When midazolam is the target molecule, the black curve represents the standard spectrum of a single midazolam, and the red curve represents the spectrum of the mixture. The algorithm selects 10 representative feature peaks from the standard spectrum as identification criteria and searches for corresponding peak positions and local waveforms in the mixture spectrum. It can be seen that although the overall peak shape and relative intensity of the mixture spectrum differ from those of the single midazolam spectrum, most feature peaks can still be found with corresponding signals in the mixture, indicating that multi-peak joint matching can effectively improve the reliability of target molecule identification.
[0055] Figure 5The algorithm evaluation index for midazolam in mixture detection is given in Figure 12. The peak position matching score is 0.7000, indicating that the main characteristic peaks of the target molecule can meet the set peak position matching requirements in the mixture; the peak intensity ratio matching score is 0.9104, indicating that the relative intensity relationship of the characteristic peaks in the mixture has high consistency with the standard spectrum; the local waveform similarity score is 0.9165, indicating that the local spectral shape near the matching peak is highly similar to the standard spectrum. After multi-index fusion, the final comprehensive confidence score reaches 0.8281, which is higher than the detection threshold of 0.6, thus determining the presence of midazolam in the mixture. This result proves that even if there are significant differences between the mixture spectrum and the single substance spectrum, the algorithm can still reliably identify the target drug based on multi-dimensional features. Further verification of the algorithm's applicability in mixture identification is conducted using other target molecules. (See Figure 12 and...) Figure 13 As shown, the algorithm analyzed the spectral identification results of mixtures of midazolam and CV, and made a comprehensive judgment through peak position matching, peak intensity ratio matching, and local waveform similarity matching. The results show that the overall confidence level of the target molecule is higher than the set detection threshold, indicating that the algorithm is not limited to a single detection object, but can be extended to the identification of mixtures of different molecular systems.
[0056] In summary, this invention proposes a method for detecting and identifying drug mixtures based on Co-assembly SERS. By introducing the analyte molecule into the assembly process of Au@Ag core-shell nanocubes, the target molecule is enriched in the interparticle gaps and hotspot regions while the nanoparticles form a dense monolayer structure. This increases the contact probability between the molecule and the plasmon enhancement region, effectively enhancing the SERS signal response. Experimental results show that this method has good applicability to different types of molecules, can improve the detection signals of model molecules and drug molecules, and can achieve low-concentration detection of drugs such as sufentanil and midazolam. Furthermore, addressing issues such as peak overlap, peak intensity variations, and background interference in mixture spectra, this invention establishes a multi-dimensional spectral matching identification method by combining peak position matching, peak intensity ratio matching, and local spectral similarity analysis. This method can evaluate the retention of target molecule characteristic peaks in the mixture from multiple perspectives and determine the presence of the target drug through comprehensive confidence. Compared with single characteristic peak interpretation methods, this strategy has better stability and anti-interference ability, improving the sensitivity and reliability of drug detection in complex systems.
[0057] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.
[0058] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A SERS substrate based on the co-assembly of noble metal nanoparticles and target molecules, characterized in that, It includes a substrate carrier and a noble metal nanoparticle film loaded on the surface of the substrate carrier; The noble metal nanoparticle film is a monolayer structure assembled from noble metal nanoparticles, and the analyte molecules are confined within the hot spot region of the nano gaps between the noble metal nanoparticles; the SERS substrate is prepared by co-assembling noble metal nanoparticles and analyte molecules at the liquid-liquid interface. The molecule to be tested is an organic molecule that can be dissolved or dispersed in an aqueous phase and has characteristic fingerprint peaks that can be identified by Raman spectroscopy. During the liquid-liquid interface co-assembly process, it is synchronously confined within the hot spot region as the gaps between nanoparticles shrink. The noble metal nanoparticles are Au@Ag core-shell nanocubes.
2. The SERS substrate according to claim 1, characterized in that, The noble metal nanoparticles comprise a gold nanosphere core and a silver shell; the gold nanosphere core has a particle size of 10-50 nm, and the silver shell has a thickness of 5-30 nm.
3. The SERS substrate according to claim 1, characterized in that, The noble metal nanoparticles are coated with PVP ligands; the substrate carrier is any one of silicon wafers, glass sheets or quartz sheets.
4. A method for preparing a SERS substrate as described in any one of claims 1-3, characterized in that, Includes the following steps: (1) Preparation of a dispersion of noble metal nanoparticles coated with PVP; (2) The noble metal nanoparticle dispersion, organic solvent and aqueous solution containing the analyte molecules are mixed to form a mixed system; (3) Add an inducer to the mixture to drive noble metal nanoparticles to migrate to the water-oil interface and undergo interfacial self-assembly. During this process, the molecule to be tested is simultaneously confined in the gaps between nanoparticles to form an interfacial nanoparticle film. (4) The interfacial nanoparticle film is transferred to the surface of the substrate carrier and dried to obtain the SERS substrate.
5. The preparation method according to claim 4, characterized in that, In step (2), the organic solvent is dichloromethane; in step (3), the inducing agent is n-hexane.
6. The preparation method according to claim 4, characterized in that, The volume ratio of the noble metal nanoparticle dispersion, organic solvent, aqueous solution and inducer is 1:0.5-1:1-2:0.3-0.
6.
7. The application of a SERS substrate as described in any one of claims 1-3 in the detection of drug mixtures, characterized in that, The applications include using the SERS substrate for SERS spectral acquisition and multidimensional spectral matching and identification.