Method for determining binder content of rca-rap hot-mix recycled asphalt mixture
By measuring the diffusion characteristics of RCA-RAP hot-mix recycled asphalt mixtures using nuclear magnetic resonance tracers and calculating the effective film-forming area, the problem of deviation in determining the amount of binder was solved, thus improving the road performance and construction quality stability of the mixture.
Patent Information
- Application Number
- CN202611501829.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies cannot accurately determine the amount of binder in RCA-RAP hot-mix recycled asphalt mixtures, leading to insufficient or excessive film formation, which affects road performance and construction quality stability.
The diffusion characteristics were measured using a nuclear magnetic resonance tracer in a state where the mineral aggregate coating was not damaged after trial mixing. The effective film-forming area was calculated by linear fitting, taking into account the effects of RAP old asphalt, recycling agent and RCA pore absorption, and iterative correction was performed to determine the amount of binder.
It enables precise determination of binder dosage under actual wrapping conditions, reduces measurement deviation, and improves road performance and construction quality stability.
Smart Images

Figure CN123155591A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of materials testing technology, and in particular to a method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixtures. Background Technology
[0002] With the continuous expansion of highway construction and maintenance, the amount of RAP (recycled asphalt pavement) generated from milling asphalt pavement and RCA (recycled aggregate) generated from crushing old cement concrete pavement is increasing. Simultaneously applying RCA and RAP to hot-mix recycled asphalt mixtures can not only facilitate the large-scale disposal of both types of solid waste, reducing the extraction of natural aggregates and asphalt consumption, but also aligns with the development direction of green highway construction and a circular economy, resulting in significant environmental and economic benefits.
[0003] However, on the one hand, the RCA surface is covered with residual cement mortar and contains a large number of open pores. During hot mixing, it absorbs some of the new asphalt binder or recycling agent, resulting in a reduction in the amount of effective binder actually participating in the formation of the aggregate film. This absorbed binder does not participate in the formation of the target asphalt film. If it is not separately included in the dosage calculation, it will lead to insufficient film-forming binder, resulting in problems such as a thin asphalt film and poor aggregate coating. On the other hand, the RAP surface is covered with an old asphalt film that has aged and hardened over a long period of use. During heating and mixing, only a portion of this old asphalt is softened and activated to participate in the formation of the new asphalt film, while the rest remains as an aged hard shell on the original RAP aggregate surface. At the same time, the recycling agent added to restore the performance of the old asphalt does not all enter the film-forming binder phase. Some may fail to form an effective film due to volatilization, absorption by the pores of the RCA, or incompatibility with other components. Furthermore, the new asphalt binder, recycling agent, and RAP old asphalt diffuse and mix with each other during the mixing process. The final film-forming state is closely related to the interaction of each component, making it difficult to estimate the film-forming area and effective film-forming quality from a single parameter. This results in the difficulty in determining the amount of binder used in RCA-RAP hot-mix recycled asphalt mixtures.
[0004] In existing technologies, the methods for determining the amount of binder are usually based on empirical asphalt-aggregate ratios, specific surface areas of the aggregate after extraction and sieving, RAP old bitumen content, or RCA adsorption capacity. The empirical asphalt-aggregate ratio method relies heavily on extensive testing and engineering experience, lacking precise characterization of material properties. RCA and RAP from different sources exhibit significant differences in adsorption and old bitumen activation levels, making empirical values often insufficiently adaptable. The extraction and sieving specific surface area method involves extracting and removing all the binder with solvent and sieving the aggregate before measuring its specific surface area to calculate the theoretical film-forming area. However, this method disrupts the true coating state of the binder on the aggregate after trial mixing, failing to reflect the binder's absorption in the RCA pores, the layering relationship between RAP old bitumen and new binder, and the film thickness distribution at different aggregate interfaces, leading to significant deviations between the calculated results and the actual film-forming area. While correction methods based on RAP old bitumen content and RCA adsorption capacity consider some material property factors, the coupling relationships between the correction terms are not incorporated into a unified analytical framework, and the determination of correction coefficients lacks objective standards.
[0005] In summary, existing technologies cannot uniformly characterize the effective film-forming area of asphalt mixtures under actual coating conditions after trial mixing. They also struggle to calculate various factors that affect the dosage of new asphalt binder and recycling agent, such as RCA pore absorption, effective participation of RAP old asphalt in film formation, and effective participation of recycling agent in film formation. This leads to a discrepancy between the binder dosage and the actual film-forming requirements, affecting the road performance and construction quality stability of recycled asphalt mixtures. Summary of the Invention
[0006] In view of this, the present invention proposes a method for determining the binder content of RCA-RAP hot-mix recycled asphalt mixture, which solves the problem that it is difficult to determine the binder content of RCA-RAP hot-mix recycled asphalt mixture in the prior art, and improves the road performance and construction quality stability of recycled mixture.
[0007] The technical solution of this invention is implemented as follows: This invention provides a method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixtures, including the following steps: S1, adding a tracer according to the initial composition ratio of the binder and preparing a sample; S2, measuring the free diffusion coefficient of the tracer in a binder with the same composition as the sample but without mineral aggregates, and measuring the apparent diffusion coefficient of the tracer in the sample, and determining the effective film-forming area of the asphalt binder by combining the calibration results of a standard sample with known mineral aggregate surface area; S3, calculating the mass of film-forming asphalt binder required to form the target asphalt film based on the effective film-forming area of the asphalt binder; S4, determining the mass of the recycling agent and the mass of the new asphalt binder based on the effective film-forming mass of the old asphalt, the effective film-forming mass of the recycling agent, and the mass of the RCA pore-absorbing asphalt binder, combined with the mass of the film-forming asphalt binder.
[0008] Based on the above technical solution, preferably, the following step is also included: S5, substituting the mass of the recycling agent and the mass of the new asphalt binder obtained in step S4 into the initial mixing ratio to prepare a new sample, and repeating steps S2 to S4 to obtain the verification results, confirming that the new sample corresponds to the effective film-forming area of the asphalt binder, the mass of the new asphalt binder and the mass of the recycling agent determined in steps S2 to S4, and then determining the mass of the recycling agent and the mass of the new asphalt binder obtained in step S4 as the final dosage.
[0009] Based on the above technical solution, preferably, step S2 includes the following steps: S21, determining the free diffusion coefficient of the tracer in a binder with the same composition as the sample but without mineral aggregate; S22, determining the apparent diffusion coefficient of the tracer in the sample at different diffusion times; S23, calculating the ratio of the apparent diffusion coefficient to the free diffusion coefficient to obtain the normalized apparent diffusion coefficient; S24, performing linear fitting on the diffusion distance scale using the normalized apparent diffusion coefficient to obtain the fitting slope, where the diffusion distance scale is characterized by the square root of the product of the free diffusion coefficient and the diffusion time; S25, determining the effective film-forming area of the asphalt binder by multiplying the absolute value of the fitting slope, the volume of the binder phase containing the tracer, and the conversion factor obtained from the standard sample calibration.
[0010] More preferably, the standard sample is an asphalt binder-coated aggregate sample with a known aggregate surface area, a known binder phase volume, and containing a tracer; the conversion factor is obtained through the following steps: S251, under the same test conditions as the sample, the slope of the normalized apparent diffusion coefficient of the standard sample on the diffusion distance scale and the binder phase volume containing the tracer are determined; S252, the conversion factor is obtained by dividing the known aggregate surface area of the standard sample by the product of the binder phase volume of the standard sample and the absolute value of the slope.
[0011] More preferably, when the normalized apparent diffusion coefficient exhibits at least two linear intervals as the diffusion distance scale changes, the effective film-forming area of the asphalt binder is determined by the fitting slope of the short diffusion time interval.
[0012] In a further preferred embodiment, when the normalized apparent diffusion coefficient exhibits at least two linear intervals as the diffusion distance scale changes, the fitting slope corresponding to the long diffusion time interval is used, combined with the calibration of the standard sample in the corresponding interval, to obtain the effective confined scale of the RAP old asphalt binder phase, and thereby correct the effective participation of old asphalt in film formation quality and the effective participation of recycling agent in film formation quality.
[0013] Based on the above technical solution, preferably, step S4 includes the following steps: S41, determining the quality of RAP old asphalt and calculating the quality of the recycling agent in combination with the recycling agent dosage coefficient; S42, determining the effective film-forming quality of RAP old asphalt based on the quality of RAP old asphalt, and determining the effective film-forming quality of the recycling agent based on the quality of the recycling agent; S43, determining the quality of RCA pore-absorbing asphalt binder, and determining the quality of the new asphalt binder based on the quality of the film-forming asphalt binder, the effective film-forming quality of RAP old asphalt, the effective film-forming quality of the recycling agent, and the quality of RCA pore-absorbing asphalt binder.
[0014] More preferably, the recycling agent dosage coefficient is the ratio of the recycling agent mass to the RAP old asphalt mass.
[0015] In a further preferred embodiment, the effective film-forming mass of RAP old asphalt does not exceed the mass of RAP old asphalt, and the effective film-forming mass of the recycling agent does not exceed the mass of the recycling agent.
[0016] Based on the above technical solutions, preferably, the tracer is an oil-soluble tracer that can generate distinguishable nuclear magnetic resonance signals in the binder phase. The tracer is compatible with the new asphalt binder and the recycling agent, and does not change the coating state of the binder after the mixture in the sample.
[0017] The method for determining the binder content in RCA-RAP hot-mix recycled asphalt mixtures according to the present invention has the following advantages over the prior art: (1) This invention uses nuclear magnetic resonance diffusion measurement on asphalt binder coated mixture samples after trial mixing without solvent extraction or sieving. The effective film-forming area of the asphalt binder is directly determined under this real coated state, avoiding the damage to the coated state caused by the extraction and sieving process and the resulting deviation in surface area measurement. Since the measurement object completely retains the in-situ state of RCA, RAP, new aggregates and mineral powder coated by the binder after trial mixing, the obtained film-forming area can truly reflect the contact situation of the interfaces of various mineral materials, making the basis for subsequent calculation of binder dosage more reliable.
[0018] (2) This invention incorporates the effective participation of RAP old asphalt in film formation quality, the effective participation of recycling agent in film formation quality, and the RCA pore absorption asphalt binder quality into the same calculation formula to determine the quality of new asphalt binder, and establishes a complete quality balance covering film formation requirements, old material contribution, and pore loss; at the same time, it takes into account the binder loss caused by RCA pore absorption and the binder replenishment brought by RAP old asphalt activation, avoiding insufficient new asphalt usage due to ignoring RCA absorption and insufficient total binder amount due to overestimating the contribution of RAP old asphalt, effectively reducing the deviation of binder usage and making the determined usage more accurate.
[0019] (3) This invention establishes a quantitative relationship between the confined diffusion behavior of nuclear magnetic resonance tracers and the surface area of minerals. It calculates the effective film-forming area using the slope of the linear fit of the normalized apparent diffusion coefficient to the diffusion distance scale and the standard sample calibration conversion factor. This achieves objective, non-destructive, and repeatable measurement of the film-forming area. Compared to traditional methods that rely on empirical judgment or indirect calculation, this measurement method has a clear physical basis and quantitative calibration criteria, improving the accuracy and reproducibility of the area measurement results.
[0020] (4) This invention includes a verification and iteration step, in which the calculated mass of the new asphalt binder and the mass of the recycling agent are reused to prepare trial samples and the diffusion measurement and mass calculation are repeated until the results are consistent with the coating state after trial mixing. This closed-loop process can verify and correct errors introduced by material variability or deviations in initial trial mixing conditions, so that the calculated results of the mass of the new asphalt binder and the effective film area of the binder are consistent with the actual trial mixing state, thereby improving the stability and engineering reliability of the binder dosage determination results.
[0021] (5) This invention further utilizes the differences in confined diffusion behavior of the normalized apparent diffusion coefficient across multiple diffusion time intervals to extract effective confined scale information of the RAP old asphalt binder phase and correct the effective film-forming quality of the old asphalt and recycling agent. This method establishes a correlation between the diffusion characteristics of the tracer in long and short diffusion time intervals and the mixing state of the new and old binder phases, providing a quantitative basis for evaluating the activation degree of RAP old asphalt and the effect of the recycling agent, improving the accuracy of binder dosage determination and adaptability to complex material systems. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 This is a flowchart illustrating the determination method of the present invention; Figure 2 This is a schematic diagram of the linear fitting of the normalized apparent diffusion coefficient as a function of the square root of diffusion time according to the present invention. Detailed Implementation
[0024] To enable those skilled in the art to better understand the technical solutions in this specification, the technical solutions in the embodiments of this specification will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0025] In the description of the embodiments of the present invention, words such as "for example" or "for instance" are used to indicate examples, illustrations, or explanations. Any embodiment or design described as "for example" or "for instance" in the embodiments of the present invention should not be construed as being more preferred or advantageous than other embodiments or designs. Rather, the use of words such as "for example" or "for instance" is intended to present the relevant concepts in a specific manner.
[0026] In the description of the embodiments of the present invention, the term "multiple" means two or more. For example, multiple systems means two or more systems, and multiple screen terminals means two or more screen terminals. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the indicated technical features. Thus, a feature defined with "first" or "second" may explicitly or implicitly include one or more of that feature. The terms "comprising," "including," "having," and variations thereof all mean "including but not limited to," unless otherwise specifically emphasized.
[0027] like Figure 1 As shown, this invention discloses a method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixtures. RCA refers to recycled cement concrete aggregate, and RAP is recycled asphalt pavement material. The core of this method lies in: after trial mixing, without solvent extraction or screening, and maintaining the aggregate in a true state where it is coated with asphalt binder, utilizing the restricted diffusion characteristics of an oil-soluble nuclear magnetic resonance tracer to calibrate the effective film-forming area of the asphalt binder. Then, the actual film-forming contributions of the old asphalt and recycling agent in RAP, as well as the pore absorption of RCA, are incorporated into the calculation of the new asphalt binder dosage. Finally, verification ensures that the dosage is consistent with the actual coating state. Specifically, the method includes the following steps:
[0028] S1. A tracer is added according to the initial composition ratio of the binder, and a sample is prepared. Specifically, according to the proposed mass blending ratio of RCA, RAP, new aggregate, and mineral powder, an initial trial mix of asphalt binder is used for laboratory mixing. An oil-soluble NMR tracer is introduced into the binder phase to obtain a mixture sample in the asphalt binder-coated state after the trial mix; this is the sample. This sample is unextracted by solvents and unsieved, fully preserving the state of RCA, RAP, new aggregate, and mineral powder coated by the asphalt binder after the trial mix. The initial trial mix of asphalt binder is only used to form a coated sample suitable for NMR measurement and is not considered as the final determined mass of the new asphalt binder or the recycling agent.
[0029] The tracer can be added by uniformly dispersing it into the new asphalt binder, into the recycling agent, or into a premixed asphalt binder formed by mixing the new asphalt binder and the recycling agent. To ensure that the tracer reliably reflects the diffusion behavior of binder molecules in the test, the tracer is preferably an oil-soluble tracer capable of generating a resolvable nuclear magnetic resonance signal in the binder phase, and its detectable nuclei can be selected from... 1 H, 2 H or 19 F. The tracer should be compatible with the new asphalt binder and recycling agent it comes into contact with, i.e., it should not cause visible stratification, precipitation, or reaction at the test mixing temperature and the test temperature, and should not change the coating state of the asphalt binder on the aggregate in the sample. Based on considerations of signal sensitivity and minimizing the impact on binder properties, the amount of tracer added is preferably 0.05% to 2.0% by weight of asphalt binder.
[0030] S2. The free diffusion coefficient of the tracer in a binder with the same composition as the sample but without mineral aggregates, and the apparent diffusion coefficient of the tracer in the sample, are determined. Combined with the calibration results of a standard sample with known mineral aggregate surface area, the effective film-forming area of the asphalt binder is determined. Specifically, at the selected test temperature T, the free diffusion coefficient D0(T) of the tracer in a pure binder containing no mineral aggregates and with the same binder composition as the sample is first determined. Then, the relationship between the apparent diffusion coefficient D(Δ,T) of the tracer in the sample and the diffusion time Δ is determined. The free diffusion coefficient reflects the intrinsic mobility of tracer molecules in the binder phase without spatial hindrance, while the apparent diffusion coefficient decreases due to the restriction of tracer molecule diffusion at the mineral aggregate interface, and its degree of restriction is closely related to the mineral aggregate surface area. Based on this, a standard sample with known mineral aggregate surface area is used for calibration, and the difference between free diffusion and apparent diffusion is converted into the effective film-forming area A of the asphalt binder. The standard sample here refers to an asphalt binder-coated aggregate sample with a known aggregate surface area, a known binder phase volume, and containing the same type of tracer, and tested under the same test temperature and NMR diffusion test conditions. By comparing the normalized diffusion-restricted behavior of the sample and the standard sample, the equivalent aggregate surface area in the sample that the asphalt binder can contact the aggregate surface and participate in the formation of the target asphalt film can be obtained, i.e., the effective film-forming area A.
[0031] S3. Calculate the mass of film-forming asphalt binder required to form the target asphalt film based on the effective film-forming area of the asphalt binder. The mass M0 of the film-forming asphalt binder is determined by the effective film-forming area A, the target asphalt film thickness h, and the density ρ of the film-forming asphalt binder; that is, M0 is the product of ρ, h, and A. This can be expressed by the following formula:
[0032] M0 = ρ × h × A, The target asphalt film thickness h is determined based on the engineering mix design requirements, target porosity, durability requirements, or preliminary test results. A typical h value can be selected between 6 μm and 10 μm depending on the mixture type. The film-forming asphalt binder density ρ refers to the binder density that ultimately constitutes the target asphalt film. It can be obtained through actual measurement of the mixture of new asphalt binder, RAP old asphalt, and recycling agent. In cases requiring iterative calculation, it can also be calculated by weighting the density of each of the new asphalt binder, RAP old asphalt, and recycling agent according to the proportion of film-forming mass corresponding to the previous iteration or the preset initial value.
[0033] S4. Based on the measured or calculated film-forming quality of old asphalt, the film-forming quality of the recycling agent, and the quality of RCA pore-absorbing asphalt binder, the quality of the film-forming asphalt binder is combined with the quality of the new asphalt binder to determine the quality of the recycling agent and the quality of the new asphalt binder. Specifically, this step first requires obtaining three key parameters: RAP (Regenerative Asphalt) effective film-forming quality M... pe Regenerants effectively contribute to film formation quality. re And the quality of RCA pore absorption asphalt binder.
[0034] Among them, RAP old asphalt effectively contributes to film formation quality M pe This refers to the portion of the old asphalt on the RAP surface that was activated during the trial mixing and recycling process and actually participated in the formation of the target asphalt film. This value does not exceed the total mass M of the old asphalt in the RAP. p That is, satisfying 0≤M pe ≤M p The specific value is determined by indoor calibration tests.
[0035] Regenerators effectively contribute to film formation quality M re This refers to the portion of the added recycling agent that actually enters the binder film phase and contributes to the formation of the asphalt film, and also does not exceed the total mass M of the recycling agent. r That is, satisfying 0≤M re ≤M r The regenerant mass M is also determined by indoor calibration tests. r By measuring the quality M of RAP old asphalt p Combined with the regenerator dosage coefficient β, it can be expressed as follows:
[0036] M r =β×M p Where M p It can be obtained by RAP extraction test or combustion method. β is determined by RAP old asphalt recycling test. The test is based on the old asphalt after recycling reaching at least one of the target penetration, viscosity, softening point or dynamic shear rheological index. β is the ratio of the mass of recycling agent to the mass of RAP old asphalt.
[0037] RCA pore-absorbing asphalt binder mass M c This refers to the portion of asphalt binder mass that is absorbed by residual mortar and open pores on the RCA surface and does not participate in the formation of the target asphalt film on the aggregate surface. This value is obtained by conducting an adsorption test on RCA with the corresponding new asphalt binder, recycling agent, or new asphalt binder-recycling agent mixture at a temperature and residence time corresponding to the trial mixing conditions.
[0038] Ultimately, the quality M of the new asphalt binder b Then, based on the aforementioned parameters, M is determined according to the following relationship: b Equals the mass of asphalt binder required for film formation M0 plus the mass of RCA pore-absorbing asphalt binder M c Subtract the effective contribution of RAP old asphalt to film formation quality M pe And regenerators effectively participate in film formation quality M re It can be expressed as the following formula:
[0039] M b =M0-M pe -M re +M c The amount of new asphalt binder obtained through the above calculations precisely compensates for the effective film-forming contribution of RAP old asphalt and recycling agent, as well as the loss due to RCA pore absorption, thus filling the gap in binder required to form a complete target asphalt film.
[0040] In one embodiment, a verification iteration step is added to ensure the consistency between the final determined amount of binder and the coating state after trial mixing. The method also includes the following steps: S5. Substitute the mass of the recycling agent and the mass of the new asphalt binder obtained in step S4 into the initial mix proportion to prepare a new sample, and repeat steps S2 to S4 to obtain the verification results. Confirm that the new sample corresponds to the effective film-forming area of the asphalt binder, the mass of the new asphalt binder and the mass of the recycling agent determined in steps S2 to S4. Then determine the mass of the recycling agent and the mass of the new asphalt binder obtained in step S4 as the final dosage.
[0041] In specific implementation, the mass M of the regenerant obtained in the previous step S4 will be... r and the quality M of the new asphalt binder bAs a new binder dosage, it is substituted into the initial proportions of RCA, RAP, new aggregates, and mineral powder to conduct a new trial mix and prepare a new asphalt binder-coated mixture sample, i.e., a new sample. Then, the nuclear magnetic resonance diffusion measurement, effective film-forming area determination, and mass calculation processes described in steps S2 to S4 above are repeated on the new sample to obtain the verification results. The core purpose of the verification is to confirm the effective film-forming area A′ of the asphalt binder exhibited by the new sample and the newly calculated mass M of the new asphalt binder. b ′, whether it matches A and M determined in steps S2 to S4 b Correspondingly.
[0042] It should be noted that in engineering practice, due to factors such as material variability and mixing uniformity, a certain reasonable deviation is allowed in the verification results. A preset deviation range can be set as a confirmation standard; for example, the mass M of the new asphalt binder. b ′ and M determined in step S4 b When the relative deviation between the two values does not exceed ±2%, and the relative deviation between the effective film-forming area A′ and the previously determined A does not exceed ±3%, the correspondence between the two can be confirmed. If the deviation exceeds the range, the parameters obtained from the verification are used as a benchmark for fine-tuning the quantity again and the verification is repeated until the self-consistency requirement is met. After confirmation, the regenerant mass M obtained in step S4 is... r And the quality M of the new asphalt binder b This serves as the final mix proportion for construction. If necessary, cross-sectional microscopic images of the RCA-RAP hot-mix recycled asphalt mixture prepared according to the final proportion can be statistically analyzed to calculate the percentage of insufficient film thickness, serving as supplementary verification of the rationality of the final binder dosage. This verification process ensures a high degree of consistency between the determined binder dosage and the coating state after trial mixing, effectively reducing the problem of insufficient or excessive actual asphalt film thickness caused by inaccurate estimations of RCA pore absorption and the participation of RAP old asphalt in film formation.
[0043] In one embodiment, a detailed process for determining the effective film-forming area of asphalt binder by nuclear magnetic resonance diffusion measurement is provided, namely, step S2 includes the following steps: S21, determine the free diffusion coefficient D0(T) of the tracer in a binder with the same composition as the sample but without mineral aggregates. This determination is performed at the same test temperature T as the sample, using a nuclear magnetic resonance spectrometer with a pulsed field gradient module. A gradient pulse sequence is applied to the pure binder sample, which contains no mineral aggregates and has the same binder composition as the sample. The binder includes new asphalt, RAP old asphalt, recycling agent, and tracer.
[0044] As the gradient intensity increases, the nuclear magnetic resonance signal attenuates due to molecular diffusion. The free diffusion coefficient D0(T) can be obtained by fitting the signal attenuation curve. This coefficient reflects the intrinsic mobility of tracer molecules in the bound phase without any spatial hindrance.
[0045] S22, The apparent diffusion coefficient D(Δ,T) of the tracer in the sample at different diffusion times Δ was determined. The same nuclear magnetic resonance pulsed gradient field method was used to measure the diffusion of the asphalt binder-coated mixture samples after trial mixing. Because the aggregate interface geometrically restricts the diffusion of tracer molecules, the actual mean square displacement of the molecules within a given diffusion time Δ is reduced, resulting in an apparent diffusion coefficient D(Δ,T) lower than the free diffusion coefficient D0(T), and this restriction becomes more pronounced with increasing diffusion time Δ. Therefore, the apparent diffusion coefficient was measured at multiple different diffusion times Δ to obtain the relationship curve of D(Δ,T) as a function of Δ.
[0046] S23, calculate the ratio of the apparent diffusion coefficient to the free diffusion coefficient to obtain the normalized apparent diffusion coefficient. Normalization eliminates the overall influence of factors such as temperature and binder viscosity on the absolute value of the diffusion coefficient, allowing for comparison of confined diffusion behavior under different samples and test conditions on the same scale. Its mathematical expression is that the normalized apparent diffusion coefficient equals the ratio of D(Δ,T) to D0(T), i.e., D(Δ,T) / D0(T).
[0047] S24, using the normalized apparent diffusion coefficient to perform a linear fit on the diffusion distance scale, yields the fitting slope k. (See also...) Figure 2 The diffusion distance scale is characterized by the square root of the product of the free diffusion coefficient and the diffusion time, i.e. This scale essentially represents the typical distance that tracer molecules can diffuse over time Δ in the absence of obstruction. Within a short diffusion time interval, tracer molecules primarily experience localized confinement at the mineral surface. The normalized apparent diffusion coefficient decreases linearly with increasing diffusion distance, and the absolute value of its slope k is proportional to the surface area of the mineral material contacted per unit volume of binder. This can be expressed by the following formula:
[0048] D(Δ,T) / D0(T)=1+k×
[0049] To ensure the reliability of the fitting results, the linear fitting is performed with the normalized apparent diffusion coefficient varying. The changes occurred within a diffusion time interval where a clear linear relationship existed, and the coefficient of determination R of the fit was [missing information]. 2Preferably, the value should not be less than 0.95. When there are multiple diffusion time intervals that satisfy the linearity condition, the fitting slope corresponding to the shorter diffusion time interval is selected as k, because the signal of the short time interval mainly reflects the contact area between the new coated binder and the surface of the aggregate, while the long time interval may be superimposed with the confining effect in the old RAP asphalt film.
[0050] S25, based on the absolute value of the fitting slope k, the volume V of the binder phase containing the tracer, and the conversion factor obtained from the standard sample calibration. Multiplication determines the effective film-forming area A of the asphalt binder. This can be expressed as the following formula:
[0051]
[0052] The volume V of the binder phase containing the tracer refers to the total volume of the asphalt binder in the sample where the oil-soluble NMR tracer is distributed, which can be obtained through NMR signal integration calibration. The calibration method is as follows: prepare a signal calibration sample, whose binder phase volume V... m It is known that the integral I of its nuclear magnetic resonance signal is measured. m Then, measure the signal integral I of the sample, then V = V m ×(I / I m This volume calibration ensures that the binder volume used for area calculations strictly corresponds to the binder phase that actually generates the NMR signal. The conversion factor is obtained by calibration using a standard sample with a known surface area.
[0053] In one embodiment, the standard sample is an asphalt binder-coated aggregate sample with known aggregate surface area, known binder phase volume, and containing a tracer. The preparation of the standard sample should simulate the binder-aggregate coating state in actual trial-mixed aggregates as closely as possible, but its aggregate surface area A... S It must be possible to know accurately in advance. A S The specific surface area can be determined using methods such as single-size minerals with known specific surface areas, area calculation of regularly shaped particles, BET nitrogen adsorption testing, microscopic image measurement, or a combination of the above methods. The type and concentration of tracer used in the standard sample, the test temperature, and the pulse sequence parameters of the NMR diffusion test must be completely consistent with the sample test conditions to ensure the conversion factor is correct. Applicability.
[0054] Among them, the conversion factor Obtained through the following steps: S251, Under the same test conditions as the sample, determine the slope k of the normalized apparent diffusion coefficient of the standard sample fitted to the diffusion distance scale. s and the volume V of the binder phase containing the tracer s The testing procedure is the same as that for the sample: first, the free diffusion coefficient D of the standard sample is measured. 0s(T) and the apparent diffusion coefficient at different diffusion times were used to calculate the normalized value, and then... The slope k is obtained by performing linear fitting. s The volume V of the binder phase of the standard sample s It is also obtained by integral calibration of nuclear magnetic resonance signals.
[0055] S252, based on the known surface area A of the standard sample. S Divide by the binder phase volume V of the standard sample s With the fitted slope k s The conversion factor is obtained by multiplying the absolute values. It can be expressed as the following formula:
[0056]
[0057] Conversion factor Essentially, a quantitative conversion relationship was established between the normalized diffusion-limited slope, the binder volume, and the mineral surface area. Since the standard sample and the test sample are identical in tracer type, test temperature, and NMR diffusion test conditions, this approach is feasible. It can be considered an instrument-material constant that is only related to the testing system and the tracer-binder system. Therefore, after measuring the V and k of the sample, the effective film-forming area A of the asphalt binder of the sample can be obtained by the previous formula without any destructive treatment of the sample itself or direct measurement of the surface area. This allows the true film-forming area to be obtained while keeping the coating state intact after the trial mixing.
[0058] In one embodiment, when the normalized apparent diffusion coefficient exhibits at least two linear intervals with respect to the diffusion distance scale, the effective film area of the asphalt binder is determined using the fitting slope of the short diffusion time interval. Specifically, in actual RCA-RAP hot-mix recycled asphalt mixture samples, due to the simultaneous presence of a new coating film of the aggregate by the new asphalt binder and the original old asphalt film on the RAP surface, the spatial confinement experienced by the tracer molecules at different diffusion distance scales may originate from different binder phase regions, leading to variations in the normalized apparent diffusion coefficient with increasing diffusion distance. The curve of change may show two or even more linear intervals with different slopes.
[0059] The reason is that within a short diffusion time interval, the diffusion displacement of tracer molecules is small, and they mainly detect the interface constraint formed by the direct contact between the new asphalt binder containing the tracer and the regenerator mixture and the mineral aggregate surface. At this time, the rate of decrease of the normalized apparent diffusion coefficient directly reflects the surface area of the mineral aggregate in contact with the new coated binder. However, within a longer diffusion time interval, the diffusion displacement of tracer molecules increases to the point that it can penetrate or sense the thickness direction constraint of the old asphalt film on the RAP surface, or sense the mineral aggregate interface at a more distant point. At this time, the slope may be mixed with the constraint information inside the old asphalt film and the influence of mass transfer resistance between different binder phases.
[0060] Therefore, when the normalized apparent diffusion coefficient exhibits at least two linear intervals as a function of diffusion distance, the effective film-forming area A of the asphalt binder is determined using the fitting slope of the short diffusion time interval. The short diffusion time interval corresponds to a smaller... Within this range, the normalized apparent diffusion coefficient decreases most steeply with increasing diffusion distance, and the absolute value of the fitted slope k is the largest. This slope is mainly attributed to the interfacial area between the new binder phase containing the tracer and the aggregate surface. Therefore, the effective film-forming area A calculated from this can more accurately reflect the actual aggregate contact area of the target asphalt film formed by the new asphalt binder and the rejuvenator. It can be expressed as follows:
[0061]
[0062] Where, k short The slope of the fit for the short diffusion time interval is given, and V is the volume of the binder phase containing the tracer. This is the conversion factor. The boundary between the short and long diffusion time intervals can be determined by the slope change point or inflection point of the normalized apparent diffusion coefficient curve, or by the behavior of the standard sample in the corresponding interval. To ensure the accuracy of area calculation, the linear fitting determination coefficient R0 within the short diffusion time interval is used. 2 It should be no less than 0.95. This treatment method effectively eliminates the interference of the internal confinement effect of the old RAP asphalt film on the determination of the effective film-forming area, ensuring that the area calibration result strictly corresponds to the calculation basis of the film-forming asphalt binder mass M0 in step S3.
[0063] In one embodiment, when the normalized apparent diffusion coefficient exhibits at least two linear intervals as the diffusion distance scale changes, the fitting slope corresponding to the long diffusion time interval is used, combined with the calibration of the standard sample in the corresponding interval, to obtain the effective confined scale of the RAP old asphalt binder phase, and accordingly correct the quality M of old asphalt effectively participating in film formation. pe And regenerators effectively participate in film formation quality M re .
[0064] In practice, within a long diffusion time interval, the diffusion of tracer molecules in the new binder phase containing the tracer has sufficiently sensed the interface between the tracer and the old RAP asphalt film, as well as the thickness direction limitations of the old asphalt film itself. The fitting slope k for the long diffusion time interval... long The absolute value is usually less than the slope k of the short-time interval. short The decay rate reflects the overall confinement of the tracer-containing binder phase on a large spatial scale, including the contribution of the RAP old bitumen film as a diffusion barrier or confined domain. By comparing the normalized apparent diffusion coefficient behavior over a long time interval with the calibration results of standard samples within the same diffusion distance scale, a parameter characterizing the effective confinement of the RAP old bitumen film can be extracted, called the effective confinement scale.
[0065] For example, by referring to the method for determining the effective film-forming area A, an equivalent long-range confined area parameter A can be defined for the long diffusion time interval. long Its value is determined by the fitting slope k over the long time interval. long Combining material phase volume V and conversion factor Multiplying them together, we get:
[0066] Among them, A long The difference between the effective film area A obtained in the short time interval and ΔA=AA long This reflects the reduction in the amount of additional confined interface perceived by the tracer over long diffusion distances due to the presence of the old RAP asphalt film, as the old asphalt film region constitutes a different confinement mode for tracer diffusion than the new binder-aggregate interface. This difference is related to the effective film-forming participation of the old RAP asphalt: if the old RAP asphalt is sufficiently softened and participates in film formation, the old and new binder phases tend to be homogeneous, and the slope difference between long and short time intervals decreases; conversely, if the old RAP asphalt is insufficiently activated, there are significant interface or viscosity differences between the old and new binder phases, resulting in a larger slope difference.
[0067] Therefore, we can use ΔA or the ratio of the slope of the long-term interval to that of the short-term interval. As a quantitative indicator, combined with the calibration curve or empirical relationship established by indoor calibration tests, the effective contribution of RAP old asphalt to film formation quality M, which was initially determined in step S4, is used to evaluate the film formation quality. pe And regenerators effectively participate in film formation quality M re Perform correction. The correction relationship can be reflected as follows:
[0068] M pe,corrected = f 1×( )×M pe Mre,corrected = f 2×( )×M re in, f 1 and f 2 represents the correction function determined by indoor calibration tests. f 1 is generally taken as a value between 0.6 and 1.2. f 2. The value is generally taken as 0.7~1.1. The calibration test uses a series of samples with known RAP old asphalt activation levels and recycling agent dosages, and determines the correlation between the slope ratio of long and short time intervals and the effective film quality. Through this correction step, the film area parameter, originally determined solely by the diffusion-restricted behavior of the new binder phase, can be correlated with the actual film-forming contribution of RAP old asphalt and the recycling agent, thus establishing the relationship between the new asphalt binder quality M in step S4. b The calculation incorporates the effective amount of old asphalt that more closely reflects the actual coating state, further improving the accuracy and reliability of determining the amount of binder.
[0069] In one embodiment, step S4 includes the following steps: S41, Determine the quality of RAP old asphalt M p And in conjunction with the regenerator dosage coefficient β, the regenerator mass M is calculated. r Specifically, the quality of RAP old asphalt M p This refers to the mass of old asphalt contained in a unit mass of RAP material, which can be obtained through RAP extraction testing or combustion methods. The extraction test uses a solvent to dissolve and separate the old asphalt on the RAP surface; after distillation to recover the solvent, the mass of the residual asphalt is weighed. The combustion method removes the asphalt through high-temperature burning, and the asphalt content is determined by the mass loss. The results obtained from the two methods should be cross-checked, and the final M... p Take the average value from multiple parallel tests, or a value that does not underestimate the quality of the old RAP asphalt according to engineering production control requirements. The recycling agent dosage coefficient β is defined as the recycling agent mass M. r Compared with RAP old asphalt quality M p The ratio, i.e., the mass percentage of the rejuvenator in the old asphalt, is determined by the RAP old asphalt recycling test. The specific procedure for the recycling test is as follows: old asphalt is extracted from RAP, and the proposed rejuvenator is added in different proportions. The penetration, viscosity, softening point, or dynamic shear rheological index of the recycled binder are measured. The amount of rejuvenator added when the performance recovers to the target design value is taken as β. The determination of β should comprehensively consider the aging degree of the old asphalt, the type and performance of the rejuvenator, and the performance grade requirements of the target binder. This yields M... p After adding β, the regenerant mass M r This can be determined by multiplying the two. It can be expressed as the following formula:
[0070] Mr =β×M p S42, based on RAP old asphalt quality M p Determine the effective contribution of RAP old asphalt to film formation quality M pe According to the regenerant mass M r Determine the effective role of regenerator in film formation quality M re .
[0071] During the trial mixing of RCA-RAP hot-mix recycled asphalt mixtures, under the combined effects of heating, mechanical mixing, and recycling agents, only a portion of the old asphalt on the RAP surface was softened, activated, and migrated to participate in the formation of the new target asphalt film. The remaining portion likely remained attached to the original RAP aggregate surface as an aged, hard shell, failing to effectively integrate into the new film-forming system. Therefore, the effective participation of old RAP asphalt in film formation quality M pe This refers to the total mass of RAP used asphalt (M). p The mass of the portion of the asphalt actually involved in forming the target asphalt film satisfies 0 ≤ M. pe ≤M p .
[0072] Similarly, during the interaction between the added rejuvenator and the old asphalt, part of it enters the old asphalt phase to soften and regenerate, and then participates in film formation. Another part may fail to form an effective film due to volatilization, absorption by RCA pores, or remaining in ineffective areas. Therefore, the effective participation of the rejuvenator in film formation affects the quality M. re Not exceeding the total mass M of the regenerant r That is, satisfying 0≤M re ≤M r .
[0073] M pe and M re All results are determined by indoor calibration tests. Indoor calibration tests should use materials corresponding to the RCA-RAP hot-mix recycled asphalt mixture to be determined, including RAP, RCA, new asphalt binder, and recycling agent from the same source, and be conducted at the same temperature and time as the actual trial mixing conditions. The determination method can be one or more of the following: microscopic image analysis, fluorescence tracer analysis, NMR signal integral change, or mass difference conversion. For example, when using the fluorescence tracer method, fluorescently labeled recycling agent or new asphalt can be added to the calibration sample, and the degree of mixing of the old and new binder phases can be statistically analyzed through fluorescence microscopy to estimate the effective film-forming proportion. When using NMR signal integral change, the effective film-forming quality can be quantitatively analyzed by comparing the changes in the binder phase signal before and after the recycling treatment of the calibration sample. When it is necessary to verify the indoor calibration results, solvent extraction comparison can be performed on the calibration sample. However, it should be noted that this extraction comparison is only used for verification of the indoor calibration test process and is not applicable to the formal samples that remain in the coated state in steps S1 and S2.
[0074] S43, Determination of the mass M of RCA pore-absorbing asphalt binder c And based on the film-forming asphalt binder quality M0 and the effective participation of RAP old asphalt in film-forming quality M pe Regenerants effectively contribute to film formation quality. re And RCA pore absorption asphalt binder quality M c Determine the quality M of the new asphalt binder. b .
[0075] Among them, the mass of RCA pore-absorbing asphalt binder M c This refers to the portion of the asphalt binder quality that is absorbed by residual mortar and open pores on the RCA surface and does not participate in the formation of the target asphalt film on the aggregate surface. M c The determination method is as follows: Take RCA samples of the same type and particle size as those in the mix proportion, and conduct an adsorption test with the proposed new asphalt binder, recycling agent, or a new asphalt binder-recycling agent mixture under conditions equivalent to the test mixing temperature and residence time. After the adsorption test, the mass of binder absorbed per unit mass of RCA is obtained by weighing the mass change of RCA before and after adsorption, or by measuring the mass difference of the remaining unadsorbed binder, etc., and then converting it into the mass of binder absorbed per unit mass of mixture according to the actual RCA content in the mix proportion. c The adsorption test should be performed in no fewer than three parallel tests, and the average value should be taken as M. c The test results, or the values that do not underestimate the quality of the new asphalt binder, should be taken according to the requirements of engineering production control.
[0076] After obtaining the above parameters, the mass M of the new asphalt binder b The following logic is used to determine the total mass of film-forming asphalt binder required to form the target asphalt film: M0. The film-forming contribution comes from three aspects: the effective participation of the old asphalt in the RAP film, M0, etc. pe The effective participation of regenerant M re And the newly added asphalt binder M b At the same time, the new asphalt binder also needs to compensate for the portion of M lost due to absorption by the RCA pores. c Therefore, the mass M of the new asphalt binder b Equals the total binder mass required for film formation M0 plus the RCA pore absorption loss M. c Subtract the effective film-forming contribution M already provided by RAP old asphalt and recycling agent. pe and M re It can be expressed as the following formula:
[0077] M b =M0-M pe -M re +Mc This embodiment integrates film-forming requirements, old material contribution, and pore absorption loss into a single quality balance framework, ensuring that the amount of new asphalt binder added is neither excessive, causing bleeding, nor insufficient, resulting in inadequate asphalt film thickness, thereby achieving precise determination of binder dosage.
[0078] In one embodiment, the regenerant dosage coefficient is the regenerant mass M. r Compared with RAP old asphalt quality M p The ratio, i.e., β=M r / M p .
[0079] The advantages of defining the recycling agent dosage coefficient using a ratio are twofold: Firstly, the physical meaning of β is clear, intuitively reflecting how much recycling agent needs to be added per unit mass of old asphalt to restore its performance, facilitating cross-sectional comparisons and experience accumulation under different RAP sources and old asphalt contents. Secondly, when the RAP blending ratio changes, leading to changes in M... p When changes occur, M can be automatically adjusted simply by maintaining the established β value. r This ensures the consistency of regeneration results and the ease of adjusting the mixing ratio.
[0080] In practice, the specific value of β is determined by the recycling test of RAP asphalt. The recycling test uses the asphalt extracted and recovered from RAP as the object, and adds the proposed recycling agent at different proportions, such as 5%, 8%, 10%, and 12% of the asphalt mass. After thorough mixing, the various performance indicators of the recycled binder are tested, including but not limited to penetration, softening point, ductility, viscosity, and dynamic shear rheological parameters. The minimum or optimal amount of recycling agent is determined based on the criterion of restoring these performance indicators to the target design value. The ratio of the recycling agent mass to the asphalt mass corresponding to this amount is β. For example, if the test determines that a certain RAP asphalt requires 8% of its mass of recycling agent to achieve the target penetration and softening point of the recycled binder, then β is taken as 0.08. For RAP with different aging degrees, different types of recycling agents, and different target performance levels, β should be determined by separate tests and should not be directly applied using empirical values. In engineering practice, the determination of β should also be comprehensively optimized by considering factors such as economy and workability.
[0081] In one embodiment, the effective film-forming mass of the RAP asphalt does not exceed the mass of the RAP asphalt, and the effective film-forming mass of the rejuvenator does not exceed the mass of the rejuvenator. This is because the portion of the RAP surface asphalt that can actually be activated and participate in the formation of the new target asphalt film cannot exceed the total amount of the asphalt itself; similarly, the portion of the rejuvenator that actually enters the binder film phase and contributes to film formation cannot exceed the total amount of rejuvenator added. Both parameters have a lower limit of zero, indicating that in extreme cases, such as severely aged RAP asphalt that cannot be activated, or the rejuvenator being completely absorbed by the RCA pores and failing to participate in film formation, the asphalt or rejuvenator may not contribute anything to the formation of the new asphalt film.
[0082] M pe The specific values are determined by indoor calibration tests. These tests simulate actual trial mixing conditions, including temperature, mixing time, and mixing intensity. The mixture containing RAP, RCA, new asphalt binder, and recycling agent is treated, and then appropriate methods are used to quantitatively distinguish which old asphalt components participated in the formation of the new film. Suitable methods include: microscopic image analysis, which involves observing the interface mixing state of the new and old binders using scanning electron microscopy or fluorescence microscopy and statistically analyzing the proportion of areas where the old asphalt film thins or disappears; fluorescence tracer analysis, which involves pre-introducing fluorescent markers into the recycling agent or new asphalt and determining the degree of intermixing and the amount of old asphalt migration through fluorescence intensity distribution; nuclear magnetic resonance signal integral change method, which utilizes the relaxation time differences of different binder components and calculates the effective participation amount by comparing the changes in binder phase signals before and after treatment; and mass difference conversion method, which calculates the amount of old asphalt transferred by accurately weighing the mass change of RAP before and after trial mixing and combining this with extraction verification. These methods can be used individually or in combination to improve the reliability of the calibration results. When it is necessary to verify the results of indoor calibration, solvent extraction can be performed on the calibration samples for comparison. The accuracy of the effective participation amount can be indirectly verified by measuring the properties of the residual binder on the surface of the mineral after extraction. It should be emphasized again that this extraction comparison is only used for the verification stage of the indoor calibration test process and is not applicable to the formal samples in the coated state used for nuclear magnetic resonance measurement in steps S1 and S2.
[0083] M re The calibration method and M pe Similarly, but with a focus on tracking the fate of the regenerator and its contribution to film formation. For example, the regenerator can be fluorescently or isotopically labeled, and after trial mixing, the proportion of the labeled material in the binder film phase and the RCA pore absorption phase can be measured to determine the effective proportion of the regenerator participating in film formation. Another example is that the effective film-forming contribution of the regenerator can be calculated from the mass difference between the film-forming binder with and without the addition of regenerator.
[0084] When the RAP old asphalt is relatively lightly aged and the old asphalt itself already has a certain film-forming ability, M pe Possibly close to M p At this point, the regenerant mainly functions to soften and reduce viscosity. re The contribution may be relatively small; conversely, when RAP old asphalt is severely aged, the film-forming contribution of the old asphalt itself is limited, M pe Possibly much smaller than M p It requires the combined action of a recycling agent and new asphalt binder to form a film, at which point M re Accurate calibration is particularly important for ensuring the precision of the total amount of binder used.
[0085] By analyzing M pe and M re Setting a reasonable range of values and quantifying the values through indoor calibration tests avoids the need to calculate the mass M of the new asphalt binder in step S43. b The underestimation of the contribution of old asphalt, resulting in insufficient new asphalt, manifests as incomplete film formation and insufficient asphalt film thickness. Conversely, the underestimation of the contribution of old asphalt, leading to an excess of binder, results in bleeding and reduced rutting resistance. These constraints, together with the calculation formula in step S43, constitute a complete mass balance system, ensuring that the contributions of each component are accurately accounted for.
[0086] In one embodiment, the tracer is an oil-soluble tracer capable of generating a recognizable nuclear magnetic resonance signal in the binder phase. The tracer is compatible with the new asphalt binder and the recycling agent, and does not change the coating state of the binder after the mixture in the sample.
[0087] The requirement that the tracer can generate a resolvable NMR signal in the binder phase is a prerequisite for implementing the NMR diffusion measurement of this invention. The tracer molecule must contain a detectable nucleus capable of generating a sufficiently strong signal in the NMR spectrometer that is distinguishable from the background signal of the binder itself. Optional detectable nuclei include... 1 H (hydrogen-1) 2 H (deuterium, hydrogen-2) or 19 F (Fluorine-19). Used 1 When the H nucleus is used, the difference between the proton peak of a specific chemical shift in the tracer molecule and the numerous aliphatic and aromatic proton signals in the asphalt binder can be used for differentiation, or the signal can be collected within the relaxation time interval where the background signal of the binder is weak. 2 When H nuclei are present, due to their extremely low natural abundance, tracers must be introduced in the form of deuterated compounds. The advantage of this is that the binder itself contains almost no deuterated compounds. 2 H, with minimal background interference and a high signal-to-noise ratio. (Using...) 19 In the F-core case, because fluorine compounds are almost non-existent in conventional asphalt binders, the signal resolution is high, and19 The nuclear magnetic resonance sensitivity of F is close to 1 H, the measurement efficiency is relatively high. The amount of tracer added is preferably 0.05% to 2.0% based on the mass of the asphalt binder. The lower limit of this range is determined by the sensitivity and signal-to-noise ratio requirements of NMR detection, while the upper limit is determined by the potential impact of the tracer on the properties of the binder and economic considerations. Too little addition may result in a weak signal and increased measurement error; too much addition may affect the rheological properties and film-forming characteristics of the binder, violating the requirement of not changing the coating state.
[0088] The compatibility requirement between the tracer and the new asphalt binder and recycling agent is that the tracer, within the range of trial mixing temperature (usually 140℃ to 180℃) and test temperature (usually room temperature to 60℃), does not exhibit visible stratification, precipitation, crystallization, or chemical reaction with the new asphalt binder and recycling agent, and can be uniformly dispersed in the binder phase at the molecular level. Compatibility can be verified through a premixing test: the tracer is mixed with the intended new asphalt binder, recycling agent, or a mixture of both at the planned dosage. After being kept at a constant temperature for a period of time at both the trial mixing temperature and the test temperature, observations are made for any stratification, turbidity, precipitation, or other phenomena. Samples are then taken for NMR signal uniformity testing. If the signal intensity remains consistent across different locations on the sample, it indicates that the tracer is uniformly distributed and has good compatibility. Optional oil-soluble NMR tracers include, but are not limited to: deuterated long-chain alkanes, deuterated aromatics, fluorinated organic compounds (such as perfluoropolyethers and fluorinated alkanes), and specific structures containing... 1 H or 19 F is an oil-soluble organic molecule. When making a specific selection, it is necessary to take into account the compatibility with the binder, the characteristics of the nuclear magnetic resonance signal (including chemical shift and relaxation time), as well as cost and safety and environmental protection requirements.
[0089] The key requirement is that the tracer does not alter the binder coating state after the trial mixing of the mixture in the sample, ensuring that the measurement results accurately reflect the film-forming behavior of the binder under actual construction conditions. If the addition of the tracer significantly alters the viscosity, surface tension, or wetting angle with the aggregate, the spreading and film-forming state of the binder on the RCA, RAP, new aggregate, and mineral powder surfaces during the trial mixing will differ from the actual working conditions without the tracer. This will affect the measured effective film-forming area A and the calculated mass M of the new asphalt binder. bThis would render it ineffective in guiding actual construction. Methods to verify whether a tracer affects the coating state include: comparing volumetric properties (such as porosity and aggregate void ratio) of trial mixtures with and without tracers under the same conditions; visually observing the uniformity and gloss of the binder coating; and statistically analyzing film thickness distribution through microscopic images. If there are no statistically significant differences in the above properties before and after adding the tracer, it can be confirmed that the tracer does not change the coating state. In engineering practice, tracer types with similar chemical structures to the binder and added in low-limit amounts are usually preferred to minimize potential interference with the coating state and binder properties.
[0090] Example 1 This embodiment uses the total mass of 1 t RCA, RAP, new aggregate, and mineral powder as the calculation basis; wherein, the mass of RAP is calculated based on the mass of RAP containing old asphalt. The mass ratio of RCA, RAP, new aggregate, and mineral powder is 25:35:36:4, and the old asphalt content of RAP is 4.8%.
[0091] Step 1: Conduct trial mixing according to the above blending ratio, and prepare a mixture sample of asphalt binder coated with oil-soluble nuclear magnetic resonance tracer after trial mixing using the initial amount of asphalt binder. The sample is unextracted by solvents, unsieved, and maintains the state where the surface of the aggregate is coated with asphalt binder.
[0092] Step 2: At the test temperature The free diffusion coefficient of the oil-soluble NMR tracer in a binder with the same composition and no mineral content was measured. The apparent diffusion coefficient of the mixture in the binder-coated state after trial mixing was measured. With diffusion time The changing relationship.
[0093] Step 3: Calibrate using standard samples prepared from minerals with known specific surface areas, where the surface area of the minerals that the binder can contact is also known. The known surface area of the minerals that the binder can contact in the standard samples is... for Combined with material phase volume for Fitting slope for ,but:
[0094]
[0095] The binder-coated mixture samples after trial mixing were tested, and the binder phase volume was measured. Fitting slope ,but:
[0096] In this embodiment, the normalized apparent diffusion coefficient is... The linear fit was performed over a short diffusion time interval, and the coefficient of determination was [value missing]. Not less than 0.95.
[0097] Step 4: Target Asphalt Film Thickness Pick Film-forming asphalt binder density Pick ,but:
[0098] Step 5: Determine the quality of RAP old bitumen by RAP extraction test:
[0099] Based on the RAP old asphalt recycling test, the recycling agent dosage coefficient β = 0.08, where β is the ratio of the recycling agent mass to the RAP old asphalt mass. Therefore:
[0100] Step 6: Determine the quality of RAP old asphalt through indoor calibration tests. The quality of the effective participation in the formation of the target asphalt film And determine the quality of the regenerant. The quality of the effective participation in the formation of the target asphalt film In this embodiment, and The indoor calibration samples prepared from RAP, RCA, new asphalt binder, and recycling agent corresponding to those in this embodiment were determined by fluorescence tracer analysis and conversion of the bonding mass difference. The mass of asphalt binder absorbed by RCA pores was measured by adsorption tests of RCA and new asphalt binder at corresponding trial mixing temperatures and residence times. The quality of the new asphalt binder is:
[0101]
[0102] Therefore, the mass of new asphalt binder corresponding to each 1t of RCA, RAP, new aggregate, and mineral powder is determined to be: The regenerant mass is .
[0103] Microscopic images, fluorescence microscopy images, or CT images capable of distinguishing the interface between binder and aggregate were used to statistically analyze the cross-sections of the test mixtures. For at least three parallel samples, at least five test areas were selected, and the binder film thickness being lower than the target asphalt film thickness within each test area was statistically analyzed. The proportion of the mineral surface area to the observed mineral surface area was used, and the average of the statistical results of each detection area was taken as the proportion of the insufficient film thickness area. According to the above method, the proportion of the insufficient film thickness area in Example 1 was 6.8%.
[0104] The determined new asphalt binder and recycling agent masses were used to re-mix the asphalt binder, and the effective film-forming area and new asphalt binder mass were repeatedly measured under the same test conditions. The verified new asphalt binder mass was 37.69 kg / t, and the verified effective film-forming area was 5756 m² / t. Based on the verification results, 37.77 kg / t was taken as the final amount of new asphalt binder used in this embodiment, and 1.34 kg / t was taken as the final amount of recycling agent used.
[0105] Example 2 This embodiment uses the total mass of 1 t of RCA, RAP, new aggregate, and mineral powder as the calculation basis; wherein, the mass of RAP is calculated based on the mass of RAP containing old asphalt. The mass ratio of RCA, RAP, new aggregate, and mineral powder is 35:25:36:4, and the old asphalt content of RAP is 4.5%. Compared with Example 1, this embodiment uses a material combination with a higher RCA content and more obvious RCA pore absorption characteristics.
[0106] Step 1: Conduct trial mixing according to the above blending ratio, and prepare a mixture sample of asphalt binder coated with oil-soluble nuclear magnetic resonance tracer after trial mixing using the initial amount of asphalt binder. The sample is unextracted by solvents, unsieved, and maintains the state where the surface of the aggregate is coated with asphalt binder.
[0107] Step 2: At the test temperature The free diffusion coefficient of the oil-soluble NMR tracer in a binder with the same composition and no mineral content was measured. The apparent diffusion coefficient of the mixture in the binder-coated state after trial mixing was measured. With diffusion time The changing relationship.
[0108] Step 3: Calibration is performed using standard samples prepared from minerals with known specific surface areas, and where the binder can contact the minerals with known surface areas. The binder-coated mixture samples after trial mixing are tested, and the binder phase volume is measured. Fitting slope The same conversion factors as in Example 1 were used. ,but:
[0109]
[0110] In this embodiment, the normalized apparent diffusion coefficient is... The linear fit was performed over a short diffusion time interval, and the coefficient of determination was [value missing]. Not less than 0.95.
[0111] Step 4: Target Asphalt Film Thickness Pick The density ρ of the film-forming asphalt binder is taken as ,but:
[0112] Step 5: Determine the quality of RAP old bitumen by RAP extraction test:
[0113] Based on the RAP old asphalt recycling test, the recycling agent dosage coefficient β = 0.08, where β is the ratio of the recycling agent mass to the RAP old asphalt mass. Therefore:
[0114] Step 6: Determine the quality of RAP old asphalt through indoor calibration tests. The quality of the effective participation in the formation of the target asphalt film And determine the quality of the regenerant. The quality of the effective participation in the formation of the target asphalt film In this embodiment, and The indoor calibration samples prepared from RAP, RCA, new asphalt binder, and recycling agent corresponding to those in this embodiment were determined by fluorescence tracer analysis and conversion of the bonding mass difference. The mass of asphalt binder absorbed by RCA pores was measured by adsorption tests of RCA and new asphalt binder at corresponding trial mixing temperatures and residence times. The quality of the new asphalt binder is:
[0115]
[0116] Therefore, the mass of new asphalt binder corresponding to each 1t of RCA, RAP, new aggregate, and mineral powder is determined to be: The regenerant mass is .
[0117] The determined new asphalt binder and recycling agent masses were used to re-mix the asphalt binder, and the effective film-forming area and mass of the new asphalt binder were repeatedly measured under the same test conditions. The verified mass of the new asphalt binder was 47.08 kg / t, and the verified effective film-forming area was 6271 m² / t. Based on the verification results, 47.21 kg / t was taken as the final amount of new asphalt binder used in this embodiment, and 0.90 kg / t was taken as the final amount of recycling agent used.
[0118] Comparative Example 1 The difference between this comparative example and Example 1 is that the binder content was determined based on the existing trial mix proportions of the same type of RCA-RAP hot-mix recycled asphalt mixture. The mass of the new asphalt binder determined from the existing trial mix proportions is... The quality of the recycling agent is determined based on the quality of the RAP old asphalt. .
[0119] The same statistical method as in Example 1 was used to analyze the cross-section of the trial mixture, and the area with insufficient film thickness accounted for 18.6%.
[0120] Comparative Example 2 The difference between this comparative example and Example 1 is that the specific surface area of the mineral obtained after solvent extraction and sieving is used instead of the effective film-forming area of the binder determined under the coating state after trial mixing; except for the above differences, the other parameters are taken with the same values as in Example 1. The calculated surface area of the extracted mineral is... ,but:
[0121]
[0122] The same RAP asphalt used in Example 1 effectively contributes to film formation quality. Regenerators effectively contribute to film formation quality. and RCA pore absorption asphalt binder quality The calculated mass of the new asphalt binder is:
[0123] The cross-section of the trial mixture was statistically analyzed using the same statistical method as in Example 1, and the area with insufficient film thickness accounted for 23.4%.
[0124] Comparative Example 3 The difference between this comparative example and Example 1 is that RCA is treated according to the adsorption characteristics of ordinary mineral materials, and the mass of RCA pore absorption binder is not separately included in the calculation. This method uses the same effective film-forming area of asphalt binder as in Example 1. Target asphalt film thickness Density of film-forming asphalt binder RAP (Reclaimed Asphalt) effectively contributes to film formation quality. Regenerators effectively contribute to film formation quality However, the mass of RCA pore absorption asphalt binder is not included separately, i.e., it is taken as... ,but:
[0125]
[0126] The cross-section of the trial mixture was statistically analyzed using the same statistical method as in Example 1, and the area with insufficient film thickness accounted for 21.7%.
[0127] The percentage of areas with insufficient film thickness in the above-mentioned trial mixtures was determined using the same statistical method, and the results are listed in Table 1.
[0128] Table 1. Percentage of Insufficient Film Thickness Area under Different Binder Dosage Determination Methods
[0129] As shown in Table 1, under the same statistical method, the proportion of insufficient film thickness area in Examples 1 and 2 is lower than that in each of the pairs.
[0130] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for determining the amount of binder for RCA-RAP hot mix recycled asphalt mixture, characterized in that, Includes the following steps: S1, add tracer according to the initial composition ratio of binder and prepare sample; S2, determine the free diffusion coefficient of the tracer in a binder with the same composition as the sample but without minerals, and determine the apparent diffusion coefficient of the tracer in the sample, and determine the effective film-forming area of the asphalt binder by combining the calibration results of a standard sample with known mineral surface area. S3, calculate the mass of film-forming asphalt binder required to form the target asphalt film based on the effective film-forming area of the asphalt binder; S4. Based on the quality of old asphalt effectively participating in film formation, the quality of recycling agent effectively participating in film formation, and the quality of RCA pore-absorbing asphalt binder, the quality of recycling agent and new asphalt binder are determined in combination with the quality of film-forming asphalt binder.
2. The method for determining the binder content of RCA-RAP hot mix recycled asphalt mixture according to claim 1, characterized in that, It also includes the following steps: S5. Substitute the mass of the recycling agent and the mass of the new asphalt binder obtained in step S4 into the initial mix proportion to prepare a new sample, and repeat steps S2 to S4 to obtain the verification results. If the new sample corresponds to the effective film-forming area of the asphalt binder, the mass of the new asphalt binder and the mass of the recycling agent determined in steps S2 to S4, then determine the mass of the recycling agent and the mass of the new asphalt binder obtained in step S4 as the final dosage.
3. The method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixture according to claim 1, characterized in that: Step S2 includes the following steps: S21, Determine the free diffusion coefficient of the tracer in a binder with the same composition as the sample but without minerals; S22, Determine the apparent diffusion coefficient of the tracer in the sample at different diffusion times; S23, calculate the ratio of the apparent diffusion coefficient to the free diffusion coefficient to obtain the normalized apparent diffusion coefficient; S24, The diffusion distance scale is linearly fitted with the normalized apparent diffusion coefficient to obtain the fitting slope, wherein the diffusion distance scale is characterized by the square root of the product of the free diffusion coefficient and the diffusion time. S25, the effective film-forming area of the asphalt binder is determined by multiplying the absolute value of the fitting slope, the volume of the binder phase containing the tracer, and the conversion factor obtained from the standard sample calibration.
4. The method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixture according to claim 3, characterized in that: The standard sample is an asphalt binder-coated aggregate sample with known aggregate surface area, known binder phase volume, and containing a tracer. The conversion factor is obtained through the following steps. S251, Under the same test conditions as the sample, determine the slope of the normalized apparent diffusion coefficient of the standard sample on the diffusion distance scale and the volume of the binder phase in which the tracer is located. S252, the conversion factor is obtained by dividing the known surface area of the standard sample by the product of the volume of the bound phase of the standard sample and the absolute value of the fitting slope.
5. The method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixture according to claim 3, characterized in that: When the normalized apparent diffusion coefficient exhibits at least two linear intervals as the diffusion distance scale changes, the effective film-forming area of the asphalt binder is determined using the fitting slope of the short diffusion time interval.
6. The method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixture according to claim 3, characterized in that: When the normalized apparent diffusion coefficient exhibits at least two linear intervals as the diffusion distance scale changes, the fitting slope corresponding to the long diffusion time interval is used, combined with the calibration of the standard sample in the corresponding interval, to obtain the effective confined scale of the RAP old asphalt binder phase, and thereby correct the effective participation of the old asphalt in film formation quality and the effective participation of the regenerator in film formation quality.
7. The method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixture according to claim 1, characterized in that: Step S4 includes the following steps: S41, Determine the quality of RAP old asphalt and calculate the quality of recycling agent by combining the recycling agent dosage coefficient; S42, determine the effective film-forming quality of RAP old asphalt based on the quality of the RAP old asphalt, and determine the effective film-forming quality of the rejuvenator based on the quality of the rejuvenator. S43, determine the quality of RCA pore-absorbing asphalt binder, and determine the quality of new asphalt binder based on the quality of film-forming asphalt binder, the quality of RAP old asphalt effectively participating in film formation, the quality of recycling agent effectively participating in film formation, and the quality of RCA pore-absorbing asphalt binder.
8. The method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixture according to claim 7, characterized in that: The recycling agent dosage coefficient is the ratio of the recycling agent mass to the RAP old asphalt mass.
9. The method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixture according to claim 7, characterized in that: The effective film-forming mass of the RAP old asphalt does not exceed the mass of the RAP old asphalt, and the effective film-forming mass of the regenerator does not exceed the mass of the regenerator.
10. The method for determining the amount of binder in RCA-RAP hot-mix recycled asphalt mixture according to claim 1, characterized in that: The tracer is an oil-soluble tracer capable of generating resolvable nuclear magnetic resonance signals in the binder phase. The tracer is compatible with new asphalt binder and recycling agent, and does not change the coating state of the binder after the mixture in the sample is mixed.