A method for measuring stress wave velocity of log cross section based on wood orthotropic symmetry
By establishing a stress wave velocity measurement method based on orthogonal symmetry of wood, the problem of insufficient accuracy caused by neglecting orthogonal symmetry in wood testing is solved. This method enables accurate prediction of stress wave velocity and improves the reliability of test results, and is applicable to hardwoods such as oak and ash.
Patent Information
- Application Number
- CN202611148649.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-24
AI Technical Summary
Existing stress wave testing technology fails to effectively consider the orthogonal symmetry of wood in the wood field, resulting in insufficient testing accuracy and ignoring the influence of grain direction, thus causing errors in the testing results.
A method for measuring stress wave velocity in log cross sections based on the orthogonal symmetry of wood is established. By establishing an orthogonal anisotropic elastic constitutive model of wood, a mathematical model of grain angle and static elastic modulus is derived. Combined with the mathematical model of stress wave propagation velocity and grain angle, stress wave parameters are measured using a stress wave meter. Outliers are eliminated, nonlinear regression analysis is performed, fitting parameters are determined, and rapid calculation of wave velocity is achieved.
It eliminates the wave velocity calculation deviation caused by texture direction, improves the accuracy and reliability of detection results, reduces the dispersion of test data, is suitable for stress wave velocity prediction under different texture angles, and improves the anti-interference and stability of detection.
Smart Images

Figure CN123155665A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of non-destructive testing technology for wood, specifically to a method for measuring the stress wave velocity of log cross sections based on the orthogonal symmetry of wood. Background Technology
[0002] Stress wave testing is one of the most commonly used testing methods in the field of non-destructive testing of wood. With its advantages of low destructiveness, high efficiency, and wide applicability, it has become an important technical means for the quality inspection of wood structures. The principle of stress wave testing relies on the correlation between the propagation law of stress waves and the physical properties of wood. The quantitative relationship between wave velocity and elastic modulus is the key theoretical basis for achieving wood performance evaluation.
[0003] However, as a naturally formed biocomposite material, wood exhibits an ordered arrangement of cellulose, hemicellulose, and lignin at the microscopic level. This structure results in significant anisotropy in its mechanical properties. The trunk, macroscopically composed of a series of concentric annual rings, gives the anisotropic wood an approximately cylindrical symmetry in space. This orthogonal symmetry significantly affects the mechanical properties of wood. Furthermore, the spatial differences in wood's mechanical parameters also have a significant impact on stress wave propagation characteristics.
[0004] Currently, most research on stress wave detection technology in the wood field is based on the isotropic assumption. However, systematic research on the correlation between orthogonal symmetry within the wood cross-section and stress wave propagation characteristics is insufficient, limiting the accuracy and reliability of stress wave detection. In recent years, the influence of wood grain direction on stress wave propagation has begun to receive attention. Studies have shown that the propagation speed of stress waves along the wood grain direction is significantly higher than that perpendicular to the grain direction; and numerical simulation analysis has confirmed that changes in the wood grain angle cause a deflection of the stress wave propagation path. Therefore, in practical testing, ignoring the anisotropic characteristics of wood and relying solely on wave velocity data obtained through linear calculations to evaluate wood performance can easily lead to erroneous test results. Summary of the Invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention aims to provide a method for measuring stress wave velocity in the cross-section of logs based on the orthogonal symmetry of wood, thereby solving the technical problem of insufficient stress wave detection accuracy caused by neglecting the orthogonal anisotropy of wood in the prior art.
[0006] The objective of this invention is achieved through the following technical solution: A method for determining the stress wave velocity of a log cross section based on the orthogonal symmetry of wood includes the following steps: Step 1: Establish an orthogonal anisotropic elastic constitutive model for wood; In the principal axis coordinate system (L,R,T), its constitutive equation is expressed in matrix form: (1) (1) In the formula: s x ,s y ,s z It is normal stress; t yz ,t zx ,t xy It is shear stress; e x ,he y ,he z It is linear strain; c yz ,c zx ,c xy It is shear strain; (1) In the formula (2) (3) (2) Where: E i、 E j This represents the static elastic modulus of tension and compression in the three principal axis directions. i or j=T,L,R ; m ij This represents 6 Poisson's ratios; i or j = T,L,R ,in i Indicates the direction of the force. j Indicates the direction of deformation; (3) Where: G LR ,G RT ,G TL It is a decision y direction and z direction, z direction and x direction, x direction and y The shear modulus of the change in the angle between directions; Step 2: Establish a mathematical model of the texture angle and static elastic modulus on the cross-section; A specimen is selected from the cross-section of the wood and rotated by an angle γ around the longitudinal axis to form a new coordinate system. Based on the principle of coordinate transformation of the elastic constants of orthotropic materials, the grain angle is derived. c Expression for the elastic modulus parameter in the direction: (4) Simplify formula (4) to its engineering application form: (5) Right now: (6) In formula (6) Indicates texture direction deflection c The simplified model of the lateral static elastic modulus after the angle not only retains the influence trend of the texture angle on the static elastic modulus, but also reduces the computational complexity, making it easier to establish a correlation with the stress wave propagation speed later. Step 3: Establish a mathematical model of the stress wave propagation velocity and texture angle; There is a positive correlation between the dynamic modulus of elasticity and the static modulus of elasticity of wood. Substitute it into the mechanical wave velocity formula , u For stress wave velocity, E For the dynamic elastic modulus of wood, D For the density of wood materials, g In the case of gravitational acceleration, we get: ; Substituting formula (6) into the relationship between the static elastic modulus of wood and the propagation velocity of stress waves: A mathematical model for the propagation velocity of stress waves under different texture angles within the cross-section was obtained: (7) Based on the mathematical model (7) relating stress wave propagation velocity to texture angle constructed above, calculating the wave velocity requires knowing the density and static elastic modulus of the wood; since the density and static elastic modulus of the same sample are constant, and the gravitational acceleration in formula (7) is... g It is 9.81 m / s². A The constant is used; to facilitate the fitting of experimental data, experimental fitting parameters are introduced. a,b,c,n ;Simplify formula (7) to its engineering application form: (8) In the formula, u γ Indicates texture angle as c Stress wave propagation speed at that time c For arbitrary texture angles a,b,c,n These are the fitting parameters.
[0007] The wood is oak or ash, and the specimens are healthy, defect-free logs with a diameter at breast height of 20-22 cm and a tree height of 15-18 m, which are processed into 8 standard specimens of 15 cm in length, with 4 specimens of each type of wood.
[0008] Stress wave parameters were measured using a stress wave meter with a time accuracy of 0.1 μs and a wave velocity measurement range of 100-6000 m / s.
[0009] The following steps are included in the setup of measuring points and data acquisition: A receiving probe is fixed 2cm from the top surface of the log, and a transmitting probe is arranged in the same cross section. The angle between the transmitting and receiving line and the tangent of the annual ring is defined as the texture angle γ. Eight vertical parallel cross sections are arranged along the log axis, with an adjacent spacing of 5cm, and numbered 1-8. The specimens were equilibrated under constant temperature and humidity for 2 weeks, and the moisture content was monitored at multiple points until it stabilized; the test section was polished to ensure clear growth ring texture. Select reference receiving points at the edges of each measurement section, fit the receiving probe tightly against the surface of the specimen, and apply Vaseline as a coupling agent. The annual ring tangent was drawn with the receiving end as the tangent point. The texture angle γ was adjusted with a protractor. The stress wave propagation time T and the probe distance L corresponding to γ = 10°--90° in 10° intervals were measured. Each group was repeated 3 times and the average value was taken. Single cross section was tested in both clockwise and counterclockwise directions. A total of 16 sets of data were collected for a single specimen. The stress wave propagation velocity u is calculated according to formula (9): (9) Where u is the propagation speed (m / s), L is the sample length (m), and T is the propagation time (s).
[0010] The box plot method was used with the interquartile range (IQR) as the criterion to identify and remove data that exceeded 1.5 times the IQR range as outliers.
[0011] The nonlinear regression analysis function of SPSS statistical software was used to fit the model, with the texture angle γ as the independent variable and the mean wave velocity u as the dependent variable. The undetermined constants a, b, c and n in the model (8) were determined by iterative calculation.
[0012] When the wood is oak, the fitting equation is: (10) The goodness of fit R² = 0.967.
[0013] When the wood is ash, the fitting equation is: (11) The goodness of fit R² = 0.939.
[0014] The method is used for non-destructive testing of stress waves in logs. It predicts the propagation speed of stress waves by using the texture angle γ, thus eliminating the wave speed calculation deviation caused by the texture direction. Beneficial effects
[0015] 1. This application breaks through the inherent defects of the isotropic assumption in traditional wood stress wave detection. Based on the orthogonal symmetric anisotropic constitutive relation of wood LRT, a quantitative correlation model of texture angle, elastic modulus and stress wave velocity is established to eliminate the wave velocity calculation deviation caused by texture direction, and the detection results are accurate.
[0016] 2. This application accurately characterizes the wave velocity-grain angle law, clearly defining the variation law of stress wave velocity in the cross section of logs as the grain angle increases (gradual increase from 0° to 40°, significant increase from 40° to 70°, and stabilization from 70° to 90°), achieving accurate prediction of wave velocity in different grain directions of oak and ash hardwood logs, with a fitting determination coefficient R² ≥ 0.939.
[0017] 3. This application enhances the anti-interference and stability of the test. By eliminating outliers using the box-line method, correcting the elastic modulus of coordinate transformation, and optimizing the interface loss reduction of the coupling agent, it effectively reduces the interference of local defects (knots), tissue dispersion, and contact loss of wood on the wave velocity test. The test data dispersion is reduced by more than 20%, and the repeatability error of a single test is ≤5%.
[0018] 4. This application optimizes the engineering applicability and universality by simplifying the complex orthogonal anisotropy theory into an engineering mathematical model with fitting parameters. It eliminates the need for complex stiffness coefficient conversion and directly achieves rapid wave velocity calculation through texture angle, making it suitable for on-site non-destructive testing of logs. It is also applicable to various hardwoods such as oak and ash, balancing theoretical rigor with practical application.
[0019] 5. This application ensures the reliability of test results by establishing a three-in-one testing system of "orthogonal symmetry theoretical modeling, experimental fitting correction, and outlier data removal." This system fundamentally avoids performance misjudgments caused by anisotropy, providing stable and accurate stress wave detection data support for timber structure safety assessment and timber grading. This invention combines experimental testing and data fitting, using nonlinear regression analysis to determine undetermined model constants and reveal the influence of the grain angle within the cross-section on wave velocity. This invention overcomes the inherent defects of the isotropic assumption in traditional timber stress wave detection, achieving rapid wave velocity calculation through the grain angle. The model determination coefficients R² for oak and ash are 0.967 and 0.939, respectively, effectively eliminating wave velocity calculation deviations caused by grain direction. This enables accurate prediction of stress wave propagation speed under different grain angles, improving the accuracy and applicability of timber stress wave detection. Attached Figure Description
[0020] Figure 1 This is a schematic diagram of an orthogonal symmetric model of wood.
[0021] Figure 2 This is a schematic diagram of a micro-element and stress symbols.
[0022] Figure 3 This is a schematic diagram of a coordinate system that rotates around a fixed axis.
[0023] Figure 4 This is a schematic diagram of the texture angle.
[0024] Figure 5 Box plot of stress wave propagation velocity corresponding to the same grain angle of oak.
[0025] Figure 6 Box plot of stress wave propagation velocity corresponding to the same texture angle of ash wood.
[0026] Figure 7 This is a graph of the oak model.
[0027] Figure 8 This is a curve diagram of the Manchurian ash model.
[0028] Figure 9 This is a test diagram. Detailed Implementation
[0029] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments: Example 1: 1. A method for determining the stress wave velocity of a log cross section based on the orthogonal symmetry of wood, comprising the following steps: Step 1: Establish an orthotropic elastic constitutive model for wood.
[0030] The orthogonal symmetry of wood is manifested in three mutually perpendicular material symmetry axes: longitudinal (L) parallel to the trunk growth direction, radial (R) along the diameter direction (from the pith to the bark), and chordal (T) perpendicular to the radial direction. For a detailed orthogonal symmetry model of wood, see [link to model]. Figure 1 .
[0031] Figure 1 A schematic diagram of an orthogonal symmetric model of wood; Based on the elastic coefficient equation of orthogonally symmetric wood, in engineering applications, wood can be approximated as a linear elastic material, and its stress-strain relationship satisfies the generalized Hooke's law. For orthotropic wood, in the principal axis coordinate system ( L,R,T Under these conditions, its constitutive equation can be expressed in matrix form: (1) (1) In the formula (2) (3) (1) In the formula: s x ,s y ,s z It is normal stress; t yz ,t zx ,t xy It is shear stress; e x ,he y ,he z It is linear strain; c yz ,c zx ,c xy Shear strain (e.g.) Figure 2 (As shown).
[0032] (2) Where: E i (E j ) Represents the tensile and compressive static elastic modulus in the three principal axis directions, ( i or j=T,L,R ); m ij Represents 6 Poisson ratios ( i or j = T,L,R ),in i Indicates the direction of the force. j It represents the direction of deformation.
[0033] (3) Where: G LR ,G RT ,G TL It is a decision y direction and z direction, z direction and x direction, x direction and y Shear modulus as the angle between directions changes.
[0034] Figure 2 Schematic diagram of infinitesimal elements and stress symbols; Step 2: Establish a mathematical model of the texture angle and static elastic modulus on the cross section.
[0035] In actual working conditions, the coordinate system of timber components often deviates from its orthogonal principal axis coordinate system. In this case, the grain direction of the specimen forms a certain angle with the principal axis direction (i.e., the grain angle), causing its static modulus of elasticity to change with the grain angle. To establish the relationship between the grain angle and the static modulus of elasticity, assume a specimen is selected on the cross-section of the timber (RT plane), and rotated by an angle γ around the longitudinal axis (y-axis) to form a new coordinate system (x′, y, z′), as follows... Figure 3 As shown.
[0036] Figure 3 A schematic diagram of a coordinate system rotating about a fixed axis y; Based on the principle of coordinate transformation of elastic constants in orthotropic materials, arbitrary texture angles... c Transverse static elastic modulus parameter in the direction ( The static elastic modulus in the direction of rotation can be derived through coordinate transformation. For RT The core of in-plane static elastic modulus parameter transformation is to convert the stiffness coefficients along the principal axes to the rotated coordinate system. Through transformation operations, combined with the generalized Hooke's law, the texture angle is finally obtained. c Expression for the elastic modulus parameter in the direction: (4) To simplify the calculation, experimental fitting parameters are introduced. By measuring the static elastic modulus at different texture angles, formula (4) can be further simplified into a form suitable for engineering applications: (5) Equation (5) can also be written as: (6) In formula (6) Indicates texture direction deflection c The simplified model of the transverse static elastic modulus after the angle not only retains the influence trend of the texture angle on the static elastic modulus, but also reduces the computational complexity, making it easier to establish a correlation with the stress wave propagation velocity later.
[0037] Step 3: Establish a mathematical model of stress wave propagation velocity and texture angle.
[0038] Studies have shown that, under the same experimental conditions, there is a positive correlation between the dynamic modulus of elasticity and the static modulus of elasticity of wood. Therefore, it can be approximately considered that... ( A (where is a constant). Substitute this into the mechanical wave velocity formula. ( u For stress wave velocity, E For the dynamic elastic modulus of wood, D For the density of wood materials, g In the case of gravitational acceleration, we can obtain: .
[0039] Substituting the derived formula (6) into the relationship between the static elastic modulus of wood and the propagation velocity of stress waves: A mathematical model for the propagation velocity of stress waves under different texture angles within the cross-section was obtained: (7) Based on the mathematical model (7) relating stress wave propagation velocity to texture angle constructed above, calculating the wave velocity requires knowledge of the wood's density and static modulus of elasticity. Since the density and static modulus of elasticity of the same sample are constant, and the gravitational acceleration in formula (7) is... g It is 9.81 m / s². A It is a constant. To facilitate the fitting of experimental data, experimental fitting parameters are introduced. a,b,c,n Formula (7) can be further simplified into a form that is easier for engineering applications: (8) In the formula, u γ Indicates texture angle as c Stress wave propagation speed at that time c For arbitrary texture angles a,b,c,n These are the fitting parameters.
[0040] Step 4: Data collection.
[0041] Log specimens were selected and equilibrated under constant temperature and humidity for two weeks, with moisture content monitored at multiple points until stable. The test sections were then sanded to ensure clear annual ring patterns. Reference receiving points were selected at the edges of each measurement section, and the receiving probes were tightly fitted to the specimen surface. Vaseline was applied as a coupling agent to reduce interfacial contact loss.
[0042] The annual ring tangent was drawn with the receiving end as the tangent point. The texture angle γ was adjusted with a protractor. The stress wave propagation time T and probe distance L were measured at γ=10°, 20°, 30°, ..., 90° intervals of 10°. Each group was repeated 3 times and the average value was taken. The single cross section was tested in both clockwise and counterclockwise directions. A total of 16 sets of data were collected for a single specimen.
[0043] The stress wave propagation velocity u is calculated according to formula (9): (9) Where u is the propagation speed (m / s), L is the sample length (m), and T is the propagation time (s).
[0044] Step 5: Data processing and outlier removal.
[0045] The box plot method was used, with the interquartile range (IQR) as the criterion, to identify and remove data that exceeded 1.5 times the IQR range as outliers.
[0046] Step Six: Model Fitting and Validation.
[0047] Based on the stress wave propagation velocity and texture angle relationship model established by formula (8), and combined with the experimental data after removing outliers, the nonlinear regression analysis function of SPSS statistical software was used to fit the model. During the fitting process, the texture angle γ was used as the independent variable and the mean wave velocity u was used as the dependent variable. The undetermined constants a, b, c and n in the model were determined by iterative calculation.
[0048] The regression analysis results show that the fitting equation for the oak sample is: (10) The goodness of fit R² = 0.967 indicates that the model can explain 96.7% of the wave velocity variation, demonstrating excellent fitting performance.
[0049] The fitting equation for the Manchurian ash sample is: (11) The goodness of fit R² = 0.939, the model's explanatory power reached 93.9%, and the fitting effect was good.
[0050] The method described is used for non-destructive testing of stress waves in logs. It predicts the propagation velocity of stress waves by using the grain angle γ, thus eliminating the wave velocity calculation deviation caused by the grain direction. Example 2: Experimental materials, instruments and methods Test materials The experiment selected two high-quality hardwoods with high economic value, oak and ash, from Fangzheng County, Heilongjiang Province. The test materials were healthy, defect-free logs with a diameter at breast height of 20-22 cm and a tree height of 15-18 m. They were processed into 8 standard specimens of 15 cm in length (4 sections of each type). The two ends of the specimens were polished flat and perpendicular to the axis to reduce the interference of stress wave interface reflection.
[0051] Test instruments Stress wave parameters were measured using a Microsecond Timer stress wave meter from FAKOPP, Hungary. The instrument has a time accuracy of 0.1 μs and a wave velocity measurement range of 100-6000 m / s, making it suitable for non-destructive testing of wood. The instrument includes a main unit, acquisition software, transceiver probes, and a firing hammer, which can excite longitudinal stress wave frequencies of 1-5 kHz.
[0052] Auxiliary equipment: 1mm precision steel tape measure, 0.1° precision digital protractor, 120 / 240 grit sandpaper, 1g precision electronic scale and moisture content meter.
[0053] Test methods Measurement point layout and texture angle definition A receiving probe is fixed 2cm from the top surface of the log, and a transmitting probe is placed on the same cross section. The angle between the transmitting and receiving line and the tangent of the growth ring is defined as the grain angle. c (See Figure 5 Eight vertical parallel sections are arranged along the axis of the log, with an adjacent spacing of 5cm, numbered 1-8.
[0054] Experimental Procedure and Data Acquisition This experiment uses the cross-sectional point-to-point stress wave propagation test method. The specific operating steps are as follows: Specimen pretreatment: The specimens were equilibrated under constant temperature and humidity for 2 weeks, and the moisture content was monitored at multiple points until it stabilized to eliminate moisture content interference; the test section was polished to ensure clear growth ring texture.
[0055] Probe installation and coupling: Select a reference receiving point at the edge of each measurement section, fit the receiving probe tightly against the surface of the specimen, and apply Vaseline as a coupling agent to reduce interface contact loss and ensure stress wave transmission efficiency.
[0056] Texture angle setting and parameter measurement: Draw the tangent line of the annual rings with the receiving end as the tangent point, and use a protractor to precisely adjust the texture angle. c Measurement c = Stress wave propagation time corresponding to 10°, 20°, 30°, ..., 90° intervals. T Spacing between probes L Each group was repeated 3 times and the average value was taken; single cross-section was tested in both clockwise and counterclockwise directions, and a total of 16 sets of data were collected for a single specimen.
[0057] Wave velocity determination: The stress wave propagation velocity is calculated according to formula (9). u Used to analyze its relationship with texture angle c The relationship between them (9) in, u The propagation speed (m / s) L The sample length is (m). T The propagation time is in seconds (s).
[0058] Figure 4 Texture angle diagram Figure 9 Test diagram; Wave velocity measurement results and analysis Tables 1 and 2 list the stress wave propagation velocities of oak and ash samples at different texture angles, as well as the average velocities at each texture angle. The average data show that, overall, the stress wave propagation velocity increases with increasing texture angle. c At a grain angle of 10°, the average stress wave propagation velocity is the lowest, with average velocities of 545.46 m / s for oak and 469.15 m / s for ash; while at a grain angle of 10°, the average velocity is the lowest. c At 90°, the average propagation speed reaches its maximum, with average speeds of 946.81 m / s for oak and 869.27 m / s for ash.
[0059] Table 1. Propagation velocity of stress waves on the cross-section corresponding to different grain angles of oak.
[0060] Note: c Let u be the texture angle, u1 be the propagation speed corresponding to the first group of different texture angles, u2 be the second group, ..., u16 be the sixteenth group, and u mean be the average value of the propagation speed corresponding to the same texture angle in the sixteen groups.
[0061] Table 2. Propagation velocity of stress waves on the cross-section corresponding to different texture angles of ash wood.
[0062] Note: c Let u be the texture angle, u1 be the propagation speed corresponding to the first group of different texture angles, u2 be the second group, ..., u16 be the sixteenth group, and u mean be the average value of the propagation speed corresponding to the same texture angle in the sixteen groups.
[0063] In this test, the average velocity measured for the ash sample at a texture angle of 30° was actually lower than the corresponding result at a texture angle of 20°. Based on the analysis of the sample cross-sectional characteristics, this abnormal fluctuation is likely related to local defects present in that texture angle direction. These defects can affect the normal propagation of stress waves to some extent, causing the measured values to deviate from the overall variation pattern.
[0064] Tables 1 and 2 show the stress wave propagation velocities and mean values of oak and ash wood at different grain angles, respectively. The experimental results show that the stress wave velocities of both types of wood exhibit an overall increasing trend with increasing grain angle, consistent with theoretical analysis. The stress wave velocity of oak is... c The value is lowest at 10°, with an average of 545.46 m / s, and increases continuously as the texture angle increases. c The wave velocity peaked at 940.56 m / s at 90°, representing a total increase of 72.4%. The rate of increase in wave velocity exhibited a phased pattern: a gradual increase from 10° to 40° (20.3%), a significant increase from 40° to 70° (34.3%), and a slower increase from 70° to 90° (6.7%). This trend is determined by the arrangement of wood cells: smaller grain angles (near radial) result in looser cells and denser wood rays, restricting wave transmission; as the grain angle increases (near tangential), the cells become more compact, enhancing the compatibility between fibers and wave propagation direction, thus increasing wave velocity. The wave velocity variation trend in ash is similar to that of oak, but the overall wave velocity is lower, consistent with the positive correlation between wood density and stress wave velocity. c =10° average wave velocity 469.15 m / s, c=90° reaches 974.24m / s, with a total increase of 107.7%; only c An anomaly occurred at 30°, with a wave velocity of 556.56 m / s lower than [previous value]. c The 578.36 m / s value at 20° was detected as being caused by a 5 mm micro-scar in that direction. The scar disrupts tissue continuity and interferes with wave propagation. This outlier needs to be removed in subsequent analyses to ensure accuracy.
[0065] Mathematical model fitting of stress wave propagation velocity and texture angle Data processing: Before modeling, outliers in the original data should be identified and removed to prevent them from reducing the accuracy of the mathematical model. This study uses box plots, with the interquartile range (IQR) as the criterion, to identify and remove data exceeding 1.5 times the IQR range as outliers.
[0066] Figure 5 Box plot of stress wave propagation velocity corresponding to the same grain angle in oak; Figure 6 Box plot of stress wave propagation velocity corresponding to the same texture angle in ash wood; Box plot analysis of the experimental data was performed using SPSS statistical software, and the results are as follows: Figure 5 and Figure 6 As shown. In the oak sample, the seventh set of data is... c The wave velocity at 80° (1675.21 m / s) exceeds the upper limit (1320.50 m / s), and the eighth set of data... c The wave velocity at 30° (936.36 m / s) exceeds the upper limit (850.20 m / s) and is therefore considered an outlier; in the Manchurian ash sample, the fifteenth set of data... c The wave velocity at γ=30° (490.80 m / s) is below the lower limit (500.10 m / s), while the wave velocity at γ=10° (563.64 m / s) in the eighth data set exceeds the upper limit (550.30 m / s), and is therefore identified as an outlier. After removing the outliers, the mean of the remaining data was recalculated to provide a reliable data foundation for subsequent model fitting.
[0067] Mathematical model fitting and evaluation: Based on the stress wave propagation velocity and texture angle relationship model established by formula (8), and combined with the experimental data after removing outliers, the nonlinear regression analysis function of SPSS statistical software was used to fit the model. During the fitting process, the texture angle γ was used as the independent variable, and the mean wave velocity was used as the mean value. u As the dependent variable, the undetermined constants in the model are determined through iterative calculation. a,b,c and n .
[0068] The regression analysis results show that the fitting equation for the oak sample is: (10) The goodness of fit R² = 0.967 indicates that the model can explain 96.7% of the wave velocity variation, demonstrating excellent fitting performance.
[0069] The fitting equation for the Manchurian ash sample is: (11) The goodness of fit R² = 0.939, the model's explanatory power reached 93.9%, and the fitting effect was good.
[0070] Figure 7 Oak model curve diagram; Figure 8 Ash tree model curve diagram; Figure 7 and Figure 8 The figures show a comparison between the model fitting curves and measured data points for oak and ash. As can be seen from the figures, the measured data points for oak are generally distributed above the fitted curve. This is because oak has smaller density fluctuations and fewer internal defects, resulting in an actual wave velocity slightly higher than the model's prediction. The measured data points for ash, on the other hand, are evenly distributed on both sides of the fitted curve, indicating that the model describes the wave velocity variation of ash more evenly. The fitted curves for both types of wood show an increasing trend with increasing grain angle, and the slope is relatively large in the range of 40°-70°, consistent with the variation characteristics of the experimental data.
[0071] This application concludes that the following conclusions are reached. (1) The propagation speed of stress waves in the cross section of wood shows a significant upward trend with the increase of the grain angle. The increase is 30%-40% in the 40°-70° range, while the changes in the 0°-40° and 70°-90° ranges are gradual, with an increase of less than 10%. This reflects the significant influence of the grain direction on the propagation path and energy dissipation of stress waves.
[0072] (2) The orthogonal symmetry principle can effectively characterize the propagation law of stress waves in the cross section of wood. By establishing an orthogonal anisotropic elastic model and deriving the analytical relationship between texture angle and wave velocity, it is confirmed that the orthogonal anisotropy of wood is an important factor affecting the propagation speed of stress waves.
[0073] (3) The fitting model constructed based on the experimental data has high accuracy. The coefficients of determination R² for oak and ash are 0.967 and 0.939, respectively, with small root mean square errors, which can accurately predict the propagation speed of stress waves under different texture angles.
[0074] (4) Local defects inside the wood can cause abnormal fluctuations in the propagation velocity of stress waves. Ash wood samples in c At 30°, the presence of knots resulted in a significantly lower wave velocity, indicating that when evaluating wood quality, it is necessary to comprehensively consider multiple aspects such as wood surface characteristics and wave velocity.
[0075] Example 3: This application breaks through the inherent defects of the isotropic assumption in traditional wood stress wave detection. Based on the orthogonal symmetric anisotropic constitutive relation of wood LRT, a quantitative correlation model of texture angle, elastic modulus and stress wave velocity is established, eliminating the wave velocity calculation deviation caused by texture direction. The reliability of the detection results is improved by more than 15% compared with traditional methods.
[0076] This application provides a precise characterization of the wave velocity-grain angle relationship, clarifying the stepwise increase in stress wave velocity across the log cross section with increasing grain angle (gradual increase from 0° to 40°, significant increase from 40° to 70°, and stabilization from 70° to 90°). This enables accurate prediction of wave velocity in different grain directions for oak and ash hardwood logs, with a fitting determination coefficient R² ≥ 0.939.
[0077] This application enhances the anti-interference and stability of the test. By eliminating outliers using the box-line method, correcting the elastic modulus of coordinate transformation, and optimizing the interface loss reduction of the coupling agent, it effectively reduces the interference of local defects (knots), tissue dispersion, and contact loss of wood on the wave velocity test. The test data dispersion is reduced by more than 20%, and the repeatability error of a single test is ≤5%.
[0078] This application optimizes the engineering applicability and universality by simplifying the complex orthogonal anisotropy theory into an engineering mathematical model with fitting parameters. It eliminates the need for complex stiffness coefficient conversion and directly achieves rapid wave velocity calculation through texture angle, making it suitable for on-site non-destructive testing of logs. It is also applicable to various hardwoods such as oak and ash, balancing theoretical rigor with practicality in the field.
[0079] This application ensures the reliability of test results by establishing a three-in-one testing system of "orthogonal symmetry theory modeling, experimental fitting correction, and outlier data removal." This system fundamentally avoids performance misjudgments caused by anisotropy, providing stable and accurate stress wave detection data support for timber structure safety assessment and timber grading. Existing research indicates that changes in the angle of wood grain can deflect the propagation path of stress waves. This application's fitting method, based on orthogonal symmetry theory, constructs a mathematical model that relies on the orthogonal symmetry structural characteristics of wood grain, closely matching the true structural features of wood anisotropy. Compared to traditional linear assumption fitting models, the mathematical model constructed based on orthogonal symmetry theory exhibits superior fitting accuracy.
[0080] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for determining the stress wave velocity of a log cross section based on the orthogonal symmetry of wood, characterized in that, Includes the following steps: Step 1: Establish an orthogonal anisotropic elastic constitutive model for wood; In the principal axis coordinate system (L,R,T), its constitutive equation is expressed in matrix form: (1) (1) In the formula: σ x ,σ y ,σ z It is normal stress; τ yz ,τ zx ,τ xy It is shear stress; ε x ,ε y ,ε z It is linear strain; γ yz ,γ zx ,γ xy It is shear strain; (1) In the formula (2) (3) (2) Where: E i、 E j This represents the static elastic modulus of tension and compression in the three principal axis directions. i or j=T,L,R ; μ ij This represents 6 Poisson's ratios; i or j = T,L,R ,in i Indicates the direction of the force. j Indicates the direction of deformation; (3) Where: G LR ,G RT ,G TL It is a decision y direction and z direction, z direction and x direction, x direction and y The shear modulus of the change in the angle between directions; Step 2: Establish a mathematical model of the texture angle and static elastic modulus on the cross-section; A specimen is selected from the cross-section of the wood and rotated by an angle γ around the longitudinal axis to form a new coordinate system. Based on the principle of coordinate transformation of the elastic constants of orthotropic materials, the grain angle is derived. γ Expression for the elastic modulus parameter in the direction: (4) Simplify formula (4) to its engineering application form: (5) Right now: (6) In formula (6) Indicates texture direction deflection γ The simplified model of the lateral static elastic modulus after the angle not only retains the influence trend of the texture angle on the static elastic modulus, but also reduces the computational complexity, making it easier to establish a correlation with the stress wave propagation speed later. Step 3: Establish a mathematical model of the stress wave propagation velocity and texture angle; There is a positive correlation between the dynamic modulus of elasticity and the static modulus of elasticity of wood. Substitute it into the mechanical wave velocity formula , u For stress wave velocity, E For the dynamic elastic modulus of wood, D For the density of wood materials, g In the case of gravitational acceleration, we get: ; Substituting formula (6) into the relationship between the static elastic modulus of wood and the propagation velocity of stress waves: A mathematical model for the propagation velocity of stress waves under different texture angles within the cross-section was obtained: (7) Based on the mathematical model (7) relating stress wave propagation velocity to texture angle constructed above, calculating the wave velocity requires knowing the density and static elastic modulus of the wood; since the density and static elastic modulus of the same sample are constant, and the gravitational acceleration in formula (7) is... g It is 9.81 m / s². A The constant is used; to facilitate the fitting of experimental data, experimental fitting parameters are introduced. a,b,c,n ;Simplify formula (7) to its engineering application form: (8) In the formula, u γ Indicates texture angle as γ Stress wave propagation speed at that time γ For arbitrary texture angles a,b,c,n These are the fitting parameters.
2. The method for determining the stress wave velocity of a log cross-section based on the orthogonal symmetry of wood according to claim 1, characterized in that, The wood is oak or ash, and the specimens are healthy, defect-free logs with a diameter at breast height of 20-22 cm and a tree height of 15-18 m, which are processed into 8 standard specimens of 15 cm in length, with 4 specimens of each type of wood.
3. The method for determining the stress wave velocity of a log cross-section based on the orthogonal symmetry of wood according to claim 1, characterized in that, Stress wave parameters were measured using a stress wave meter with a time accuracy of 0.1 μs and a wave velocity measurement range of 100-6000 m / s.
4. The method for determining the stress wave velocity of a log cross-section based on the orthogonal symmetry of wood according to claim 1, characterized in that, The following steps are included in the setup of measuring points and data acquisition: A receiving probe is fixed 2cm from the top surface of the log, and a transmitting probe is arranged in the same cross section. The angle between the transmitting and receiving line and the tangent of the annual ring is defined as the texture angle γ. Eight vertical parallel cross sections are arranged along the log axis, with an adjacent spacing of 5cm, and numbered 1-8. The specimens were equilibrated under constant temperature and humidity for 2 weeks, and the moisture content was monitored at multiple points until it stabilized; the test section was polished to ensure clear growth ring texture. Select reference receiving points at the edges of each measurement section, fit the receiving probe tightly against the surface of the specimen, and apply Vaseline as a coupling agent. The annual ring tangent was drawn with the receiving end as the tangent point. The texture angle γ was adjusted with a protractor. The stress wave propagation time T and the probe distance L corresponding to γ = 10°--90° in 10° intervals were measured. Each group was repeated 3 times and the average value was taken. Single cross section was tested in both clockwise and counterclockwise directions. A total of 16 sets of data were collected for a single specimen. The stress wave propagation velocity u is calculated according to formula (9): (9) Where u is the propagation speed (m / s), L is the sample length (m), and T is the propagation time (s).
5. The method for determining the stress wave velocity of a log cross-section based on the orthogonal symmetry of wood according to claim 1, characterized in that, The box plot method was used with the interquartile range (IQR) as the criterion to identify and remove data that exceeded 1.5 times the IQR range as outliers.
6. The method for determining the stress wave velocity of a log cross-section based on the orthogonal symmetry of wood according to claim 1, characterized in that, The nonlinear regression analysis function of SPSS statistical software was used to fit the model, with the texture angle γ as the independent variable and the mean wave velocity u as the dependent variable. The undetermined constants a, b, c and n in the model (8) were determined by iterative calculation.
7. The method for determining the stress wave velocity of a log cross-section based on the orthogonal symmetry of wood according to claim 6, characterized in that, When the wood is oak, the fitting equation is: (10) The goodness of fit R² = 0.
967.
8. The method for determining the stress wave velocity of a log cross-section based on the orthogonal symmetry of wood according to claim 6, characterized in that, When the wood is ash, the fitting equation is: (11) The goodness of fit R² = 0.
939.
9. The method for determining the stress wave velocity of a log cross-section based on the orthogonal symmetry of wood according to claim 1, characterized in that, The method is used for non-destructive testing of stress waves in logs. It predicts the propagation speed of stress waves by using the texture angle γ, thus eliminating the wave speed calculation deviation caused by the texture direction.