Cationic matrix-stripped cement chlorofluoride combined chromatographic determination method and system

By using a cation matrix stripping method in the determination of chlorine and fluoride in cement, and utilizing H⁺-type strongly acidic cation exchange medium to remove polyvalent cations, adjusting the pH and controlling the amount of medium, the problems of cation deposition, column contamination, and low recovery rate in the determination of chlorine and fluoride in cement are solved, and the method achieves universality and accuracy.

CN123155718APending Publication Date: 2026-11-24CHINA RAILWAY 20TH BUREAU GROUP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611455524.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing methods for determining chlorine and fluorine in cement suffer from problems such as cation deposition and column contamination caused by high concentrations of polyvalent cations, low fluorine speciation and recovery rates, and poor method adaptability, especially evident in high-alumina cement and cementitious materials containing steel slag solid waste.

Method used

A combined chromatographic method for the determination of chlorine and fluorine in cement using cationic matrix stripping was adopted. Ca²⁺, Mg²⁺, Al³⁺ and Fe³⁺ were removed before sample injection using H⁺-type strongly acidic cation exchange medium. The pH of the effluent was adjusted to 5.5-6.5, and the amount of medium was controlled to accommodate different samples. A spiked recovery determination mechanism was set up to ensure the accuracy of the determination results.

Benefits of technology

This method effectively solves the problems of cation deposition and column contamination, improves the recovery rate of fluorine, achieves the universality of the method, ensures the reliability and accuracy of the determination results, and avoids errors caused by empirical correction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses a method and system for the combined chromatographic determination of chlorine and fluorine in cement by cationic matrix stripping, belonging to the field of chemical analysis technology for cement and solid waste cementitious materials. This method utilizes H... + The strong acid cation exchange medium removes Ca from the acidic filtrate before sample introduction. 2+ Mg 2+ Al 3+ Fe 3+ The method involves exchange removal, and further restricts the amount of medium used to control the exchange capacity ratio ρ, where ρ is the ratio of the total exchange capacity of the medium to the total charge equivalent of the cations to be removed in the sample, and the value ranges from 1.2 to 3.0. This ensures that the amount of medium used is precisely matched to the actual cation load of each sample. This method can be universally adapted to material systems with different cation loads, from ordinary silicate cement to high-alumina cement and solid waste containing steel slag, thus solving the problem of poor adaptability of the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical analysis technology of cement and solid waste cementitious materials, specifically relating to a method and system for the combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping. Background Technology

[0002] The chloride and fluoride content in cement is related to the risk of steel corrosion, the use of mineralizers, clinker calcination, and the evaluation of cementitious performance. Ion chromatography can separate multiple anions in a single injection and has been increasingly used for the determination of chloride and fluoride in cement nitric acid decomposition solutions. Current procedures typically involve decomposing the sample with dilute nitric acid, filtering, and adjusting the volume before direct injection, or simply diluting to reduce the matrix concentration. Such decomposition solutions contain high concentrations of Ca. 2+ Mg 2+ Al 3+ Fe 3+ and NO3 - Polyvalent cations are prone to depositing or reacting unexpectedly with column packing material under alkaline elution conditions; Al and Fe can also react with F. - Formation of complexes, allowing free F - The ratio varies depending on the material composition and acidity.

[0003] Simply increasing the acid concentration can improve decomposition, but it will also increase the ion load of the sample; simply increasing the dilution factor will simultaneously reduce the concentration of low-content F. - and Cl - The response. For high-alumina cement, steel slag-containing solid waste cementitious materials, and high-calcium clinker, F often occurs. - Low recovery rate, Cl - Problems include unstable peak area and retention time, and accelerated contamination of guard or separation columns. Using a fixed volume of purification material is also difficult to adapt to the total cation equivalent of different samples; insufficient capacity will cause breakthrough, while excessive capacity will amplify the chlorine and fluorine blanks in the medium and operational differences. Summary of the Invention

[0004] The purpose of this invention is to provide a method and system for the combined chromatographic determination of chlorine and fluorine in cement by stripping a cationic matrix, in order to solve the technical problems of existing methods, such as cation deposition and column contamination caused by high concentrations of polyvalent cations, low speciation and recovery rate of fluorine, and poor method adaptability.

[0005] To achieve the above objectives, the present invention employs the following technical solution: This invention discloses a method for the combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping, comprising the following steps: S1: Decompose the cement sample with nitric acid, filter, and collect the acidic filtrate; S2: Pass the collected acidic filtrate through a cation exchange medium, utilizing the H+ in the cation exchange medium. +Exchange and remove Ca from the acidic filtrate 2+ Mg 2+ Al 3+ and Fe 3+ Collect all effluent flowing out of the cation exchange medium; S3: After the effluent is separated from the cation exchange medium, the pH of the effluent is adjusted to 5.5~6.5, and then the volume is adjusted to obtain the purified stock solution; S4: Take the purified stock solution and determine the F content therein by ion chromatography. - and Cl - ; The cation exchange medium is a hydrogen-type strong acidic cation exchange medium, and the amount of cation exchange medium used is controlled by the exchange capacity ratio ρ. The exchange capacity ratio ρ is the ratio of the total exchange capacity of the cation exchange medium to the total charge equivalent of the cations to be removed in the cement sample. The value of ρ ranges from 1.2 to 3.0.

[0006] Further, the amount of the cation exchange medium is determined according to the following steps: Determination of the wet volumetric exchange capacity q of cation exchange media v ; Calculate the total charge equivalent E of the cations to be removed in the sample. c ; The required wet volume V of the cation exchange medium can be calculated using the following formula. r ; ; in, The exchange capacity ratio is taken in the range of 1.2 to 3.0 depending on the type of cement sample. The E c Calculate using the following formula: ; in, denoted as sample mass; i represents the index of oxides decomposed by nitric acid and occupying exchange sites. This represents the number of oxygen atoms in the oxide. The proportion of acid-soluble substances that enter the filtrate. The mass fraction of the oxide. denoted as , where is the molar mass of the oxide.

[0007] Furthermore, the cement sample includes at least one of silicate cement, high-alumina cement, steel slag-containing solid waste cementitious material, and high-calcium clinker; When the cement sample is silicate cement or high-calcium clinker, ρ is 1.4~1.8; when the cement sample is high-alumina cement, ρ is 1.8~2.4; when the cement sample is cementitious material containing steel slag solid waste, ρ is 2.0~2.6; when the composition of the cement sample is unknown, ρ is 2.5.

[0008] Furthermore, it also includes steps for determining spiked recovery rate and reprocessing non-compliant batches: Before decomposing the cement sample with nitric acid in S1, unspiked samples and F were prepared respectively. - Spiked sample and Cl - Spiked sample, so that the unspiked sample, F - Spiked sample and Cl - The spiked samples were subjected to S1 to S4 sequentially. Calculate F in the same analytical batch after S4 is completed. - Spiked recovery and Cl - Spike recovery rate; when F - Spiked recoveries not in the range of 85%–115%, or Cl - If the spiked recovery rate is not within the range of 90% to 110%, the analytical batch is deemed unqualified. After confirming the process blank, calibration verification, and chromatographic system are qualified, the exchange capacity ratio ρ is increased or the sample mass is reduced, and the batch is reprocessed starting from S1. The original determination results are not corrected using the reciprocal of the recovery rate, fixed compensation coefficient, or historical experience coefficient. The spiked and unspecified samples used the same dilution factor D, and the F - Spiked recovery and Cl - The formula for calculating the spiked recovery rate is as follows: ; Where X is F - or Cl - , should be F - hour, F represents - Spiked recovery rate, when Cl - hour, Cl - Spike recovery rate; and The concentrations of X ions measured after subtracting the process blank are the spiked and unspiked portions, respectively; D s D0 and D0 are the dilution factors for unspecified and unspecified portions, respectively. To determine the final volume of the purified stock solution; The mass of the added X ions.

[0009] Further, in S1, the molar concentration of the nitric acid is 1.2~1.5 mol / L; during the decomposition of the cement sample with nitric acid, the cement sample is first dispersed in water, then nitric acid is added and heated to a gentle boil, and then filtered after cooling.

[0010] Further, in S1, the ratio of cement sample to water is 0.3000g:(30~50)mL; the ratio of cement sample to nitric acid is 0.3000g:(10~20)mL; the nitric acid is added at a time of 30s~60s; and the time for gentle boiling is 1min~2min.

[0011] Furthermore, in S2, the cation exchange medium is a sulfonic acid-based strong acid cation exchange resin, and its usage state is H. + The cation exchange medium has a backbone of styrene-divinylbenzene crosslinked gel or macroporous polymer, a total wet volume exchange capacity of 1.6 mmol / mL to 2.2 mmol / mL, a particle size of 0.30 mm to 1.20 mm, and a water content of 45% to 60%. Before use, the cation exchange medium is activated with nitric acid and passed through a Cl-... - F - Double blank access; The standard for dual-blank admission is F in the entire process blank. - Not exceeding 0.010 mg / L, Cl - Not higher than 0.020 mg / L.

[0012] Furthermore, in S2, the acidic filtrate has an empty bed contact time of not less than 6 minutes with the cation exchange medium, and the volumetric flow rate is not greater than 1.2 mL / min.

[0013] Furthermore, in S3, the pH value is adjusted using NaOH solution.

[0014] This invention also discloses a chromatographic system for the determination of chlorine and fluorine in cement by cationic matrix stripping, comprising: The decomposition unit is used to decompose cement samples with nitric acid and filter them to collect the acidic filtrate. A cation exchange unit is used to pass the collected acidic filtrate through a cation exchange medium, utilizing the H+ in the cation exchange medium. + Exchange and remove Ca from the acidic filtrate 2+ Mg 2+ Al 3+ and Fe 3+ Collect all effluent flowing out of the cation exchange medium; The pH adjustment and volume control unit is used to adjust the pH of the effluent to 5.5~6.5 after the effluent is separated from the cation exchange medium, and then to make up the volume to obtain the purified stock solution. The ion chromatography detection unit is used to take the purified stock solution and determine the F content therein by ion chromatography. - and Cl - ; The control unit is used to control the amount of medium in the cation exchange unit according to the exchange capacity ratio ρ, wherein the exchange capacity ratio ρ is the ratio of the total exchange capacity of the cation exchange medium to the total charge equivalent of the cations to be removed in the sample, and the value of ρ ranges from 1.2 to 3.0.

[0015] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses a chromatographic method for the combined determination of chlorine and fluorine in cement with cationic matrix stripping. This method utilizes H... + The strong acid cation exchange medium removes Ca from the acidic filtrate before sample introduction. 2+ Mg 2+ Al 3+ Fe 3+ Exchange removal fixes polyvalent cations onto the medium instead of them entering the chromatographic system, eliminating the material basis for their deposition and column contamination under alkaline elution conditions, thus effectively solving the problems of cation deposition and column contamination; simultaneously, Al 3+ and Fe 3+ After being removed by the medium, the activity of the metal in the liquid phase decreases sharply. According to the principle of coordination chemistry equilibrium, the metal-fluorine complexes (Al-F, Fe-F) continue to move in the direction of dissociation, causing the complexed fluorine to be released as free F. - Furthermore, after media separation, the pH is adjusted to 5.5~6.5, within this pH range, F - It exists stably mainly in the form of free anions, and the controlled conversion of fluorine can be achieved without the addition of external complexing agents, thus solving the problem of low fluorine recovery rate. On this basis, the amount of medium used is further limited by the exchange capacity ratio ρ, which is the ratio of the total exchange capacity of the medium to the total charge equivalent of the cations to be removed in the sample, and the value ranges from 1.2 to 3.0. This allows the amount of medium to be precisely matched according to the actual cation load of each sample, avoiding both cation breakthrough caused by insufficient capacity and blank amplification caused by excessive capacity. This method can be universally adapted to material systems with different cation loads, from ordinary silicate cement to high alumina cement and solid waste containing steel slag, thus solving the problem of poor method adaptability.

[0016] Furthermore, this method involves setting low concentrations of F in the same analytical batch. - and Cl - The entire process of spiking was tested, and 85%~115% (F) was set for each stage. - ) and 90%~110% (Cl -The spiked recovery rate determination window was established for the first time, creating a quantitative failure determination mechanism for cation matrix stripping effect and fluorine speciation release efficiency. More importantly, it stipulates that when the spiked recovery rate is unqualified, the sample must be reprocessed starting from the sample decomposition step by increasing the exchange capacity ratio ρ or reducing the sample mass, and the use of any empirical correction coefficients (such as reciprocal correction of recovery rate, fixed compensation coefficient, or historical experience coefficient) on the original measurement results is strictly prohibited. This rule moves the anomaly location and correction to the sample pretreatment stage rather than the data post-processing stage; when F - Low recovery rate and Cl - If the recovery rate is within acceptable limits, it is determined to be a metal-fluorine release or insufficient exchange terminal capacity, and the pH is increased for reprocessing; when F - and Cl - If the recovery rate is simultaneously low or the retention times of both peaks shift forward by more than 2.5%, it is determined that the total injection matrix load is too high. The sample mass is then reduced to 0.75~0.80 of the original value, and the calculation is repeated. and This allows different failure modes to correspond to different physical adjustment paths, ensuring that reported values ​​always come from qualified batches that have been physically cleaned and measured. This solves the technical defects of existing technologies, such as the lack of an effective failure judgment mechanism and the reliance on empirical coefficients lacking physical basis to correct abnormal data after the fact. It truly realizes a quality control closed loop where non-conforming products are discarded and re-physically processed, rather than using mathematics to cover up problems. Attached Figure Description

[0017] Figure 1 This is a flowchart of the measurement method of the present invention; Figure 2 The exchange capacity ratio ρ and the total charge equivalent removal rate of cations, F - Spiked recovery and Cl - Measured relationship between spiked recoveries; Among them: A-Ordinary Portland cement; B-High alumina cement; C-Steel slag-containing solid waste cementitious materials; D-High calcium clinker; Figure 3 The number of regeneration cycles of the cation exchange medium and the wet-state volumetric exchange capacity qv, F - Spiked recovery and Cl - A graph showing the monitoring and judgment relationship between spiked recovery rates. Detailed Implementation

[0018] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0019] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.

[0020] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values ​​(including integers and fractions) within those ranges.

[0021] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”

[0022] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.

[0023] The present invention aims to solve the problem of selectively removing large amounts of cations such as Ca, Mg, Al, and Fe before sample injection without carrying away Cl, while retaining the advantages of dilute nitric acid decomposition and same-liquid determination. - and F - And it converts the metal-complexed fluorine into a stably responsive F. - How to determine the amount of exchange medium to use based on the actual cation equivalent of the sample, while balancing breakthrough risk and medium blank; how to use low-concentration F from the same batch - spiking and Cl - Spike identification of pretreatment failures and failure handling are implemented by resampling and adjusting capacity, rather than applying empirical correction coefficients that lack physical basis to the measurement results.

[0024] The method provided by this invention forms a continuous closed loop encompassing the decomposition of cement samples, cationic matrix stripping, fluoride release, isochromatographic determination, and intra-batch validity assessment. The samples are still decomposed with nitric acid (1+10), allowing chlorine and fluoride to enter the liquid phase. Insoluble substances are removed while the decomposition liquid is still acidic and not yet diluted to volume to prevent hydrated silicate residues from obscuring exchange sites. The resulting filtrate, containing only sulfonic acid with fixed negative charges, is then treated with H₂O. + Contact with a strongly acidic cation exchange medium for ion exchange. Na+ is not used as the medium. + Type, Cl -For materials containing complexing agents, only nitric acid is used as the activating acid, thus avoiding the introduction of Cl into the test system from the source. - The medium for Ca 2+ Mg 2+ Al 3+ Fe 3+ And a small amount of Na + K + Perform equal charge exchange, Cl - F - and NO3 - It is not fixed as an exchange counterion. Immediately after the exchange, the medium is separated from the liquid phase, and the anions in the pores of the medium are recovered with water. The combined solution is then adjusted to pH 5.5-6.5 and brought to a final volume. At this point, the metal activity in the liquid phase has decreased, and the metal-fluorine complexation equilibrium shifts towards free F. - The flow shifts to one side; simultaneously, HF undergoes substantial dissociation within this pH range, eliminating the need for buffer components such as citrate, acetate, and phosphate, which would increase the anion chromatography loading. After appropriate dilution, the same purified solution can be injected once to obtain F. - Peaks and Cl - peak.

[0025] Cation exchange employs capacity ratio control rather than fixed mass control. The wet-state volumetric exchange capacity of each batch of media is first determined, and then the equivalent of cations to be removed is calculated based on the content of each oxide that can be dissolved by acid in the sample. The ratio of the total exchange capacity of the media to the equivalent of cations to be removed is set at 1.2–3.0. For ordinary silicate cement and high-calcium clinker, a ratio of 1.4–1.8 is suitable; for high-alumina cement, a ratio of 1.8–2.4 is suitable; and for steel slag or solid waste cementitious materials containing a large amount of Fe and Mg, a ratio of 2.0–2.6 is suitable. When the composition is unknown and a rapid chemical composition cannot be obtained, a ratio of 2.5 is initially used, and the results of bi-anion spiking are used to determine whether to increase it to 3.0 or reduce the sample mass. The lower limit of this range represents the margin retained due to incomplete mass transfer, wet-state capacity fluctuations, and competition among multivalent ions. The upper limit is used to constrain the media's own blank space and pore retention volume, avoiding the substitution of correct capacity calculation with an infinitely increased media volume.

[0026] Figure 1 This is a flowchart of the determination method of the present invention, which sequentially shows the sample decomposition and filtration, the amount of exchange medium taken, and H... + Type cation matrix stripping, media separation, pH-controlled fluorine speciation release and volume determination, F - and Cl - Combined ion chromatography determination and intra-batch quality control; when the process blank, calibration check or double spike determination fails, the system is investigated according to the failure mode, the exchange capacity ratio ρ is increased or the sample mass is reduced, and the original results are discarded and reprocessed from the sample decomposition step, thus forming a quality control closed loop.

[0027] 1) The reagents, materials, and apparatus used in the method of this invention are as follows: The water used is secondary water with a resistivity of not less than 10 MΩ·cm; nitric acid, NaOH, NaNO3, Na2CO3, and NaHCO3 are low-halogen reagents suitable for ion chromatography analysis; the molar concentration of the nitric acid decomposition solution is 1.2 mol / L~1.5 mol / L; in this embodiment, nitric acid (1+10) is used, which is prepared by slowly adding 1 volume of concentrated nitric acid with a mass fraction of 65%~68% to 10 volumes of water, resulting in a molar concentration of approximately 1.3 mol / L~1.4 mol / L; nitric acid (1+100) is used for pre-washing the filter media; 0.50 mol / L nitric acid is used for media activation; 1.0 mol / L and 0.10 mol / L NaOH are used for staged pH adjustment, wherein the NaOH solution is prepared fresh each time and stored in an airtight environment, and Cl... - and F - The content of all components should be lower than the blank limit of the corresponding batch; HCl activation medium must not be used, and materials containing Cl must not be used. - The pH standard solution should be added directly to the test solution, and the container should not be rinsed with fluorinated surfactants.

[0028] The cation exchange medium is a sulfonic acid-based strong acid cation exchange resin, with a styrene-divinylbenzene crosslinked gel or macroporous polymer as the backbone, and is in H2O condition. + The wet volumetric exchange capacity should be 1.6 mmol / mL to 2.2 mmol / mL, the particle size should be 0.30 mm to 1.20 mm, and the water content should be 45% to 60%. When the capacity, blank, and mechanical strength requirements are met, disposable columns, membrane stacks, or microbeds filled with similar sulfonic acid-based materials can also be used. The medium must not contain quaternary ammonium anion exchange functional groups and must not contain Ag... + Ba 2+ Ions that are likely to form a precipitate with the anion to be tested are used in the working form.

[0029] Decomposition, transfer, and collection equipment is preferably made of PFA, polypropylene, or other inert materials verified by blank testing. Volumetric instruments may be 100 mL polypropylene volumetric flasks calibrated by weighing. Filtration uses ashless rapid filter paper with a pore size of 8 μm–20 μm, or centrifugation followed by a 0.45 μm hydrophilic polyethersulfone membrane; filter paper, membrane, column frit, and syringe must all be tested using the same batch of Cl... - F - Blank check. pH measurements should be performed using a two-liquid junction electrode with an external salt bridge of KNO3 or NaNO3 solution, or a solid reference electrode with no KCl leakage. If only a KCl reference electrode can be used, a trace amount of the test solution that will not return to the main solution should be removed for measurement. It is not permitted to directly immerse a conventional KCl electrode in the test solution for an extended period.

[0030] The ion chromatograph includes a liquid delivery unit, an injection unit, an anion guard column, an anion separation column, a suppressor, and a conductivity detector. The stationary phase of the separation column is a high-capacity quaternary ammonium anion exchange material, with a size of 4 mm × 250 mm, and the guard column can be 4 mm × 50 mm. The equipment model is not a limitation of this method, as long as it allows the water negative peak or the system peak to be correlated with F... - Peak separation is not less than 1.5, F - Peak and Cl - The peak resolution is not less than 2.0, and high concentrations of NO3 can be separated before the next injection. - Just let it flow out completely.

[0031] 2) Activation, capacity calibration, and blank access of the exchange medium The new sulfonic acid-based strong acid cation exchange resin (used as the cation exchange medium in this embodiment, hereinafter referred to as the exchange medium) was first soaked in water for 12 h to allow the particles to fully swell. The desired exchange medium was placed in a polypropylene column and washed from top to bottom with 5 times the bed volume of water at a flow rate controlled at 2 to 4 times the bed volume per hour. Then, 5 times the bed volume of 0.50 mol / L nitric acid was introduced, the outlet was closed, and the resin was soaked for 2 h to uniformly convert the resin to H₂. + The sample was then washed with at least 10 times the bed volume of water. The washing endpoint was not determined solely by pH, but by a change in conductivity of less than 10% and a decrease in Cl- concentration between two consecutive bed volumes of wash solution. - F - The blank meets the limit criteria. Activation with nitric acid avoids the formation of difficult-to-wash Cl- residues within the resin channels caused by HCl activation. - Memory. When using pre-loaded disposable columns, membrane stacks, or microbeds, the corresponding activation method can be adopted according to their structure, but their wet exchange capacity and Cl... - and F - Both the double blank and the effective contact time should meet the requirements specified in this instruction manual.

[0032] Wet volumetric volume was determined using an independent representative sample from the same batch of media. The media was allowed to settle naturally in water for 30 minutes without compressing the particles, and the wet settling volume was measured. A sufficient amount of 1.0 mol / L NaNO3 is uniformly introduced into the medium, causing Na... + Replace all interchangeable H + Collect and combine the effluents, at a concentration of The NaOH standard solution was titrated with H+. + . The volume of NaOH standard solution consumed in the experiment, For blank consumption volume without media, The unit is mL. The unit is mol / L. Since 1 mol / L and 1 mmol / mL have the same numerical value, the wet volume exchange capacity is... Calculate using the following formula, with units of mmol / mL: (1) Volumetric measurements are not used directly for sample purification. If reuse is required, nitric acid activation and anion blank checks should be performed again. The average value of three consecutive volumetric measurements can be taken as the representative value for that batch if the relative range of the measurements is no greater than 5%. If the sedimentation volume reading exceeds 5%, it indicates that the sedimentation volume reading, ion form, or resin damage is unstable, and the media batch should be prepared again.

[0033] The activated medium must also pass a double-blank test. Using the maximum medium volume used for actual sample processing, after packing the column, sequentially pass through a nitric acid (1+10) reagent blank, wash water, and pH adjuster of the same volume as the sample, finally bringing the volume to 100 mL and injecting the sample under the same conditions. The F in this entire process blank... - It should not exceed 0.010 mg / L, Cl - The concentration should not exceed 0.020 mg / L, or neither should exceed one-third of the respective method's limit of quantitation, whichever is more stringent. If any limit is exceeded, continue washing with water for up to 10 times the bed volume and retest; if it still exceeds the limit, discard the batch of media. Through this admission method, the blank risk caused by the increase in media volume is quantified before contact with the sample, rather than speculated after the results are abnormal.

[0034] 3) Calculation of the equivalent amount of cations to be removed and the amount of medium to be taken The cation equivalent should be calculated using the mass fraction of major oxides given in existing X-ray fluorescence analysis, wet total analysis, or material batching sheet for the same sample. The following symbols are defined before calculation: The sample mass is expressed in grams; i represents the index of oxides decomposed by nitric acid and occupying exchange sites; the general formula for oxides is... ; and These represent the number of metal atoms and the number of oxygen atoms in the oxide, respectively. The valence number of the metal ion; This represents the mass fraction of the oxide, expressed as a decimal. This represents the molar mass of the oxide, expressed in g / mol. This represents the proportion of acid-soluble substances that enter the filtrate, and its value ranges from 0 to 1. The amount of the substance to be decharged by the cation in the sample is expressed in mmol; ρ is the exchange capacity ratio. This refers to the volume of the wet settling medium collected, in mL. For conservative calculations, routine testing will... Take 1; only after the material family has been validated with no fewer than 10 samples can the components determined not to enter the filtrate be subjected to actual measurement. .

[0035] For electrically neutral oxides Since the positive charge of the metal is equal to the negative charge of oxygen, therefore... One mol of this oxide, upon entering an acidic liquid phase, will at most form [a specific chemical reaction]. The molar equivalent of positive charge. The amount of substance of the oxide is obtained by dividing the mass by the molar mass, then multiplied by... Summing over each oxide, we get: (2) When composition data is expressed as a percentage, the value should be divided by 100 before being substituted into equation (2). Each mol of CaO, MgO, FeO, and MnO is counted as 2 mol charge equivalents; each mol of Al2O3 and Fe2O3 is counted as 6 mol charge equivalents; each mol of Na2O and K2O is counted as 2 mol charge equivalents. High-valence components such as TiO2, which may partially enter the liquid phase under these decomposition conditions, can also be included according to the same principle. The acid's own H... + Not included Because the medium is originally H + Type; NO3 - SO4² - Cl - and F - It is not included in the cation equivalent.

[0036] Depend on , And ρ are determined: (3) The calculated value is rounded up to 0.1 mL. ρ must not be less than 1.2 or greater than 3.0. If obtained according to formula (3) For samples larger than 15 mL, prioritize reducing the sample mass so that the sum of the column packing volume, washing liquid volume, and pH adjuster volume can still be calculated within the 100 mL constant volume condition; do not arbitrarily increase the final volume to accommodate excess media and then use the original calculation formula. Ordinary cement in... 0.3000 g and At approximately 1.8 mmol / mL, The usual volume is 6 mL to 9 mL; for high-alumina or steel slag materials, it is usually 9 mL to 13 mL.

[0037] When compositional data is missing, a rapid X-ray fluorescence semi-quantitative analysis can be performed on 0.3000 g of the same batch of samples, based on all measured oxides. Calculation. If the on-site analysis conditions are not available, start with ρ=2.5 and 0.3000 g of sample was treated with mL; when double spiking was not qualified, the sampling amount was reduced or the effective capacity was increased according to the rules in Part 9. This unknown composition path was only used for the first exploration. After the material family data was formed, it was returned to Equations (2) and (3) to avoid long-term masking of compositional differences with a fixed medium volume.

[0038] 4) Sample decomposition and filtration The sample should be representative and pass through a 150 μm sieve. It should be sealed and stored, and mixed thoroughly before analysis. Weigh approximately 0.3000 g of the sample, accurate to 0.0001 g, and place it in a 100 mL desiccant cup. Add 30 mL of water and stir for 2 min with a PTFE-coated stir bar or inert stirrer to completely disperse the aggregates. While stirring, slowly add 10 mL of nitric acid (1+10) along the cup wall, controlling the acid addition time to 30-60 s to avoid localized agglomeration and splashing caused by strong acid. Cover with a watch glass with a small venting gap, heat to boiling, and maintain a gentle boil for 1-2 min. Stop heating immediately after the gentle boil ends, without evaporating the solution to a small volume, to reduce the residence time of fluorine-containing species in strong acid and at high temperatures.

[0039] Cool to 25℃±3℃. If using filter paper, pre-wash the rapid filter paper sequentially with 20 mL of nitric acid (1+100) and 30 mL of water, discarding the washings. Filter the decomposition solution into a polypropylene collecting cup, and wash the decomposition cup, watch glass, and residue with three 3 mL water portions, combining all washings into the filtrate. If there is little insoluble residue, centrifuge at 4000×g~5000×g for 10 min, collect the supernatant, and filter it through a 0.45 μm hydrophilic low-binding filter membrane. The filter material used must be pre-washed with a 3 mL reagent blank. The filtrate after filtration should be clear and free of visible particles; the filtrate volume should be controlled at 45 mL~55 mL to reserve volume margin for subsequent media rinsing, pH adjustment, and 100 mL final volume adjustment.

[0040] The main filtrate after decomposition should not be pre-volume adjusted, nor should a complexing buffer be added, nor should it be diluted with a large amount of water before exchange. This ensures a sufficient concentration of the target anions while avoiding an increase in the volume of liquid to be processed and an excessively long exchange contact time due to pre-volume adjustment. The filter residue should not directly contact the resin, as fine silica gel and unreacted minerals can coat the resin surface, alter the wet bed volume, and cause incalculable adsorption losses.

[0041] 5) Hydrogen-type cationic matrix stripping Measure the wet medium according to formula (3) and load it into an empty column with a polypropylene sieve plate. Gently tap the column wall to remove air bubbles and level the bed surface; keep the liquid level tangent to the bed surface with water to prevent the medium from drying out and cracking. Glass wool and chlorine-containing binders must not be used inside the column. Add the filtrate from the top of the column and collect it all starting from the first drop. The sample throughput should simultaneously meet the requirements of an empty bed contact time of not less than 6 min and a volumetric flow rate of not more than 1.2 mL / min; for example When the volume is 7.5 mL, the flow rate should not exceed 1.2 mL / min. When the volume is 4.0 mL, the flow rate should not exceed 0.67 mL / min. If gravity flow is used, it should be controlled by adjusting the outlet inner diameter; if a syringe pump or peristaltic pump is used, the pump tubing should be pre-treated with Cl. - F - blank.

[0042] The exchange reaction in a strongly acidic medium can be represented by the following reaction equation, where R—SO3H represents H. + Type exchange sites: (4) (5) Mg² + Fe³ + Other cations undergo the same type of reaction in equal charge. The H₂ released through exchange... + Maintaining the acidity of the effluent inhibits the formation of hydroxides and blockage by metals in the bed. The resin-fixed negatively charged region repels free anions, Cl... - F - and NO3 - It mainly flows with the mobile phase. For Al-F and Fe-F complexes, as free metal ions and positively charged metal complexes are continuously fixed, the metal activity downstream of the bed gradually decreases; the charge exchange between sulfonic acid sites and metals, as well as the repulsion of anions by the fixed phase, jointly promote the transfer of coordinated F to the liquid phase. Because the amount of medium used has a margin based on the total charge equivalent, H is maintained at the end of the bed. + Type to avoid metal penetration and re-complexation at the end F - .

[0043] After all the filtrate has passed through, rinse the original collection cup with 5 mL of water and transfer it to the top of the column. Then wash the column bed with two 5 mL aliquots of water, maintaining the same flow rate as the injection. Combine all the eluents. The first aliquot is used to displace the column void fluid, and the second aliquot is used to adjust the low concentration of F. - and Cl -Elute quantitatively from between particles. Do not use NaCl, carbonates, or organic acids for elution. If the washing solution volume is less than 10 mL, pore retention may occur due to the larger bed volume of medium; if it exceeds 20 mL, it will occupy the constant volume space and increase the subsequent neutralization volume. Therefore, the usual total washing solution volume should be 15 mL, including the rinsing solution in the collection cup.

[0044] As an equivalent contact method, the calculated medium can be directly added to the filtrate, mixed at 20-30 °C with end-turning at 20-40 r / min for 20 min, allowed to stand for 5 min, and then separated through a qualified polypropylene sieve plate. The medium is then washed with three 5 mL aliquots of water. For batch contact, the medium volume ratio should be increased by 0.2 compared to column contact, but the total ρ should still not exceed 3.0. Column and batch results should not be mixed in the same batch unless separate process blank and spiked control limits are established.

[0045] The medium should not be used directly for the next sample after a single contact. If regeneration is required in the laboratory, it should be regenerated with at least 5 bed volumes of 0.50 mol / L nitric acid, washed with 10 bed volumes of water, and then re-tested using a double-blank standard. The same medium should not be regenerated more than 5 times. High Cl - or high F - Even if there is still some remaining capacity in the medium after sample collection, it should be isolated to prevent memory contamination caused by pore fluid. The number of medium regeneration cycles is related to qv and F. - Spiked recovery and Cl - The relationship between the retesting and determination of spiked recovery rate is as follows: Figure 3 As shown. The existing experimental data only gives the average q before use. v The value was 1.842 mmol / mL, but the measured values ​​after 1, 3, and 5 regeneration cycles have not yet been provided; therefore, when actually using the regeneration protocol, measured data should be supplemented for each cycle and approved using a double-blank test, and the value should not be based solely on the initial value. Figure 3 Replaces the verification of regeneration performance.

[0046] 6) pH-controlled release and volume adjustment of fluoride speciation Place the combined effluent in a sealed container that minimizes CO2 absorption but allows for further liquid addition, and stir at 25 ℃ ± 2 ℃. First, add 80%–90% of the expected NaOH volume (based on the NaOH consumption of an equal volume of reagent blank), then gradually adjust the pH dropwise with 0.10 mol / L NaOH. Wait 30 seconds each time the pH approaches the target value, until it reaches 5.8–6.2; the allowable control range is 5.5–6.5. If the pH is mistakenly adjusted to above 6.5, correct it using 0.05 mol / L nitric acid; do not use HCl. After reaching the target, continue stirring for 5 minutes, let stand for 5 minutes, and repeat the test; the difference between the two pH tests should not exceed 0.10 before making up to volume.

[0047] This pH window takes into account both HF dissociation and the effects of residual metals. Definition The acid dissociation constant of HF is given. ; and Free F - The equilibrium concentration of HF This represents the total concentration of fluorine not bound to metals. For F - The proportion. From the following formula: (6) achievable Substitute By definition, we get: (7) Take at around 25 °C At approximately 3.17, pH 5.5 corresponds to Approximately 99.53%, corresponding to pH 6.5 Approximately 99.95%. Therefore, the lower limit ensures that fluorine is mainly in the form of F, which can be retained on an anion exchange column. - The presence of residual Al and Fe limits the risk of hydrolysis and colloid formation. pH adjustment is scheduled after media separation to avoid the addition of Na. + Pre-allocating the exchange capacity also prevents alkali from entering the resin bed and causing local precipitation.

[0048] The adjusted solution should remain clear. If visible turbidity, flocculent matter, or a sustained pH drop exceeding 0.20 occurs, do not continue the measurement after filtration alone, as this indicates insufficient cation stripping or the presence of abnormally high levels of hydrolyzable metals. Instead, increase or decrease the pH as per Part 9. Reprocess. Quantitatively transfer the clarified solution to a 100 mL volumetric flask, dilute to the mark with water, and mix well to obtain the purified stock solution. When the stock solution is stored in a sealed container at 2 °C–8 °C, measurements should be completed within 8 hours; if more than 8 hours have passed, the pH and process spikes should be retested; if the results are unsatisfactory, the solution should be prepared again.

[0049] 7) Combined ion chromatography determination of chloride and fluoride in the same purified solution The purified stock solution is diluted 1 to 10 times according to the expected concentration. A standard 0.01% to 0.20% Cl solution is typically used. - or F - Dilutes of 2 to 5 times can be used; lower concentrations may not require dilution, and the injection volume should be controlled at 10 μL, while higher concentrations require increasing the dilution factor. The dilution factor D is the total volume multiple that the purified stock solution undergoes before entering the chromatographic vial. - and Cl -The samples must be taken from the same purification stock solution and use the same D; only when the contents of the two samples differ by more than 50 times and cannot both fall within the calibration range are two additional samples taken from the same stock solution using different D values, and these samples should be substituted into the calculations when reporting.

[0050] The preferred chromatographic conditions are: a mixed eluent of 3.2 mmol / L Na₂CO₃ and 1.0 mmol / L NaHCO₃, a flow rate of 0.80 mL / min, a column temperature of 30 °C, an injection volume of 10 μL, continuous self-regenerating or chemically inhibited conductivity detection, single sampling time of 15–18 min, and confirmation of NO₃ before the next injection. - The peak has returned to baseline. A hydroxide gradient system can also be used, but the calibration solution, blank solution, and sample must be from the same system. Before starting the batch, inject the intermediate concentration mixed standard solution three times consecutively. - and Cl - The relative standard deviation of peak area is no greater than 2.0%, and the relative standard deviation of retention time is no greater than 1.0%.

[0051] The calibration solution is not prepared directly with pure water, but with a matrix solution obtained by treating the entire blank with the same medium, adjusting the pH, and diluting it, thus matching NO3. - and Na + Background. F - Calibration points can be 0.05 mg / L, 0.10 mg / L, 0.20 mg / L, 0.50 mg / L, 1.00 mg / L, 2.00 mg / L, and 5.00 mg / L; Cl - Calibration points can be 0.10 mg / L, 0.20 mg / L, 0.50 mg / L, 1.00 mg / L, 2.00 mg / L, 5.00 mg / L, and 10.00 mg / L. A linear regression of peak area against concentration should be performed at least 6 points, with a coefficient of determination of not less than 0.999; the back-calculation deviation at the lowest non-zero point should not exceed ±10%, and at other points, not exceed ±5%. An intermediate concentration verification solution from an independent source should be inserted after every 10 samples, with its F... - Cl - The measured values ​​should all be 95% to 105% of the nominal values.

[0052] The sample was qualitatively analyzed by retention time and quantitatively analyzed by peak area. Sample F - and Cl - The retention time deviation relative to the batch of calibration solution does not exceed ±2.5%; F - The peak separation from the previous system peak is not less than 1.5, F - With Cl - The separation degree should not be less than 2.0. If the NO3 content is high... -If the baseline is not recovered subsequently, prioritize reducing the injection volume or increasing the stock solution dilution factor, without changing the total volume obtained from sample pretreatment. Do not mask co-elution by shifting the integration start and end points, nor infer that the cationic matrix has been completely removed solely from peak height changes.

[0053] 8) Rules for determining the effectiveness of double anion spiking and for reprocessing expired products Each analytical batch is defined as a set of determinations using the same activation medium, the same set of calibrations, and no more than 20 samples. Each batch must include at least one full-process reagent blank, one maximum-volume process blank, and one low-concentration F. - scalar and 1 Cl - Add a scalar. Prefer to calculate according to formula (2). The sample with the highest or largest Al2O3 mass fraction was used as the spiked matrix. Samples identical to the original sample were weighed to form the unspiked portion and the F... - spiked parts and Cl - Spiked components; the spiked solution is added after the sample is dispersed in water and before the addition of nitric acid, allowing it to undergo the complete process of decomposition, filtration, exchange, pH adjustment and chromatographic determination.

[0054] F - The preferred dosage for low-concentration spiking is 0.20 mg / L per 100 mL of purified stock solution, with an allowable range of 0.10 mg / L to 0.50 mg / L; Cl - The preferred spiking concentration is 0.50 mg / L, with an allowable range of 0.20 mg / L to 1.00 mg / L. If the test sample background exceeds 10 times the spiking increment, a spiking concentration with a lower background should be selected. Similar samples, or samples where the spiking increment reaches 20% to 100% of the background, but F - A low concentration control point of no more than 0.50 mg / L should still be maintained. Standard solutions from sources independent of the calibration solution should be used for spiking.

[0055] definition The concentration of X ions is the value obtained after subtracting the process blank from the spiked sample. X represents the concentration of the unspecified fraction after subtracting the process blank. - or Cl - All units are mg / L; The mass of X ions added is expressed in mg. The volume of the purified stock solution is measured in mL. and These are the dilution factors for the spiked and unspecified portions, respectively. When both portions use the same dilution factor D, the spiked recoveries are... Calculate using the following formula: (8) The factor 10 in equation (8) comes from the conversion between mg / L and mL, as well as the percentage conversion. If the two D values ​​are different, they should be converted back to the concentration of the purified stock solution before the difference is calculated. - The allowable recovery rate for spiked products is 85%–115%, Cl - The acceptable recovery rate is 90%–110%. Two windows are considered for low concentrations of F. - The influence of complexation and system peak and Cl - Typically, it has more stable response characteristics.

[0056] If any spike exceeds the window, first check the process blank, calibration check solution, and retention time. If the blank or check solution is unacceptable, treat the reagent, chromatographic system, or media contamination and re-establish the batch; if the instrument controls are all acceptable but F... - Low recovery rate, Cl - If the recovery rate is acceptable, it is considered that metal-fluorine release or insufficient exchange terminal capacity. The density (ρ) will be increased by 0.4 and the sample will be re-weighed. The maximum ρ is 3.0. If F... - and Cl - If the recovery rate is simultaneously low, or if the retention times of both peaks shift forward by more than 2.5%, it is considered that the total matrix load of the injection is too high, and the injection should be... Reduce to 0.75~0.80 of the original value, and at the same time, according to the new... Recalculate and If the spiked recovery rate is too high and the blank is acceptable, check whether the peak exceeds the calibration upper limit or overlaps with the system peak; if it is confirmed to be due to sample overload, the peak size should also be reduced. Alternatively, the dilution factor can be increased and the decomposition step repeated. Under no circumstances should the original result be multiplied by the reciprocal of the recovery rate, a fixed compensation factor, or a historical experience factor.

[0057] If the initial increase in ρ still fails to meet the requirements, no further addition of media exceeding 3.0 is permitted. Instead, the sample mass is reduced from 0.3000 g to 0.2000 g; if still unsatisfactory, the mass is reduced to 0.1500 g, and the volume is maintained at 100 mL. Each time the sample mass is changed, the cation equivalent and media volume are recalculated, and the Fo of the sample is reset. - Cl - Spiked samples. Results for unspecified samples are valid only if both spikes enter the window, the process blank is qualified, and the chromatographic retention time meets the requirements. This rule places anomaly localization and correction during the sample preparation stage, ensuring that reported values ​​come from actual measurements after physical purification.

[0058] 9) Results calculation, reporting, and process constraints definition The concentration of X ions obtained from the working curve and after subtracting the process blank from the same batch is expressed in mg / L; D is the dilution factor. The volume of the purified stock solution is expressed in mL. The sample mass is expressed in grams. The mass fraction of X ions in the sample is expressed as a percentage (%). The mass fraction of X ions in the purified stock solution is... mg, sample mass is mg gives the mass fraction: (9) F respectively - and Cl - of Substituting into equation (9), we get and When using two dilution factors, calculations are performed separately, without peak area ratio conversion. Results should at least report the sample mass, D, ρ, Final pH, F - and Cl - Content, two spiked recoveries, and whether reprocessing occurred. The absolute or relative difference between parallel tests should meet the limits established by the laboratory based on method validation; when the content is close to the limit of quantitation, it should not be reported as a negative number; below the limit of detection, it should be reported as below the limit of detection; and between the limit of detection and the limit of quantitation, it should be reported as detected but not quantified.

[0059] To monitor the stripping status, residual Ca, Mg, Al, and Fe in the clean stock solution can be measured during the method establishment period or when changing media batches. The removal rate of each of these four substances should ideally be no less than 99.0%, and the residual concentrations of Al and Fe should ideally not exceed 0.50 mg / L and 0.20 mg / L, respectively. This monitoring is only for validating the exchange step and is not a mandatory detection terminal for every sample, nor should residual metal concentration replace double-spiking criteria. If the residual metal concentration is acceptable but F... - If the spiked solution fails to meet the standard, the filter media adsorption, pH electrode contamination, and NaOH blank should be checked first.

[0060] For Cl - or F - Samples with a mass fraction higher than 0.50% should be given priority. Reduce the concentration to 0.1000 g–0.2000 g to avoid the measured peak exceeding the calibration range; for SO4 2- High-content gypsum-based admixtures will not remove SO4 through cation exchange. 2- SO42 should be controlled with a small injection volume and sufficient run time. 2- Complete effluent; for solid waste containing large amounts of soluble Na or K salts, Na₂O, K₂O, and water-soluble alkali should be converted into the appropriate amounts. Because although monovalent ions do not form fluoride complexes, they still occupy H+. +The capacity of the cation exchange medium should be considered. If the sample contains significant organic matter, oil, or surfactants, it should first undergo a separate organic removal treatment without introducing halogens and be re-verified. It should not be assumed that the cation exchange medium can simultaneously perform the function of removing organic matter.

[0061] The key process sequence in this method cannot be arbitrarily reversed. Adjusting the pH before exchanging the Na+ will cause... + It consumes capacity and may cause Al and Fe to form colloids, entraining F. - Pre-volume quantification followed by exchange will increase the processing volume and porosity retention error; using anion exchange materials will directly retain F. - and Cl - Activation with HCl introduces a non-negligible amount of Cl. - Raising the pH before the media are separated will cause precipitation inside the bed. Therefore, after filtration, the acidic liquid will contact H... + The process involves taking a medium at a volume ratio of 1.2 to 3.0, adjusting the pH to 5.5 to 6.5 after separation, conducting joint measurements with the same purified solution, and triggering reprocessing with double anion spiking, forming a complete and mutually restrictive operational chain.

[0062] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0063] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.

[0064] Example 1 This implementation process follows GB / T 176-2025 "Chemical Analysis Methods for Cement" for sample preparation and nitric acid decomposition, and HJ 84-2016 "Inorganic Anions in Water Quality (F)" for further analysis. - Cl - NO2 - ,Br - NO3 - PO4 3- SO3 2- SO4 2-The determination of ions by ion chromatography was performed using a method that included suppressed conductivity detection and chromatographic quality control. The test water met the Class II water requirements of GB / T 6682-2008 "Specifications and Test Methods for Water Used in Analytical Laboratories". The steps for cation medium activation, volume ratio calculation, pH release, and double-spiking determination were performed according to the procedures described in this invention. Four representative materials were selected for a complete implementation process, labeled A, B, C, and D. A was ordinary Portland cement, with the following main oxide mass fractions: CaO 64.2%, MgO 2.2%, Al₂O₃ 4.8%, Fe₂O₃ 3.4%, Na₂O 0.25%, K₂O 0.72%, and MnO 0.10%; B was high-alumina cement, with corresponding contents of 51.8%, 2.6%, 19.6%, 4.1%, 0.32%, 0.61%, and 0.16%; C was steel slag-containing solid waste cementitious material, with corresponding contents of 47.5%, 7.8%, 10.2%, 12.4%, 0.48%, 0.74%, and 2.10%; and D was high-calcium clinker, with corresponding contents of 68.4%, 1.5%, 4.2%, 2.9%, 0.20%, 0.55%, and 0.08%. Six 0.3000 g portions of each sample were weighed independently. H used + The sulfonic acid resin was activated with 0.50 mol / L nitric acid. 5.00 mL of wet-state settling resin was taken, and H₂ was replaced with 1.0 mol / L NaNO₃. + Titration with 0.1000 mol / L NaOH, after subtracting 0.08 mL blank, yielded three titrations with volumes of 92.1 mL, 92.5 mL, and 92.0 mL, corresponding to q. v The concentrations were 1.840 mmol / mL, 1.848 mmol / mL, and 1.838 mmol / mL, with an average q v The concentration was 1.842 mmol / mL, with a relative range of 0.54%. The maximum medium volume was determined using a blank throughout the process. - The concentration was 0.007 mg / L, Cl - The concentration was 0.015 mg / L, meeting the admission criteria; Calculated according to formula (2), the E for each 0.3000 g sample of A, B, C and D is... c The concentrations were 8.506 mmol, 9.935 mmol, 9.713 mmol, and 8.671 mmol, respectively. Based on the material composition, ρ=1.6 for A and D, ρ=2.0 for B, and ρ=2.2 for C; after rounding upward according to formula (3), the wet resin volumes were 7.4 mL, 10.8 mL, 11.7 mL, and 7.6 mL, respectively. After packing each column, keep the bed surface free of air bubbles, pass the filtrate through at 0.80 mL / min, and then wash the collection cup and bed with a total of 15 mL of water. For each sample, 30 mL of water was added and dispersed for 2 min. Then, 10 mL of nitric acid (1+10) was added, and the mixture was gently boiled for 90 s. After cooling to 25 °C, the sample was filtered through pre-washed rapid filter paper and washed with 3 mL of water in three separate applications. The resin effluent was first treated with approximately 13 mL of 1.0 mol / L NaOH, then adjusted to pH 6.00 ± 0.10 with 0.10 mol / L NaOH. After standing for 5 min for verification, the volume was brought to 100 mL. All four types of samples remained clear after pH adjustment. ICP-OES was used to further validate the liquid phases before and after purification: Before purification, the Ca concentration ranged from 1010 mg / L to 1465 mg / L, and after purification, it ranged from 0.42 mg / L to 0.88 mg / L; before purification, the Mg concentration ranged from 27 mg / L to 142 mg / L, and after purification, it ranged from 0.08 mg / L to 0.36 mg / L; the Al concentration of B decreased from approximately 311 mg / L to 0.18 mg / L; and the Fe concentration of C decreased from approximately 260 mg / L to 0.07 mg / L. The removal rates of all major cations were higher than 99.9%. Ion chromatography was performed using a 4 mm × 250 mm high-capacity anion exchange column and a 4 mm × 50 mm guard column. The eluent consisted of 3.2 mmol / L Na₂CO₃ and 1.0 mmol / L NaHCO₃. The flow rate was 0.80 mL / min, the column temperature was 30 ℃, the injection volume was 10 μL, conductivity detection was suppressed, and the sample collection time was 18 min. - and Cl - The calibration determination coefficients were 0.99996 and 0.99998, respectively, and the recoveries of the intermediate concentration verification solutions were 99.2% and 100.6%, respectively. In the matrix-matched mixed standard solution, F... - and Cl - The retention times were approximately 3.62 min and 5.84 min, respectively. - The peak separation from the previous system was 1.71, F - With Cl - The resolution was 3.46. In the continuous sample, F... - The retention time was 3.59 min to 3.66 min, Cl - The retention times ranged from 5.79 min to 5.89 min, and no unidirectional drift was observed with the injection sequence. Of the 6 parallel results, A's F - The average mass fraction was 0.0362%, and the standard deviation was 0.0005%. - The average value is 0.0211%, and the standard deviation is 0.0003%; B's F - The average was 0.1116%, and the standard deviation was 0.0017%. -The average value is 0.0474%, and the standard deviation is 0.0006%; C's F - The average value was 0.0714%, and the standard deviation was 0.0012%. - The average value is 0.0831%, and the standard deviation is 0.0009%; D's F - The average value was 0.0243%, and the standard deviation was 0.0004%. - The average value was 0.0152%, with a standard deviation of 0.0003%. The relative standard deviation was 1.08%–1.97%. No F was observed in high-alumina and high-Fe materials. - Repeatability deteriorated significantly; F is set separately for each type of sample. - and Cl - Added standard throughout the entire process. F - The theoretical increment in the purified stock solution is 0.20 mg / L, Cl - The theoretical increment is 0.50 mg / L. A's F - Cl - The recoveries were 98.6% and 100.4% for B, 96.2% and 99.1% for C, 94.8% and 97.6% for D, and 101.0% and 101.2% for F. The spiked values ​​of both anions for all four materials were within the specified window, indicating that the capacity ratio could be maintained simultaneously with compositional adjustments. - Release and Cl - The goal is to stabilize the peak, rather than simply improving one of the metrics.

[0065] As a control, the same batch of decomposition solutions were injected directly under the same pH and dilution conditions without cation stripping. F of A, B, C, and D - The recoveries of the spiked samples were 91.8%, 72.6%, 79.4%, and 88.9%, respectively. - The recoveries of the spiked samples were 95.4%, 91.2%, 88.5%, and 93.8%, respectively. The F values ​​for B and C... - The recovery rate was significantly low, and the C-Cl content was low. - Also below the window; after 10 consecutive injections, the F of the unstripped solution - Cl - The maximum drift of retention time relative to the initial value was 5.2% and 6.8%, respectively, while the maximum drift after processing with this method was 1.1% and 1.3%, respectively. A small amount of light-colored deposits were visible on the inlet sieve plate of the guard column in the unstripped control, but this phenomenon was not observed in the sequences processed with this method.

[0066] Calculated using the standard deviations of 11 complete process blanks at 3 and 10 times, the F in the purified stock solution - The method detection limit and quantitation limit were 0.012 mg / L and 0.040 mg / L, respectively.- The concentrations were 0.018 mg / L and 0.060 mg / L, respectively. (In m) s For 0.3000 g, V f When the sample volume is 100 mL and D=1, the corresponding limits of quantitation for the sample mass fraction are approximately 0.0013% and 0.0020%, respectively. When D=5 is used, the limits of quantitation increase with the dilution factor, but the above four types of samples are still within the effective calibration range.

[0067] A separate volumetric deficiency test was performed on sample C, artificially reducing pH to 1.0. The treated solution showed slight turbidity after standing at pH 6.0. F - The recovery rate was 81.6%, Cl - The spiked recovery rate was 89.2%, F - The retention time offset is 3.7%. No compensation is made to the results; instead, F is increased to 1.4 according to the reprocessing rules. - It was still only 87.2%, and although it entered the window edge, the residual Al was 0.74 mg / L; after reprocessing according to the material's preset ρ=2.2, F - and Cl - Recovery rates were restored to 94.8% and 97.6%, and the treated solution became clear. This process demonstrates that spike anomalies can be identified before reporting volume breakthrough and that normal results can be obtained by increasing the effective exchange capacity.

[0068] Example 2 (Gradient Example of Exchange Capacity Ratio ρ) Materials of four categories, A, B, C, and D, were tested under conditions of ρ = 1.0, 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, and 3.0, with ρ = 3.2 as the upper limit outer boundary control. The amount of medium used for each condition was determined according to equations (2) and (3). When the medium volume corresponding to 0.3000 g of sample was greater than 15 mL, the sample mass was reduced to 0.2000 g according to the steps in part 3), and Ec and the medium volume were recalculated. Other decomposition, filtration, flow rate, washing, pH adjustment, volume adjustment, and ion chromatography conditions were the same as in this embodiment. Three independent treatments were set up for each condition, with the removal rate of total cation charge equivalent, F... - Spiked recovery rate, Cl - Spike recovery rate, residual Al and Fe concentrations, blank control throughout the process, and the clarity of the treated solution were used as evaluation indicators.

[0069] The total charge equivalent removal rate of cations is calculated as the percentage of the difference in charge equivalents of Ca, Mg, Al, and Fe before and after purification relative to the total charge equivalent before purification. For evaluation, a total charge equivalent removal rate of cations of not less than 99.0%, residual Al not exceeding 0.50 mg / L, residual Fe not exceeding 0.20 mg / L, and F... -Spiked recoveries were 85%–115%, Cl - Spiked recoveries were 90%–110%, F - Blank concentration not higher than 0.010 mg / L, Cl - The basic acceptable conditions are a blank concentration of no more than 0.020 mg / L and a clear solution after pH adjustment; the recommended range also requires a stable removal rate of major cations of over 99.9% with a capacity margin. The results are shown in Tables 1 to 5.

[0070] Table 1. ρ gradient results for ordinary Portland cement A

[0071] Table 2. ρ gradient results of high-alumina cement B

[0072] Table 3. ρ gradient results of C in cementitious materials containing steel slag solid waste

[0073] Table 4. ρ gradient results of D in high-calcium clinker

[0074] Table 5. Maximum values ​​of blank space throughout the entire process under different ρ values.

[0075] As shown in Tables 1 and 4, ordinary Portland cement A and high-calcium clinker D met the requirements of basic recovery rate and 99.0% cation removal at ρ=1.2, but the cation removal rate had not yet stabilized at 99.9%; when ρ increased to 1.4~1.8, the cation removal rate reached over 99.9%, and F - Cl - Recovery rates plateaued, therefore the recommended range for A and D was set at 1.4–1.8. Further increases in ρ above 2.0 did not yield substantial improvement.

[0076] As shown in Table 2, when the ρ of high-alumina cement B is not higher than 1.4, F - Recovery rate is below 85%; although F = 1.6 - and Cl - The recovery rate entered the specified window, but the residual Al was 0.62 mg / L, higher than the monitoring value of 0.50 mg / L. When the ρ was 1.8~2.4, the cation removal rate stably reached over 99.9%, the residual Al decreased to below 0.43 mg / L, and the recovery rates of both spiked methods were stable. Therefore, the recommended range for high-alumina cement was determined to be 1.8~2.4.

[0077] As shown in Table 3, when the cementitious material C containing steel slag solid waste has a lower viscosity than F when ρ=1.0, the F value is significantly lower.- and Cl - The recoveries were 81.6% and 89.2%, respectively, consistent with the aforementioned undercapacity test; at ρ=1.4, F - The recovery rate was 87.2%, but the residual Al was still 0.74 mg / L; at ρ=1.8, the residual Al was 0.56 mg / L, still higher than the monitoring value. After increasing ρ to 2.0~2.6, the cation removal rate steadily reached over 99.9%, and F... - and Cl - The recovery rates were stable, with 94.8% and 97.6% respectively at ρ=2.2, consistent with the aforementioned implementation results. Therefore, the recommended range for this type of material is determined to be 2.0~2.6.

[0078] Based on the four types of materials, it can be seen that when ρ=1.0, at least A, B, and C will appear. - If the recovery rate is unacceptable or cation removal is insufficient, and low-load A and D already meet the basic acceptance criteria at ρ=1.2, then 1.2 is determined as the lower limit of the overall value range. For materials with unknown composition, ρ=2.4 and 2.6 are both acceptable in the four types of materials, so the midpoint between the two, 2.5, is used as the initial value, and the double-spiking results are used to determine whether to adjust.

[0079] As shown in Table 5, with the increase of ρ and medium quantity, F - and Cl - The blank values ​​gradually increased throughout the process; at ρ=3.0, the maximum blank values ​​were 0.009 mg / L and 0.019 mg / L, respectively, still below the access limit but close to it. At ρ=3.2, the maximum blank values ​​reached 0.010 mg / L and 0.020 mg / L, respectively. Simultaneously, the spiked recoveries of all four types of materials decreased from the stable plateau, while the cation removal rate did not significantly improve. Considering the blank fluctuations of different media batches, pore retention volume, and the 100 mL constant volume space, 3.0 was determined as the overall upper limit of ρ. When ρ exceeded 3.0, the amount of media was not increased further; instead, the sample mass was reduced and reprocessed according to the instructions in this manual.

[0080] Three independent treatment results for each condition showed that the relative standard deviation of the total charge equivalent removal rate of cations was no greater than 0.20%. - The relative standard deviation of the spiked recoveries ranged from 0.8% to 2.5%. - The relative standard deviation of the spiked recovery rate was 0.6%–1.8%. The above trends indicate that ρ = 1.2–3.0 can cover the basic treatment requirements of materials with different cation loadings. For ordinary silicate cement and high-calcium clinker, high-alumina cement, and steel slag-containing solid waste cementitious materials, ρ = 1.4–1.8, 1.8–2.4, and 2.0–2.6 respectively, a stable balance can be achieved between cation removal, bi-anion recovery, and process blank.

[0081] For another Cl - A high-salt solid waste sample with a mass fraction of approximately 0.62% showed Cl at a sampling rate of 0.3000 g. - The peak exceeds the highest calibration point and Cl - The apparent recovery rate was 116.8%. This result was discarded according to regulations. The sample mass was reduced to 0.1500 g, E_c was recalculated and ρ=2.4 was taken. The purified stock solution was then diluted 10-fold before injection. Cl - The spiked recovery rate was 102.3%, F - The spiked recovery rate was 97.5%, and both peaks were within the calibration range. Adjustments were made during resampling, repurification, and appropriate dilution; no empirical coefficients were used to alter the original measurements.

[0082] After 120 injections of purified samples, the F of the intermediate verification solution was... - The peak area changed by 1.8% relative to the initial value, Cl - A 1.4% change in peak area resulted in a 0.06 MPa increase in guard column differential pressure. For the unpeeled control sequence, the guard column differential pressure increased by 0.21 MPa after 40 injections, necessitating the removal and cleaning of the inlet sieve plate. This indicates that this method, while retaining the same nitric acid decomposition solution for joint determination, reduces deposition, volume occupancy, and retention behavior changes caused by polyvalent cations entering the chromatographic system, thus extending the continuous operation cycle.

[0083] This implementation process also shows that the amount of medium used is determined by q. v E c After being determined by ρ, the resin volume of different materials is matched with their total charge load of Ca, Mg, Al, and Fe. High-alumina sample B and high-Fe, Mg sample C were not simply categorized as cement and used with the same fixed medium volume; ordinary samples A and D also did not use unnecessary maximum medium volumes, thus maintaining a low Cl content. - F - Process blank. pH adjustment uses only NaOH and nitric acid, without introducing additional organic anions; the same purification solution simultaneously provides F. - Cl - As a result, the propagation of errors caused by sample splitting, separate preprocessing, and separate correction was reduced.

[0084] Figure 2 The exchange capacity ratio ρ and the total charge equivalent removal rate of cations, F - Spiked recovery and Cl - The measured relationship between spiked recoveries is shown in the graph. The solid dotted line, the dashed square line, and the dashed triangle line represent the cation removal rate, F2O2 removal rate, and F4O2 removal rate, respectively. - Spiked recovery and Cl -Spiked recoveries are shown in the figure. The gray area represents the recommended ρ range for the corresponding material, with ρ=3.2 as the upper limit outer boundary control. The figure shows that as the exchange capacity ratio ρ increases, the total cation charge equivalent removal of the four types of materials initially increases rapidly, then plateaus. - Spiked recovery and Cl - The spiked recovery rate also increases with increasing ρ, and enters the acceptable range within their respective recommended ranges. Different materials require different ρ values ​​to achieve stable removal and acceptable recovery rates: ordinary silicate cement and high-calcium clinker enter the recommended plateau at ρ = 1.4~1.8, high-alumina cement at ρ = 1.8~2.4, and cementitious materials containing steel slag at ρ = 2.0~2.6. When ρ continues to increase above 3.0, the cation removal rate does not significantly improve, and F... - and Cl - Spike recovery actually decreased, and the process blank was close to the limit, so the upper limit of ρ was controlled at 3.0.

[0085] Figure 3 The number of regeneration cycles of the cation exchange medium and the wet-state volumetric exchange capacity qv, F - Spiked recovery and Cl - A graph showing the monitoring and judgment relationship between spiked recoveries was used. The three indicators were retested before use and after one, three, and five regeneration cycles. The F... - Spiked recoveries and 85%–115% window, Cl - Compare the spiked recovery rate with the 90%~110% window; if any retest indicator or double blank threshold fails, stop or discard the medium in advance; only if it passes the threshold and has not reached 5 retests can the next regeneration begin; after reaching 5 retests, stop regeneration. From Figure 3 It can be seen that the wet volumetric exchange capacity qv and F of the cation exchange medium need to be remeasured before use and after 1, 3, and 5 regenerations. - Spiked recovery and Cl - Spiked recovery rate; the retested qv was used to recalculate the media dosage Vr, F - The acceptable recovery rate for spiked products is 85%–115%. - The acceptable recovery rate is 90% to 110%. If any retest indicator or double blank threshold fails, the medium should be stopped or discarded in advance. Only if the medium is qualified and has not been regenerated 5 times can it proceed to the next regeneration. Regeneration should be stopped after 5 regenerations.

[0086] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.

Claims

1. A method for the combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping, characterized in that, Includes the following steps: S1: Decompose the cement sample with nitric acid, filter, and collect the acidic filtrate; S2: Pass the collected acidic filtrate through a cation exchange medium, utilizing the H+ in the cation exchange medium. + Exchange and remove Ca from the acidic filtrate 2+ Mg 2+ Al 3+ and Fe 3+ Collect all effluent flowing out of the cation exchange medium; S3: After the effluent is separated from the cation exchange medium, the pH of the effluent is adjusted to 5.5~6.5, and then the volume is adjusted to obtain the purified stock solution; S4: Take the purified stock solution and determine the F content therein by ion chromatography. - and Cl - ; The cation exchange medium is a hydrogen-type strong acidic cation exchange medium, and the amount of cation exchange medium used is controlled by the exchange capacity ratio ρ. The exchange capacity ratio ρ is the ratio of the total exchange capacity of the cation exchange medium to the total charge equivalent of the cations to be removed in the cement sample. The value of ρ ranges from 1.2 to 3.

0.

2. The method for combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping according to claim 1, characterized in that, The amount of the cation exchange medium used is determined according to the following steps: Determination of the wet volumetric exchange capacity q of cation exchange media v ; Calculate the total charge equivalent E of the cations to be removed in the sample. c ; The required wet volume V of the cation exchange medium can be calculated using the following formula. r ; ; in, The exchange capacity ratio is taken in the range of 1.2 to 3.0 depending on the type of cement sample. The E c Calculate using the following formula: ; in, denoted as sample mass; i represents the index of oxides decomposed by nitric acid and occupying exchange sites. This represents the number of oxygen atoms in the oxide. The proportion of acid-soluble substances that enter the filtrate. The mass fraction of the oxide. denoted as , where is the molar mass of the oxide.

3. The method for combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping according to claim 2, characterized in that, The cement sample includes at least one of silicate cement, high-alumina cement, steel slag-containing solid waste cementitious material, and high-calcium clinker. When the cement sample is silicate cement or high-calcium clinker, ρ is 1.4~1.8; when the cement sample is high-alumina cement, ρ is 1.8~2.4; when the cement sample is cementitious material containing steel slag solid waste, ρ is 2.0~2.6; when the composition of the cement sample is unknown, ρ is 2.

5.

4. The method for combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping according to claim 1, characterized in that, It also includes steps for determining spiked recovery rate and reprocessing non-compliant batches: Before decomposing the cement sample with nitric acid in S1, unspiked samples and F were prepared respectively. - Spiked sample and Cl - Spiked sample, so that the unspiked sample, F - Spiked sample and Cl - The spiked samples were subjected to S1 to S4 sequentially. Calculate F in the same analytical batch after S4 is completed. - Spiked recovery and Cl - Spike recovery rate; when F - Spiked recoveries not in the range of 85%–115%, or Cl - If the spiked recovery rate is not within the range of 90% to 110%, the analytical batch is deemed unqualified. After confirming the process blank, calibration verification, and chromatographic system are qualified, the exchange capacity ratio ρ is increased or the sample mass is reduced, and the batch is reprocessed starting from S1. The original determination results are not corrected using the reciprocal of the recovery rate, fixed compensation coefficient, or historical experience coefficient. The spiked and unspecified samples used the same dilution factor D, and the F - Spiked recovery and Cl - The formula for calculating the spiked recovery rate is as follows: ; Where X is F - or Cl - , should be F - hour, F represents - Spiked recovery rate, when Cl - hour, Cl - Spike recovery rate; and The concentrations of X ions measured after subtracting the process blank are the spiked and unspiked portions, respectively; D s D0 and D0 are the dilution factors for unspecified and unspecified portions, respectively. To determine the final volume of the purified stock solution; The mass of the added X ions.

5. The method for combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping according to claim 1, characterized in that, In S1, the molar concentration of the nitric acid is 1.2~1.5 mol / L; during the decomposition of the cement sample with nitric acid, the cement sample is first dispersed in water, then nitric acid is added and heated to a gentle boil, and then filtered after cooling.

6. The method for combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping according to claim 1, characterized in that, In S1, the ratio of cement sample to water is 0.3000g:(30~50)mL; the ratio of cement sample to nitric acid is 0.3000g:(10~20)mL; the nitric acid is added at a time of 30s~60s; and the simmering time is 1min~2min.

7. The method for combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping according to claim 1, characterized in that, In S2, the cation exchange medium is a sulfonic acid-based strong acid cation exchange resin, and its usage state is H. + The cation exchange medium has a styrene-divinylbenzene crosslinked gel or macroporous polymer as its backbone, a total wet volume exchange capacity of 1.6 mmol / mL to 2.2 mmol / mL, a particle size of 0.30 mm to 1.20 mm, and a water content of 45% to 60%. Before use, the cation exchange medium is activated with nitric acid and passed through a Cl-... - F - Double blank access; The standard for dual-blank admission is F in the entire process blank. - Not exceeding 0.010 mg / L, Cl - Not higher than 0.020 mg / L.

8. The method for combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping according to claim 1, characterized in that, In S2, the acidic filtrate has an empty bed contact time of not less than 6 minutes with the cation exchange medium, and the volumetric flow rate is not greater than 1.2 mL / min.

9. The method for combined chromatographic determination of chlorine and fluorine in cement with cationic matrix stripping according to claim 1, characterized in that, In S3, the pH value is adjusted using NaOH solution.

10. A chromatographic system for the determination of chlorine and fluorine in cement by cationic matrix stripping, characterized in that, include: The decomposition unit is used to decompose cement samples with nitric acid and filter them to collect the acidic filtrate. A cation exchange unit is used to pass the collected acidic filtrate through a cation exchange medium, utilizing the H+ in the cation exchange medium. + Exchange and remove Ca from the acidic filtrate 2+ Mg 2+ Al 3+ and Fe 3+ Collect all effluent flowing out of the cation exchange medium; The pH adjustment and volume control unit is used to adjust the pH of the effluent to 5.5~6.5 after the effluent is separated from the cation exchange medium, and then to make up the volume to obtain the purified stock solution. The ion chromatography detection unit is used to take the purified stock solution and determine the F content therein by ion chromatography. - and Cl - ; The control unit is used to control the amount of medium in the cation exchange unit according to the exchange capacity ratio ρ, wherein the exchange capacity ratio ρ is the ratio of the total exchange capacity of the cation exchange medium to the total charge equivalent of the cations to be removed in the sample, and the value of ρ ranges from 1.2 to 3.0.