Method for determining the oxidation rate of polymetallic ores
By employing multi-stage fine screening and sample preparation processes, combined with economic weighting and liberation degree correction, the accuracy and economic guidance issues of polymetallic ore oxidation rate determination have been resolved, enabling more accurate oxidation rate calculation and optimization of mineral processing technology.
Patent Information
- Application Number
- CN202611676510.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies are insufficient to accurately determine the oxidation rate of polymetallic ores, especially in complex polymetallic ores. The calculation benchmark for the oxidation rate is unclear, making it difficult to make horizontal comparisons of the results and reflect the actual degree of oxidation and metal loss. Existing methods are also complex to operate and have large errors.
By employing multi-particle fine sieving, graphite doping and embedding with secondary cutting sample preparation, calculation of oxidation loss of undissociated portion, economic weighting, and correction of dissociation standard deviation, the basis for calculating oxidation rate is clarified, thereby improving the accuracy and economic guidance of the determination.
Through refined screening and sample preparation processes, the accuracy and representativeness of oxidation rate determination are improved, enabling a more accurate reflection of metal loss during mineral processing and providing a reliable basis for mineral processing optimization and resource evaluation.
Smart Images

Figure CN123155773A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of process mineralogy, specifically to a method for determining the oxidation rate of polymetallic ores. Background Technology
[0002] In the process of mineral resource development and utilization, the degree of oxidation of ore is one of the key parameters determining the beneficiation and metallurgical process route, recovery rate, and economic benefits. Accurately determining the effective oxidation rate of target elements in the ore not only helps in the rational formulation of flotation, leaching, and other process flows, but also provides important basis for resource reserve assessment and comprehensive utilization. Especially for polymetallic ores containing copper, lead, zinc, gold, silver, etc., the oxidation rate directly affects the blending ratio of sulfide minerals and oxide minerals, reagent formulation, and tailings management strategies.
[0003] Currently, methods for determining the oxidation rate of ores targeting a single element are mainly divided into two categories: chemical analysis and mineralogical analysis. Chemical analysis often employs phase analysis, such as selective dissolution, acid leaching, or potentiometric titration, to distinguish between oxidized and sulfide mineral phases using different solvents, and then calculates the oxidation rate using stoichiometry. This type of method is relatively complex to operate and has the following shortcomings: (1) Selective dissolution conditions are difficult to control precisely, and cross-phase dissolution or cross-phase occurrence is prone to occur, leading to result deviations; (2) For finely embedded or complexly connected particles after grinding, inclusions cannot be effectively distinguished, especially the oxidized / sulfide components within them, thus underestimating the actual content; (3) The analysis cycle is long, and there is a lack of ability to simultaneously determine multi-element systems. On the other hand, methods based on automated mineralogical analysis (such as MLA, QEMSCAN, TIMA, etc.) can achieve mineral type identification, particle dissociation statistics, and elemental distribution characterization by relying on high-resolution backscattered electron imaging (BEI) and energy dispersive spectroscopy (EDS) quantitative technology, and have been widely recognized in process mineralogical research. However, existing automated mineralogical analysis workflows still face several challenges: First, in the sample preparation stage, improper epoxy resin embedding or poor polishing quality can easily cause mineral particles to detach or agglomerate, resulting in surface scratches or poor conductivity, affecting image recognition accuracy. Second, for ultrafine-grained minerals with a particle size less than 0.010 mm, due to similar BEI gray levels or blurred particle boundaries, oxide minerals and sulfide minerals are easily misidentified, and there is a significant random error in the degree of liberation statistics, which lacks a unified and effective correction method. Third, existing oxidation rate calculation methods mostly use simple mass weighting or single-element phase ratios, failing to fully consider the differences in the contribution of mineral liberation states in different particle sizes to the "effective loss" of oxidation, and also failing to introduce economic value weights, making it difficult to objectively reflect the actual industrial utilization value of the ore. Currently, there is a lack of a unified definition and benchmark selection standard for the determination of oxidation rate in polymetallic ores. Existing technologies have not provided a clear definition of which target element or mineral should be used as the benchmark for oxidation rate calculation. Therefore, existing oxidation rate results are difficult to compare horizontally and cannot accurately reflect the actual oxidation degree of polymetallic ores and the metal loss during the beneficiation process.
[0004] In view of this, it is necessary to develop a method for determining the oxidation rate of polymetallic ores, so as to clarify the calculation benchmark for oxidation rate and improve the accuracy, representativeness and economic guidance of the determination. Summary of the Invention
[0005] In view of the technical problems existing in the background art, this application provides a method for determining the oxidation rate of polymetallic ores. This method uses multi-particle fine sieving, graphite doping and embedding and secondary cutting sample preparation, conversion of oxidation loss of undissociated part, economic weighting and standard deviation correction of dissociation degree to clarify the oxidation rate calculation benchmark, thereby improving the accuracy, representativeness and economic guidance of oxidation rate determination.
[0006] To achieve the above objectives, embodiments of this application provide a method for determining the oxidation rate of polymetallic ores, comprising: S1, the sample to be tested is ground and sieved to obtain ore samples of various particle sizes, with a mass of A. n The yield is a n ; S2, ore samples of various particle sizes were selected and subjected to initial embedding, vertical cutting, and secondary embedding processes to obtain sample B for automated mineralogical analysis. n ; S3, for analyzing sample B n Perform automated mineralogical analysis to determine the type of target mineral and its mass fraction (b) in the analytical sample. i e .n Mass fraction c of the target element in the target mineral i e .n and dissociation parameter d i e .s.n ; S4. Based on the results of automated mineralogical analysis, calculate the mass fraction of the target element in oxidized minerals, the mass fraction of the target element in specific intergrowths and inclusions of sulfide minerals, and the total mass fraction of the target element in the analyzed sample to obtain the effective oxidation rate W of the target element. i ; S5. Based on the effective oxidation rate of the target element and combined with the market price of the target element as a value weighting factor, the economic weighted oxidation rate W of the ore is obtained. S6, based on the liberation degree parameter d of the target mineral. i e .s.n Calculate the degree of liberation correction factor K to obtain the corrected economic weighted oxidation rate W' of the ore; where, n represents the particle size, and n can be 1 to m, where 2 ≤ m ≤ 4; i represents the type of target element, and e represents the type of target mineral; s represents sulfide minerals in the target mineral.
[0007] Furthermore, based on the results of automated mineralogical analysis, the steps for calculating the effective oxidation rate of the target element, including calculating the mass fraction of the target element in oxidized minerals, the mass fraction of the target element in specific intergrowths and inclusions of sulfide minerals, and the total mass fraction of the target element in the analyzed sample, include: Calculate the mass fraction of the target element in oxidized minerals, and the mass fraction M of the target element in specific intergrowths and inclusions of sulfide minerals. i.1 =Σa n ×b ie .x.n ×c i e .x.n +Σa n ×b i e .s.n ×c i e .s.n ×d i e .s.n ; Calculate the total mass fraction M of the target element in each particle size. i.2 =Σa n ×b i e .n ×c i e .n ; Calculate the effective oxidation rate W of the target element i =M i.1 / M i.2 ;in, x represents an oxidized mineral in the target mineral.
[0008] Furthermore, the steps to obtain the economically weighted oxidation rate of the ore, based on the effective oxidation rate of the target element and combined with its market price as a value weighting factor, include: Introducing the market price Q of the target element i Calculate the economically weighted oxidation rate of the ore W = Σ(W i ×M i.2 ×Q i ) / Σ(M i.2 ×Q i ).
[0009] Furthermore, the steps for calculating the liberation degree correction coefficient based on the liberation degree parameter of the target mineral to obtain the corrected economic weighted oxidation rate of the ore include: Calculate the economic weighted value of each target mineral, and select the target mineral with the highest weighted value as the key target mineral; Different fields of view of the analytical samples of key target minerals were selected, and the degree of dissociation parameters were repeatedly measured. The standard deviation σ and the average value d were calculated to obtain the degree of dissociation deviation coefficient k=2σ / d. Calculate the degree of dissociation correction coefficient K = 1 / (1-k) based on the degree of dissociation deviation coefficient k. The corrected economic weighted oxidation rate of ore, W' = K × W, is calculated based on the degree of liberation correction factor.
[0010] Furthermore, the steps for calculating the economic weighted value of each target mineral and selecting the target mineral with the highest weighted value as the key target mineral include: Obtain the mass fraction of sulfide minerals containing each target element in the sample to be tested, the mass fraction of the target element in the sulfide, and the market unit price of each target element; The economic contribution of a target mineral is calculated as the product of the mass fraction of sulfide minerals containing each target element, the mass fraction of the target element in the sulfide minerals, and the market price of the target element. The sulfide minerals that contribute the most to economic growth were identified as the key target minerals in the samples to be tested.
[0011] Furthermore, the degree of dissociation parameter should be measured at least 10 times.
[0012] Furthermore, the degree of dissociation parameter d i e .s.n This represents the mass fraction of sulfide mineral inclusions and intergrowths within mineral particles with a diameter ≤ 0.010 mm in the nth particle size analysis sample, relative to the total mass of the target mineral.
[0013] Furthermore, the grinding particle size is ≤0.074mm.
[0014] Furthermore, the particle size range of the ore sample includes at least two of the following four particle size ranges: Greater than 0.037 mm; Less than or equal to 0.037 mm and greater than 0.010 mm; Less than or equal to 0.010 mm and greater than 0.005 mm; Less than or equal to 0.005 mm.
[0015] Furthermore, the steps for obtaining automated mineralogical analysis samples by selecting ore samples of various particle sizes and performing initial embedding, vertical cutting, and secondary embedding processes include: After mixing the analytical sample with graphite powder, epoxy resin was used for initial embedding and curing. The initial embedded body was cut vertically to obtain a slice containing the cross section of the analytical sample; The slices were then embedded and cured with their cut surfaces facing down. The embedded body obtained by secondary embedding and solidification is ground and polished to expose the cutting surface and form a polished surface. After carbon spraying, an automated mineralogical analysis sample is obtained.
[0016] The beneficial technical effects of this application are as follows: In the technical solution of this application, considering the complex mineral composition, wide particle size distribution, and close symbiotic relationship between sulfide and oxide minerals in polymetallic ores, the samples are first finely sieved to obtain multiple narrow-particle-size samples, which are then prepared and analyzed separately to reduce the impact of particle size differences and sampling deviations on the measurement results, thereby improving sample representativeness and data comparability. In the sample preparation stage, an optimized graphite doping and embedding process combined with a secondary cutting process is used to fully expose the cross-section of mineral particles, thereby improving the resolution and statistical representativeness of automated mineralogical analysis for identifying fine-grained minerals, inclusions, and intergrowths. In the calculation model, in addition to statistically analyzing conventional oxide minerals, the portion of sulfide minerals that has not been liberated due to inclusions or intergrowths is also converted into oxidation loss to more accurately reflect the metal loss caused by insufficient liberation during mineral processing. Simultaneously, the market price of the target element is introduced as an economic weighting factor to weight the oxidation loss of different target elements based on economic value; and a correction coefficient is constructed based on the standard deviation of liberation obtained from repeated measurements to effectively correct for misjudgment of fine particles and statistical errors. Thus, an accurate, comprehensive, and economically significant oxidation rate determination result is obtained, providing a reliable basis for mineral processing optimization, resource evaluation, and metallurgical process design.
[0017] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description
[0018] To more clearly illustrate the technical solution of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.
[0019] Figure 1 This is a backscattering image of chalcopyrite and chalcocite in Example 1 of this application; Figure 2 for Figure 1 Elemental surface scans of chalcopyrite and chalcocite in the particles; Figure 3 for Figure 1 Energy dispersive spectroscopy (EDS) analysis of the target element in the particle; Figure 4 This is a backscattering image of molybdenite and tungsten-molybdenite in Example 1 of this application; Figure 5 for Figure 4 Elemental surface scans of molybdenite and tungsten-molybdenite in the particles; Figure 6 for Figure 4 Energy spectrum analysis of the target element in the particle. Detailed Implementation
[0020] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.
[0022] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0023] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0024] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0025] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0026] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0027] Unless otherwise specified, the terms "comprising" and "including" as used in this application are open-ended. For example, "comprising" and "including" may mean that other components not listed may also be included or contained.
[0028] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0029] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.
[0030] In the process of mineral resource development and utilization, the degree of oxidation of ore is one of the key parameters determining the beneficiation and metallurgical process route, recovery rate, and economic benefits. Accurately determining the effective oxidation rate of target elements in the ore not only helps in the rational formulation of flotation, leaching, and other process flows, but also provides important basis for resource reserve assessment and comprehensive utilization. Especially for polymetallic ores containing copper, lead, zinc, gold, silver, etc., the oxidation rate directly affects the blending ratio of sulfide minerals and oxide minerals, reagent formulation, and tailings management strategies.
[0031] Currently, methods for determining the oxidation rate of ores targeting a single element are mainly divided into two categories: chemical analysis and mineralogical analysis. Chemical analysis often employs phase analysis, such as selective dissolution, acid leaching, or potentiometric titration, to distinguish between oxidized and sulfide mineral phases using different solvents, and then calculates the oxidation rate using stoichiometry. This type of method is relatively complex to operate and has the following shortcomings: (1) Selective dissolution conditions are difficult to control precisely, and cross-phase dissolution or cross-phase occurrence is prone to occur, leading to result deviations; (2) For finely embedded or complexly connected particles after grinding, inclusions cannot be effectively distinguished, especially the oxidized / sulfide components within them, thus underestimating the actual content; (3) The analysis cycle is long, and there is a lack of ability to simultaneously determine multi-element systems. On the other hand, methods based on automated mineralogical analysis (such as MLA, QEMSCAN, TIMA, etc.) can achieve mineral type identification, particle dissociation statistics, and elemental distribution characterization by relying on high-resolution backscattered electron imaging (BEI) and energy dispersive spectroscopy (EDS) quantitative technology, and have been widely recognized in process mineralogical research. However, existing automated mineralogical analysis workflows still face several challenges: First, in the sample preparation stage, improper epoxy resin embedding or poor polishing quality can easily cause mineral particles to detach or agglomerate, resulting in surface scratches or poor conductivity, affecting image recognition accuracy. Second, for ultrafine-grained minerals with a particle size less than 0.010 mm, due to similar BEI gray levels or blurred particle boundaries, oxide minerals and sulfide minerals are easily misidentified, and there is a significant random error in the degree of liberation statistics, which lacks a unified and effective correction method. Third, existing oxidation rate calculation methods mostly use simple mass weighting or single-element phase ratios, failing to fully consider the differences in the contribution of mineral liberation states in different particle sizes to the "effective loss" of oxidation, and also failing to introduce economic value weights, making it difficult to objectively reflect the actual industrial utilization value of the ore. Currently, there is a lack of a unified definition and benchmark selection standard for the determination of oxidation rate in polymetallic ores. Existing technologies have not provided a clear definition of which target element or mineral should be used as the benchmark for oxidation rate calculation. Therefore, existing oxidation rate results are difficult to compare horizontally and cannot accurately reflect the actual oxidation degree of polymetallic ores and the metal loss during the beneficiation process.
[0032] To address the aforementioned technical problems, this application provides a method for determining the oxidation rate of polymetallic ores, comprising: S1, the sample to be tested is ground and sieved to obtain ore samples of various particle sizes, with a mass of A. n The yield is a n ; S2, ore samples of various particle sizes were selected and subjected to initial embedding, vertical cutting, and secondary embedding processes to obtain sample B for automated mineralogical analysis. n ; S3, for analyzing sample B nPerform automated mineralogical analysis to determine the type of target mineral and its mass fraction (b) in the analytical sample. i e .n Mass fraction c of the target element in the target mineral i e .n and dissociation parameter d i e .s.n ; S4. Based on the results of automated mineralogical analysis, calculate the mass fraction of the target element in oxidized minerals, the mass fraction of the target element in specific intergrowths and inclusions of sulfide minerals, and the total mass fraction of the target element in the analyzed sample to obtain the effective oxidation rate W of the target element. i ; S5. Based on the effective oxidation rate of the target element and combined with the market price of the target element as a value weighting factor, the economic weighted oxidation rate W of the ore is obtained. S6, based on the liberation parameter of the target mineral .s.n Calculate the degree of liberation correction factor K to obtain the corrected economic weighted oxidation rate W' of the ore; where, n represents the particle size, and n can be 1 to m, where 2 ≤ m ≤ 4; i represents the type of target element, and e represents the type of target mineral; s represents sulfide minerals in the target mineral.
[0033] In the technical solution of this application, considering the characteristics of polymetallic ores—complex mineral composition, wide particle size distribution, and close coexistence of sulfide and oxide minerals—the sample is first ground and finely sieved in step S1 to obtain multiple narrow-size samples. The mass fraction of each size sample is then determined, and the yield 'a' of each size sample is calculated. n =A n / ΣA n Where n represents the particle size, n ranges from 1 to m, 2 ≤ m ≤ 4, to facilitate subsequent fine calculations based on particle size. In step S2, after the initial embedding and fixing of the sample, vertical cutting ensures that the particles are cut in random directions, guaranteeing a random cross-section for analysis and reducing statistical bias caused by mineral orientation. Secondary embedding improves the hardness of the embedding body and the stability of particle support, facilitating high-precision grinding and polishing to obtain a smooth, clean analytical surface with sufficient particle exposure, thereby improving the statistical representativeness and accuracy of oxidation rate calculation in automated mineralogical analysis. In step S3, the analytical sample B... n Perform automated mineralogical analysis to determine the type of target mineral and its mass fraction (b) in the analytical sample. i e .n Mass fraction c of the target element in the target minerali e .n and dissociation parameter d i e .s.n Where i represents the type of target element, e represents the type of target mineral, and s represents the sulfide mineral within the target mineral. Based on backscattered electron imaging and combined with energy dispersive spectroscopy (EDS) analysis, mineral types are identified particle by particle, and the area fraction of each mineral is calculated and converted to mass fraction using theoretical density. Simultaneously, sample B is measured. n The types and contents of target elements are identified, their occurrence minerals, distribution ratios, and sulfidation or oxidation states are determined, and the grain size distribution, degree of liberation, and intergrowth relationships of the target minerals are obtained. This provides basic data for subsequent oxidation rate calculations and screening of key target minerals. In step S4, based on the results of automated mineralogical analysis, the mass fraction of target elements in oxidized minerals, the mass fraction of target elements in specific intergrowths and inclusions of sulfide minerals, and the total mass fraction of target elements in the analyzed sample are calculated to obtain the effective oxidation rate W of the target elements. i In addition to statistically analyzing conventional oxidized minerals, the portion of sulfide minerals that remains undissociated due to encapsulation or specific intergrowth is also considered as oxidation loss, to more accurately reflect metal loss caused by insufficient dissociation during mineral processing. In step S5, based on the effective oxidation rate of the target element and its market price as a value weighting factor, the economically weighted oxidation rate W of the ore is obtained. This takes into account the difference between the degree of mineral oxidation and the economic value of the element, making the oxidation rate measurement results closer to actual mineral processing and enhancing its economic guidance significance. In step S6, based on the liberation parameter d of the target mineral... i e .s.n The degree of liberation correction coefficient K is calculated to obtain the corrected economic weighted oxidation rate W' of the ore, which corrects the statistical error of fine-grained minerals and improves the accuracy of ore oxidation rate determination.
[0034] It can be explained that automated mineralogical analysis uses scanning electron microscopy (SEM) as a platform, combined with energy dispersive spectroscopy (EDS) to automatically acquire backscattered electron images and elemental spectra. It then automatically identifies minerals through a mineral database and statistically analyzes parameters such as mineral composition, grain size, degree of liberation, and intergrowth relationships. The main systems include MLA (Mineral Liberation Analyzer), QEMSCAN (Quantitative Mineral Scanning Electron Microscopy Analysis System), TIMA (Integrated Mineral Analyzer), and AMICS (Automatic Mineral Identification and Characterization System).
[0035] In some embodiments, the step of calculating the mass fraction of the target element in oxidized minerals, the mass fraction of the target element in specific intergrowths and inclusions of sulfide minerals, and the total mass fraction of the target element in the analyzed sample based on the results of automated mineralogical analysis, to obtain the effective oxidation rate of the target element, includes: Calculate the mass fraction of the target element in oxidized minerals, and the mass fraction M of the target element in specific intergrowths and inclusions of sulfide minerals. i.1 =Σa n ×b i e .x.n ×c i e .x.n +Σa n ×b i e .s.n ×c i e .s.n ×d i e .s.n ; Calculate the total mass fraction M of the target element in each particle size. i.2 =Σa n ×b i e .n ×c i e .n ; Calculate the effective oxidation rate W of the target element i =M i.1 / M i.2 ; where x represents the oxidized mineral in the target mineral.
[0036] In this embodiment, b i e .x.n c represents the mass fraction of the oxidized mineral phase x corresponding to the target mineral e containing target element i in the analytical sample of particle size n. i e .x.n b represents the mass fraction of target element i in the oxidized mineral phase x of target mineral e in an analytical sample of particle size n; i e .s.n c represents the mass fraction of the sulfide mineral phase s corresponding to the target mineral e containing the target element i in the analytical sample of particle size n. i e .s.n This represents the mass fraction of target element i in the sulfide mineral phase s of target mineral e in an analytical sample of particle size n. Based on the results of automated mineralogical analysis, the mass fraction of the target element in the oxidized mineral and the mass fraction of the target element in the sulfide mineral that is not dissociated due to encapsulation or intergrowth are calculated. The portion that is actually difficult to react with the reagent is included in the oxidation rate calculation to more accurately reflect the metal loss caused by insufficient dissociation of the target element and improve the accuracy of oxidation rate determination.
[0037] In some embodiments, the step of obtaining the economically weighted oxidation rate of the ore based on the effective oxidation rate of the target element and combining the market price of the target element as a value weighting factor includes: Introducing the market price Q of the target element i Calculate the economically weighted oxidation rate of the ore W = Σ(W i ×M i.2 ×Q i ) / Σ(M i.2 ×Q i ).
[0038] In this embodiment, the unit price of the target element is introduced as a value weighting factor, and the economic weighted percentages of the oxidation state and total content of the target element are calculated respectively to evaluate the overall economics of the ore system in which the target element is located.
[0039] In some embodiments, the step of calculating a liberation degree correction coefficient based on the liberation degree parameter of the target mineral to obtain the corrected economic weighted oxidation rate of the ore includes: Calculate the economic weighted value of the target element in each target mineral, and select the target mineral with the highest weighted value as the key target mineral; Different fields of view of the analytical samples of key target minerals were selected, and the degree of dissociation parameters were repeatedly measured. The standard deviation σ and the average value d were calculated to obtain the degree of dissociation deviation coefficient k=2σ / d. Calculate the degree of dissociation correction coefficient K = 1 / (1-k) based on the degree of dissociation deviation coefficient k. The corrected economic weighted oxidation rate of ore, W' = K × W, is calculated based on the degree of liberation correction factor.
[0040] In this embodiment, the target mineral with the highest weighted value is selected as the key target mineral, so that subsequent liberation degree correction focuses on the target mineral with the greatest impact on the overall economic evaluation. Liberation degree parameters are repeatedly measured from different perspectives to reduce random bias in liberation degree measurement. The liberation degree correction coefficient K is used to correct W, achieving deviation correction for the economically weighted oxidation rate, making W' more representative of the overall oxidation degree of the ore, reducing errors caused by single perspective or local measurement, and improving the representativeness and reliability of the evaluation results.
[0041] In some embodiments, the step of calculating the economic weighted value of each target mineral and selecting the target mineral with the highest weighted value as the key target mineral includes: Obtain the mass fraction of sulfide minerals containing each target element in the sample to be tested, the mass fraction of the target element in the sulfide, and the market unit price of each target element; The economic contribution of a target mineral is calculated as the product of the mass fraction of sulfide minerals containing each target element, the mass fraction of the target element in the sulfide minerals, and the market price of the target element. The sulfide minerals that contribute the most to economic growth were identified as the key target minerals in the samples to be tested.
[0042] In this embodiment, calculating the economic weighted value of the target mineral requires a combination of the unit price of the target element and the content of the target element in the ore sample. By comparing the economic contribution of each target element in the sulfide, the economic value of the target mineral can be objectively screened, and the target mineral with the highest economic value can be identified as the key target mineral. This ensures the representativeness of the key target mineral and improves the economic guidance of the determination of oxidation rate of polymetallic ores.
[0043] In some embodiments, the degree of dissociation parameter is measured at least 10 times.
[0044] In this embodiment, the number of repeated measurements of the dissociation parameter is controlled to be at least 10 times to reduce random errors and sampling randomness, improve the reliability of the dissociation correction coefficient, and at the same time take into account both measurement accuracy and measurement efficiency.
[0045] In some embodiments, the degree of dissociation parameter d i e .s.n This indicates the mass fraction of sulfide mineral inclusions and intergrowths in the target mineral within analytical mineral particles with a particle size ≤ 0.010 mm, relative to the total mass of the target mineral.
[0046] In this embodiment, the degree of dissociation parameter d i e .s.n This represents the proportion of particles in the nth-sized sample (within 0.010 mm diameter) that are either encapsulated or intergrowths, representing the eth metal sulfide target mineral corresponding to the i-th target element. Fine-grained samples are difficult to dissociate, and the influence of intergrowths and encapsulated particles is significant. Therefore, the evaluation of the degree of dissociation is highly targeted. For analytical samples of different sizes, the degree of dissociation parameter obtained from the smallest grain size is used for calculation.
[0047] In some embodiments, the grinding particle size is ≤0.074 mm.
[0048] In this embodiment, the sample to be tested is ground to a particle size of 0.074 mm to pass through completely. Grinding to this particle size can improve the separation degree between the target metal sulfide mineral and gangue, improve the identification efficiency of encapsulated particles and intergrowth particles, and reduce the interference of coarse, undissociated particles.
[0049] In some embodiments, the particle size range of the ore sample includes at least two of the following four particle size ranges: Greater than 0.037 mm; Less than or equal to 0.037 mm and greater than 0.010 mm; Less than or equal to 0.010 mm and greater than 0.005 mm; Less than or equal to 0.005 mm.
[0050] In this embodiment, the sample to be tested is ground and then sieved into at least two particle sizes in order to distinguish the dissociation characteristics of different particle sizes, reduce the interference between mixed coarse and fine particles in the identification of intergrowths and inclusions, and improve the accuracy of the measurement results.
[0051] In some embodiments, the steps of selecting ore samples of various particle sizes and performing initial embedding, vertical cutting, and secondary embedding processes to obtain automated mineralogical analysis samples include: After mixing the analytical sample with graphite powder, epoxy resin was used for initial embedding and curing. The initial embedded body was cut vertically to obtain a slice containing the cross section of the analytical sample; The slices were then embedded and cured with their cut surfaces facing down. The embedded body obtained by secondary embedding and solidification is ground and polished to expose the cutting surface and form a polished surface. After carbon spraying, an automated mineralogical analysis sample is obtained.
[0052] In this embodiment, samples were taken from each particle size obtained by sieving. The samples were mixed with graphite powder with a particle size less than 0.037 mm at a volume ratio of 1:(2~5), and dispersed by shaking in at least 1.5 times the volume of anhydrous ethanol for at least 10 min. After air drying and removal of free water, the samples were crushed until the particles were fully dispersed to obtain a dry sample. Epoxy resin and curing agent were mixed at a volume ratio of 1:(0.2~0.8) to prepare an epoxy resin curing solution. The dry sample and epoxy resin curing solution were then mixed in a mold at a solid-liquid ratio of 1:(2~3), ultrasonically vibrated for 15~20 min, and cured at room temperature for 10~12 h. The primary embedded body was then demolded. The primary embedded body was cut vertically along its center position, and then placed with the cut surface facing down in the mold. Epoxy resin curing solution was injected again until the curing liquid level reached 1.0~1.3 cm. The mold was heated to 45~60℃ until cured, and the secondary embedded body was demolded. The lower surface of the secondary embedded body was subjected to coarse grinding, fine grinding, high-precision grinding, and polishing in sequence to obtain a smooth and clean analytical surface. After coarse grinding, the sample surface morphology was observed under an optical microscope, with a particle exposure rate of no less than 90%. Fine grinding and high-precision grinding were performed sequentially using 200-grit, 500-grit, 1000-grit, and 2000-grit silicon carbide sandpaper to reduce interference from the encapsulation on oxidation rate determination. Polishing was performed using 0.5–1.0 μm diamond polishing agent until the sample surface was smooth and free of scratches. Subsequently, a 10–30 nm thick carbon layer was sprayed onto the polished sample surface to improve conductivity, thus obtaining the sample for automated mineralogical analysis.
[0053] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0054] Example 1 S1. Take 200g of the sample to be tested, grind it to a particle size ≤0.045mm, sieve all the sample to be tested into 3 particle sizes, dry them at 105℃ for 2h to constant weight, and weigh the mass A of each particle size sample. n Calculate the yield a of each particle size sample. n =A n / ΣA n The mass and yield of each particle size sample are shown in Table 1. Table 1. Mass and Yield of Each Particle Size S2. 1.5g of each particle size of ore sample was selected and mixed with graphite (0.02mm particle size) at a volume ratio of 1:3. The mixture was then shaken in twice the volume of anhydrous ethanol for 15 minutes, air-dried, and rolled until the particles were uniformly dispersed to obtain the dried sample. Epoxy resin and curing agent were mixed at a volume ratio of 1:0.5 to prepare an epoxy resin curing solution. The dried sample and epoxy resin curing solution were mixed in a mold at a solid-liquid ratio of 1:2, ultrasonically vibrated for 15 minutes, and cured at room temperature for 10 hours before demolding. The resulting primary inclusions were vertically cut along the center position and placed in the mold with the cut surface facing down. Epoxy resin curing solution was poured in again until the liquid level reached 1.2cm. The mold was then heated to 55℃ for curing and demolded. The resulting secondary inclusions were successively ground using 200-grit, 500-grit, 1000-grit, and 2000-grit silicon carbide sandpaper, and finally polished with 0.5μm diamond polishing agent until the surface was smooth and free of scratches. A 15nm thick layer of carbon was sprayed onto the polished sample using a multi-functional coating instrument to obtain analytical sample B. n ; S3, for analyzing sample B n Automated mineralogical analysis was performed. The results showed that the copper mineral particles mainly contain chalcopyrite and chalcocite as sulfides, and malachite as an oxide. The molybdenum mineral particles mainly contain molybdenite as a sulfide, and tungsten-molybdenite as an oxide. Figures 1-3 The images show scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS) analyses of copper mineral grains. Figure 2 Showing chalcocite (red) surrounding chalcopyrite (light green); Figures 4-6 The image shows scanning electron microscopy and energy dispersive spectroscopy (EDS) analysis of molybdenum mineral grains. Figure 5The sample shows molybdenite (pink) intergrowth with tungsten-molybdenite (light green). The type of target mineral and its mass fraction (b) in the analytical sample were determined. i e .n Mass fraction c of the target element in the target mineral i e .n and dissociation parameter d i e .s.n The results of the automated mineralogical analysis are shown in Tables 2 and 3. Table 2 Results of Automatic Mineralogical Analysis of Copper Minerals Table 3 Results of Automated Mineralogical Analysis of Molybdenum Minerals S4. Based on the results of automated mineralogical analysis, calculate the mass fraction of the target element in oxidized minerals, the mass fraction of the target element in specific intergrowths and inclusions of sulfide minerals, and the total mass fraction of the target element in the analyzed sample to obtain the effective oxidation rate W of the target element. i ; Calculate the mass fraction of the target element in oxidized minerals, and the mass fraction M of the target element in specific intergrowths and inclusions of sulfide minerals. i.1 =Σa n ×b i e .x.n ×c i e .x.n +Σa n ×b i e .s.n ×c i e .s.n ×d i e .s.n ; Calculate the total mass fraction M of the target element in each particle size. i.2 =Σa n ×b i e .n ×c i e .n ; Calculate the effective oxidation rate W of the target element i =M i.1 / M i.2 The calculation results are shown in Table 4. Table 4 Calculation Results of Copper Minerals Effective oxidation rate W of copper minerals i =M i.1 / M i.2 =0.20153043 ÷ 0.591535714 = 34.07% Table 5 Calculation Results for Molybdenum Minerals Effective oxidation rate W of molybdenum minerals i =M i.1 / M i.2 =0.044233181÷0.237773405=18.60% S5. Based on the effective oxidation rate of the target element and combined with the market price of the target element as a value weighting factor, the economic weighted oxidation rate W of the ore is obtained. According to the information obtained, the international market prices (converted to RMB) on August 28, 2026 were: RMB 109,600 / ton for copper (purity > 99.50%) and RMB 615,000 / ton for molybdenum (purity > 99.50%).
[0055] W=Σ(W i ×M i.2 ×Q i ) / Σ(M i.2 ×Q i = (34.07% × 0.591535714 × 10.96 + 18.60% × 0.237773405 × 61.50) ÷ (0.591535714 × 10.96 + 0.237773405 × 61.50) = 23.35% S6, based on the liberation degree parameter d of the target mineral. i e .s.n Calculate the degree of dissociation correction factor K to obtain the corrected economic weighted oxidation rate of ore W'. The mass fraction of copper in chalcopyrite = Σa n ×b i e .s.n ×c i e .s.n =(18.78%×0.58%×34.52%+59.16%×0.49%×34.52%+22.06%×0.67%×34.52%)=0.1887%, The mass fraction of copper in chalcocite = Σa n ×b ie .s.n ×c i e .s.n =(18.78%×0.23%×79.84%+59.16%×0.27%×79.84%+22.06%×0.34%×79.84%)=0.2219%, Mass fraction of molybdenum in molybdenite = Σa n ×b i e .s.n ×c i e .s.n =(18.78%×0.31%×58.26%+59.16%×0.35%×58.26%+22.06%×0.40%×58.26%)=0.2060%; Based on the combined international market prices of copper and molybdenum, the economic contribution of chalcopyrite is 0.1887 × 10.96 = 20,700 yuan / ton, that of chalcocite is 0.2219 × 10.96 = 24,300 yuan / ton, and that of molybdenite is 0.2060 × 61.50 = 126,700 yuan / ton. Molybdenite was selected as the key target mineral for calculating the degree of liberation correction coefficient. Analysis yielded the following 10 sets of data for the degree of liberation parameters of molybdenite: 6.04%, 6.12%, 6.10%, 5.95%, 5.90%, 5.81%, 6.08%, 6.24%, 6.04%, 6.02%; The mean was calculated to be d = 6.03%, and the standard deviation was σ = 0.1147%. The dissociation deviation coefficient k is calculated as k = 2σ / d = 2 × 0.1147% ÷ 6.03% = 0.03084; The dissociation correction factor K is calculated as follows: K = 1 / (1-k) = 1 ÷ (1-0.03084) = 1.03182; The corrected economic weighted oxidation rate of the ore is calculated as W' = K × W = 23.35% × 1.03182 = 24.09%.
[0056] Flotation verification: a closed-circuit mixed flotation process of "rough grinding - rough concentrate regrinding - one roughing, two cleaning, and three scavenging - middlings mixed and returned to roughing". The ore was ground to a particle size of -0.074 mm (75%), the pulp pH was adjusted to 10, and 150 g / t of water glass was added as a gangue dispersion inhibitor. A combination of 20 g / t MCO and 60 g / t kerosene was used as a collector, and 50 g / t MIBC was used as a frother for copper-molybdenum mixed roughing. The resulting rough concentrate was directly refmilled to a particle size of -0.038 mm (90%) to enhance the liberation of copper-molybdenum intergrowths. After two stages of cleaning and three stages of scavenging, the middlings were combined and returned to the roughing stage to form a closed circuit. Finally, a copper-molybdenum mixed concentrate was obtained with a total copper recovery of 65.51% and a total molybdenum recovery of 81.56%. Considering the overall copper and molybdenum value, the total recovery rate was approximately 75.25%, which is in good agreement with the measured value of 24.09% based on the corrected economic weighted oxidation rate of the ore, indicating that the oxidation rate measured by this method accurately reflects the actual flotation behavior of the ore. This method is simple to operate and quick, with the entire process completed within 12 hours.
[0057] Comparative Example 1 The same ore sample as that in Example 1 was selected, and the oxidation rate of the ore was determined using chemical methods. The specific steps are as follows: Following the methods described in the papers "Application of Inductively Coupled Plasma Atomic Emission Spectrometry in Copper Phase Analysis of Copper Ore" and "Research on Tungsten Phase Analysis and Detection in Tungsten Polymetallic Ore," the oxidation rates of individual elements in ore samples from the same source as in Example 1 were determined. The copper oxidation rate was 31.54%, and the molybdenum oxidation rate was 14.25%, both lower than the oxidation rates obtained by the method in this application. This is because fine-grained inclusions exist in the ore, and some sulfide minerals are not dissociated, leading to cross-contamination during chemical leaching, resulting in the leaching of some oxidized minerals and causing systematic bias. Based on the copper oxidation rate, leaching should be the primary process, and based on the molybdenum oxidation rate, a full-process flotation process should be used. If the separation process is determined separately based on the chemical oxidation rates of copper and molybdenum, contradictory process directions will be obtained, indicating that single-element chemical phase analysis is poorly adapted to this polymetallic ore, potentially leading to further loss of valuable metals and increased costs. Comparative Example 1 used a single-element determination method, which is time-consuming, with the entire determination process taking approximately 3 days.
[0058] In summary, the determination method of this invention has been verified by both mineral processing tests and economic benefit analysis, proving that its accuracy, practicality and convenience are significantly better than traditional methods, and can provide a reliable basis for the design of beneficiation and metallurgical processes and economic evaluation of polymetallic ores.
[0059] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing embodiments by combining some of the constituent elements, are also included in the scope of this application without departing from the spirit of this application.
[0060] Furthermore, although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A method for determining the oxidation rate of polymetallic ores, characterized in that, include: S1, the sample to be tested is ground and sieved to obtain ore samples of various particle sizes, with a mass of A. n The yield is a n ; S2, Select the ore samples of each particle size, and after initial embedding, vertical cutting, and secondary embedding, obtain sample B for automated mineralogical analysis. n ; S3, for the analytical sample B n Perform automated mineralogical analysis to determine the type of target mineral and its mass fraction (b) in the analyzed sample. i e .n The mass fraction c of the target element in the target mineral i e .n and dissociation parameter d i e .s.n ; S4. Based on the results of automated mineralogical analysis, calculate the mass fraction of the target element in oxidized minerals, the mass fraction of the target element in specific intergrowths and inclusions of sulfide minerals, and the total mass fraction of the target element in the analyzed sample to obtain the effective oxidation rate W of the target element. i ; S5. Based on the effective oxidation rate of the target element, and combined with the market price of the target element as a value weighting factor, the economic weighted oxidation rate W of the ore is obtained. S6, based on the degree of liberation parameter d of the target mineral. i e .s.n Calculate the degree of liberation correction factor K to obtain the corrected economic weighted oxidation rate W' of the ore; where, n represents the particle size, and n can be 1 to m, where 2 ≤ m ≤ 4; i represents the type of target element, and e represents the type of target mineral; s represents sulfide minerals in the target mineral.
2. The method for determining the oxidation rate of polymetallic ores according to claim 1, characterized in that, The step of calculating the effective oxidation rate of the target element based on the results of automated mineralogical analysis, including calculating the mass fraction of the target element in oxidized minerals, the mass fraction of the target element in specific intergrowths and inclusions of sulfide minerals, and the total mass fraction of the target element in the analyzed sample, comprises: Calculate the mass fraction of the target element in oxidized minerals, and the mass fraction M of the target element in specific intergrowths and inclusions of sulfide minerals. i.1 =Σa n ×b i e .x.n ×c i e .x.n +Σa n ×b i e .s.n ×c i e .s.n ×d i e .s.n ; Calculate the total mass fraction M of the target element in each particle size. i.2 =Σa n ×b i e .n ×c i e .n ; Calculate the effective oxidation rate W of the target element i =M i.1 / M i.2 ;in, x represents an oxidized mineral in the target mineral.
3. The method for determining the oxidation rate of polymetallic ores according to claim 1, characterized in that, The step of obtaining the economically weighted oxidation rate of the ore based on the effective oxidation rate of the target element and using the market price of the target element as a value weighting factor includes: Introducing the market price Q of the target element i Calculate the economically weighted oxidation rate of the ore W = Σ(W i ×M i.2 ×Q i ) / Σ(M i.2 ×Q i ).
4. The method for determining the oxidation rate of polymetallic ores according to claim 1, characterized in that, The step of calculating the liberation degree correction coefficient based on the liberation degree parameter of the target mineral to obtain the corrected economic weighted oxidation rate of the ore includes: Calculate the economic weighted value of each target mineral, and select the target mineral with the highest weighted value as the key target mineral; Different fields of view of the analytical samples of the key target minerals were selected, and the degree of dissociation parameters were repeatedly measured. The standard deviation σ and the average value d were calculated to obtain the degree of dissociation deviation coefficient k = 2σ / d. Calculate the degree of dissociation correction coefficient K = 1 / (1-k) based on the degree of dissociation deviation coefficient k. The corrected economic weighted oxidation rate of the ore, W' = K × W, is calculated based on the dissociation correction coefficient.
5. The method for determining the oxidation rate of polymetallic ores according to claim 4, characterized in that, The step of calculating the economic weighted value of each target mineral and selecting the target mineral with the highest weighted value as the key target mineral includes: Obtain the mass fraction of sulfide minerals containing each target element in the sample to be tested, the mass fraction of the target element in the sulfide, and the market unit price of each target element; The economic contribution of the target mineral is the product of the mass fraction of the sulfide mineral containing each target element, the mass fraction of the target element in the sulfide mineral, and the market price of the target element. The sulfide minerals that contribute the most to economic growth were identified as the key target minerals in the samples to be tested.
6. The method for determining the oxidation rate of polymetallic ores according to claim 4, characterized in that, The degree of dissociation parameter is measured at least 10 times.
7. The method for determining the oxidation rate of polymetallic ores according to claim 1, characterized in that, The degree of dissociation parameter d i e .s.n This represents the mass fraction of sulfide mineral inclusions and intergrowths within mineral particles with a diameter ≤ 0.010 mm in the nth particle size analysis sample, relative to the total mass of the target mineral.
8. The method for determining the oxidation rate of polymetallic ores according to claim 1, characterized in that, The particle size of the grinding process is ≤0.074mm.
9. The method for determining the oxidation rate of polymetallic ores according to claim 1, characterized in that, The particle size range of the ore sample includes at least two of the following four particle size ranges: Greater than 0.037 mm; Less than or equal to 0.037 mm and greater than 0.010 mm; Less than or equal to 0.010 mm and greater than 0.005 mm; Less than or equal to 0.005 mm.
10. The method for determining the oxidation rate of polymetallic ores according to claim 1, characterized in that, The steps of selecting ore samples of each particle size and performing initial embedding, vertical cutting, and secondary embedding to obtain automated mineralogical analysis samples include: After mixing the analytical sample with graphite powder, epoxy resin was used for initial embedding and curing. The initial embedded body was cut vertically to obtain a slice containing the cross section of the analytical sample; The slice is then embedded and cured with its cut surface facing down. The embedded body obtained by secondary embedding and solidification is ground and polished to expose the cutting surface and form a polished surface. After carbon spraying, an automated mineralogical analysis sample is obtained.